Lithium battery composite packaging material and lithium battery having high corrosion resistance
By controlling the composition and structure of the internal corrosion-resistant layer in the lithium battery composite packaging material, a stable corrosion-resistant cross-linking structure is formed, which solves the problem of short service life and risk of liquid leakage in harsh environments, and achieves a longer Lifespan and greater safety.
Patent Information
- Application Number
- CN202210654920.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-10
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-06-10
AI Technical Summary
The composite packaging materials of existing lithium batteries have a short service life under harsh environments, and are prone to separation of the intermediate metal layer from the hot-weld resin layer due to corrosive substances, losing their protection function, and leading to the risk of liquid leakage.
By controlling the content of chromium, moisture, carbon and metal elements in the internal corrosion-proof layer, a stable and corrosion-resistant crosslinking structure is formed, ensuring stable contact between the intermediate metal layer and the internal corrosion-proof layer, and increasing electrolytes and The resistance of hydrofluoric acid.
Extend the service life of lithium batteries, improve the shelf life and safety in harsh environments, prevent the separation of the intermediate metal layer and the hot-spread resin layer, and avoid the corrosion of liquid leakage and corrosive substances.
Smart Images

Figure CN115000596B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a battery packaging material, in particular to a composite packaging material suitable for lithium batteries and having high corrosion resistance; and to a lithium battery having high corrosion resistance. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density, light weight, and thinness, so they are widely used. Among them, in order to protect the battery from damage and prevent the electrolyte in the battery from leaking, aluminum-plastic composite film is usually used as the main outer packaging material of soft-package lithium-ion batteries. Specifically, the aluminum-plastic composite film includes: an intermediate metal layer and a heat-welding resin layer in order from the outside of the battery to the inside, wherein: when the electrolyte inside the lithium battery reacts with the moisture in the heat-welding resin layer, hydrofluoric acid will be generated. If the side of the intermediate metal layer close to the electrolyte does not form an anti-corrosion layer, the corrosive substances inside the battery will directly contact the intermediate metal layer, causing it to dissolve, crack, or produce pinholes. In existing lithium-ion batteries, although an anti-corrosion layer is formed between the intermediate metal layer and the heat-welding resin layer, the anti-corrosion property and structural strength of the formed anti-corrosion layer are not good. Therefore, the shelf life of lithium-ion batteries made of it as an anti-corrosion material is short, and it is less able to withstand harsh use environments, so the scope of use is greatly limited.
[0003] In addition, when the intermediate metal layer is corroded by the corrosive substances inside the lithium battery, it is easy to cause the peel strength between the intermediate metal layer and the heat-welding resin layer to decrease, causing the two to delaminate. If delamination occurs, the side of the intermediate metal layer close to the electrolyte will lose its protective power, making it easier for the corrosive substances to corrode and damage the intermediate metal layer, and eventually lead to leakage, making the lithium battery dangerous when used. Therefore, in order to avoid the above situation, it is necessary to provide a lithium battery composite packaging material with a good anti-corrosion layer formed on the side of the intermediate metal layer close to the electrolyte, so that the lithium battery can be stored for a long time, maintain normal performance in harsh environments, and improve safety in use. Summary of the invention
[0004] The purpose of the present invention is to provide a lithium battery composite packaging material with high corrosion resistance, wherein the chromium content, moisture content, carbon content, and metal element content from the intermediate metal layer contained in the inner corrosion protection layer are controlled to form a stable and corrosion-resistant cross-linked structure between the inner corrosion protection layer and the intermediate metal layer, so as to prevent the intermediate metal layer from directly contacting the corrosive substances inside the lithium-ion battery.
[0005] To achieve the above-mentioned object, the present invention provides a lithium battery composite packaging material with high corrosion resistance, comprising:
[0006] an intermediate metal layer;
[0007] an inner corrosion protection layer formed on one side of the intermediate metal layer, wherein the inner corrosion protection layer contains, per square meter of area: 5 to 100 mg of chromium, 0.5 to 65 mg of water, carbon, the content of which gradually decreases from the side of the inner corrosion protection layer opposite to the intermediate metal layer toward the side of the inner corrosion protection layer in contact with the intermediate metal layer, and metal elements from the intermediate metal layer, the content of which gradually decreases from the side of the inner corrosion protection layer in contact with the intermediate metal layer toward the side of the inner corrosion protection layer opposite to the intermediate metal layer; and
[0008] A heat-welding resin layer is formed on the side of the inner anti-corrosion layer opposite to the intermediate metal layer.
[0009] More preferably, it further comprises: an outer base resin layer formed on a side of the intermediate metal layer opposite to the inner anti-corrosion layer.
[0010] More preferably, it further comprises: an outer adhesive layer formed on a side of the intermediate metal layer opposite to the inner anti-corrosion layer.
[0011] More preferably, it further comprises: an inner adhesive layer formed between the inner anti-corrosion layer and the hot-melt resin layer.
[0012] Better yet, wherein: in the layered structure of the inner anti-corrosion layer on the side opposite to the intermediate metal layer, the carbon content is c, and the metal content is d1, based on the total weight of the inner anti-corrosion layer, and 40wt%≤c≤100wt%, and d1≤5wt%; in the layered structure of the inner anti-corrosion layer on the side opposite to the intermediate metal layer moving 20nm toward the intermediate metal layer, the metal content is d2, based on the total weight of the inner anti-corrosion layer, and 10wt%≤d2≤70wt%; or in the layered structure of the inner anti-corrosion layer on the side opposite to the intermediate metal layer moving 40nm toward the intermediate metal layer, the metal content is d3, based on the total weight of the inner anti-corrosion layer, and 20wt%≤d3≤100wt%.
[0013] Better yet, after the lithium battery composite packaging material with high corrosion resistance is immersed in an electrolyte, the inner anti-corrosion layer further contains fluorine element, wherein: in the layered structure of the inner anti-corrosion layer moving 20nm toward the intermediate metal layer on the side relative to the intermediate metal layer, the content of fluorine element is e1, and the content of metal element is d2, based on the total weight of the inner anti-corrosion layer, and e1≤30wt%, 10wt%≤d2≤70wt%, and e1 / d2≤2; or in the layered structure of the inner anti-corrosion layer moving 40nm toward the intermediate metal layer on the side relative to the intermediate metal layer, the content of fluorine element is e2, and the content of metal element is d3, based on the total weight of the inner anti-corrosion layer, and e2≤20wt%, 20wt%≤d3≤100wt%, and e2 / d3≤1.
[0014] More preferably, the inner anti-corrosion layer is formed by coating an anti-corrosion liquid on one side of the intermediate metal layer, and heating and drying the anti-corrosion liquid.
[0015] More preferably, the anti-corrosion liquid is heat treated at a temperature of 120 to 200° C. for 0.5 to 5 minutes to dry the anti-corrosion liquid.
[0016] More preferably, the components of the anti-corrosion liquid include: a solute including: a trivalent chromium compound, an inorganic acid, and an organic resin; and a solvent including: water or an organic solvent.
[0017] More preferably, based on the total weight of the anti-corrosion liquid, the weight ratio of the trivalent chromium compound, the inorganic acid, the organic resin, and the solvent is 1.9 to 6: 0.3 to 6: 0.6 to 6: 78.6 to 97.2.
[0018] More preferably, the solute further comprises a titanium compound, and the content of the titanium compound is 0 to 0.6 wt % based on the total weight of the anti-corrosion liquid; or the solute further comprises a zirconium compound, and the content of the zirconium compound is 0 to 2.8 wt % based on the total weight of the anti-corrosion liquid.
[0019] More preferably, the anti-corrosion liquid further comprises a cross-linking agent; the cross-linking agent comprises: an amino resin, a melamine resin, a phenolic resin, an epoxy compound, a blocked isocyanate compound, an oxazoline compound, or a carbodiimide compound; and the content of the cross-linking agent is 0.1 to 50 wt % based on the total weight of the solute.
[0020] More preferably, the anti-corrosion liquid further comprises a cross-linking agent; the cross-linking agent comprises: a condensation product of formaldehyde and an alkyl monohydric alcohol having 1 to 4 carbon atoms, or a condensation product of carbolic acid and formaldehyde; and the content of the cross-linking agent is 0.01 to 1.0 wt % based on the total weight of the solute.
[0021] More preferably, the trivalent chromium compound comprises chromium nitrate or chromium fluoride; the inorganic acid comprises phosphoric acid, nitric acid, or hydrofluoric acid; the organic resin comprises acrylic resin, methacrylic resin, hydroxy acrylic resin, polyvinyl alcohol resin, olefin resin, or fenaldehyde resin; the titanium compound comprises titanium fluoride or titanium nitrate; the zirconium compound comprises zirconium fluoride or zirconium nitrate; and the organic solvent comprises isopropyl alcohol, ethanol, or ethylene glycol butyl ether.
[0022] More preferably, the intermediate metal layer comprises: aluminum alloy, stainless steel, titanium steel, or nickel-plated iron plate.
[0023] The present invention further provides a lithium battery, comprising:
[0024] A lithium battery composite packaging material with high corrosion resistance; and an electrolyte, which is coated by the lithium battery composite packaging material with high corrosion resistance and contacts with the side of the heat-welding resin layer opposite to the intermediate metal layer.
[0025] Preferably, it further comprises:
[0026] an outer base resin layer formed on a side of the intermediate metal layer opposite to the inner anti-corrosion layer;
[0027] an outer adhesive layer formed on a side of the intermediate metal layer opposite to the inner anti-corrosion layer; or
[0028] An inner adhesive layer is formed between the inner anti-corrosion layer and the thermal welding resin layer.
[0029] The beneficial effect of the present invention is that when the moisture content contained in the inner anti-corrosion layer is too high or too low, the structural strength of the inner anti-corrosion layer will be unstable, resulting in a decrease in the peel strength between the intermediate metal layer and the heat-melting resin layer, which can easily lead to stratification of the two. In order to solve the above-mentioned problem, the present invention controls the moisture content contained in the inner anti-corrosion layer to form a stable cross-linked structure between the intermediate metal layer and the inner anti-corrosion layer, thereby preventing the electrolyte, hydrofluoric acid, or corrosive substances inside the lithium battery from dissolving the inner anti-corrosion layer through the heat-melting resin layer, and avoiding direct contact between the corrosive substances and the intermediate metal layer, causing the intermediate metal layer to rupture or perforate, resulting in leakage. Specifically, the lithium battery composite packaging material of the present invention has good corrosion resistance, so it can be stored for a long time, maintain normal performance in harsh environments, and improve safety in use. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figures 1A to 1B A series of structural diagrams are used to illustrate the structural features of the lithium battery composite packaging material with high corrosion resistance of the present invention;
[0031] Figures 2A to 2B It is a series of structural diagrams used to illustrate the structural features of the lithium battery of the present invention. DETAILED DESCRIPTION
[0032] In order to make the above and / or other purposes, effects, and features of the present invention more clearly understood, preferred embodiments are specifically described below in detail:
[0033] See also Figure 1A , which is used to represent the structural features of the present invention, wherein, Figure 1A As shown, the present invention provides a lithium battery composite packaging material 100 with high corrosion resistance, comprising: an intermediate metal layer 1; an inner anti-corrosion layer 5, formed on one side of the intermediate metal layer 1, wherein the inner anti-corrosion layer 5 per square meter area contains: 5 to 100 mg of chromium, 0.5 to 65 mg of water, and carbon, the content of which gradually decreases from the side of the inner anti-corrosion layer 5 relative to the intermediate metal layer 1 to the side where the inner anti-corrosion layer 5 contacts the intermediate metal layer 1, and metal elements from the intermediate metal layer 1, the content of which gradually decreases from the side where the inner anti-corrosion layer 5 contacts the intermediate metal layer 1 to the side where the inner anti-corrosion layer 5 relative to the intermediate metal layer 1; and a hot-melt resin layer 7, formed on the side of the inner anti-corrosion layer 5 relative to the intermediate metal layer 1.
[0034] Preferably, if Figure 1BAs shown, it further includes: an outer base resin layer 3, formed on the side of the intermediate metal layer 1 relative to the inner anti-corrosion layer 5. In a preferred embodiment, it further includes: an outer adhesive layer 4, formed on the side of the intermediate metal layer 1 relative to the inner anti-corrosion layer 5. In another preferred embodiment, it further includes: an outer anti-corrosion layer 2, formed on the side of the intermediate metal layer 1 relative to the inner anti-corrosion layer 5. In another preferred embodiment, it further includes: an inner adhesive layer 6, formed between the inner anti-corrosion layer 5 and the hot-melt resin layer 7.
[0035] Preferably, wherein: in the layered structure of the inner anti-corrosion layer 5 on one side relative to the intermediate metal layer 1, the carbon element content is c, and the metal element content is d1, based on the total weight of the inner anti-corrosion layer 5, and 40wt%≤c≤100wt%, and d1≤5wt%; in the layered structure of the inner anti-corrosion layer 5 on one side relative to the intermediate metal layer 1 moving 20nm toward the intermediate metal layer 1, the metal element content is d2, based on the total weight of the inner anti-corrosion layer 5, and 10wt%≤d2≤70wt%; or in the layered structure of the inner anti-corrosion layer 5 on one side relative to the intermediate metal layer 1 moving 40nm toward the intermediate metal layer 1, the metal element content is d3, based on the total weight of the inner anti-corrosion layer 5, and 20wt%≤d3≤100wt%.
[0036] Preferably, after the lithium battery composite packaging material 100 with high corrosion resistance is immersed in an electrolyte 8, the inner anti-corrosion layer 5 further contains fluorine element, wherein: in the layered structure of the inner anti-corrosion layer 5 moving 20nm toward the intermediate metal layer 1 on one side of the intermediate metal layer 1, the content of fluorine element is e1, and the content of metal element is d2, based on the total weight of the inner anti-corrosion layer 5, and e1≤30wt%, 10wt%≤d2≤70wt%, and e1 / d2≤2; or in the layered structure of the inner anti-corrosion layer 5 moving 40nm toward the intermediate metal layer 1 on one side of the intermediate metal layer 1, the content of fluorine element is e2, and the content of metal element is d3, based on the total weight of the inner anti-corrosion layer 5, and e2≤20wt%, 20wt%≤d3≤100wt%, and e2 / d3≤1.
[0037] Preferably, the inner anti-corrosion layer 5 is formed by applying an anti-corrosion liquid to one side of the intermediate metal layer 1 and heating and drying the anti-corrosion liquid. In a preferred embodiment, the anti-corrosion liquid is heat-treated at a temperature of 120 to 200°C for 0.5 to 5 minutes to dry the anti-corrosion liquid. In another preferred embodiment, the anti-corrosion liquid comprises a solute comprising a trivalent chromium compound, an inorganic acid, and an organic resin, and a solvent comprising water or an organic solvent. In another preferred embodiment, the weight ratio of the trivalent chromium compound, the inorganic acid, the organic resin, and the solvent is 1.9 to 6: 0.3 to 6: 0.6 to 6: 78.6 to 97.2 based on the total weight of the anti-corrosion liquid. In another preferred embodiment, the solute further comprises a titanium compound, and the content of the titanium compound is 0 to 0.6 wt% based on the total weight of the anticorrosion liquid; or the solute further comprises a zirconium compound, and the content of the zirconium compound is 0 to 2.8 wt% based on the total weight of the anticorrosion liquid. In another preferred embodiment, the anticorrosion liquid further comprises a crosslinking agent; the crosslinking agent comprises: an amino resin, a melamine resin, a phenolic resin, an epoxy compound, a blocked isocyanate compound, an oxazoline compound, or a carbodiimide compound; and the content of the crosslinking agent is 0.1 to 50 wt% based on the total weight of the solute. In another preferred embodiment, the anticorrosion liquid further comprises a crosslinking agent; the crosslinking agent comprises: a condensate of formaldehyde and a monohydric alcohol having 1 to 4 carbon atoms, or a condensate of carbolic acid and formaldehyde; and the content of the crosslinking agent is 0.01 to 1.0 wt% based on the total weight of the solute. In another preferred embodiment, the trivalent chromium compound comprises chromium nitrate or chromium fluoride; the inorganic acid comprises phosphoric acid, nitric acid, or hydrofluoric acid; the organic resin comprises acrylic resin, methacrylic resin, hydroxy acrylic resin, polyvinyl alcohol resin, olefin resin, or fenaldehyde resin; the titanium compound comprises titanium fluoride or titanium nitrate; the zirconium compound comprises zirconium fluoride or zirconium nitrate; and the organic solvent comprises isopropyl alcohol, ethanol, or ethylene glycol butyl ether. In another preferred embodiment, the intermediate metal layer 1 comprises aluminum alloy, stainless steel, titanium steel, or nickel-plated iron plate.
[0038] Preferably, the present invention further provides a lithium battery, such as Figure 2A As shown, it comprises: a lithium battery composite packaging material 100 with high corrosion resistance; and an electrolyte 8, which is coated by the lithium battery composite packaging material 100 with high corrosion resistance and contacts with the side of the heat-welding resin layer 7 relative to the intermediate metal layer 1. In a preferred embodiment, as Figure 2BAs shown, it further includes: an outer base resin layer 3, formed on the side of the intermediate metal layer 1 relative to the inner anti-corrosion layer 5; an outer adhesive layer 4, formed on the side of the intermediate metal layer 1 relative to the inner anti-corrosion layer 5; an outer anti-corrosion layer 2, formed on the side of the intermediate metal layer 1 relative to the inner anti-corrosion layer 5; or an inner adhesive layer 6, formed between the inner anti-corrosion layer 5 and the hot melt resin layer 7.
[0039] Preferably, in the lithium battery composite packaging material 100 with high corrosion resistance provided by the present invention, the outer substrate resin layer 3 is used as the outermost layer of the lithium ion battery to provide an insulating effect to prevent leakage; and the heat-melting resin layer 7 is used as the innermost layer of the packaging material to block the electrolyte to prevent the electrolyte 8 from flowing out of the lithium ion battery. In a preferred embodiment, in order to make the lithium battery composite packaging material 100 with high corrosion resistance provided by the present invention have a specific color, a coloring layer can be formed on the outer substrate resin layer 3, but it is not limited to this. In order to more fully describe the detailed structure of the present invention and the type of materials used, the detailed implementation of the outer substrate resin layer 3, the outer adhesive layer 4, the coloring layer, the outer anti-corrosion layer 2, the intermediate metal layer 1, the inner anti-corrosion layer 5, the inner adhesive layer 6, and the heat-melting resin layer 7 is specifically provided below; and the "lithium battery composite packaging material 100 with high corrosion resistance" of the present invention is referred to as "metal-plastic composite film" below.
[0040] 1. Related embodiments of the outer base resin layer 3.
[0041] Preferably, the outer substrate resin layer 3 is arranged on the outermost side of the metal-plastic composite film, and its function includes: exerting the substrate function of the metal-plastic composite film, so it can be understood that the raw material of the outer substrate resin layer 3 should at least have insulation. In a preferred embodiment, the method for making the outer substrate resin layer 3 includes: directly forming a resin film product from a resin; or coating a resin product, and is not limited to this. Among them, the resin film includes: an unstretched film; or a stretched film, wherein the stretched film includes: a uniaxial stretched film, or a biaxial stretched film, and is not limited to this. In a preferred embodiment, the stretched film is preferably a biaxial stretched film, and its preparation method includes: a step-by-step biaxial stretching method, a blown film method, or a synchronous stretching method, and is not limited to this. The preparation method of the coated resin product includes: a roller coating method, a micro-concave coating method, or an extrusion coating method, and is not limited to this.
[0042] Preferably, the raw material of the outer substrate resin layer 3 includes: polyester, polyamide, polyolefin, epoxy resin, acrylic resin, fluororesin, polyurethane, silicone resin, phenolic resin, modified products of the above-listed resins, copolymers of the above-listed resins, modified products of the copolymers of the above-listed resins, mixtures of the above-listed resins, or combinations thereof. In a preferred embodiment, the raw material of the outer substrate resin layer 3 is preferably polyester or polyamide. Among them, polyester includes: polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyethylene isophthalate, or copolyester, but is not limited thereto. Specifically, the copolyester is a copolymer polyester formed by polymerizing ethylene terephthalate as a main body of repeating units; polymerizing ethylene terephthalate as a main body of repeating units with ethylene isophthalate; polymerizing terephthalate with isophthalate; polymerizing terephthalate with adipate; polymerizing terephthalate with sodium isophthalate; polymerizing terephthalate with phenyl-dicarboxylate; or polymerizing terephthalate with decanedicarboxylate. In a preferred embodiment, one polyester can be used alone; or two or more polyesters can be used in combination.
[0043] Preferably, the polyamide comprises: nylon 6, nylon 66, nylon 610, nylon 12, nylon 46, nylon 6, or nylon 66 copolymer. In a preferred embodiment, the polyamide comprises structural units of terephthalic acid (t) or isophthalic acid (I), specifically: nylon 6I, nylon 6T, nylon 6IT, or nylon 6I6T. In another preferred embodiment, the polymer raw material of the polyamide comprises: hexamethylenediamine, isophthalic acid, terephthalic acid, or a combination thereof, but is not limited thereto. In another preferred embodiment, the polyamide includes: PA4T, PA6T, PA9T, PA10T, PA11T, PA12T, PA6I, PA9I, PA10I, PA12I, PA46, PA6, PA66, PA69, PA10, PA11, PA12, PA610, PA612, PA1010, PA1112, PA1011, PA1012, PA1212, PA MXD6, PA MXD9, PA MXD10, PA MXD12, PA PACM6, PA PACM9, PA PACM10, PAPACM12, PA6N, PA12N, PA10N, PA9N, or a combination thereof. In another preferred embodiment, the polyamide is PA6T / 61, PA6T / 66, PA6T / 610, PA6T / 612, PA6T / 12, PA6T / 11, PA6T / 6, PA6T / 10T, PA6T / 101, PA6T / 106, PA6T / 1010, PA6T / 66 / 106, PA6T / MACM10, PA6T / MACM12, PA6T / MACM18, PA6T / MACM1, PAMACMT / 61, PA6T / PACM6, PA6T / PACM10, PA6T / PACM12, PA6T / PACM18, PA6T / PACM1, PACMT / 61, PA MPT / MP1, PA MPT / MP6, PA6T / MP1, PA6T / 9T, PA6T / 12T, PA6T / 6I / 66, PA6T / 6I / 6, PA6T / 6I / 12, PA6T / 66 / 6, PA6T / 66 / 12, PA6T / 6I / MACM1, or PA6T / 66 / PACM6, but not limited thereto. It can be understood that the polyamide may include one or a combination of two or more of the above-mentioned polyamides.
[0044] Preferably, the outer substrate resin layer 3 comprises: a polyester film, a polyamide film, a polyolefin film, or a combination thereof; further preferably comprises: a stretched polyester film, a stretched polyamide film, a stretched polyolefin film, or a combination thereof; further preferably comprises: a stretched polyethylene terephthalate film, a stretched polybutylene terephthalate film, a stretched nylon film, a stretched polypropylene film, or a combination thereof; further preferably comprises: a biaxially stretched polyethylene terephthalate film, a biaxially stretched polybutylene terephthalate film, a biaxially stretched nylon film, a biaxially stretched polypropylene film, or a combination thereof.
[0045] Preferably, the outer substrate resin layer 3 can be a single-layer structure, or a multi-layer structure of more than one layer. Wherein, when the outer substrate resin layer 3 is composed of more than one layer, the outer substrate resin layer 3 is a composite film formed by the interaction of an adhesive and a multi-layer structure; or a multi-layer resin composite film made of resin by "co-extrusion technology", but not limited to this. In a preferred embodiment, the multi-layer resin composite film can be used as the outer substrate resin layer 3 in an unstretched state; after uniaxial stretching; or after biaxial stretching. In another preferred embodiment, when the outer substrate resin layer 3 is composed of more than one layer, its structure is: a composite film of polyester film and nylon film; a composite film composed of more than one layer of nylon film; or a composite film composed of more than one layer of polyester film; further preferably, a composite film composed of stretched nylon film and stretched polyester film, a composite film composed of more than one layer of stretched nylon film, or a composite film composed of more than one layer of stretched polyester film. Specifically, the multilayer resin composite film is a composite film composed of a polyester resin film and a polyester resin film; a composite film composed of a polyamide resin film and a polyamide resin film; or a composite film composed of a polyester resin film and a polyamide resin film, wherein: the multilayer resin composite film is further preferably a composite film composed of a polyethylene terephthalate film and a polyethylene terephthalate film; a composite film composed of a polybutylene terephthalate film and a polybutylene terephthalate film; a composite film composed of a nylon film and a nylon film; or a composite film composed of a polyethylene terephthalate film and a nylon film, and is not limited to these.
[0046] Preferably, since polyester resin has the problem of being difficult to change color when the electrolyte 8 is attached to the surface, in order to improve the above disadvantages, when the outer substrate resin layer 3 is a resin composite film of more than two layers, the polyester resin film is preferably arranged on the outermost layer of the outer substrate resin layer 3. In a preferred embodiment, the two or more resin films can be composited by acting with an adhesive, wherein the adhesive is preferably a glue having the same composition as the outer adhesive layer 4.
[0047] Preferably, the method for compounding more than two layers of resin film includes: dry compounding method, sandwich compounding method, extrusion compounding method, thermal compounding method, and is not limited thereto, wherein dry compounding method is preferred. Specifically, when compounding a multilayer resin film by dry compounding method, the reactive adhesive as the outer layer is preferably a reactive polyurethane adhesive, and the thickness of the outer adhesive layer 4 is about 2 to 5 μm. In a preferred embodiment, when the outer substrate resin layer 3 is formed by a resin coating method, the resin can be first dissolved in an organic solvent, and then the outer substrate resin layer 3 is formed by coating. In another preferred embodiment, the coating resin used in the resin coating method is a phenol resin, and its types include: polyamide resin, polyimide resin, polyurethane resin, epoxy resin, acrylic resin, polyester resin, polyamide resin, polyimide resin, fluorine copolymer resin, polyester resin, etc.; or an amino resin, and its types include: polyester resin, polycarbonate resin, urea resin, or melamine resin.
[0048] Preferably, one or more additives may be added to the surface or inside of the outer substrate resin layer 3, wherein the additives include: lubricants, flame retardants, anti-adhesive agents, antioxidants, light stabilizers, tackifiers, or antistatic agents. In a preferred embodiment, in order to improve the formability of the lithium battery composite packaging material, a layered structure composed of a lubricant is preferably formed on the surface of the outer substrate resin layer 3. The lubricant is preferably an amide lubricant, including: saturated fatty acid amide, unsaturated fatty acid amide, substituted amide, hydroxymethyl amide, saturated fatty acid bisamide, unsaturated fatty acid bisamide, fatty acid amide, or aromatic bisamide. In another preferred embodiment, the saturated fatty acid amide comprises: lauric acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, or hydroxystearic acid amide; the unsaturated fatty acid amide comprises: oleic acid amide, or erucic acid amide; the substituted amide comprises: N-oleyl palmitic acid amide, N-stearic acid amide, N-stearic acid amide, N-oleostearic acid amide, or N-stearic acid amide; the hydroxymethyl amide comprises: hydroxymethyl stearic acid amide; the saturated fatty acid bisamide comprises: methylene bis stearic acid amide, ethylene bis caprylic acid amide, ethylene bis lauric acid amide, ethylene bis stearic acid amide, ethylene bis hydroxystearic acid amide, ethylene bis behenic acid amide, or ethylene bis caprylic acid amide. The unsaturated fatty acid bisamides include: ethylene bisoleamide, ethylene biserucic acid amide, hexamethylene bisoleamide, n,n'-dioleyl adipamide, or n,n'-dioleyl sebacic acid amide; the fatty acid ester amides include: stearamide ethyl stearate; the aromatic bisamides include: isophthalic acid bisstearamide, isophthalic acid bishydroxystearamide, or n,n'-distearylisophthalic acid amide. In another preferred embodiment, the lubricant may include one or more of the above-listed ones, but is not limited thereto.
[0049] Preferably, when a lubricant is formed on the surface of the outer base resin layer 3, the coating amount of the lubricant is preferably 3 mg / m 2 More preferably, 4 to 30 mg / m 2 , but not limited thereto. In a preferred embodiment, the lubricant formed on the surface of the outer substrate resin layer 3 is exuded from the outer substrate resin layer 3 containing the lubricant; or the lubricant is applied to the surface of the outer substrate resin layer 3. In another preferred embodiment, when the outer substrate resin layer 3 is a resin composite film with more than one layer, the thickness of the resin film constituting each layer is preferably 2 to 30 μm, wherein the thickness of the outer substrate resin layer 3 can meet the basic requirements as a substrate, and therefore the thickness is not limited thereto.
[0050] Preferably, the outer substrate resin layer 3 is a single layer or a composite film formed by one or more of the above-listed polymer materials, or a combination of materials, such as blown film nylon, synchronous biaxially stretched nylon, asynchronous biaxially stretched nylon, synchronous biaxially stretched polyethylene terephthalate (PET), asynchronous biaxially stretched polyethylene terephthalate (PET), synchronous biaxially stretched polybutylene terephthalate (PBT), asynchronous biaxially stretched polybutylene terephthalate (PBT), polyimide (PI), or one or more of the above-listed polymer materials. In a preferred embodiment, the outer substrate resin layer 3 can be bonded to the intermediate metal layer 1 by extrusion, coating, compounding, hot pasting, or a combination of the above methods. In another preferred embodiment, the total thickness of the outer substrate resin layer 3 is preferably 5 to 35 μm. Specifically, when the thickness is less than 5 μm, the formability and insulation of the outer substrate resin layer 3 are poor; if the thickness exceeds 35 μm, the total thickness of the metal-plastic composite film will be too thick, resulting in poor softness of the metal-plastic composite film.
[0051] 2. Related embodiments of the outer adhesive layer 4.
[0052] Preferably, in the state where the outer substrate resin layer 3 and the intermediate metal layer 1 are compounded, in order to improve the adhesion between the two, an outer adhesive layer 4 is preferably formed between the two. It can be understood that the outer adhesive layer 4 is an adhesive, including: a two-component curing adhesive (two-component adhesive), or a single-component curing adhesive (single-component adhesive). In a preferred embodiment, the type of adhesive used to form the outer adhesive layer 4 includes: a chemical reaction type, a solvent evaporation type, a hot melt type, or a hot pressing type, but is not limited thereto. In addition, the outer adhesive layer 4 can be a single-layer structure, or a multi-layer structure of more than one layer.
[0053] Preferably, the outer adhesive layer 4 comprises a main agent and a curing agent, specifically, a two-component polyurethane adhesive formed by using polyester polyol and polyol modified with polyol as diol main agents and aromatic or aliphatic isocyanate as curing agent. The main agent used includes: polyester resin, including: polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyethylene isophthalate, or copolymerized polyester; polyether resin; polyurethane resin; epoxy resin; phenolic resin; polyamide resin, including: nylon 6, nylon 66, nylon 12, or copolymerized polyamide; polyolefin resin, including: polyolefin, cyclic polyolefin, acid-modified polyolefin, or acid-modified cyclic polyolefin; polyvinyl acetate; cellulose; (meth) acrylic resin; polyimide resin; polycarbonate; amino resin, including: urea resin or melamine resin; rubber, including: chloroprene rubber, nitrile rubber, or styrene-butadiene rubber; or silicone resin. The curing agent used can be selected according to the functional groups of the components of the adhesive, including: multifunctional epoxy resin, polymer containing methyl sulfonic acid, polyamine resin, or inorganic acid. It is understood that the adhesive may be composed of one or a combination of more than one of the components listed above.
[0054] Preferably, the outer adhesive layer 4 comprises: a binary or polyvalent polyester; one, two, or more than two polyurethane-modified polyesters; and an isocyanate. Among them, the isocyanate is a compound having two or more isocyanate groups in the molecule, but is not limited thereto. Specifically, the isocyanate comprises: isophorone diisocyanate (IPDI), toluene diisocyanate (TDI), diphenylmethane-4,4'-diisocyanate (MDI), 1,6-hexamethylene diisocyanate (HDI), or a mixture formed by combining the above polymers.
[0055] 3. Related embodiments of the coloring layer.
[0056] Preferably, a coloring layer can be formed between the outer substrate resin layer 3 and the intermediate metal layer 1 according to the coloring requirements. The coloring layer can be formed by adding a colorant to the outer adhesive layer 4; forming a coloring layer between the outer substrate resin layer 3 and the outer adhesive layer 4; or setting a coloring layer on the side of the outer substrate resin layer 3 relative to the intermediate metal layer 1, but not limited thereto. Specifically, a coloring layer can be formed by applying an ink containing a colorant to the surface of the outer substrate resin layer 3; the surface of the outer adhesive layer 4; or the surface of the intermediate metal layer 1. In a preferred embodiment, the colorant is formed by a plurality of pigment particles bonded to each other, and the particle size range of the pigment particles is 0.05 to 5 μm, preferably 0.08 to 2 μm. The median particle size of the pigment particles can be measured using a laser diffraction device or a scattering particle size distribution measuring device, but not limited thereto. In another preferred embodiment, the content of the colorant is 5 to 60wt%, preferably 10 to 40wt%, based on the total weight of the outer adhesive layer 4, but not limited thereto. In another preferred embodiment, the thickness of the coloring layer is sufficient to bond the intermediate metal layer 1 and the outer substrate resin layer 3, preferably 1 to 10μm, more preferably 2 to 5μm, but not limited thereto. In another preferred embodiment, under the premise of not affecting the adhesion of the outer adhesive layer 4, the raw materials of the outer adhesive layer 4 can be added with an additive, including: a colorant, a thermoplastic elastomer, a tackifier, or a filler, but not limited thereto. In another preferred embodiment, when the outer adhesive layer 4 contains a colorant, the lithium battery composite packaging material can be colored. Among them, the colorant can be a pigment, including: organic pigments, including: azo, phthalocyanine, quinacridone, anthraquinone, dioxazine, indigothioindigo, perylene, or isoindoline pigments; and inorganic pigments, including: carbon black, titanium oxide, cadmium, lead, or isoindoline pigments; or dyes, but not limited to this. In addition, it can be understood that the colorant includes one or more combinations of the above-listed ones. It can be understood that in order to make the appearance of the metal-plastic composite film black, the color of the pigment or dye used is preferably carbon black, but not limited to this.
[0057] 4. Related embodiments of the anti-corrosion layer.
[0058] Preferably, in the metal-plastic composite film, in order to prevent the hydrogen fluoride generated by the reaction of the electrolyte in the lithium battery with water from corroding the surface of the intermediate metal layer 1, an anti-corrosion layer can be formed on at least one side of the intermediate metal layer 1, wherein the purpose of forming the anti-corrosion layer includes: maintaining the uniformity of the surface of the intermediate metal layer 1; and reducing the change in adhesion (wettability), thereby preventing the intermediate metal layer 1 from separating or stratifying from the heat-melting resin layer 7, or preventing the intermediate metal layer 1 from separating or stratifying from the outer base resin layer 3.
[0059] Preferably, an anti-corrosion liquid can be applied to the side of the intermediate metal layer 1 facing the outer substrate resin layer 3 to form an "external anti-corrosion layer 2"; and an anti-corrosion liquid can be applied to the side of the intermediate metal layer 1 facing the heat-welding resin layer 7 to form an "internal anti-corrosion layer 5". Specifically, the main components of the anti-corrosion liquid used include: a solute including: a trivalent chromium compound, an inorganic acid, and an organic resin, and a solvent including: water, an organic solvent, or a combination thereof, but not limited thereto. In a preferred embodiment, based on the total weight of the anti-corrosion liquid, the weight ratios of the trivalent chromium compound, the inorganic acid, the organic resin, and the solvent are 1.9 to 6wt%, 0.3 to 6wt%, 0.6 to 6wt%, and 78.6 to 97.2wt%, respectively.
[0060] Preferably, the anti-corrosion liquid of the present invention can be evenly spread and wetted on the intermediate metal layer 1 through a coating process, and after the anti-corrosion liquid is spread, it is heat treated under high temperature conditions for a period of time to evaporate the water or organic solvent in the anti-corrosion liquid to form an outer anti-corrosion layer 2 or an inner anti-corrosion layer 5, and the obtained anti-corrosion layer is in close contact with the intermediate metal layer 1 and is not easy to fall off. In a preferred embodiment, the anti-corrosion layer of the present invention includes the following features: the content of chromium in the anti-corrosion layer is 5 to 100 mg / m 2 ; The moisture content in the anti-corrosion layer is controlled between 0.5 and 65 mg / m 2 ; and the carbon content from the anti-corrosion layer and the metal element content from the intermediate metal layer 1 are distributed in a gradient or linearly increased or decreased, based on the total weight of the anti-corrosion layer. Specifically, taking the "external anti-corrosion layer 2" as an example, based on the total weight of the external anti-corrosion layer 2, the carbon element content in the outermost layer relative to the intermediate metal layer 1 is a, and 40wt%≤a≤100wt%, and the metal element content from the intermediate metal layer 1 is b1, and 5wt%≤b1≤30wt%; the metal element content from the intermediate metal layer 1 in the layered structure moving 20nm from the outermost layer relative to the intermediate metal layer 1 to the intermediate metal layer 1 is b2, and 10wt%≤b2≤70wt%; and the metal element content from the intermediate metal layer 1 in the layered structure moving 40nm from the outermost layer relative to the intermediate metal layer 1 to the intermediate metal layer 1 is b3, and 20wt%≤b3≤100wt%.
[0061] Preferably, in the anticorrosion liquid, the trivalent chromium compound used contains at least chromium nitrate or chromium fluoride, the purpose of which is to form a coordination cross-linked structure centered on chromium (Cr) atoms on the surface of the intermediate metal layer 1. Specifically, the trivalent chromium compound is used to increase the degree of cross-linking between the intermediate metal layer 1 and the anticorrosion layer. In addition, chromium nitrate and chromium fluoride react with the resin in the anticorrosion layer, the intermediate metal layer 1, and the inorganic acid; and chromium fluoride can improve the ability of the anticorrosion layer to resist hydrogen fluoride, and can maintain the adhesion between the intermediate metal layer 1 and the outer substrate resin layer 3, or the adhesion between the intermediate metal layer 1 and the heat-welding resin layer 7 during long-term storage. In a preferred embodiment, the inorganic acid at least includes: phosphoric acid, nitric acid, or hydrofluoric acid, wherein the function of adding the inorganic acid is to remove the oxide film on the surface of the intermediate metal layer 1, so that the metal can react quickly with the components in the anti-corrosion layer to form a strong chromium reaction product, thereby ensuring the bonding strength between the intermediate metal layer 1 and the outer substrate resin layer 3, or the intermediate metal layer 1 and the hot-melt resin layer 7 when the metal-plastic composite film is stored for a long time, so that it is not easy to separate. In another preferred embodiment, the organic resin at least includes: acrylic resin, methacrylic resin, hydroxy acrylic resin, polyvinyl alcohol resin, olefin resin, phenolic resin, or phenolic resin, wherein the function of adding the organic resin is to improve the film-forming property of the anti-corrosion layer on the surface of the intermediate metal layer 1; and to enhance the bonding force and bonding stability between the outer anti-corrosion layer 2 and the outer adhesive layer 4, or the inner anti-corrosion layer 5 and the inner adhesive layer 6. In another preferred embodiment, the organic solvent at least comprises: isopropanol, ethanol, or ethylene glycol butyl ether, wherein: the function of adding the organic solvent is to reduce the surface tension of the anticorrosive liquid to increase the leveling property of the anticorrosive liquid on the surface of the intermediate metal layer 1. In addition, the organic solvent can be used alone or added to water to improve the wettability of the anticorrosive liquid and the stability of the anticorrosive layer and the intermediate metal layer 1. In another preferred embodiment, in order to enhance the anticorrosive power of the anticorrosive layer, wherein: the anticorrosive liquid further comprises: titanium (Ti) compound or zirconium (Zr) compound, preferably, the titanium compound at least comprises: titanium fluoride or titanium nitrate; and the zirconium compound at least comprises: zirconium fluoride or zirconium nitrate, but not limited thereto, more preferably, based on the total weight of the anticorrosive liquid, the content of the titanium compound is 0 to 0.6wt%; and the content of the zirconium compound is 0 to 2.8wt%. Specifically, titanium compounds or zirconium compounds can serve as secondary central crosslinking points to enhance the anti-corrosion effect of the anti-corrosion layer on the surface of the intermediate metal layer 1; and titanium compounds or zirconium compounds can improve the stability of the reaction between chromium and resin, metal, and inorganic acid.In another preferred embodiment, in the anti-corrosion layer, the reaction products of chromium, titanium and zirconium are resistant to the battery electrolyte 8 or the hydrogen fluoride produced by the electrolyte 8, thereby improving the bonding strength between the intermediate metal layer 1 and the outer substrate resin layer 3, or the intermediate metal layer 1 and the heat-melting resin layer 7, making it difficult for them to separate.
[0062] Preferably, taking the "external anti-corrosion layer 2" as an example, the purpose of controlling the minimum value of the water content in the external anti-corrosion layer 2 is to control the crosslinking density of the external anti-corrosion layer 2 to avoid the crosslinking density of the external anti-corrosion layer 2 being too high. When the crosslinking density is too high, the external anti-corrosion layer 2 will become hard and brittle, so that the external substrate resin layer 3 and the external anti-corrosion layer 2 cannot form a good mechanical property match, which easily causes the intermediate metal layer 1 to break or separate from the external substrate resin layer 3. In a preferred embodiment, when the water content in the external anti-corrosion layer 2 is less than or equal to 0.5 mg / m 2 When the water content in the outer anti-corrosion layer 2 is less than 0.5 mg / m3, the intermediate metal layer 1 will be cracked or corroded. Therefore, the water content in the outer anti-corrosion layer 2 should be between 0.5 and 65 mg / m3. 2 The above-mentioned risks can only be avoided if the moisture content of the intermediate metal layer 1 is within the range of . In another preferred embodiment, the present invention can adjust the surface tension of the intermediate metal layer 1 by controlling the moisture content, so as to improve the surface wettability of the intermediate metal layer 1, and improve the adhesion between the outer adhesive layer 4 and the intermediate metal layer 1, and improve the adhesion between the outer substrate resin layer 3 and the intermediate metal layer 1. Specifically, the metal-plastic composite film of the present invention has stable performance and can be used as an outer packaging material for lithium batteries for a long time, so that the battery has a longer service life. In another preferred embodiment, the purpose of controlling the minimum value of the moisture content in the "inner anti-corrosion layer 5" is to avoid the intermediate metal layer 1 from breaking or separating from the hot-melt resin layer 7. Since the purpose of controlling the moisture content of the inner and outer anti-corrosion layers 2 is roughly the same, no further elaboration is given here.
[0063] Preferably, when the water content in the outer anti-corrosion layer 2 is controlled, the water content in the inner anti-corrosion layer 5 is also controlled. Specifically, when the water content in the inner anti-corrosion layer 5 is appropriate, the inner anti-corrosion layer 5 can be improved to resist the penetration, swelling, or destruction of the electrolyte 8 or hydrofluoric acid, so as to protect the intermediate metal layer 1 from the corrosion of hydrofluoric acid, and maintain good and stable bonding between the heat-welding resin layer 7 and the intermediate metal layer 1.
[0064] Preferably, in the present invention, the content of elements contained in the anti-corrosion layer is in a gradient distribution or linear increase and decrease, wherein, by controlling the carbon (C) content and the metal element content of the anti-corrosion layer relative to the outermost layer of the intermediate metal layer 1; the metal element content in the layered structure of the anti-corrosion layer relative to the outermost layer of the intermediate metal layer 1 moving 20nm toward the intermediate metal layer 1; and the metal element content in the layered structure of the anti-corrosion layer relative to the outermost layer of the intermediate metal layer 1 moving 40nm toward the intermediate metal layer 1, the bonding stability between the intermediate metal layer 1 and the outer substrate resin layer 3; or between the intermediate metal layer 1 and the hot-melt resin layer 7 can be improved to prevent the two from being delaminated. In summary, the present invention can effectively block the electrolyte 8 inside the battery and the corrosive substances outside the battery, so that the battery can maintain stability and safety in harsh environments or during long-term storage, without the risk of leakage, short circuit, or explosion due to corrosion or rupture of the intermediate metal layer 1.
[0065] Preferably, the surface wettability of the intermediate metal layer 1 is 65 dyn / cm, preferably 70 dyn / cm or more; or the angle of the titration contact angle between the intermediate metal layer 1 and distilled water is 15° or less, preferably 10° or less. Specifically, if the wettability of the intermediate metal layer 1 or the contact angle between its surface and water exceeds the range interval listed above, the intermediate metal layer 1 may have rolling oil remaining on its surface during the manufacturing process. It can be understood that when the rolling oil exists, the interface adhesion between the intermediate metal layer 1, the inner anti-corrosion layer 5, and the hot-melt resin layer 7 will be poor, so that the battery made of the intermediate metal layer 1 has the risk of falling off between the intermediate metal layer 1 and the hot-melt resin layer 7 during long-term storage, making the battery prone to leakage. In a preferred embodiment, in order to avoid the above situation, the intermediate metal layer 1 can be annealed at 150°C or above; or the intermediate metal layer 1 can be deoiled by plasma, corona method, or alkali solution. In another preferred embodiment, the degreasing method using alkaline solution includes: immersing the intermediate metal layer 1 in an alkaline solution at 50 to 65° C. for a certain period of time; washing the immersed intermediate metal layer 1 twice with deionized water; and drying, thereby completing the degreasing treatment of the intermediate metal layer 1.
[0066] Preferably, the method of forming the anti-corrosion layer on the intermediate metal layer 1 includes: coating the anti-corrosion liquid on both sides of the intermediate metal layer 1; heat treating the anti-corrosion liquid at high temperature for a period of time to form the anti-corrosion layer. In a preferred embodiment, the anti-corrosion liquid can be simultaneously coated on the corresponding two sides of the intermediate metal layer 1 by a one-step method using a double-sided coating method, and subjected to a high-temperature heat treatment for a period of time to obtain an intermediate metal layer 1 having an anti-corrosion layer on both sides. In another preferred embodiment, the anti-corrosion liquid can be first coated on one side of the intermediate metal layer 1 by a two-step method, and heat treated at high temperature for a period of time to form an intermediate metal layer 1 having an anti-corrosion layer on one side, and then a second coating is performed to coat the anti-corrosion liquid on the other side of the intermediate metal layer 1, and heat treated at high temperature for a period of time to finally form an intermediate metal layer 1 having an anti-corrosion layer on both sides.
[0067] Preferably, the outer adhesive layer 4 is formed by forming a polyurethane adhesive dissolved by an organic solvent on the side of the intermediate metal layer 1 facing the outer base resin layer 3 or the side of the outer base resin layer 3 facing the intermediate metal layer 1, and heating at a certain temperature for a certain time to volatilize the organic solvent to form the outer adhesive layer 4. In a preferred embodiment, the outer adhesive layer 4 is compounded by compounding the outer base resin layer 3, the outer adhesive layer 4 and the intermediate metal layer 1 at a certain temperature and pressure, and after storing at a certain temperature for a certain time, the outer adhesive layer 4 undergoes a curing reaction to obtain a composite resin layer composed of the outer base resin layer 3, the outer adhesive layer 4 and the intermediate metal layer 1 in sequence. In another preferred embodiment, when the outer substrate resin layer 3 and the intermediate metal layer 1 are composited without using the outer adhesive layer 4, the intermediate metal layer 1 and the outer substrate resin layer 3 can be composited by heating and pressurizing. Specifically, the outer substrate resin layer 3 can be film-formed by heating treatment, ultraviolet treatment, or electron beam treatment to obtain a composite resin layer composed of the outer substrate resin layer 3 and the intermediate metal layer 1.
[0068] Preferably, the composite film composed of the outer substrate resin layer 3 and the intermediate metal layer 1 can be appropriately selected to be composited with the hot melt resin layer 7 in different composite methods. Specifically, the composite method of the hot melt resin layer 7 can use a dry composite method, including: applying a solution-type inner layer adhesive to the side of the intermediate metal layer 1 relative to the outer substrate resin layer 3, wherein the components of the solution-type inner layer adhesive include a main agent, a curing agent, and an organic solvent; drying the solution-type inner layer adhesive to form an inner layer adhesive layer 6; under a certain temperature and pressure, the hot melt resin layer 7 is brought into contact with the side of the inner layer adhesive layer 6 relative to the intermediate metal layer 1 to perform thermal composite, and perform a aging treatment to form a composite product composed of the outer substrate resin layer 3, the outer layer adhesive layer 4, the intermediate metal layer 1, the inner layer adhesive layer 6, and the hot melt resin layer 7 in sequence. In a preferred embodiment, before the hot melt resin layer 7 is brought into contact with the inner layer adhesive layer 6, the hot melt resin layer 7 can be pre-corona treated. In another preferred embodiment, the inner adhesive layer 6 may be subjected to a aging treatment. Preferably, the aging temperature does not exceed the melting point of the inner adhesive layer 6. More preferably, the aging temperature does not exceed 60°C. In another preferred embodiment, an outer anti-corrosion layer 2 may be formed between the outer adhesive layer 4 and the intermediate metal layer 1; and an inner anti-corrosion layer 5 may be formed between the inner adhesive layer 6 and the intermediate metal layer 1.
[0069] Preferably, the composite method of the hot-melt resin layer 7 can use a melt extrusion method, including: forming a hot-melt inner layer adhesive layer 6 of a certain thickness on the side of the inner anti-corrosion layer 5 relative to the intermediate metal layer 1 by melt extrusion of a hot-melt inner layer adhesive resin; and thermally compounding the surface of the hot-melt inner layer adhesive layer 6 with a hot-melt resin layer 7. In a preferred embodiment, the composite method of the hot-melt resin layer 7 can use a melt co-extrusion method, including: contacting the hot-melt inner layer adhesive resin and the hot-melt resin with the side of the inner anti-corrosion layer 5 relative to the intermediate metal layer 1 by co-extrusion, so that the inner anti-corrosion layer 5 relative to the intermediate metal layer 1 sequentially forms a hot-melt inner layer adhesive layer 6 and a hot-melt resin layer 7. In another preferred embodiment, the hot-melt resin layer 7 can be composited by a thermal bonding method, including: dissolving a resin main agent with a melting point above 100°C and a curing agent in an aqueous solvent or an organic solvent to form an aqueous solution type inner layer adhesive; applying the aqueous solution type inner layer adhesive to the side of the inner anti-corrosion layer 5 relative to the intermediate metal layer 1, and drying it to obtain a solution type inner layer adhesive layer 6; and thermally composite the solution type inner layer adhesive layer 6 and the hot-melt resin layer 7 at a certain temperature and pressure. The obtained composite product includes: an outer base resin layer 3, an outer adhesive layer 4, an outer anti-corrosion layer 2, an intermediate metal layer 1, an inner anti-corrosion layer 5, an inner adhesive layer 6, and a hot-melt resin layer 7 in sequence along an extension direction. In another preferred embodiment, in order to enhance the bonding strength between the intermediate metal layer 1 and the heat-melting resin layer 7 to avoid peeling between the two, the heat-melting resin layer 7 and the inner adhesive layer 6 can be subjected to heat treatment at a temperature not exceeding the melting point (60°C) of the inner adhesive layer 6 after the heat-melting resin layer 7 and the inner adhesive layer 6 are compounded. In another preferred embodiment, the heat-melting resin layer 7 can be formed by extrusion or using a film. Preferably, when a film is used, the bonding surface of the heat-melting resin layer 7 on the side in contact with the inner adhesive layer 6 is pre-corona treated.
[0070] Preferably, the anti-corrosion liquid can be coated on the surface of the intermediate metal layer 1 by rod coating, roller coating, gravure coating, or dipping, and then the anti-corrosion liquid is dried at high temperature to react with the surface of the intermediate metal layer 1 at high temperature. In a preferred embodiment, the coating amount of the anti-corrosion liquid on the intermediate metal layer 1 is in the range of 1.6 to 3.2 g / m 2, but not limited thereto; and the heating temperature after the anti-corrosion liquid is applied is 120 to 200°C, and the heating time is 0.5 to 5 minutes, but not limited thereto. Specifically, after heat treatment, the water and solvent in the anti-corrosion liquid can be volatilized, and the contact amount between the trivalent chromium compound, the inorganic acid, and the organic resin can be increased. Therefore, a cross-linking reaction is easily generated between the trivalent chromium compound, the inorganic acid, and the organic resin to form a cross-linked network structure, wherein it can be understood that the obtained cross-linked network structure is the anti-corrosion layer. In addition, since the surface of the intermediate metal layer 1 is activated by reaction with the inorganic acid, the adhesion between the anti-corrosion layer and the intermediate metal layer 1 can be further improved, making it difficult for the two to peel off or fall off.
[0071] Preferably, the water content in the inner anti-corrosion layer 5 will affect the degree of cross-linking reaction between the trivalent chromium compound, the inorganic acid, and the organic resin. If the water content in the inner anti-corrosion layer 5 is low, the volatilization amount of water is small during the high-temperature heating process, so that the cross-linking reaction is incomplete, and a cross-linked network structure with a low cross-linking density is formed. Specifically, in this state, the electrolyte 8 and hydrofluoric acid coated inside the lithium-ion battery can easily penetrate into the inner anti-corrosion layer 5, so that the cross-linked network structure is dissolved or destroyed, and finally the electrolyte 8 and hydrofluoric acid contact the intermediate metal layer 1, so that the intermediate metal layer 1 is corroded; and the adhesion strength between the intermediate metal layer 1 and the heat-melting resin layer 7 is greatly reduced. Therefore, it can be understood that it is necessary to effectively control the water content in the inner anti-corrosion layer 5 so that the inner anti-corrosion layer 5 has a certain corrosion resistance, so as to stabilize the adhesion between the intermediate metal layer 1 and the heat-melting resin layer 7. In addition, water vapor, acidic chemicals, alkaline chemicals, hydrogen sulfide, or corrosive gases or salts outside the lithium-ion battery will come into contact with the outer anti-corrosion layer 2 after passing through the outer substrate resin layer 3. If the cross-linking density of the outer corrosion layer is too low, the outer anti-corrosion layer 2 will also be dissolved by the corrosive components, causing the intermediate metal layer 1 to be corroded, thereby reducing the bonding strength between the intermediate metal layer 1 and the outer substrate resin layer 3, and easily causing peeling. Specifically, when peeling occurs between the intermediate metal layer 1 and the outer substrate resin layer 3 or the heat-melting resin layer 7, and the intermediate metal layer 1 is exposed to corrosive components, it is easy to cause fractures or pinholes. It can be understood that if the electrolyte 8 located inside the lithium-ion battery leaks due to the fracture of the intermediate metal layer 1, it may be dangerous to the user or cause mechanical equipment loaded with the lithium-ion battery to malfunction. Therefore, the water content contained in the anti-corrosion layer is effectively maintained, the outer substrate resin layer 3 and the heat-melting resin layer 7 are tightly bonded to the intermediate metal layer 1, and the intermediate metal layer 1 is protected, so as to effectively avoid dangers or accidents when using lithium-ion batteries.
[0072] In addition, when the degree of cross-linking reaction is low, the organic resin in the anti-corrosion layer will have a strong adhesiveness. Specifically, when the adhesiveness of the organic resin is high, foreign matter will adhere to the surface of the intermediate metal layer 1, resulting in pinholes; or when the organic resin contacts the roller in the processing device, the anti-corrosion layer is easily peeled off from the surface of the intermediate metal layer 1, resulting in its inability to exhibit sufficient anti-corrosion function and inability to form a stable and strong adhesion with the intermediate metal layer 1. It can be understood that when the anti-corrosion layer cannot effectively adhere to the surface of the intermediate metal layer 1, in a high temperature and high humidity environment, the intermediate metal layer 1 is easy to delaminate from the outer base material resin layer 3; or the intermediate metal layer 1 is easy to delaminate from the heat-welding resin layer 7, resulting in a shortened service life of the lithium-ion battery.
[0073] When the water content in the anti-corrosion liquid is too high, during the high-temperature heating process, the water content in the anti-corrosion liquid will be too much volatilized, which will increase the cross-linking reaction and increase the density and hardness of the cross-linked network structure. Specifically, when the density of the formed cross-linked network structure is too high or the hardness is too large, the mechanical properties of the anti-corrosion layer will not match the mechanical properties of the intermediate metal layer 1, so that during the processing of the metal-plastic composite film, the anti-corrosion layer is easily peeled off from the intermediate metal layer 1, and delamination will occur between the heat-welding resin layer 7 or the outer substrate resin layer 3 and the intermediate metal layer 1. In addition, when the moisture content in the anti-corrosion liquid is high, it will directly affect the performance of the anti-corrosion layer produced, including: when the electrolyte 8 in the battery penetrates the heat-melting resin layer 7 and the inner adhesive layer 6 and contacts the anti-corrosion layer, the electrolyte 8 will react with the remaining moisture in the anti-corrosion layer to produce hydrofluoric acid, among which: the hydrofluoric acid will directly dissolve and destroy the inner anti-corrosion layer 5, and will also dissolve the surface of the intermediate metal layer 1, thereby reducing the adhesion strength between the intermediate metal layer 1 and the heat-melting resin layer 7, causing the intermediate metal layer 1 and the heat-melting resin layer 7 to easily peel off.
[0074] Preferably, in order to avoid peeling between the intermediate metal layer 1 and the outer substrate resin layer 3 or the heat-welding resin layer 7, the water content in the anti-corrosion liquid needs to be controlled. Specifically, the water content in the anti-corrosion liquid should be between 0.5 and 65 mg / m 2 In the range of 0.5 to 49 mg / m 2 In a preferred embodiment, the residual amount of water contained in the anti-corrosion layer is affected by the temperature and heating time of the heat treatment. Specifically, when the coating range of the anti-corrosion liquid on the intermediate metal layer 1 is 1.6 to 3.2 g / m 2Under the conditions of , when heat treatment is carried out at a high temperature of 120 to 200°C for 0.5 to 5 minutes, the residual water content in the formed anti-corrosion layer is within an appropriate range. Therefore, it can be understood that in the metal-plastic composite film, controlling the residual water content in the anti-corrosion layer within an appropriate range can prevent the electrolyte and hydrogen fluoride generated by the reaction with water from corroding the surface of the intermediate metal layer 1; prevent the intermediate metal layer 1 from being separated from the heat-welding resin layer 7; prevent the moisture, acidic chemicals, alkaline chemicals, hydrogen sulfide, corrosive gases or salts outside the lithium-ion battery from corroding the intermediate metal layer 1; prevent the intermediate metal layer 1 from being separated from the outer substrate resin layer 3; and maintain the uniformity of the surface of the intermediate metal layer 1, so that its adhesion (wettability) changes little.
[0075] Preferably, the following specifically provides the relevant content of "internal corrosion protection layer 5". Specifically, based on the total weight of the internal corrosion protection layer 5, the carbon content contained in the outermost layer of the internal corrosion protection layer 5 relative to the intermediate metal layer 1 is c, and 40wt%≤c≤100wt%, and the content of the metal element from the intermediate metal layer 1 is d1, and d1≤5wt%; in the layered structure of the inner corrosion protection layer 5 relative to the outermost layer of the intermediate metal layer 1 moving 20nm toward the middle gold intermediate metal layer 1, the content of the metal element from the intermediate metal layer 1 is d2, and 10wt%≤d2≤70wt%; in the layered structure of the inner corrosion protection layer 5 relative to the outermost layer of the intermediate metal layer 1 moving 40nm toward the middle gold intermediate metal layer 1, the content of the metal element from the intermediate metal layer 1 is d3, and 20wt%≤d3≤100wt%. Among them, if c<40wt% or d1>5wt%, the bonding strength between the inner anti-corrosion layer 5 and the inner adhesive layer 6 will be unstable, which may be affected by the electrolyte 8 and cause the peel strength to decrease during the storage process; or due to the increase in the metal element content, the insulation of the inner anti-corrosion layer 5 is reduced, wherein: when the insulation of the inner anti-corrosion layer 5 is reduced, the life of the lithium-ion battery made of the inner anti-corrosion layer 5 will be reduced; or due to the metal-plastic composite film and the electrical short circuit inside the battery, the electrolyte 8 will leak.
[0076] Preferably, after the intermediate metal layer 1 with the inner anti-corrosion layer 5 is formed and compounded with the inner adhesive layer 6 and the hot-melt resin layer 7, the metal-plastic composite film is immersed in an electrolyte 8 containing 1000PPM of water for 5 days to observe the fluorine content contained in the inner anti-corrosion layer 5, wherein: the electrolyte 8 contains an EC mixed solvent, a DEC mixed solvent, and a DMC mixed solvent containing 1mol / L LiPF6, and the weight ratio of the EC mixed solvent, the DEC mixed solvent, and the DMC mixed solvent is 1:1:1. After the metal-plastic composite film is immersed, based on the total weight of the inner anti-corrosion layer 5, the layered structure of the inner anti-corrosion layer 5 moving 20nm relative to the outermost layer of the intermediate metal layer 1 toward the side where the inner anti-corrosion layer 5 contacts the intermediate metal layer 1 contains fluorine elements, wherein the content of the fluorine elements is e1, and 30wt%≥e1, and 2≥e1 / d2; the layered structure of the inner anti-corrosion layer 5 moving 40nm relative to the outermost layer of the intermediate metal layer 1 toward the side where the inner anti-corrosion layer 5 contacts the intermediate metal layer 1 contains fluorine elements, wherein the content of the fluorine elements is e2, and 20wt%≥e2, and 1≥e2 / d3. Specifically, if e1>30wt%, the tilt distribution in the inner anti-corrosion layer 5 will be uneven, resulting in a reduction in the resin component, and the bonding strength between the inner anti-corrosion layer 5 and the inner adhesive layer 6 will tend to be unstable. In a preferred embodiment, if e1 / d2>2, the corrosion effect of the inner anti-corrosion layer 5 in suppressing the hydrogen fluoride generated by the reaction of the electrolyte 8 and water will be reduced, and under long-term storage, the peel strength of the inner adhesive layer 6 and the intermediate metal layer 1 will be greatly reduced, making the two easy to separate. In another preferred embodiment, if e2>20wt%, the reaction product between the inner anti-corrosion layer 5 and the intermediate metal layer 1 will be reduced, so that during long-term storage, the peel strength between the inner adhesive layer 6 and the intermediate metal layer 1 may be greatly reduced. In another preferred embodiment, if e2 / d3>1, the corrosion effect of the inner anti-corrosion layer 5 in suppressing the hydrogen fluoride generated by the electrolyte 8 will be reduced, so that during long-term storage, the peel strength between the inner adhesive layer 6 and the intermediate metal layer 1 will be greatly reduced.
[0077] Preferably, the carbon content of the inner anti-corrosion layer 5 on the side relative to the intermediate metal layer 1 is high, but as it gets closer to the intermediate metal layer 1, the content of the metal elements contained in the inner anti-corrosion layer 5 gradually increases, forming an inclined structure, so that the inner anti-corrosion layer 5 can maintain a certain bonding strength with the heat-melting resin layer 7, and even if the inner anti-corrosion layer 5 contacts the electrolyte 8, the electrolyte 8 is infiltrated, or the electrolyte 8 reacts with water to produce corrosive hydrogen fluoride, it still has the ability to inhibit the penetration of hydrogen fluoride to prevent hydrogen fluoride from corroding the intermediate metal layer 1. In a preferred embodiment, in order to inhibit the penetration of hydrogen fluoride and the electrolyte 8, the inclined structure is a cross-linked structure, wherein: in order to form the cross-linked structure, an anti-corrosion liquid containing specific components is used to react with the intermediate metal layer 1; and a specific heat treatment process is used to dry the anti-corrosion liquid to form an inner anti-corrosion layer 5 with protective ability. It can be understood that when the heat treatment conditions are not appropriate, sufficient adaptability to the battery contents cannot be obtained. In another preferred embodiment, in the inner anti-corrosion layer 5, the ratio of the fluorine element (F) to the metal element (e1 / d2 or e2 / d3) refers to: the content of the metal element in the inner anti-corrosion layer 5 is detected by (XPS-ESCA method), and its value is set to 1, and the value of the fluorine (F) element relative to the metal element is obtained to obtain the ratio of the two. In another preferred embodiment, the "metal element" refers to the element composition constituting the intermediate metal layer 1. Specifically, when the anti-corrosion liquid contacts the intermediate metal layer 1, part of the elements of the intermediate metal layer 1 will dissolve in the anti-corrosion liquid, so the "metal element" that is the same as the element of the intermediate metal layer 1 can be detected in the anti-corrosion liquid.
[0078] Preferably, in the metal-plastic composite film of the present invention, and the preparation method or steps thereof, in addition to controlling the moisture residue of the anti-corrosion layer, it is also necessary to control the elements and element content in the anti-corrosion layer. Wherein, the "content of metal elements" refers to the metal elements mixed into the anti-corrosion layer by the intermediate metal layer 1 when the intermediate metal layer 1 and the anti-corrosion layer undergo a cross-linking reaction. In a preferred embodiment, if b1>30wt%, it means that the degree of cross-linking reaction inside the outer anti-corrosion layer 2 is too high. At this time, the outer anti-corrosion layer 2 will be hard and brittle, resulting in low composite strength, and in the subsequent molding process of the composite film, the outer anti-corrosion layer 2 is prone to cracking or pinholes; and the heat and moisture resistance are not good, resulting in easy stratification between the outer substrate resin layer 3 and the outer anti-corrosion layer 2. In another preferred embodiment, the carbon content can ensure the bonding stability between the intermediate metal layer 1 and the outer substrate resin layer 3, or between the intermediate metal layer 1 and the hot melt resin layer 7. It can be understood that if the adhesion is unstable, the lithium-ion battery will be easily peeled off from the outer substrate resin layer 3 or the hot melt resin layer 7 when stored for a long time in a high temperature or high humidity environment.
[0079] Preferably, the content of metal elements contained in the anticorrosion layer changes with the distance from the intermediate metal layer 1. When the specific position in the anticorrosion layer is closer to the intermediate metal layer 1, the content of metal elements contained will be higher, the adhesion to the intermediate metal layer 1 will be stronger, and the ability to resist the penetration of external moisture will be better. It must be noted that if b1>30wt%; or b2>70wt%, it means that the cross-linking reaction between the intermediate metal layer 1 and the anticorrosion liquid is excessive, resulting in the hardness of the outer anticorrosion layer 2 formed on the surface of the intermediate metal layer 1 being too high and the brittleness being too large. If it is used for the subsequent processing of lithium ion packaging materials in this state, the outer anticorrosion layer 2 is prone to rupture or pinholes during the processing, resulting in the intrusion of external moisture into the outer anticorrosion layer 2, reducing the adhesion between the outer substrate resin layer 3 and the intermediate metal layer 1, and finally causing delamination between the outer substrate resin layer 3 and the intermediate metal layer 1. In addition, if a<40wt%, or b1>30wt%, the bonding strength between the outer anti-corrosion layer 2 and the outer base resin layer 3 will be unstable. When the two are affected by the external temperature and humidity, they are prone to peeling during storage. Therefore, it is understandable that if it is used as a battery packaging material, the quality and safety of the manufactured battery products may be insufficient, and accidents or dangers may occur during easy use or storage.
[0080] Preferably, the intermediate metal layer 1 may include a main component and a secondary component. Specifically, when the main component is aluminum, the secondary component may include: iron, nickel, copper, or silicon dioxide; when the main component is stainless steel, the secondary component may include: chromium, iron, or nickel, but not limited thereto. In a preferred embodiment, when the intermediate metal layer 1 is a steel plate, its main component is iron, and other alloy components may be added as secondary components; when the intermediate metal layer 1 is a nickel-plated steel plate, its main component is nickel, and other alloy components may be added as secondary components. In another preferred embodiment, when the elemental composition contained in the inner anti-corrosion layer 5 is determined, in addition to the metal elements from the intermediate metal layer 1, it also includes the constituent elements in the anti-corrosion layer and the electrolyte 8, such as: carbon (C), oxygen (O), nitrogen (N), chromium (Cr), phosphorus (P), silicon (Si), fluorine (F), titanium (Ti), zirconium (Zr), or cerium (Ce), but not limited thereto. In another preferred embodiment, sometimes a trace amount of metal elements are added to the material of the anticorrosive liquid. If the source of the metal elements in the anticorrosive liquid cannot be distinguished, all of them can be regarded as metal elements from the intermediate metal layer 1, so as to facilitate the measurement of the metal element content; or it can be assumed that the metal elements added to the anticorrosive liquid are uniformly dispersed in the anticorrosive liquid, and the amount of metal elements added to the anticorrosive liquid is subtracted from the total metal element content detected to obtain the content of the metal elements from the intermediate metal layer 1. In another preferred embodiment, the anticorrosive layer can be a single layer or multiple layers, wherein: when the anticorrosive layer is multi-layered, when determining the element content contained therein, it can be judged by the single layer in contact with the intermediate metal layer 1, or by the entire multi-layer anticorrosive layer.
[0081] Preferably, the anti-corrosion layer of the present invention is a thin film obtained by applying an anti-corrosion liquid to the intermediate metal layer 1. In a preferred embodiment, the anti-corrosion liquid contains a rare earth element oxide sol, an anionic polymer, a cationic polymer, or a combination thereof; or contains phosphoric acid, a phosphate, or a cross-linking agent that cross-links the polymer, but is not limited thereto. In another preferred embodiment, the rare earth element oxide sol refers to: microparticles of rare earth element oxide (for example, particles with an average particle size of less than 100 nm) dispersed in a liquid dispersion medium. In another preferred embodiment, the rare earth element oxide includes: cerium oxide, yttrium oxide, neodymium oxide, or lanthanum oxide, but is not limited thereto, and cerium oxide is preferred. In another preferred embodiment, the rare earth element oxide contained in the anticorrosive liquid can be used alone or in combination of two or more; as the liquid dispersion medium of the rare earth element oxide sol, it includes: water, alcohol solvent, hydrocarbon solvent, ketone solvent, ester compound solvent, or ether solvent, preferably water; and as the cationic polymer, it includes: polyethylene imine, a complex ion polymer complex formed by a polymer having polyethylene imine and carboxylic acid, a primary amine Graf To acrylic resin grafted with a primary amine on an acrylic main chain, polyacetic acid or its derivatives, or aminophenol, but not limited thereto, preferably poly (methyl) acrylic acid or its salt, or a co-polymer with (methyl) acrylic acid and its salt as the main component. In another preferred embodiment, the crosslinking agent is preferably a compound having an isocyanate chemical group, a glycidyl chemical group, a carboxyl chemical group, or an oxazoline chemical group; or a silane coupling agent, but not limited thereto.
[0082] Preferably, the anti-corrosion liquid is mainly an aqueous solution composed of a trivalent chromium compound, an inorganic acid, an organic resin, a titanium (Ti) compound or a zirconium (Zr) compound, an organic solvent, and water, wherein, based on the total weight of the anti-corrosion liquid, the proportions of the trivalent chromium compound, the inorganic acid, the organic resin, the titanium (Ti) compound, the zirconium (Zr) compound, the organic solvent and water are 1.9 to 6wt%, 0.3 to 6wt%, 0.6 to 6wt%, 0 to 0.6wt%, 0 to 2.8wt%, and 78.6 to 97.2wt%, respectively. In a preferred embodiment, the trivalent chromium compound at least includes: chromium nitrate or chromium fluoride; the inorganic acid at least includes: phosphoric acid, nitric acid, or hydrofluoric acid; the organic resin at least includes: acrylic resin, methacrylic resin, hydroxy acrylic resin, polyvinyl alcohol resin, olefin resin, or phenolic resin; the titanium (Ti) compound at least includes: titanium fluoride or titanium nitrate; the zirconium (Zr) compound at least includes: zirconium fluoride or zirconium nitrate; and the organic solvent at least includes isopropyl alcohol, ethanol, or ethylene glycol butyl ether. In another preferred embodiment, a crosslinking agent can be added to the anticorrosion liquid. Specifically, by adding a crosslinking agent to the anticorrosion liquid, the crosslinking density of the anticorrosion layer can be increased, the tolerance of the anticorrosion layer to hydrogen fluoride can be increased, and its own stability can be maintained. In another preferred embodiment, the crosslinking agent includes: an organic crosslinking agent, or an inorganic crosslinking agent, wherein: the inorganic crosslinking agent includes: a silicon dioxide compound, including: silicon dioxide; a zirconium compound, including: ammonium zirconium fluoride, or ammonium zirconium carbonate; a metal chelate, including: a titanium chelate; a metal salt, including: metal ions such as Ca, Al, Mg, Fe, or Zn. In another preferred embodiment, the organic crosslinking agent includes: an amino resin, a melamine resin, a phenolic resin, an epoxy compound, a blocked isocyanate compound, an oxazoline compound, a carbodiimide compound, a condensate of formaldehyde and a monoalcohol having 1 to 4 carbon atoms, or a condensate of carbolic acid and formaldehyde. Wherein, when the crosslinking agent is an inorganic crosslinking agent, or an organic crosslinking agent is used, including: amino resin, melamine resin, phenolic resin, epoxy compound, blocked isocyanate compound, oxazoline compound or carbodiimide compound, the amount of the crosslinking agent added is 0.1 to 50wt%, preferably 0.5 to 30wt%, based on the total solid content of the anti-corrosion liquid. In another preferred embodiment, when the content of the crosslinking agent is less than 0.5wt%, the corrosion resistance of the anti-corrosion layer cannot be effectively improved; when the content of the crosslinking agent exceeds 50wt%, the crosslinking density of the anti-corrosion layer is too large and too hard, therefore, in the process of subsequent molding and processing, the anti-corrosion layer is prone to cracking or peeling, resulting in a decrease in its corrosion resistance.In another preferred embodiment, when the cross-linking agent is a condensation product of formaldehyde and an alkyl alcohol having 1 to 4 carbon atoms, or a condensation product of carbolic acid and formaldehyde, and, based on the total weight of the solid components of the anti-corrosion liquid, when the added amount of the cross-linking agent is less than 0.01wt%, the corrosion resistance of the corrosion-resistant layer cannot be effectively improved by adding the cross-linking agent; and when the added amount of the cross-linking agent exceeds 1.0wt%, the cross-linking density of the anti-corrosion layer is too large and too hard. Therefore, during the subsequent molding process, the anti-corrosion layer is prone to cracking or peeling, resulting in a decrease in its corrosion resistance.
[0083] 5. Related embodiments of the intermediate metal layer 1.
[0084] Preferably, the function of the intermediate metal layer 1 includes: providing a barrier effect to prevent moisture from penetrating into the interior of the lithium battery. Wherein: the material of the intermediate metal layer 1 includes: at least one of aluminum alloy, stainless steel, titanium steel, and nickel-plated iron plate; and the structure includes: a single layer of metal foil, or a multi-layer metal foil stacked on each other. In a preferred embodiment, the metal foil is selected from the following group: aluminum alloy foil, nickel-plated iron plate, stainless steel foil, or a combination of the above. It can be understood that in order to improve the formability of the metal-plastic composite film, the aluminum alloy foil used is a soft aluminum alloy foil made of aluminum alloy after annealing, and iron metal can be added to the raw material of the aluminum alloy foil as needed to further improve the formability of the aluminum alloy foil; and in order to resist the erosion of the electrolyte 8 or avoid being decomposed by the electrolyte 8, silicon dioxide or magnesium metal can be added to the raw material of the aluminum alloy foil, but it is not limited to this. In another preferred embodiment, the types of the stainless steel foil include: austenitic; ferritic; austenite-ferrite dual phase; martensitic; or precipitation hardened stainless steel foil, but not limited thereto. In order to improve the formability of the metal-plastic composite film, austenitic stainless steel is selected to make the stainless steel foil, and the types of stainless steel used include: SUS304, SUS301, or SUS316L, and preferably SUS304. In another preferred embodiment, when the intermediate metal layer 1 is composed of one or more layers of metal foil, the thickness of the intermediate metal layer 1 should at least meet the minimum requirement for preventing moisture intrusion. Preferably, the thickness of the intermediate metal layer 1 is 9 to 200 μm, but not limited thereto. In another preferred embodiment, the thickness of the intermediate metal layer 1 does not exceed 100 μm, more preferably, does not exceed 50 μm, but not limited thereto.
[0085] Preferably, the intermediate metal layer 1 is a steel plate, and a nickel plating treatment is performed on the side of the steel plate in contact with the hot-melt resin layer 7, so that the steel plate has rust and corrosion resistance. It can be understood that after the nickel plating treatment, when an anti-corrosion layer is formed on the surface of the nickel-plated layer, the rust and corrosion resistance of the intermediate metal layer 1 can be significantly improved. In a preferred embodiment, the thickness of the nickel-plated layer is less than or equal to 20 μm, preferably 1 to 5 μm. Specifically, when the thickness of the nickel-plated layer exceeds 20 μm, although it can effectively improve the corrosion resistance of the intermediate metal layer 1, due to its excessive thickness, it is easily affected by the external pressure load and cracked, so that it loses its corrosion resistance function.
[0086] Preferably, when alloy components are added to the composition of the intermediate metal layer 1, the alloy components will be precipitated on the surface of the intermediate metal layer 1; or in the annealing step after the rolling process, the volatility of the rolling oil is affected. Therefore, in the adjustment of the alloy components, the surface cleanliness needs to be managed. Among them, the management method of surface cleanliness includes: using a wetting reagent to test wettability as an indicator, wherein the method mentioned in "National Standard of the People's Republic of China GB / T225638.5-2016, Aluminum Foil Test Method, Part 5: Detection of Wettability" can be adopted; or using the contact angle as an indicator, wherein the method mentioned in "National Standard of the People's Republic of China GB / T22638.9-2008, Aluminum Foil Test Method Part 9: Hydrophilicity Measurement" can be adopted.
[0087] Preferably, when the wettability is tested with a wetting agent as an indicator, the rating obtained should be greater than or equal to Class D, preferably greater than or equal to Class B; when the contact angle is used as an indicator, the contact angle when tested with pure water is less than 25°, preferably less than 20°, and more preferably less than 15°. Specifically, when the wettability rating is lower than Class D; or the contact angle exceeds 25°, the reactivity or initial adhesion between the intermediate metal layer 1 and the anti-corrosion layer will deteriorate. It can be understood that when the reactivity deteriorates, the reaction between the anti-corrosion layer and the intermediate metal layer 1 is insufficient, so the resistance to penetration of the battery electrolyte 8; and the resistance to hydrogen fluoride produced by the reaction between the electrolyte and water will decrease, resulting in the adhesion of the anti-corrosion layer to the intermediate metal layer 1 decreasing over time; the anti-corrosion layer dissolving; or the intermediate metal layer 1 and the anti-corrosion layer peeling off, resulting in a reduction in the service life of the battery. In addition, it can be understood that when the initial adhesion between the anti-corrosion layer and the intermediate metal layer 1 deteriorates, the same situation will occur.
[0088] In summary, in order to avoid the above-mentioned risks, the present invention suppresses the precipitation of alloy from the intermediate metal layer 1 by adjusting the alloy composition and the alloy ratio within a certain range; or makes it easy to manage the temperature and time conditions in the annealing step during rolling.
[0089] 6. Related embodiments of the inner adhesive layer 6.
[0090] In order to make the intermediate metal layer 1 and the hot-melt resin layer 7 bond tightly, an inner adhesive layer 6 can be formed between the two. Wherein, the hot-melt resin layer 7 comprises: polyolefin, cyclic polyolefin, carboxylic acid-modified polyolefin, carboxylic acid-modified cyclic polyolefin, methacrylic acid-modified polyolefin, acrylic acid-modified polyolefin, crotonic acid-modified polyolefin, or imide-modified polyolefin, but not limited thereto. In order to improve the bonding between the intermediate metal layer 1 and the hot-melt resin layer 7, wherein the modified polyolefin is preferably acrylic acid, methacrylic acid, maleic acid, anhydrous maleic anhydride, or polyamide. In a preferred embodiment, the resin component of the inner adhesive layer 6 may or may not contain a polyolefin main chain, wherein it preferably contains a polyolefin main chain. In order to test whether the resin constituting the inner adhesive layer 6 contains a polyolefin main chain, infrared spectroscopy or gas chromatography-mass spectrometry can be used for analysis, but the analysis method is not limited thereto.
[0091] Preferably, the inner adhesive layer 6 and the heat-melting resin layer 7 contain the same polyolefin and modified resin, wherein polypropylene resin or propylene and ethylene copolymer is preferred. In a preferred embodiment, in order to maintain the stability of the metal-plastic composite film during long-term use, the inner adhesive layer 6 comprises: acid-modified polyolefin and a resin of a curing agent. The acid-modified polyolefin is preferably maleic anhydride or acrylic acid-modified polyolefin; the purpose of the curing agent is to cure the acid-modified polyolefin, and epoxy curing agents, multifunctional isocyanate curing agents, carbodiimide curing agents, or oxazoline curing agents can be used, but are not limited thereto. Among them, the epoxy curing agent used is a compound having at least one epoxy group, but not limited to this; the multifunctional isocyanate curing agent used is a compound having two or more isocyanate groups in the molecule, but not limited to this; the carbodiimide curing agent used is a compound having at least one carbodiimide group (-N=C=N-) in the molecule, but not limited to this, among which a polycarbodiimide compound having at least two or more carbodiimide groups is preferred; the oxazoline curing agent used is a compound having an oxazoline skeleton, but not limited to this. Specifically, the epoxy curing agent includes: bisphenol A diglycidyl ether, modified bisphenol A diglycidyl ether, novolac glycidyl ether, glycerol polyglycidyl ether, or polyglycerol polyglycidyl ether; or the multifunctional isocyanate curing agent includes: isophorone diisocyanate (PDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), or the components after polymerization or addition of the above substances or the reaction products of such mixtures and other polymers. In another preferred embodiment, in order to improve the adhesion between the inner adhesive layer 6 and the hot-melt resin layer 7, the curing agent component used includes more than one compound.
[0092] Preferably, the function of the inner adhesive layer 6 is to act as an adhesive layer to tightly fix the materials on the corresponding two sides, and the thickness of the inner adhesive layer 6 is preferably 1 to 80 μm, more preferably 1 to 50 μm, but not limited thereto. In a preferred embodiment, the main components of the inner adhesive layer 6 include: a modified polyolefin resin, a polyolefin resin, a block copolymer polypropylene resin (B-PP) with a polypropylene (PP) content exceeding 50%, a random copolymer polypropylene resin (R-PP), a homopolymer polypropylene resin (H-PP), or a single layer or more than two layers of a film layer formed by a mixture of the above components. In another preferred embodiment, when the inner adhesive layer 6 is used to compound the intermediate metal layer 1 and the hot melt resin layer 7, the compounding method includes: a method of using a solution-type inner adhesive layer 6; or a method of using a hot melt inner adhesive resin layer, but not limited thereto. The raw materials of the solution-type inner adhesive layer 6 include: a main agent, including: acid-modified polyolefin resin; and a hardener, including: isocyanate, epoxy resin, oxazoline resin, triethylamine, N,N-dimethylethanolamine, or a combination of the above components. Specifically, the method for forming the solution-type inner adhesive layer 6 includes: a dissolving step, adding the main agent and the hardener into a solvent to dissolve to form a mixed liquid, wherein the solvent includes: water, ethanol, isopropanol, ethyl acetate, methyl ethyl ketone, toluene, methylcyclohexane, or a combination of the above; a coating step, uniformly coating the mixed liquid on the surface of the intermediate metal layer 1 on which the anti-corrosion layer has been formed; and a heating step, heating the mixed liquid coated on the metal surface to volatilize the solvent in the mixed liquid to form the inner adhesive layer 6. The thickness of the inner adhesive layer 6 is preferably 1 to 10 μm, and more preferably 1 to 5 μm, but not limited thereto. Among them, when the thickness of the inner adhesive layer 6 is less than 1 μm, due to the thin thickness, the bonding force between the intermediate metal layer 1 and the hot-melt resin layer 7 is reduced, and they cannot be tightly bonded; when the thickness exceeds 10 μm, although the bonding can be maintained, under the action of the curing agent reaction, the inner adhesive layer 6 will be too hard and the bending resistance will deteriorate, resulting in a decrease in the flexibility of the metal-plastic composite film, and when the bending state occurs, cracks may occur, causing peeling between the intermediate metal layer 1 and the hot-melt resin layer 7.
[0093] Preferably, in the solution-type inner layer adhesive, the melting point of the acid-modified polyolefin resin used is 60 to 155°C; the weight average molecular weight is 10,000 to 150,000; or the acid value is 0.5 to 200 mgKOH / g. In a preferred embodiment, the solution-type inner layer adhesive may not add a curing agent, wherein, in the absence of a curing agent, the components of the solution-type inner layer adhesive include: acid-modified polyolefin, and amine compounds, which are used as hardeners. Among them, the weight ratio of the acid-modified polyolefin to the amine compound is 10 to 125:1, preferably 15 to 50:1. In another preferred embodiment, in the acid-modified polyolefin, the acid used includes: maleic acid, fumaric acid, or methacrylic acid; and the amine compound is triethylamine, N, N-2 methylethanolamine, or a combination of the above. In another preferred embodiment, the acid-modified polyolefin is a polypropylene having a melting point above 110°C, and the content of polypropylene is above 50wt%. Among them, if the melting point is below 60°C, it will lead to low heat resistance, causing the intermediate metal layer 1 and the heat-melting resin layer 7 to peel off at high temperatures; if the melting point exceeds 155°C, although the heat resistance is good, when reacting with the curing agent, a hard resin layer will be formed, resulting in poor bending and reduced flexibility of the metal-plastic composite film, and it is easy to crack when bending, resulting in peeling between the intermediate metal layer 1 and the heat-melting resin layer 7. In another preferred embodiment, when the weight average molecular weight of the acid-modified polyolefin resin is below 10,000, in the heating step, although its fluidity is high, it will cause the thickness to be seriously thinned during heat sealing, resulting in reduced adhesion strength between the intermediate metal layer 1 and the heat-melting resin layer 7, and there is a problem of sealing, and even if a curing agent is added, this situation will still occur; when the weight average molecular weight of the acid-modified polyolefin resin exceeds 150,000, it will cause the resin layer to be too hard, thereby reducing the flexibility and bending resistance of the metal-plastic composite film, making it easy to crack when bending, or causing When the acid value of the acid-modified polyolefin resin is less than 0.5 mgKOH / g, the curing reaction points between the acid-modified polyolefin resin and the curing agent are small, resulting in unstable adhesion between the intermediate metal layer 1 and the thermally-fused resin layer 7; or when the acid value exceeds 200 mgKOH / g, the curing reaction of the curing agent is too intense, resulting in the resin layer being too hard, thereby reducing the flexibility and bending resistance of the metal-plastic composite film, making it easy to crack when bent, or causing peeling between the intermediate metal layer 1 and the thermally-fused resin layer 7.
[0094] Preferably, the inner adhesive layer 6 is a hot melt inner adhesive, wherein the melting point of the acid-modified polyolefin resin used in the hot melt inner adhesive layer 6 is 135 to 165° C., and the melt index (MFR) is 3 to 15 g / 10min at a temperature of 230° C. In a preferred embodiment, the thickness of the hot melt inner adhesive layer 6 is 2 to 80 μm, and preferably 5 to 50 μm; and the degree of modification of the acid-modified polyolefin resin used in the hot melt inner adhesive is 1% to 15%, and preferably 3% to 12%. Among them, when the melting point of the acid-modified polyolefin resin is below 135°C, heating in the heating step will cause the fluidity of the resin to increase, and during pressurized heat sealing, the thickness will be seriously thinned, which will reduce the adhesion strength between the intermediate metal layer 1 and the heat-welding resin layer 7, making the sealing unstable; and when the melting point is above 165°C, although the fluidity is relatively low during pressurized heat sealing and the heat resistance is improved, when it is compounded with the intermediate metal layer 1, it will cause an increase in thermal shrinkage, which will increase the internal stress and cause the adhesion ability of the hot-melt type inner layer adhesive to the intermediate metal layer 1 to decrease, and, in a long-term storage state, it may peel off from the intermediate metal layer 1, and due to the heating during heat sealing, further thermal shrinkage will occur, which will reduce the adhesion between it and the intermediate metal layer 1, causing the problem of low sealing strength.
[0095] Preferably, if the melt index (MFR) of the acid-modified polyolefin resin is lower than 3 g / 10 min at a temperature of 230°C, when it is extruded onto the intermediate metal layer 1 for compounding after hot melting, the extrusion film-forming property may be unstable; and if the melt index (MFR) is higher than 15 g / 10 min, the resin fluidity may increase during the heating step, and the thickness may be seriously reduced during pressurized heat sealing, thereby reducing the adhesion strength between the intermediate metal layer 1 and the heat-melting resin layer 7, and causing sealing problems. In a preferred embodiment, when the thickness of the hot melt type inner adhesive layer 6 is less than 2 μm, when it is compounded with the intermediate metal layer 1, it will not be able to absorb the heat shrinkage due to excessive heat shrinkage, and due to the increase of internal stress, the adhesion between it and the intermediate metal layer 1 will be reduced, and even the intermediate metal layer 1 will be peeled off during long-term storage; and when the thickness of the hot melt type inner adhesive layer 6 exceeds 80 μm, although there will be no physical property problems, it will lead to an increase in production prices, which is not in line with the actual benefits of mass production. In another preferred embodiment, when the modification degree of the hot melt type inner adhesive layer 6 is less than 1%, it will cause the adhesion between it and the intermediate metal layer 1 to be unstable; and when it exceeds 15%, although there will be no physical property problems, it will lead to an increase in production prices, which is not in line with the actual benefits of mass production.
[0096] 7. Related embodiments of the heat-welding resin layer 7.
[0097] Preferably, the heat-melting resin layer 7 is arranged in the innermost layer of the metal-plastic composite film, and its main function is to exert its heat-melting property to seal the battery assembly when assembling the battery. It can be understood that the heat-melting resin layer 7 is used as a heat-sealing layer. The resin contained in the heat-melting resin layer 7 is based on the principle that it can be heat-melted, including: polyolefins, acid-modified polyolefins, or resins containing polyolefin main chains, but not limited to this. Specifically, polyolefins include: low-density polyethylene; medium-density polyethylene; high-density polyethylene; linear low-density polyethylene; ethylene-α-olefin copolymers; homopolypropylene; polypropylene block copolymers, including: block copolymers of propylene and ethylene; random copolymers of polypropylene, including: random copolymers of propylene and ethylene; propylene-α-olefin copolymers; or ethylene-butene-propylene terpolymers. It can be understood that when used as a copolymer, the polyolefin resin can be a block copolymer; or a random copolymer, and the polyolefin resin used can be one or more of the above-listed ones. In a preferred embodiment, the resin contained in the heat-melting resin layer 7 is preferably polypropylene.
[0098] Preferably, the acid-modified polyolefin used is a polymer modified by block polymerization or graft polymerization of an acid component and a polyolefin. The acid-modified polyolefin is a copolymer formed by copolymerization of a polar molecule, including polyacrylic acid or methacrylic acid, and a polyolefin. In a preferred embodiment, the acid component used includes maleic acid, acrylic acid, itaconic acid, crotonic acid, maleic anhydride, itaconic anhydride, anhydrides of the above components, or a combination of the above components, wherein acrylic acid, maleic acid, anhydrides of the above components, or a combination of the above components are preferably used. In another preferred embodiment, the hot-melt resin layer 7 may be a single-layer structure or a multi-layer structure; and its components may include one or more resins, wherein when its structure is multi-layer, the resin material of each layer may be the same or different.
[0099] Preferably, in order to improve the formability of the metal-plastic composite film, a lubricant may be added to the heat-melting resin layer 7. The lubricant may be any product disclosed in the current public information, without any particular limitation, and one or more lubricants may be used. In a preferred embodiment, an amide lubricant is preferably used, and is preferably used on the surface of the heat-melting resin layer 7. When the surface of the heat-melting resin layer 7 is formed or coated with a lubricant, the content of the lubricant used is not particularly limited, and in order to improve the formability of the metal-plastic composite film, the content is preferably 10 to 50 mg / m 2 , more preferably 15 to 40 mg / m 2. It can be understood that the lubricant is formed by: seeping from the resin of the heat-melting resin layer 7 to its surface; or coating the lubricant on the surface of the heat-melting resin layer 7. In another preferred embodiment, the heat-melting resin layer 7 can achieve the function of sealing the battery assembly after heat-melting, and there is no special restriction on its thickness. The thickness of the heat-melting resin layer 7 is less than 100 μm, and more preferably 25 to 80 μm, but not limited thereto.
[0100] Preferably, an antioxidant can be added to the composition of the heat-melting resin layer 7 as required to suppress the risk of thermal degradation during the manufacturing process. Among them, the antioxidant can use the products disclosed in the current public information without special restrictions, and one or more antioxidants can be used. In a preferred embodiment, the composition of the inner heat-melting resin layer 7 includes: acid-modified polyolefin resin, homopolymer polypropylene resin, block copolymer polypropylene resin, random copolymer polypropylene resin, polyethylene resin, a single layer or a composite layer of a combination of the above, or a mixture of the above combination. In another preferred embodiment, the melting point of the resin used in the heat-melting resin layer 7 is 120 to 162°C, preferably 130 to 162°C; the MFR under the temperature condition of 230°C is 2 to 15g / 10min, preferably 3 to 12g / 10min; and the heat-melting resin layer 7 can be a single layer or multiple layers, and its thickness is 20 to 120μm, preferably 25 to 80μm. In another preferred embodiment, when the inner heat-melting resin layer 7 is a composite layer, the thickness of the resin on the other side in contact with the intermediate metal layer 1 is more than 2 μm; and the melting point is 130 to 152°C. Among them, when the melting point is below 120°C, its fluidity will increase during the heating step; during the pressurized heat sealing, its thickness will become thinner, resulting in a decrease in its adhesion to the intermediate metal layer 1, and when pressurized, the resin in the squeezed part inside the lithium battery will flow to the edge part that is not squeezed, and because the lithium battery is expanded, contracted, or bent, external forces may cause cracks, and the electrolyte 8 will penetrate into the intermediate metal layer 1 through the cracks, causing the insulation resistance of the heat-melting resin layer 7 to decrease, leakage to occur, or the battery life to be shortened.
[0101] Preferably, when the melting point of the resin used in the heat-welding resin layer 7 exceeds 162°C, its crystallinity will increase, resulting in a decrease in its fluidity during pressurized heat sealing. Although the heat resistance can be improved, a hard and brittle resin layer will be formed during heat sealing of a high-crystallinity resin. Specifically, under the action of external forces such as expansion and contraction of the lithium battery or bending processing, the heat-welding resin layer 7 will be prone to cracking, and the sealing property cannot be maintained stably for a long time. In a preferred embodiment, at a temperature of 230°C, when the MFR of the resin is lower than 2g / 10min, the fluidity of the resin will be low during pressurized heat sealing, so it is difficult to obtain stable sealing; when the MFR of the resin exceeds 15g / 10min, the fluidity of the resin will be too high during pressurized heat sealing, resulting in a serious thinning of the resin thickness, so it is also difficult to maintain stable sealing. In another preferred embodiment, when pressurization is performed, the resin in the squeezed part inside the lithium battery will flow to the edge part that is not squeezed. Under the influence of external factors such as expansion and contraction or bending of the lithium battery, the heat-melting resin layer 7 is likely to crack, and the electrolyte 8 will penetrate through the cracks to contact the intermediate metal layer 1, causing the insulation resistance of the heat-melting resin layer 7 to decrease, resulting in leakage, which will shorten the battery life.
[0102] Preferably, when the thickness of the heat-melting resin layer 7 is less than 20 μm, its thickness cannot fully cover the deviation of the mechanical processing dimensions of the battery assembly or the heat sealing device, or the deviation of the conditions, so it is impossible to obtain a uniform heat-melting part, and it is impossible to effectively maintain a stable and long-term sealing. In a preferred embodiment, when pressurized, the resin of the squeezed part inside the lithium battery will flow to the edge part that is not squeezed, making the thickness of the heat-melting resin layer 7 thinner, and under the action of external factors such as the expansion and contraction of the lithium battery or bending processing, it is easy to cause cracks in the heat-melting resin layer 7, and the electrolyte 8 penetrates through the cracks to contact the intermediate metal layer 1, causing the insulation resistance of the heat-melting resin layer 7 to decrease, and leakage occurs, resulting in a shortened battery life. In another preferred embodiment, when the thickness of the heat-melting resin layer 7 exceeds 120 μm, the amount of water vapor penetration will increase, causing more water inside the battery. When water reacts with the electrolyte 8 in the battery, gas will be generated, making the battery prone to expansion, rupture, or leakage, etc., reducing the battery life. In another preferred embodiment, when water reacts with the electrolyte 8, hydrogen fluoride will be generated, and excessive hydrogen fluoride will corrode the intermediate metal layer 1 that has been treated with corrosion resistance, resulting in a decrease in the adhesion strength between the intermediate metal layer 1 and the heat-melting resin layer 7, and creating the risk of electrolyte 8 leakage.
[0103] 8. The preparation method of the present invention.
[0104] The metal-plastic composite film of the present invention is formed by stacking a plurality of layered structures, wherein the metal-plastic composite film comprises in sequence along one direction: an outer substrate resin layer 3, an outer adhesive layer 4, an intermediate metal layer 1, an inner adhesive layer 6, and a hot-melt resin layer 7. It can be understood that the thickness of the outer substrate resin layer 3 and the intermediate metal layer 1 can be adjusted according to individual embodiments. In a preferred embodiment, the thickness of the outer adhesive layer 4 is preferably 3 μm, but is not limited thereto. In another preferred embodiment, an outer anti-corrosion layer 2 is formed between the intermediate metal layer 1 and the outer adhesive layer 4; and an inner anti-corrosion layer 5 is formed between the intermediate metal layer 1 and the inner adhesive layer 6.
[0105] Preferably, the preparation method of the metal-plastic composite film comprises: subjecting the outer substrate resin layer 3 film to corona treatment; applying the anti-corrosion liquid on the intermediate metal layer 1 to form an outer anti-corrosion layer 2 on one side of the intermediate metal layer 1 facing the outer substrate resin layer 3 film, and an inner anti-corrosion layer 5 on the other side; applying the outer layer adhesive liquid on the side of the outer anti-corrosion layer 2 facing the intermediate metal layer 1 to form an outer layer adhesive layer 4, wherein: the outer layer adhesive liquid is composed of a non-crystalline polyester polyol with a weight average molecular weight of 5000, a Tg of 50°C, and a hydroxyl value of 25 mg KOH / g, and a polyol with a weight average molecular weight of 20000, a Tg of -17°C, and a hydroxyl value of 8 mg The non-crystalline polyester polyol of KOH / g is mixed in a weight ratio of 3:2, and toluene diisocyanate (TDI) is added, and the NCO / OH ratio of the outer adhesive liquid is 6.2; and the outer adhesive layer 4 and the outer substrate resin layer 3 are thermally laminated and cured at a temperature of 80°C for 3 days to obtain a metal-plastic semi-finished composite film. In a preferred embodiment, the anti-corrosion liquid is added at every m 2 The amount coated on the intermediate metal layer 1 is 5 g, but not limited to this.
[0106] Preferably, the preparation method of the metal-plastic composite film further comprises: applying an inner adhesive liquid to the side of the inner anti-corrosion layer 5 relative to the intermediate metal layer 1 to form an inner adhesive layer 6; compounding the inner adhesive layer 6 with the hot-melt resin layer 7 to obtain a composite layer; and compounding the composite layer onto the metal-plastic semi-finished composite film by melt coextrusion, so that the inner adhesive layer 6 is in contact with the side of the inner anti-corrosion layer 5 relative to the intermediate metal layer 1. In a preferred embodiment, the inner adhesive liquid comprises: 60 wt% of anhydrous maleic anhydride modified random copolymer polypropylene with a melting point of 140°C and an MFR of 5 g / 10min at an environmental condition of 230°C; a melting point of 160°C, an MFR of 2.6 g / 10min at an environmental condition of 230°C, and a density of 0.87 g / cm 324 wt% of a copolymer elastomer of propylene and butene; a melting point of 130°C, an MFR of 9.5 g / 10 min at 230°C, and a density of 0.91 g / cm 3 The present invention relates to a mixture of 8 wt% of a crystalline copolymer elastomer of ethylene and propylene; and 8 wt% of a low-density polyethylene having a melting point of 105°C and an MFR of 12 g / 10min under an environmental condition of 230°C. The degree of modification of the random copolymer polypropylene by anhydrous maleic anhydride is 10%. In another preferred embodiment, the thickness of the inner adhesive layer 6 is 15 μm, and the thickness of the hot-melt resin layer 7 is 30 μm, but not limited thereto. In another preferred embodiment, the hot-melt resin layer 7 comprises: an inner hot-melt resin layer 7, which is in contact with the inner adhesive layer 6; and an outer hot-melt resin layer 7, which is formed on one side of the inner hot-melt resin layer 7 relative to the inner adhesive layer 6. Wherein: the composition of the inner heat-melting resin layer 7 comprises: 62wt% of random copolymer polypropylene with a melting point of 155°C and an MFR of 4g / 10min at an environmental condition of 230°C; 33wt% of non-crystalline propylene-based elastomer; and 5wt% of low-density polyethylene with a melting point of 110°C and an MFR of 7.5g / 10min at an environmental condition of 230°C; and the outer heat-melting resin layer 7 is composed of random copolymer polypropylene with a melting point of 155°C and an MFR of 15g / 10min at an environmental condition of 230°C. In another preferred embodiment, the thickness ratio of the inner heat-melting resin layer 7 to the outer heat-melting resin layer 7 is 8:2, but not limited thereto. In another preferred embodiment, the preparation method of the metal-plastic composite mold further comprises: a heat treatment step, when the composite layer and the metal-plastic semi-finished composite film are composited, the obtained composite is heat-treated at a temperature of 180°C for 2 seconds to obtain the metal-plastic composite film.
[0107] Preferably, the compounding method of the solution-type inner adhesive layer 6 comprises: forming a solution-type mixture with an anhydrous maleic anhydride-modified polypropylene solution having a weight average molecular weight of 80,000, a melting point of 80°C, and an acid value of 2 mg KOH / g and an aromatic isocyanate (HDI system, hexamethylene diisocyanate) solution at a solid ratio of 20:1; applying the solution-type mixture to the side of the inner anti-corrosion layer 5 relative to the intermediate metal layer 1, and drying it to form an inner adhesive layer 6 having a thickness of 4 μm; thermally compounding a 25 μm thick hot-melt resin layer 7 and the inner adhesive layer 6 at a temperature of 80°C; and performing an aging treatment at a temperature of 60°C for 7 days. In a preferred embodiment, before the hot-melt resin layer 7 and the inner adhesive layer 6 are compounded, the hot-melt resin layer 7 has been pre-corona treated.
[0108] In a preferred embodiment, the heat-melting resin layer 7 comprises: an inner heat-melting resin layer 7, which is in contact with the inner adhesive layer 6, wherein: the composition of the inner heat-melting resin layer 7 is composed of random copolymer polypropylene with a melting point of 145°C and an MFR of 7.5g / 10min under an environmental condition of 230°C; a medium heat-melting resin layer 7, which is formed on the side of the inner heat-melting resin layer 7 in contact with the inner adhesive layer 6, wherein: the composition of the medium heat-melting resin layer 7 is composed of: 40wt% of block copolymer polypropylene with a melting point of 162°C and an MFR of 2g / 10min under an environmental condition of 230°C; 40wt% of block copolymer polypropylene with a melting point of 160°C and an MFR of 5g / 10min under an environmental condition of 230°C; and a melting point of 130°C and an MFR of 9.5g / 10min under an environmental condition of 230°C, and a density of 0.91g / cm 3 The outer heat-melting resin layer 7 is in contact with the side of the middle heat-melting resin layer 7 opposite to the inner heat-melting resin layer 7, wherein the outer heat-melting resin layer 7 is composed of a random copolymer polypropylene having a melting point of 145°C and an MFR of 7.5 g / 10 min under an environmental condition of 230°C. In another preferred embodiment, the thickness ratio of the inner heat-melting resin layer 7, the middle heat-melting resin layer 7, and the outer heat-melting resin layer 7 is 1:8:1, but is not limited thereto.
[0109] 9. Related tests of the present invention on lithium battery composite packaging materials.
[0110] Preferably, the method for testing the moisture content in the anti-corrosion layer comprises: cutting the intermediate metal layer 1 after the anti-corrosion liquid is applied into pieces; and drying the cut intermediate metal layer 1 in a drying room, wherein: the moisture content of the intermediate metal layer 1 is measured in the drying room using a Karl Fischer moisture meter, wherein the instrument setting parameters are: temperature of 160°C, air flow rate of 50ml / min, blowing time of 600s, speed of 8 gears, pre-balance time of 40s, and pre-balance waiting time of 60s. After the above test method, the final moisture content in mg / m 2 The value is a unit of unit, wherein, because the moisture content of the intermediate metal layer 1 is zero, the moisture content obtained by the test represents the residual moisture content in the anti-corrosion layer. In a preferred embodiment, the above method is only applicable to the test of "intermediate metal layer 1 containing only outer anti-corrosion layer 2" or "intermediate metal layer 1 containing only inner anti-corrosion layer 5". In another preferred embodiment, multiple samples can be tested at the same time to obtain more accurate test results when the number of samples is large, wherein the number of samples is at least 5, but not limited to this. In a preferred embodiment, in the preparation process of the metal-plastic composite film, the moisture content in the anti-corrosion layer is preferably 0.5 to 65 mg / m2 , more preferably 0.5 to 49 mg / m 2 Only within the specified range can the anti-corrosion layer have sufficient corrosion resistance and structural strength.
[0111] Preferably, in the present invention, XPS (Axis supra, produced by Shimadzu, UK) is used to determine the element distribution in the anti-corrosion layer by ESCA method. In a preferred embodiment, the intermediate metal layer 1 is sputtered by Ar ions to form a surface of the anti-corrosion layer, wherein: the ion beam diameter of the Ar ions is 800 μm, the voltage is 15 KV, the ion beam sputtering depth is 5 nm, the sputtering rate is 3 nm / min, the number of sputterings is 7 times, the signal source detection depth is 5 nm, the detection limit is 1‰, and the number of detections is 8 times.
[0112] Preferably, in the finished product of the metal-plastic composite film, the test method of the initial peel strength between the intermediate metal layer 1 and the heat-melting resin layer 7 includes: preparing the finished product of the metal-plastic composite film into a straight strip of 100 (TD) * 15 (MD) mm; and using a tensile test device to test the peel strength between the intermediate metal layer 1 and the heat-melting resin layer 7, including: placing the peeled heat-melting resin layer 7 film in the upper clamping plate of the telescopic test device, and placing the intermediate metal layer 1 in the lower clamping plate, and then performing a T-shaped peeling with a peeling surface of 180° at a telescopic speed of 50 mm / min. In a preferred embodiment, the peel strength is read as follows: when the moving distance between the heat-melting resin layer 7 and the intermediate metal layer 1 is 50 mm, the average value of the peel strength between the moving distance of 10 mm and 40 mm is selected. In another preferred embodiment, multiple samples can be tested at the same time to obtain more accurate test results when the number of samples is large, wherein the number of samples is at least 5, but not limited thereto.
[0113] Preferably, the method of "anhydrous electrolyte resistance 8 test" of the finished metal-plastic composite film includes: directly immersing the finished metal-plastic composite film sample in a mixed solvent of dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethylene carbonate (EC) containing 1 mol / L LiPF6 at a temperature of 85°C for 3 days, and the weight ratio of the above components in the mixed solution is 1:1:1 based on the total weight of the mixed solvent; and after the immersion is completed, taking out the sample, washing it with water for 15 minutes, and wiping off the moisture on the surface of the sample, and then measuring the peel strength between the intermediate metal layer 1 and the thermally welded resin layer 7 by comparing with the initial peel strength test method.
[0114] Preferably, the method of "water resistance to electrolyte 8 test" of the finished metal-plastic composite film comprises: peeling the intermediate metal layer 1 and the heat-melting resin layer 7 of the finished metal-plastic composite film strip by 20 mm, then immersing it in a mixed solution of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethylene carbonate (EC) containing 1 mol / L Li PF6 and water accounting for 1000 PPM of the total mass of the electrolyte 8 at a temperature of 85°C for 3 days, wherein: in the above-mentioned mixed solution, except for water, the proportions of each component are the same; taking out the strip, washing it with water for 15 minutes, not wiping off the water, and then measuring the peel strength between the intermediate metal layer 1 and the heat-melting resin layer 7 according to the method of initial peel strength test. In a preferred embodiment, the test method is to peel it in a state where there is residual water between the intermediate metal layer 1 and the heat-melting resin layer 7, and measure the peel strength between the intermediate metal layer 1 and the heat-melting resin layer 7 from the pre-peeled part.
[0115] Preferably, in the present invention, a German KRUSS DSA25 contact angle measuring instrument is used to measure the water contact angle of the surface of the intermediate metal layer 1. Specifically, the test method includes: placing the intermediate metal layer 1 flat on the instrument workbench, injecting water drops on the intermediate metal layer 1 with a syringe, and recording the contact angle value when the water droplets just drip onto the surface of the intermediate metal layer 1, wherein: the water output of the syringe each time is controlled to be 2μml, and the liquid addition speed is 2.67μmL / s.
[0116] Preferably, in the present invention, the German Arcotest dyne pen is used to measure the dyne value of the intermediate metal layer 1. Specifically, the test method includes: using the German Arcotest dyne pen to draw two 10 cm long straight lines on the surface of the intermediate metal layer 1. If the straight line shrinks by more than 10% within 3 seconds, it means that the dyne value of the surface of the intermediate metal layer 1 does not reach the dyne value of the dyne pen, so it is necessary to select a dyne pen with a lower dyne value to re-measure until the intermediate metal layer 1 corresponds to the dyne value of the dyne pen.
[0117] Preferably, in order to test whether the metal-plastic composite film can still maintain its bonding strength when stored under harsh environmental conditions and avoid delamination between the intermediate metal layer 1 and the hot-melt resin layer 7, a high temperature and high humidity resistance test is performed. Specifically, the test method includes: preparing the finished metal-plastic composite film into a sheet of 92 (TD) * 76 (MD) mm; using a deep punching experimental device to form the metal-plastic composite film, wherein: the forming depth is 7 mm, the surface pressure of the formed metal-plastic composite film is 1 MPa, the forming time is 5 seconds, and the forming size is 62 (TD) * 46 ( MD) mm; after the metal-plastic composite film is formed, the sample is placed in a dark room, and the integrity of the sample is observed by a light source to confirm whether the four corners are damaged or cracked. If the sample is broken, it will be discarded and re-cut and molded until a good sample is selected; the groove of the punched part of the good sample is facing downward and set corresponding to the module, wherein: the size of the module is 61*45mm and the height is 5.5mm; and downward pressure is applied directly above the sample groove to deform the sample, wherein the deformation depth is 1.5mm. In addition, a constant temperature and humidity chamber is prepared, the temperature is adjusted to 65°C and the humidity is adjusted to 90%RH, and the above-mentioned deformed samples are placed in a constant temperature and humidity chamber and laid flat, and the samples are observed after 5 days, 10 days, and 30 days of placement respectively to detect whether floating occurs between the intermediate metal layer 1 and the heat-melting resin layer 7. It can be understood that in order to pursue detection efficiency or detection accuracy, multiple samples can be tested in parallel at the same time.
[0118] The following provides 6 sets of examples and 2 sets of comparative examples to show the influence of different parameter conditions on whether the battery packaging structure will produce floating and delamination. Among them: Examples 1 to 6 and Comparative Examples 1 to 2 are all coated with an anti-corrosion liquid at a rate of 5g / m 2 The wet film is uniformly coated on the side of the intermediate metal layer 1 that contacts the heat-soluble resin layer, and the anti-corrosion liquid is dried under different temperature conditions and heat treatment time. In order to clearly indicate the content of elements contained in each layer structure of the inner anti-corrosion layer 5, the inner anti-corrosion layer 5 is defined as the "first layer" relative to the outermost layer of the intermediate metal layer 1; the layered structure of the inner anti-corrosion layer 5 relative to the outermost layer of the intermediate metal layer 1 moving 20nm toward the direction of the intermediate metal layer 1 is defined as the "second layer"; and the layered structure of the inner anti-corrosion layer 5 relative to the outermost layer of the intermediate metal layer 1 moving 40nm toward the direction of the intermediate metal layer 1 is defined as the "third layer".
[0119] 10. The test results of Example 1 are provided below.
[0120] In this embodiment, the material used for the intermediate metal layer 1 is aluminum foil, and has the following characteristics: thickness of 40μm; water contact angle of 15°; 8021 series annealed metal; the side of the intermediate metal layer 1 in contact with the hot-melt resin layer 7 is anti-corrosion treated; and the anti-corrosion liquid used contains a cross-linking agent. As shown in Table 1 below, the test results obtained under various test conditions of Example 1 are shown, from which it can be seen that in the inner anti-corrosion layer 5, the proportion of the content of each layer of the elements contained, specifically, the content ratio of chromium nitrate, phosphoric acid, and acrylic resin on the surface of the intermediate metal layer 1 is 2:2:1; and the content of chromium (Cr) coated on the surface of the intermediate metal layer 1 is 15mg / m 2 In addition, in this embodiment, the inner adhesive layer is compounded with the heat-melting resin layer 7 by using a "solution-type inner adhesive layer compounding method".
[0121] Table 1
[0122]
[0123]
[0124] 11. The test results of Example 2 are provided below.
[0125] In this embodiment, the material used for the intermediate metal layer 1 is aluminum foil, and has the following characteristics: thickness of 40μm; water contact angle of 15°; 8021 series annealed metal; and the side of the intermediate metal layer 1 in contact with the heat-welding resin layer 7 is anti-corrosion treated. As shown in Table 2 below, the test results obtained under various test conditions in Example 2 are shown, from which it can be seen that in the inner anti-corrosion layer 5, the proportion of the content of each layer of the elements contained in each layer, specifically, the content ratio of chromium fluoride, hydrofluoric acid, and polyvinyl alcohol resin on the surface of the intermediate metal layer 1 is 2:1:5; and the content of chromium (Cr) coated on the surface of the intermediate metal layer 1 is 15mg / m 2 .
[0126] The inner adhesive layer is laminated with the heat-welding resin layer 7 by a "solution-type inner adhesive layer lamination method".
[0127] Table 2
[0128]
[0129]
[0130] 12. The test results of Example 3 are provided below.
[0131] In this embodiment, the material used for the intermediate metal layer 1 is aluminum foil, and has the following characteristics: thickness of 40μm; dyne value of 75dyn / cm; 8021 series annealed metal; and the side of the intermediate metal layer 1 in contact with the heat-welding resin layer 7 is anti-corrosion treated. As shown in Table 3 below, the test results obtained under various test conditions in Example 3 are shown, from which it can be seen that in the inner anti-corrosion layer 5, the proportion of the content of each layer of the elements contained in the inner anti-corrosion layer 5 is 2:2:1; and the content of chromium (Cr) coated on the surface of the intermediate metal layer 1 is 15mg / m 2 .
[0132] The inner adhesive layer is laminated with the heat-welding resin layer 7 by a "solution-type inner adhesive layer lamination method".
[0133] Table 3
[0134]
[0135] 13. The test results of Example 4 are provided below.
[0136] In this embodiment, the material used for the intermediate metal layer 1 is aluminum foil, and has the following characteristics: thickness of 40μm; dyne value of 75dyn / cm; 8021 series annealed metal; and the side of the intermediate metal layer 1 in contact with the heat-welding resin layer 7 is anti-corrosion treated. As shown in Table 4 below, the test results obtained under various test conditions in Example 4 are shown, from which it can be seen that in the inner anti-corrosion layer 5, the proportion of the content of each layer of elements contained, specifically, the content ratio of chromium fluoride, hydrofluoric acid, polyvinyl alcohol resin, and titanium fluoride on the surface of the intermediate metal layer 1 is 15:1:3:2; and the content of chromium (Cr) coated on the surface of the intermediate metal layer 1 is 15mg / m 2 .
[0137] The inner adhesive layer is compounded with the heat-welding resin layer 7 by a "melt-type inner adhesive layer compounding method".
[0138] Table 4
[0139]
[0140]
[0141] 14. The test results of Example 5 are provided below.
[0142] In this embodiment, the material used for the intermediate metal layer 1 is aluminum foil, and has the following characteristics: thickness is 33μm; water contact angle is 15°; it is 8021 series annealed metal; the intermediate metal layer 1 is cleaned by alkaline cleaning solution; and the side of the intermediate metal layer 1 in contact with the hot-melt resin layer 7 is anti-corrosion treated. As shown in Table 5 below, the test results obtained under various test conditions of Example 5 are shown, from which it can be seen that in the inner anti-corrosion layer 5, the proportion of the content of each layer of the elements contained, specifically, the content ratio of chromium nitrate, phosphoric acid, and acrylic resin on the surface of the intermediate metal layer 1 is 2:2:1; and the content of chromium (Cr) coated on the surface of the intermediate metal layer 1 is 15mg / m 2 .
[0143] The inner adhesive layer is laminated with the heat-welding resin layer 7 by a "solution-type inner adhesive layer lamination method".
[0144] Table 5
[0145]
[0146]
[0147] 15. The test results of Example 6 are provided below.
[0148] In this embodiment, the material used for the intermediate metal layer 1 is a nickel-plated steel plate, and has the following characteristics: thickness of 50 μm; water contact angle of 15°; intermediate metal layer 1 is cleaned by alkaline cleaning solution; and the side of the intermediate metal layer 1 in contact with the hot-melt resin layer 7 is treated with anti-corrosion. As shown in Table 6 below, the test results obtained under various test conditions of Example 6 are shown, from which it can be seen that in the inner anti-corrosion layer 5, the proportion of the content of each layer of the elements contained, specifically, the content ratio of chromium nitrate, phosphoric acid, and acrylic resin on the surface of the intermediate metal layer 1 is 2:2:1; and the content of chromium (Cr) coated on the surface of the intermediate metal layer 1 is 15 mg / m 2 .
[0149] The inner adhesive layer is compounded with the heat-welding resin layer 7 by a "melt-type inner adhesive layer compounding method".
[0150] Table 6
[0151]
[0152]
[0153] 16. The test results of Comparative Example 1 are provided below.
[0154] In this embodiment, the material used for the intermediate metal layer 1 is aluminum foil, and has the following characteristics: thickness of 40 μm; dyne value of 75 dyn / cm; 8021 series annealed metal; and the side of the intermediate metal layer 1 in contact with the heat-welding resin layer 7 is anti-corrosion treated. As shown in Table 7 below, the test results obtained under various test conditions for Comparative Example 1 are shown, from which it can be seen that in the inner anti-corrosion layer 5, the proportion of the content of each layer of the elements contained, specifically, the content ratio of chromium nitrate, phosphoric acid, and acrylic resin on the surface of the intermediate metal layer 1 is 1:2:1; and the content of chromium (Cr) coated on the surface of the intermediate metal layer 1 is 15 mg / m 2 Among them, in this comparative example, the inner adhesive layer is compounded with the heat-melting resin layer 7 by a "solution-type inner adhesive layer compounding method".
[0155] Compared with Examples 1 to 6, the heating condition for forming the inner anti-corrosion layer 5 in this comparative example is heating at 100° C. for 50 seconds, and the residual water content in the inner anti-corrosion layer 5 is as high as 71 mg / m 2 , which is higher than the result detected in the embodiment. In addition, in this comparative example, in the "first layer", the carbon content is 38wt%, which is low, and the metal element content from the intermediate metal layer 1 is 3.0wt%, which is low; in the "second layer", the metal element content from the intermediate metal layer 1 is 6.0wt%, which is low; and in the "third layer", the metal element content from the intermediate metal layer 1 is 12wt%, which is low. The above results show that the anti-corrosion liquid forms an unstable cross-linked network structure on the intermediate metal layer 1.
[0156] In addition, after the metal-plastic composite film was immersed in electrolyte 8 for 5 days, in the second layer, the ratio of the content of fluorine element contained to the content of metal element contained from the intermediate metal layer 1 was 3.5; in the third layer, the ratio of the content of fluorine element contained to the content of metal element contained from the intermediate metal layer 1 was 2.0, and the content of fluorine element contained was 32wt%, which was high. At this time, the initial peel strength between the intermediate metal layer 1 and the hot-melt resin layer 7 was 15.8 (N / 15mm); in the electrolyte 8 resistance test, under the condition of no water addition, the peel strength maintenance rate was 22%; and in the electrolyte 8 resistance test, under the condition of adding water, the peel strength maintenance rate was 11%. Compared with the embodiment, the peel strength maintenance rate of the comparative example is significantly lower.
[0157] In Example 2, the heating condition for forming the inner anti-corrosion layer 5 is heating at 120° C. for 50 seconds, and the residual water content in the obtained inner anti-corrosion layer 5 is 47 mg / m 2, which is the highest among all the embodiments, and is only lower than the value of Comparative Example 1. It can be seen from the test results of Example 2 and Comparative Example 1 that when the moisture content contained in the inner anti-corrosion layer 5 is lower, the maintenance rate of the electrolyte 8 resistance test is higher. In addition, the maintenance rate of the electrolyte 8 resistance test in Example 1 is the highest among all the tests, which is due to the fact that the anti-corrosion liquid in Example 1 contains a cross-linking agent. Therefore, it can be understood that the cross-linking agent can indeed improve the ability of the anti-corrosion layer to resist electrolyte 8 and hydrofluoric acid.
[0158] Table 7
[0159]
[0160]
[0161] 16. The test results of Comparative Example 2 are provided below.
[0162] In this embodiment, the material used for the intermediate metal layer 1 is aluminum foil, and has the following characteristics: thickness of 40 μm; water contact angle of 15°; 8021 series annealed metal; and the side of the intermediate metal layer 1 close to the heat-welding resin layer 7 is anti-corrosion treated. As shown in Table 8 below, the test results obtained under various test conditions for Comparative Example 2 are shown, from which it can be seen that in the inner anti-corrosion layer 5, the proportion of the content of each layer of the elements contained, specifically, the content ratio of chromium fluoride, hydrofluoric acid, and polyvinyl alcohol resin on the surface of the intermediate metal layer 1 is 2:1:5; and the content of chromium (Cr) coated on the surface of the intermediate metal layer 1 is 15 mg / m 2 Among them, in this comparative example, the inner adhesive layer is compounded with the heat-melting resin layer 7 by a "solution-type inner adhesive layer compounding method".
[0163] Compared with Examples 1 to 6, the heating conditions for forming the inner anti-corrosion layer 5 in this comparative example are heating at 500° C. for 300 seconds, and the residual water content in the inner anti-corrosion layer 5 is 0.5 mg / m 2 , which is lower than the result detected in the embodiment. In addition, in the present comparative example, in the "first layer", the carbon content is 55wt%, and the metal content from the intermediate metal layer 1 is 2.0wt%; in the "second layer", the metal content from the intermediate metal layer 1 is 50wt%; and in the "third layer", the metal content from the intermediate metal layer 1 is 80wt%. In addition, after the metal-plastic composite film is immersed in the electrolyte 8 for 5 days, in the second layer, the ratio of the content of the fluorine element to the content of the metal element from the intermediate metal layer 1 is 0.5; in the third layer, the ratio of the content of the fluorine element to the content of the metal element from the intermediate metal layer 1 is 0.4.
[0164] In this comparative example, the initial peel strength between the intermediate metal layer 1 and the heat-melting resin layer 7 is 15.6 (N / 15mm); in the electrolyte resistance test 8, the peel strength maintenance rate is 90% under the condition of no water addition; and in the electrolyte resistance test 8, the peel strength maintenance rate is 71% under the condition of adding water. It can be found that the peel strength maintenance rate of comparative example 2 is similar to that of the embodiment, so it can be understood that when the water content contained in the inner anti-corrosion layer 5 is too low, the peel strength between the intermediate metal layer 1 and the heat-melting resin layer 7 is not greatly affected. However, when the storage test is carried out under high temperature and high humidity environmental conditions, when the water content contained in the inner anti-corrosion layer 5 is too low, the phenomenon of delamination and floating between the intermediate metal layer 1 and the heat-melting resin layer 7 will occur. To sum up, it can be inferred that: when the moisture content in the inner anti-corrosion layer 5 is too low, causing its texture to be hard and brittle, it is not conducive to molding and is prone to cracking or pinholes. As a result, when stored in a harsh environment, moisture can easily invade the damaged parts of the inner anti-corrosion layer 5, causing stratification and floating between the intermediate metal layer 1 and the hot-melt resin layer 7.
[0165] Table 8
[0166]
[0167]
[0168] Compared with the prior art, the present invention has the following positive effects: in the process of preparing the metal-plastic composite film, the water content in the inner anti-corrosion layer 5 is controlled and the water content contained therein is controlled within a range of 0.5 to 65 mg / m 2 The range of the inner anti-corrosion layer 5 is as follows: since the residual water content contained in the inner anti-corrosion layer 5 can ensure that a large amount of water in the anti-corrosion liquid volatilizes, the trivalent chromium compound, the inorganic acid, the organic acid, and the cross-linking agent can fully produce a cross-linking reaction to increase the cross-linking density of the cross-linked network structure in the inner anti-corrosion layer 5. Since the cross-linked network structure of the inner anti-corrosion layer 5 has sufficient strength and density, when the electrolyte 8, hydrofluoric acid, or corrosive substances from the inside of the metal-plastic composite film passes through the hot-melt resin layer 7 and contacts the inner anti-corrosion layer 5, the inner anti-corrosion layer 5 can protect the intermediate metal layer 1 and prevent the above-mentioned corrosive substances from corroding the intermediate metal layer 1, so that the intermediate metal layer 1 and the hot-melt resin layer 7 have a stable adhesion, and are not easily separated by the storage environment or storage time of the battery. It can be understood that when the hot-melt resin layer 7 is tightly combined with the intermediate metal layer 1, the hot-melt resin layer 7 can buffer the stress on the intermediate metal layer 1 to avoid the intermediate metal layer 1 from breaking or pinholes, thereby extending the service life of the battery. In addition, the purpose of controlling the moisture content in the outer anti-corrosion layer 2 is roughly the same as that of the inner anti-corrosion layer 5, so it will not be elaborated here.
[0169] However, what is described above is only a preferred embodiment of the present invention, but it cannot be used to limit the patent protection scope of the present invention; therefore, all simple equivalent changes and modifications made according to the patent protection scope of the present invention and the contents of the specification still fall within the patent protection scope of the present invention.
Claims
1. A lithium battery composite packaging material with high corrosion resistance, characterized in that: Include: an intermediate metal layer; an inner anti-corrosion layer formed on one side of the intermediate metal layer, wherein the inner anti-corrosion layer contains 5 to 100 mg of chromium and 0.5 to 65 mg of water per square meter; as well as a heat-welding resin layer formed on a side of the inner anti-corrosion layer opposite to the intermediate metal layer; The inner anti-corrosion layer contains carbon, and the carbon content gradually decreases from the side of the inner anti-corrosion layer opposite to the intermediate metal layer to the side of the inner anti-corrosion layer in contact with the intermediate metal layer; wherein the inner anti-corrosion layer contains metal elements from the intermediate metal layer, and the content of the metal elements gradually decreases from the side of the inner anti-corrosion layer in contact with the intermediate metal layer to the side of the inner anti-corrosion layer opposite to the intermediate metal layer; and Wherein, in the layered structure on one side of the inner anti-corrosion layer relative to the intermediate metal layer, based on the total weight of the inner anti-corrosion layer, the carbon content is c, and the metal element content is d1, and 40 wt% ≤ c ≤100 wt%, and d1 ≤5 wt%; Wherein, after the lithium battery composite packaging material with high corrosion resistance is immersed in an electrolyte, the inner anti-corrosion layer further contains fluorine element, wherein: In a layered structure where the inner anti-corrosion layer is moved 20 nm toward the intermediate metal layer on one side of the inner anti-corrosion layer relative to the intermediate metal layer, based on the total weight of the inner anti-corrosion layer, the content of the fluorine element is e1, and the content of the metal element is d2, and e1≤30 wt%, 10 wt% ≤ d2 ≤70 wt%, and e1 / d2≤2; and In the layered structure where the inner anti-corrosion layer is moved 40 nm toward the intermediate metal layer on one side relative to the intermediate metal layer, the content of fluorine element is e2, and the content of metal element is d3, based on the total weight of the inner anti-corrosion layer, and e2≤20 wt%, 20 wt% ≤ d3 ≤100 wt%, and e2 / d3≤1.
2. The lithium battery composite packaging material with high corrosion resistance according to claim 1, characterized in that: It further comprises: an outer base resin layer formed on a side of the intermediate metal layer opposite to the inner anti-corrosion layer.
3. The lithium battery composite packaging material with high corrosion resistance according to claim 1, characterized in that: It further comprises: an outer adhesive layer formed on a side of the intermediate metal layer opposite to the inner anti-corrosion layer.
4. The lithium battery composite packaging material with high corrosion resistance according to claim 1, characterized in that: It further comprises: an inner adhesive layer formed between the inner anti-corrosion layer and the hot-melt resin layer.
5. The lithium battery composite packaging material with high corrosion resistance according to any one of claims 1 to 4, characterized in that: The inner anti-corrosion layer is formed by coating an anti-corrosion liquid on one side of the intermediate metal layer and heating and drying the anti-corrosion liquid.
6. The lithium battery composite packaging material with high corrosion resistance according to claim 5, characterized in that: The anti-corrosion liquid is heat-treated at a temperature of 120 to 200° C. for 0.5 to 5 minutes to dry the anti-corrosion liquid.
7. The lithium battery composite packaging material with high corrosion resistance according to claim 5, characterized in that: The components of the anti-corrosion liquid include: a solute including: a trivalent chromium compound, an inorganic acid, and an organic resin; and a solvent including: water or an organic solvent.
8. The lithium battery composite packaging material with high corrosion resistance according to claim 7, characterized in that: Based on the total weight of the anti-corrosion liquid, the weight ratio of the trivalent chromium compound, the inorganic acid, the organic resin, and the solvent is 1.9 to 6: 0.3 to 6: 0.6 to 6: 78.6 to 97.
2.
9. The lithium battery composite packaging material with high corrosion resistance according to claim 7, characterized in that: The solute further comprises a titanium compound, and the content of the titanium compound is 0 to 0.6 wt % based on the total weight of the anti-corrosion liquid; or the solute further comprises a zirconium compound, and the content of the zirconium compound is 0 to 2.8 wt % based on the total weight of the anti-corrosion liquid.
10. The lithium battery composite packaging material with high corrosion resistance according to claim 7, characterized in that: The components of the anti-corrosion liquid further include a cross-linking agent; the cross-linking agent includes: amino resin, melamine resin, phenolic resin, epoxy compound, blocked isocyanate compound, oxazoline compound, or carbodiimide compound; and the content of the cross-linking agent is 0.1 to 50 wt% based on the total weight of the solute.
11. The lithium battery composite packaging material with high corrosion resistance according to claim 7, characterized in that: The components of the anti-corrosion liquid further include a cross-linking agent; the cross-linking agent includes: a condensate of formaldehyde and an alkyl monohydric alcohol having 1 to 4 carbon atoms, or a condensate of carbolic acid and formaldehyde; and the content of the cross-linking agent is 0.01 to 1.0 wt % based on the total weight of the solute.
12. The lithium battery composite packaging material with high corrosion resistance according to claim 9, characterized in that: The trivalent chromium compound includes: chromium nitrate or chromium fluoride; the inorganic acid includes: phosphoric acid, nitric acid, or hydrofluoric acid; the organic resin includes: acrylic resin, methacrylic resin, hydroxy acrylic resin, polyvinyl alcohol resin, olefin resin, or fenaldehyde resin; the titanium compound includes: titanium fluoride or titanium nitrate; the zirconium compound includes: zirconium fluoride or zirconium nitrate; and the organic solvent includes: isopropyl alcohol, ethanol, or ethylene glycol butyl ether.
13. The lithium battery composite packaging material with high corrosion resistance according to any one of claims 1 to 4, characterized in that: The intermediate metal layer comprises: aluminum alloy, stainless steel, titanium steel, or nickel-plated iron plate.
14. A lithium battery, characterized in that: Include: A lithium battery composite packaging material with high corrosion resistance as claimed in claim 1; and An electrolyte is coated by the lithium battery composite packaging material with high corrosion resistance and contacts the side of the heat-welding resin layer opposite to the intermediate metal layer.
15. The lithium battery according to claim 14, characterized in that: Also includes: an outer base resin layer formed on a side of the intermediate metal layer opposite to the inner anti-corrosion layer; an outer adhesive layer formed on a side of the intermediate metal layer opposite to the inner anti-corrosion layer; or An inner adhesive layer is formed between the inner anti-corrosion layer and the thermal welding resin layer.