Structure and preparation method of back-incident near-infrared enhanced silicon avalanche photodetector
By adopting a back-incidence structure and a micron-scale silicon pillar design in the silicon-based avalanche photodetector, combined with a channel-type guard ring, the problem of low responsivity and noise in the near-infrared band is solved, and the effects of high responsivity and low noise are achieved.
Patent Information
- Application Number
- CN202110222821.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-02-26
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-02-26
AI Technical Summary
Existing silicon-based avalanche photodetectors have low optical responsivity to the near-infrared band, and the nanoscale process cost is high and it is difficult to accurately design the enhanced response at different wavelengths. The front-side incidence method requires a low n+ zone layer thickness to reduce noise, but Lateral diffusion and lattice damage will be introduced.
The structure of the back-incident near-infrared enhanced silicon avalanche photodetector is used, including the substrate, π-type layer, p-type layer, n+ layer, channel-type protection trench and silicon dioxide insulating layer. Micron-scale silicon pillars are etched by inductively coupled plasma. , design different silicon pillar diameters and spacing, and etch channel-type guard rings to regulate the edge electric field, reduce noise and enhance near-infrared band response.
A near-infrared band photodetector with high responsivity under low-precision technology has been achieved, reducing excess noise, adjusting quantum efficiency, and effectively suppressing edge breakdown through the channel protection ring, improving the three characteristics of the avalanche photodetector.
Smart Images

Figure CN114975672B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to photoelectric detection research and avalanche photoelectric detector structure, and in particular to a structure and a preparation method of a back-incident near-infrared enhanced silicon avalanche photoelectric detector. Background Art
[0002] With the continuous development of cutting-edge technologies such as autonomous driving, the performance requirements for devices at the detection receiving end, namely photodetectors, are becoming increasingly higher. At the same time, photodetectors are used in optical fiber communication systems, radar imaging systems, laser ranging systems, etc. Avalanche photodetectors, especially silicon-based avalanche photodetectors, stand out among a number of detectors due to their small size, high internal gain, and easy integration.
[0003] At present, the main incident modes of avalanche photodetectors are front incidence, back incidence and side incidence, among which front incidence requires n + The layer thickness of the region is low to minimize the excess noise of photogenerated holes introduced by the multiplication region. When using a guard ring to suppress edge breakdown, ion implantation can accurately control the depth of the guard ring, but it will cause lateral diffusion and damage the internal lattice; due to the light absorption coefficient of silicon materials, the light response to the near-infrared band is very low. Nanoimprinting and other technologies can be used to enhance infrared absorption, but the cost of introducing nano-microstructures is too high, and it is difficult to accurately design different wavelengths in the near-infrared to enhance the response. Summary of the invention
[0004] In view of this, the main purpose of the present invention is to provide a structure and a preparation method of a back-incident near-infrared enhanced silicon avalanche photodetector, in order to at least partially solve at least one of the above-mentioned technical problems.
[0005] To achieve the above object, as one aspect of the present invention, the present invention provides a structure of a back-incident near-infrared enhanced silicon avalanche photodetector, comprising:
[0006] substrate;
[0007] A π-type layer, disposed on the upper surface of the substrate, for absorbing incident light;
[0008] A p-type layer disposed on the π-type layer;
[0009] n + layer, disposed on the p-type layer, wherein the p-type layer and the n + The layers together form an avalanche zone;
[0010] A channel type protection groove runs through the p-type layer and is used to increase the breakdown voltage;
[0011] The trench-type protection groove divides the upper surface of the p-type layer into a middle circular portion and a peripheral circular portion; wherein n +The layer is located on the middle circular part of the p-type layer;
[0012] Silicon dioxide insulating layer, covering the n + The layer, the channel protection groove and the outer ring part of the p-type layer are used as a surface passivation layer;
[0013] The first electrode, covering n + The silicon dioxide insulating layer above the layer is used to form an ohmic contact anode;
[0014] The substrate hollowing region is arranged on the lower surface of the substrate to reduce the optical loss of the incident light outside the absorption region and reduce the transit time of the carriers;
[0015] A silicon pillar region is arranged at the bottom of the groove in the hollowed-out region of the substrate and is used to enhance the absorption of light in the near-infrared band;
[0016] The second electrode covers the bottom of the substrate and is located at the periphery of the hollowed-out region of the substrate, and is used to form an ohmic contact cathode.
[0017] As another aspect of the present invention, a method for preparing a back-incident near-infrared enhanced silicon avalanche photodetector is also disclosed, comprising:
[0018] Prepare a π-type layer on the upper surface of the substrate;
[0019] preparing a p-type layer on the π-type layer;
[0020] forming a silicon dioxide layer on the p-type layer;
[0021] Etching the silicon dioxide layer to form an ion implantation window;
[0022] Preparation of n in ion implantation window + layer;
[0023] Etch the p-type layer and part of the n + A layer is formed to form a channel type protection groove; the p-type layer is divided into a middle circular part and a peripheral circular ring part by the channel type protection groove;
[0024] In the p-type layer, the channel protection trench and the n + A silicon dioxide insulating layer is prepared on the layer;
[0025] In n + A first electrode is formed on the silicon dioxide insulating layer above the layer;
[0026] Etching a groove on the lower surface of the substrate to prepare a substrate hollowing area;
[0027] A second electrode is prepared on the lower surface of the substrate and is located at the periphery of the hollowed-out region of the substrate;
[0028] A silicon pillar region is prepared at the bottom of the groove in the hollowed-out region of the substrate to complete the preparation of the novel back-incident near-infrared enhanced silicon avalanche photodetector.
[0029] Based on the above technical solution, it can be seen that the structure and preparation method of the back-incident near-infrared enhanced silicon avalanche photodetector of the present invention have at least one of the following advantages over the prior art:
[0030] 1. The present invention adopts an inductively coupled plasma etching method to etch micron-sized silicon pillars, and no nano-scale process is used in the preparation process, so that the preparation method has lower precision requirements than the nano-scale process, higher process fault tolerance, lower preparation cost and better repeatability, while still maintaining enhanced response to the near-infrared band, making it possible to realize avalanche photodetectors with high responsiveness in the near-infrared band under low precision;
[0031] 2. The present invention can enhance the response of different wavelengths in the near-infrared band and adjust the quantum efficiency by designing different silicon column diameters and silicon column intervals and etching silicon column regions of different depths;
[0032] 3. The present invention can adjust the edge electric field distribution by etching a channel-type guard ring (Guard-Ring), that is, a channel-type protection groove, and effectively suppress the breakdown of the edge electric field of the active area. At the same time, by designing different etching depths, the breakdown characteristics of the device can be effectively adjusted, so that the low-precision process has the characteristics of channel-controlled electric field;
[0033] 4. The present invention adopts the back-incident method to improve the near-infrared band response while reducing excess noise. At the same time, through the precise design of the channel guard ring area, the edge electric field can be accurately controlled, thereby achieving the effect of simultaneously improving the three characteristics of the avalanche photodetector (i.e., suppressing edge breakdown, low noise, and near-infrared band response). BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 is a schematic cross-sectional structure diagram of a back-incident near-infrared enhanced silicon avalanche photodetector in an embodiment of the present invention;
[0035] Figure 2 1 is a schematic diagram of a top plan structure of a back-incident near-infrared enhanced silicon avalanche photodetector according to an embodiment of the present invention;
[0036] Figure 3 is a top-view planar structural diagram of a back-incident near-infrared enhanced silicon avalanche photodetector according to an embodiment of the present invention;
[0037] Figure 4 4 is a curve diagram showing the relationship between the channel protection groove depth and the breakdown voltage in an embodiment of the present invention.
[0038] Description of reference numerals:
[0039] 1- substrate;
[0040] 2- substrate hollowing area;
[0041] 3-Silicon column area;
[0042] 4-Trench type protection groove;
[0043] 5-π-type layer;
[0044] 6-p-type layer;
[0045] 7-n + layer;
[0046] 8-silicon dioxide insulating layer;
[0047] 9- a first electrode;
[0048] 10- Second electrode. DETAILED DESCRIPTION
[0049] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings.
[0050] The main purpose of the present invention is to provide a structure and preparation method of a back-incident near-infrared enhanced silicon avalanche photodetector, which aims to use a channel-etched guard ring to regulate the edge electric field distribution, and further etch out micron-scale silicon pillars after hollowing out the back substrate to a certain thickness, so that the detector has the characteristics of channel regulation of the electric field and back silicon pillar regulation of the near-infrared band response under low-precision process.
[0051] The present invention discloses a structure of a back-incident near-infrared enhanced silicon avalanche photodetector, comprising:
[0052] Substrate 1;
[0053] The π-type layer 5 is disposed on the upper surface of the substrate 1 and is used to absorb incident light;
[0054] A p-type layer 6, disposed on the π-type layer 5;
[0055] n + Layer 7 is disposed on the p-type layer 6, wherein the p-type layer 6 and the n + Layer 7 together forms the avalanche zone;
[0056] A channel type protection groove 4, penetrating the p-type layer 6, is used to increase the breakdown voltage;
[0057] The channel protection groove 4 divides the upper surface of the p-type layer 6 into a middle circular part and a peripheral circular ring part; wherein, n + Layer 7 is located on the middle circular portion of p-type layer 6;
[0058] The silicon dioxide insulating layer 8 covers the n + Layer 7, the channel protection groove 4 and the outer ring portion of the p-type layer 6 are used as a surface passivation layer;
[0059] The first electrode 9 covers n + On the silicon dioxide insulating layer 8 above the layer 7, for forming an ohmic contact anode;
[0060] The substrate hollowing region 2 is arranged on the lower surface of the substrate 1 and is used to reduce the optical loss of the incident light outside the absorption region and reduce the transit time of the carriers;
[0061] The silicon pillar region 3 is arranged at the bottom of the groove of the substrate hollowing region 2 and is used to enhance the absorption of near-infrared light;
[0062] The second electrode 10 covers the bottom of the substrate 1 and is located outside the substrate hollowing region 2 to form an ohmic contact cathode.
[0063] In some embodiments of the present invention, the thickness of the substrate 1 is 70 to 150 μm.
[0064] In some embodiments of the present invention, the depth of the substrate hollowing region 2 is 30 to 60 μm, for example, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, or 60 μm;
[0065] In some embodiments of the present invention, the substrate hollowed-out region 2 is in the shape of a cylindrical groove.
[0066] In some embodiments of the present invention, the silicon column region 3 includes at least 2 silicon columns;
[0067] In some embodiments of the present invention, the shape of the silicon pillar comprises a cylinder;
[0068] In some embodiments of the present invention, the height of the silicon pillar is 8 to 15 μm, for example, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm;
[0069] In some embodiments of the present invention, the interval period of the silicon pillars is 5 to 10 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm;
[0070] In some embodiments of the present invention, when the silicon column is in the shape of a cylinder, the bottom diameter of the silicon column is 3 to 8 μm, for example, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, or 8 μm.
[0071] In some embodiments of the present invention, the thickness of the π-type layer 5 is 30 to 70 μm;
[0072] In some embodiments of the present invention, the doping concentration of the π-type layer 5 is 1×10 14 Up to 5×10 14 cm -3 .
[0073] In some embodiments of the present invention, the thickness of the p-type layer 6 is 4 to 10 μm, for example, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, or 10 μm;
[0074] In some embodiments of the present invention, the doping concentration of the p-type layer 6 is 1×10 15 cm -3 Up to 3×10 15 cm -3 ;
[0075] In some embodiments of the present invention, the n + The thickness of the layer 7 is 0.1 to 0.5 μm, for example, 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, or 0.5 μm.
[0076] In some embodiments of the present invention, the shape of the channel-type protection groove 4 includes an annular groove;
[0077] In some embodiments of the present invention, the width of the channel type protection groove 4 is 1 to 6 μm, for example, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm;
[0078] In some embodiments of the present invention, the depth of the channel protection groove 4 is greater than the thickness of the p-type layer 6 and less than the sum of the thickness of the p-type layer 6 and the thickness of the π-type layer 5 .
[0079] In some embodiments of the present invention, the material used for the first electrode 9 includes aluminum, gold, titanium-gold or titanium-platinum-gold alloy;
[0080] In some embodiments of the present invention, the thickness of the first electrode 9 is 300 to 600 nm.
[0081] In some embodiments of the present invention, the material used for the second electrode 10 includes aluminum, gold, titanium-gold or titanium-platinum-gold alloy;
[0082] In some embodiments of the present invention, the thickness of the second electrode 10 is 300 to 600 nm.
[0083] The present invention also discloses a method for preparing a back-incident near-infrared enhanced silicon avalanche photodetector, comprising:
[0084] Prepare a π-type layer 5 on the upper surface of the substrate 1;
[0085] Preparing a p-type layer 6 on the π-type layer 5;
[0086] preparing a silicon dioxide layer on the p-type layer 6;
[0087] Etching the silicon dioxide layer to form an ion implantation window;
[0088] Preparation of n in ion implantation window + Layer 7;
[0089] Etch the p-type layer 6 and part of the n + Layer 7, forming a channel type protection groove 4; the p-type layer 6 is divided into a middle circular part and a peripheral circular ring part by the channel type protection groove 4;
[0090] In the p-type layer 6, the channel type protection groove 4 and the n + A silicon dioxide insulating layer 8 is prepared on the layer 7;
[0091] In n + A first electrode 9 is formed on the silicon dioxide insulating layer 8 above the layer 7;
[0092] Etching a groove on the lower surface of the substrate 1 to prepare a substrate hollowing region 2;
[0093] A second electrode 10 is formed on the lower surface of the substrate 1 and is located outside the hollowed-out region 2 of the substrate;
[0094] A silicon column region 3 is prepared at the bottom of the groove of the substrate hollowed-out region 2 to complete the preparation of the novel back-incident near-infrared enhanced silicon avalanche photodetector.
[0095] In some embodiments of the present invention, when preparing the channel type protection groove 4, the n + The width of the layer 7 is 2 to 4 μm.
[0096] In order to further understand the content, characteristics and beneficial effects of the technical solution of the present invention, the following is further described by several preferred embodiments. Among them, the materials used in the following embodiments are all commercially available, or prepared by methods reported in the literature. It should be noted that the following embodiments are only used to illustrate the present invention, rather than to limit the present invention.
[0097] In one embodiment of the present invention, a novel back-incident near-infrared enhanced silicon avalanche photodetector is disclosed, such as Figure 1 , Figure 2 and Figure 3 As shown, including: thinned p + type substrate (i.e., substrate 1), a region hollowed out to a certain depth (i.e., substrate hollowed-out region 2), an epitaxial π-type layer (i.e., π-type layer 5) located above the substrate 1, an epitaxial p-type layer 6 located above the π-type layer 5, and an n-type layer adjacent to the p-type layer 6. + Layer 7, located at n+ The channel-type protection grooves 4 on both sides of the layer 7, the middle micron-sized silicon column region (i.e., silicon column region 3) located directly below the light absorbing π-type layer (i.e., π-type layer 5), and the lower electrode (i.e., the second electrode 10) below the substrate 1 and the n + The upper electrode 9 (ie, the first electrode 9) is above the layer 7.
[0098] The substrate hollowing region 2 has a depth of 30-60 μm, so as to leave etching space for the next step of silicon column etching.
[0099] The thinned p + The substrate type (i.e., substrate 1) is p + The type is highly doped to form an ohmic contact with the lower electrode (i.e., the second electrode 10), and the specific doping concentration is 1×10 19 cm -3 ~1×10 21 cm -3 .
[0100] The middle silicon column region (ie silicon column region 3) etched on the back is obtained by inductively coupled plasma etching, and the silicon column has a diameter of 3 to 8 μm, a height of 8 to 15 μm, and a silicon column interval of 5 to 10 μm, which is evenly spaced.
[0101] The π-type layer 5 is a thinned p + The substrate (i.e., substrate 1) is obtained by epitaxial growth, with a thickness of 30 to 70 μm and a doping concentration of 1×10 14 cm -3 ~5×10 14 cm -3 .
[0102] The p-type layer 6 is obtained by epitaxial growth on the π-type layer 5, and has a thickness of 4 to 10 μm and a doping concentration of 1×10 15 cm -3 ~3×10 15 cm -3 .
[0103] The + Layer 7 is obtained after phosphorus ions are implanted twice into the p-type layer 6. The first phosphorus ion implantation dose is 3×10 15 cm -3 ~5×10 14 cm -3 The implantation energy is 50keV~200keV, the annealing temperature is 850℃~1050℃, and the annealing time is 50~80s; the second phosphorus ion implantation dose is 1×10 14 cm -3 ~5×10 15 cm -3The implantation energy is 30keV~60keV, the annealing temperature is 850℃~950℃, and the annealing time is 50s~80s.
[0104] The trench protection groove 4 is obtained by inductively coupled plasma etching and is located at the aforementioned n + Layer 7 on both sides but the etched area is the same as the aforementioned n + The layer 7 partially overlaps, the width of the channel protection grooves 4 on both sides is 2-6 μm, the etching depth is 0-6 μm, and the avalanche region is never etched (that is, the etching depth is less than the sum of the thickness of the p-type layer 6 and the π-type layer 5), and the n + The width of the overlapping portion of layer 7 is 2 to 4 μm.
[0105] The first electrode 9 and the second electrode 10 are metal film electrodes with a thickness of 300-600 nm. The metal material may be aluminum Al, gold Au, titanium-gold alloy Ti / Au or titanium-platinum-gold alloy Ti / Pt / Au.
[0106] When the device is working, the light radiation or various reflected lasers excited by the detected material are absorbed by the photosensitive surface (including the silicon column area 3) and the π-type layer 5 of the new back-incident near-infrared enhanced silicon avalanche photodetector, generating photogenerated carriers, among which the photogenerated electrons drift to the avalanche region, i.e., the p-type layer 6 and the n-type layer 5. + Multiplication occurs in the interface region of layer 7, and the original photogenerated charge and the avalanche multiplied charge continue to drift toward the electrodes at both ends, thereby generating photocurrent.
[0107] The method for preparing the novel back-incident near-infrared enhanced silicon avalanche photodetector comprises the following steps:
[0108] Step 1: Prepare a clean and dry p-type highly doped silicon single crystal wafer substrate material (i.e., substrate 1) with a crystal orientation of (111);
[0109] Step 2: Grow a π-type layer 5 on a silicon single crystal wafer (i.e., substrate 1) by vapor phase epitaxy, with a doping concentration of 1×10 14 cm -3 ~5×10 14 cm -3 , with a thickness of 30 to 70 μm, used to absorb incident light;
[0110] Step 3: On the π-type layer 5 obtained by the above-mentioned vapor phase epitaxial growth, a p-type layer 6 is further vapor phase epitaxially grown with a doping concentration of 1×10 15 cm -3 ~3×10 15 cm -3 , with a thickness of 4 to 10 μm; wherein the p-type layer (6) and the n+ layer (7) together form an avalanche region;
[0111] At this point, the epitaxial growth of the epitaxial wafers used for subsequent tape-out has been completed.
[0112] Step 4: Grow a layer of silicon dioxide on the silicon epitaxial wafer by magnetron sputtering or PECVD, with a thickness of about 0.2 to 0.5 μm;
[0113] Step 5: Spin-coat a layer of photoresist on the surface of the SiO2 film layer, and pattern the photoresist using a mask pattern, and photolithograph the ion implantation area of the SiO2 film layer to be etched silicon dioxide;
[0114] Step 6: Etching the patterned area with silicon dioxide to remove the unprotected SiO2 film layer to form a phosphorus ion implantation window;
[0115] Step 7: Remove the remaining photoresist in step 5 and use the silicon dioxide mask layer in step 6 to perform phosphorus ion implantation with an implantation dose of 3×10 15 cm -3 ~5×10 16 cm -3 , the injection energy is 50keV~200keV;
[0116] Step 8: Perform rapid thermal annealing in an annealing furnace, the annealing temperature is 850° C. to 1050° C., and the annealing time is 50 to 80 seconds;
[0117] Step 9: Use the silicon dioxide mask layer in step 6 again to perform phosphorus ion implantation with an implantation dose of 1×10 14 cm -3 ~5×10 15 cm -3 , the injection energy is 30keV~60keV;
[0118] Step 10: Annealing is performed again, this time using rapid thermal annealing, the annealing temperature is 850°C to 950°C, and the annealing time is 50s to 80s;
[0119] Steps 7 to 10 work together to form n + Layer 7, the junction depth formed with the p-type layer 6 is 0.1 to 0.5 μm;
[0120] Among them, to increase n + The surface doping concentration of layer 7 is 1.5, and it forms an ohmic contact with the electrode. Three ion implantations are used to form n + Layer 7;
[0121] Step 11: Spin-coat a layer of photoresist on the front side of the silicon epitaxial wafer (the thickness of the photoresist must be greater than 1 μm), pattern the photoresist again using the mask pattern, and photolithograph a channel-type protection groove area to be etched;
[0122] Step 12: Using the remaining photoresist from step 11 as a mask, etching out the protection ring trenches on both sides (i.e., the trench protection grooves 4) to increase the breakdown voltage; the width of the trench protection grooves 4 on both sides is 2 to 6 μm, and the etching depth is 0 to 6 μm (from the unetched to the etched avalanche region), which is consistent with n + The width of the overlapping portion of layer 7 is 2 to 4 μm.
[0123] Step 13: depositing a layer of silicon dioxide with a thickness of 100 to 500 nm on the front side of the silicon epitaxial wafer by PECVD to form a silicon dioxide insulating layer 8;
[0124] Step 14: remove all the photoresist remaining in the previous steps, and continue to deposit a metal film layer (Ti / Au) on the front side of the epitaxial wafer, and etch out a metal electrode pattern to form an upper electrode (ie, the first electrode 9).
[0125] At this point, the process processing of the front side of the device is completed.
[0126] Step 15: Grinding and polishing the silicon epitaxial wafer substrate (i.e., substrate 1) to a thickness of 100 to 150 μm;
[0127] Step 16: Spin-coat a layer of photoresist on the silicon epitaxial wafer substrate (i.e., substrate 1), and pattern the photoresist using a mask pattern, and photoetch out a substrate hollowing area to be etched on the photoresist;
[0128] Step 17: Using the remaining photoresist in step 16 as a mask, perform back silicon etching with an etching depth of 30 to 60 μm to form a substrate hollowing region 2;
[0129] Step 18: remove the photoresist produced previously, deposit a metal film layer (Ti / Au) on the back of the silicon epitaxial wafer, etch out a metal electrode pattern, and form a lower electrode (i.e., the second electrode 10);
[0130] Step 19: Spin-coat a layer of photoresist (thickness of about 1 μm) on the silicon epitaxial wafer substrate again, and pattern the photoresist using a mask pattern, and photoetch out a silicon column pattern area on the photoresist to be etched;
[0131] Step 20: using the photoresist patterned in step 23 as a mask, etching the silicon in the unprotected area to a depth of 8 to 15 μm to form a silicon column region 3;
[0132] Step 21: Remove all the remaining photoresists from the previous steps to complete the design and preparation of the back-incident near-infrared enhanced silicon avalanche photodetector.
[0133] like Figure 4As shown in the figure, with the increase of the etching depth of the channel protection groove 4, the breakdown voltage of the back-incident near-infrared enhanced silicon avalanche photodetector shows an overall upward trend. When the depth of the channel protection groove 4 is 0, the breakdown voltage of the back-incident near-infrared enhanced silicon avalanche photodetector is 72V; and when the depth of the channel protection groove 4 is 3μm, the breakdown voltage of the back-incident near-infrared enhanced silicon avalanche photodetector is 87V, and the breakdown voltage increases by 20.8%. Therefore, by etching the channel protection groove 4, the device breakdown voltage can be effectively improved, and the device breakdown characteristics can be suppressed, so that the back-incident near-infrared enhanced silicon avalanche photodetector has the characteristics of channel regulation electric field under low-precision process.
[0134] The novel micron-scale silicon pillar back-incident near-infrared enhanced silicon avalanche photodetector prepared in this embodiment improves the response in the near-infrared band while reducing excess noise. At the same time, through the precise design of the channel guard ring area, the edge electric field can be accurately controlled, achieving the effect of simultaneously improving the three characteristics of the avalanche photodetector (suppressing edge breakdown, low noise, and near-infrared band response).
[0135] Another embodiment of the present invention provides a method for preparing a novel back-incident near-infrared enhanced silicon avalanche photodetector, comprising the following steps:
[0136] Step 1: Prepare a clean and dry p-type highly doped silicon single crystal wafer substrate material (i.e., substrate 1) with a crystal orientation of (111);
[0137] Step 2: Grow a π-type layer 5 on a silicon single crystal wafer (i.e., substrate 1) by vapor phase epitaxy with a doping concentration of 5×10 14 cm -3 , thickness is 50μm;
[0138] Step 3: On the π-type layer 5 obtained by the above-mentioned vapor phase epitaxial growth, a p-type layer 6 is further vapor phase epitaxially grown with a doping concentration of 3×10 15 cm -3 , thickness is 7μm;
[0139] At this point, the epitaxial growth of the epitaxial wafers used for subsequent tape-out has been completed.
[0140] Step 4: grow a layer of silicon dioxide with a thickness of 0.5 μm on the silicon epitaxial wafer by magnetron sputtering;
[0141] Step 5: Spin-coat a layer of photoresist on the surface of the SiO2 film layer, and pattern the photoresist using a mask pattern, and photolithograph the ion implantation area of the SiO2 film layer to be etched silicon dioxide;
[0142] Step 6: Etching the patterned area with silicon dioxide to remove the unprotected SiO2 film layer to form a phosphorus ion implantation window;
[0143] Step 7: Remove the remaining photoresist in step 5 and use the silicon dioxide mask layer in step 6 to perform phosphorus ion implantation with an implantation dose of 3×10 15 cm -3 , the injection energy is 150keV;
[0144] Step 8: Perform rapid thermal annealing in an annealing furnace, the annealing temperature is 1000°C, and the annealing advancement time is 80s;
[0145] Step 9: Use the silicon dioxide mask layer in step 6 again to perform phosphorus ion implantation with an implantation dose of 3×10 14 cm -3 , the injection energy is 30keV;
[0146] Step 10: Rapid thermal annealing is performed again, the annealing temperature is 850°C, and the annealing time is 50s;
[0147] Steps 7 to 10 work together to form n + The junction depth formed by layer 7 and p-type layer 6 is 0.5 μm.
[0148] Step 11: Spin-coat a layer of photoresist on the front of the silicon epitaxial wafer (the thickness of the photoresist should be guaranteed to be
[0149] The photoresist is patterned again using the mask pattern to photolithography a channel-type protection groove area to be etched;
[0150] Step 12: Using the remaining photoresist from step 11 as a mask, etching out the protection ring trenches on both sides (i.e., the trench protection trenches 4). The width of the obtained trench protection trenches 4 on both sides is 5 μm, and the etching depth is 0 to 6 μm (from unetched to etched avalanche region), which is the same as n + The width of the overlapping portion of layer 7 is 2 to 4 μm;
[0151] Step 13: depositing a layer of silicon dioxide with a thickness of 100 to 500 nm on the front side of the silicon epitaxial wafer by PECVD to form a silicon dioxide insulating layer 8;
[0152] Step 14: remove all the photoresists remaining in the previous steps, and continue to deposit a metal film layer (Ti / Au) on the front side of the epitaxial wafer, and etch out a metal electrode pattern to form a first electrode 9.
[0153] At this point, the process processing of the front side of the device is completed.
[0154] Step 15: Grinding and polishing the silicon epitaxial wafer substrate (i.e., substrate 1) to a thickness of 120 μm;
[0155] Step 16: Spin-coat a layer of photoresist on the silicon epitaxial wafer substrate (i.e., substrate 1), and pattern the photoresist using a mask pattern, and photoetch out a substrate hollowing area to be etched on the photoresist;
[0156] Step 17: Using the remaining photoresist in step 16 as a mask, perform back silicon etching with an etching depth of 40 μm to form a substrate hollowing region 2;
[0157] Step 18: remove the photoresist produced previously, deposit a metal film layer (Ti / Au) on the back of the silicon epitaxial wafer, and etch out a metal electrode pattern to form a second electrode 10.
[0158] Step 23: Spin-coat a layer of photoresist (thickness of about 1 μm) on the silicon epitaxial wafer substrate again, and pattern the photoresist using a mask pattern, and photoetch out a silicon column pattern area on the photoresist to be etched;
[0159] Step 24: using the photoresist patterned in step 23 as a mask, etching the silicon in the unprotected area to a depth of 10 μm to form a silicon column region 3;
[0160] Step 25: Remove all the remaining photoresists from the previous steps to complete the design and preparation of the back-incident near-infrared enhanced silicon avalanche photodetector.
[0161] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A structure of a back-incident near-infrared enhanced silicon avalanche photodetector, characterized in that: include: Substrate (1); A π-type layer (5) is arranged on the upper surface of the substrate (1) and is used to absorb incident light; A p-type layer (6) disposed on the π-type layer (5); n + The layer (7) is arranged on the p-type layer (6), wherein the p-type layer (6) and the n-type layer (7) are connected to each other. + Layer (7) together forms the avalanche zone; A channel-type protection groove (4) penetrates the p-type layer (6), and the bottom of the channel-type protection groove (4) is located on the π-type layer (5), and is used to increase the breakdown voltage; The channel-type protection groove (4) is in the shape of an annular groove, and the channel-type protection groove (4) divides the upper surface of the p-type layer (6) into a middle circular portion and an outer circular portion, and the depth of the channel-type protection groove (4) is greater than the thickness of the p-type layer (6) and less than the sum of the thickness of the p-type layer (6) and the thickness of the π-type layer (5); wherein n + Layer (7) is located on the middle circular portion of the p-type layer (6); The silicon dioxide insulating layer (8) covers the n + The layer (7), the channel type protection groove (4) and the outer ring portion of the p-type layer (6) are used as a surface passivation layer; The first electrode (9) covers n + On the silicon dioxide insulating layer (8) above the layer (7), used to form an ohmic contact anode; A substrate hollowing region (2) is arranged on the lower surface of the substrate (1) and is used to reduce light loss of incident light outside the absorption region and simultaneously reduce the transit time of carriers; A silicon column region (3) is arranged at the bottom of the groove of the substrate hollowed-out region (2) and is used to enhance the absorption of near-infrared light; the silicon column is in the shape of a cylinder, the silicon column spacing between the plurality of silicon columns is 5 to 10 μm, and the plurality of silicon columns are evenly spaced; The second electrode (10) covers the bottom of the substrate (1) and is located outside the substrate hollowed-out region (2), and is used to form an ohmic contact cathode.
2. The structure according to claim 1, characterized in that: The thickness of the substrate (1) is 70 to 150 μm.
3. The structure according to claim 1, characterized in that: The depth of the substrate hollowed-out region (2) is 30 to 60 μm; The substrate hollowed-out area (2) is in the shape of a cylindrical groove.
4. The structure according to claim 1, characterized in that The height of the silicon pillars is 8 to 15 μm; When the silicon column is in the shape of a cylinder, the bottom diameter of the silicon column is 3 to 8 μm.
5. The structure according to claim 1, characterized in that: The thickness of the π-type layer (5) is 30 to 70 μm; The doping concentration of the π-type layer (5) is 1×10 14 Up to 5×10 14 cm -3 ; The thickness of the p-type layer (6) is 4 to 10 μm; The doping concentration of the p-type layer (6) is 1×10 15 cm -3 Up to 3×10 15 cm -3 ; The + The thickness of the layer (7) is 0.1 to 0.5 μm.
6. The structure according to claim 1, characterized in that The width of the trench type protection groove (4) is 1 to 6 μm.
7. The structure according to claim 1, characterized in that The material used for the first electrode (9) includes aluminum, gold, titanium, or titanium-platinum alloy; The thickness of the first electrode (9) is 300 to 600 nm.
8. The structure according to claim 1, characterized in that The material used for the second electrode (10) includes aluminum, gold, titanium-gold or titanium-platinum-gold alloy; The thickness of the second electrode (10) is 300 to 600 nm.
9. A method for preparing a back-incident near-infrared enhanced silicon avalanche photodetector, characterized in that: include: Preparing a π-type layer (5) on the upper surface of the substrate (1); Preparing a p-type layer (6) on the π-type layer (5); Preparing a silicon dioxide layer on the p-type layer (6); Etching the silicon dioxide layer to form an ion implantation window; Preparation of n in ion implantation window + Layer (7); Etch the p-type layer (6) and part of the n + The p-type layer (6) is provided with a plurality of protective grooves (4) formed therein; the ... In the p-type layer (6), the channel type protection groove (4) and the n + A silicon dioxide insulating layer (8) is formed on the layer (7); In n + A first electrode (9) is formed on the silicon dioxide insulating layer (8) above the layer (7); Etching a groove on the lower surface of the substrate (1) to prepare a substrate hollowed-out region (2); A second electrode (10) is prepared on the lower surface of the substrate (1) and is located at the periphery of the substrate hollowed-out region (2); A silicon pillar region (3) is prepared at the bottom of the groove of the substrate hollowed-out region (2), thereby completing the preparation of the back-incident near-infrared enhanced silicon avalanche photodetector; The silicon pillars are in the shape of cylinders, the interval between the silicon pillars is 5 to 10 μm, and the silicon pillars are evenly spaced.
10. The preparation method according to claim 9, characterized in that: When preparing the channel type protection groove (4), the n + The width of the layer (7) is 2 to 4 μm.