Application Number
CN202210625341.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-02
Publication Date
2024-11-15
Estimated Expiration
2042-06-02

AI Technical Summary

Technical Problem

In the miniaturization packaging process of existing quartz crystal resonators, the parallel sealing method causes the base ceramic to crack easily, and the high-temperature welding equipment is expensive, making it difficult to meet the packaging requirements of sizes below 1210 and 1008.

Method used

The top cover is preformed using gold-tin soldering. The Kovar substrate is ground, nickel-plated, and gold-plated, and etched to form a multi-microporous structure. It is then fused to the base at a low temperature using a gold-tin eutectic furnace to reduce the welding temperature.

Benefits of technology

It effectively avoids base cracking, reduces welding temperature and equipment costs, achieves miniaturized packaging, and improves welding reliability and airtightness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115001444B_ABST
    Figure CN115001444B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of resonators, and in particular, is a quartz crystal resonator gold-tin solder preformed upper cover and a manufacturing method thereof. The present invention comprises the following steps: S1, grinding the surface of the Kovar substrate once; S2, sequentially performing nickel plating and gold plating on the surface of the Kovar substrate, so that a nickel layer and a gold layer are sequentially formed on the surface of the Kovar substrate; S3, etching pretreatment is performed on the side of the Kovar substrate to which the gold-tin solder frame is welded in step S2; S4, the gold-tin solder frame is welded to the outer surface of the etched part of the Kovar substrate to obtain a preformed upper cover. The present invention adopts the method of pre-welding a gold-tin solder frame with a low welding temperature on the upper cover, so that the upper cover can be welded to the base at a relatively low temperature, which is convenient for preparing a resonator with a small package size, and the base will not crack.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of resonators, and in particular relates to a gold-tin soldering preformed upper cover of a quartz crystal resonator and a manufacturing method thereof. Background Art

[0002] With the development of electronic information technology, electronic products are developing towards miniaturization, low power consumption and high integration, especially smart phones, smart wearables and other products are getting smaller and smaller, and electronic devices must also be miniaturized and thin. As a key device in the field of communication technology, the package size of quartz crystal resonators is getting smaller and smaller, from 5032 and 3225 to 1612, 1210 and 1008. The package size of 3225 refers to the total thickness of the product is about 0.7 mm, and the package size of 1008 refers to the total thickness of the product is 0.25 mm.

[0003] The existing quartz crystal resonator upper cover and base are mainly welded together by parallel sealing. The principle is that the current flows out from one end of the welding wheel, passes through the metal welding ring (thickness is 0.2mm) on the upper cover body and the base, and then returns to the other end of the welding wheel to form a loop, and then the upper cover sealing edge generates a large contact resistance, which causes local heating to melt the upper cover. The melted upper cover and the metal welding ring formed integrally on the base are welded together to form an airtight cavity. When the package size reaches 1210 and 1008, the original parallel sealing method is no longer applicable. The main reason is that the upper cover surface is electroplated with a nickel layer, and it takes a temperature of more than 1450℃ to melt it, which is very high in heat. The thickness of the ceramic base plate of the resonator below 1210 size is only 0.1 mm. The high heat can easily cause it to crack, and it is impossible to form an airtight cavity after welding. Summary of the invention

[0004] In order to overcome the defects in the prior art, the present invention provides a quartz crystal resonator gold-tin solder preformed upper cover and a manufacturing method thereof. The present invention reduces the welding temperature with the base and can effectively avoid the ceramic base from cracking during welding.

[0005] To achieve one of the above purposes, the present invention adopts the following technical solution:

[0006] A method for manufacturing a gold-tin solder preformed upper cover of a quartz crystal resonator comprises the following steps:

[0007] S1. Grind the surface of the Kovar substrate once, because the base is ceramic, and the thermal expansion coefficient of the Kovar material is similar to that of ceramic;

[0008] S2, sequentially performing nickel plating and gold plating on the surface of the Kovar substrate, so that a nickel layer and a gold layer are sequentially formed on the surface of the Kovar substrate;

[0009] S3, performing etching pretreatment on the side of the Kovar substrate welded to the gold-tin solder frame in step S2, so that the outer size of the etched part of the Kovar substrate is consistent with the inner size of the gold-tin solder frame;

[0010] S4. A gold-tin solder frame is welded onto the outer peripheral surface of the etched portion of the Kovar substrate to obtain a preformed upper cover.

[0011] Preferably, the surface roughness Ra of the kovar substrate after grinding in step S1 is less than 0.05 μm.

[0012] Preferably, in step S2, the thickness of the nickel layer is 3-5 μm, and the thickness of the gold layer is 0.01-0.02 μm; both the nickel layer and the gold layer are made by a roll plating process.

[0013] Preferably, in step S3, the etching width of the etching portion is 0.2 mm-0.4 mm, and the etching depth is 0.02-0.05 μm.

[0014] Preferably, after the gold-tin soldering frame is welded to the Kovar substrate, the upper cover is subjected to secondary grinding to remove the gold-plated layer on other parts of the surface of the Kovar substrate upper cover and the oxide layer on the surface of the gold-tin soldering frame; the thickness of the gold-tin soldering frame is 10-15um.

[0015] Preferably, the grinding speed of the first grinding treatment is 450 rpm, the grinding time is 20 minutes, the volume ratio of the brown corundum abrasive of the grinder to the Kovar substrate is 20:1, and the total volume is 2L; the grinding speed of the second grinding treatment is 200 rpm, the grinding time is 30 minutes, the volume ratio of the cylindrical high-alumina porcelain abrasive of the grinder to the Kovar substrate after the gold-tin solder frame is fused is 30:1, and the total volume is 3L.

[0016] Preferably, the welding equipment in step S4 is a gold-tin eutectic furnace; the process route is to evacuate the furnace chamber of the gold-tin eutectic furnace, heat it to 250°C, fill the furnace chamber with formic acid for 3-5 minutes, and then heat it to 310°C-320°C at a rate of 1-2°C per second, keep it warm for 30 seconds, then cool it down to 100°C at a rate of 2-4°C per second and take it out of the furnace.

[0017] Preferably, the material of the gold-tin soldering frame is a tin-rich gold-tin eutectic material, and the weight content of gold in the gold-tin soldering frame is 78%-79.5%.

[0018] Preferably, the Kovar substrate and the gold-tin soldering frame need to be stamped before the Kovar substrate is subjected to a primary grinding process.

[0019] A second object of the present invention is to provide a gold-tin soldering preformed upper cover for a quartz crystal resonator.

[0020] The advantages of the present invention are:

[0021] (1) The present invention pre-welds a low-melting-point gold-tin solder frame onto a Kovar substrate (upper cover), so that the upper cover can be welded to the base at a relatively low temperature, thereby facilitating the preparation of a resonator with a small package size without causing the base to crack.

[0022] (2) The welding temperature between the existing base and the ordinary Kovar upper cover is above 1450°C. This is because the welding of the general ceramic base and the upper cover (the surface of the Kovar substrate is nickel-plated) is carried out by a parallel sealing machine, and the nickel-plated layer on the Kovar substrate has a high melting point. When welding with the base at a higher welding temperature, a large amount of heat will be generated, which can easily cause the thin base to crack. In the present invention, the temperature when the upper cover welded with the gold-tin solder frame is welded to the base is only 280-300°C. This is because the present invention welds the gold-tin solder frame to the upper cover of the Kovar substrate in advance instead of welding it to the base. The gold-tin solder has a low melting point and generates less heat, so the base is not easy to crack, thereby greatly reducing the influence of temperature on product performance. The packaging size of the resonator can be less than 1008. Moreover, the welding of the gold-tin solder upper cover and the base only requires a welding furnace, and the cost of the welding furnace is much lower than that of the parallel sealing machine, which greatly reduces the investment in expensive equipment and saves production costs.

[0023] (3) In the present invention, the surface roughness Ra of the kovar substrate after grinding is less than 0.05 μm, which is convenient for improving the wettability and infiltration of the kovar substrate; the nickel plating of the kovar substrate in the present invention can play an anti-corrosion role, and the gold plating layer can increase the wettability and infiltration of the welding surface, which is convenient for subsequent welding and improves the airtightness with the gold-tin solder frame; in the present invention, the surface of the upper cover is partially etched to remove the gold plating layer on its surface and to form a microporous hydrophobic structure with the nickel plating layer, so that the gold-tin solder frame can preserve the status quo of the solder ring after melting, and will not be spread or gathered together on the upper cover.

[0024] (4) The thickness of the nickel layer of the present invention is 3-5 μm, so that the nickel layer has a good protective ability to prevent the substrate from rusting; the gold-plated layer with a thickness of 0.01-0.02 μm can make the welding surface have just the right wettability. This is because too low wettability is not conducive to welding and tightness, while too high wettability will, firstly, lead to higher costs, and secondly, when the gold-tin solder frame is melted, the excessively thick gold will migrate into the gold-tin solder frame, which will affect the gold-tin composition ratio of the gold-tin solder frame, and further affect the melting point temperature during re-welding.

[0025] (5) The purpose of the first grinding in the present invention is to remove stamping burrs and correct surface roughness; the purpose of the second grinding is to remove the gold-plated layer on other parts of the upper cover surface (specifically, to remove the excess gold layer on the surface of the kovar substrate and the side wall) and recycle it, and at the same time, it can also remove oxides and impurities on the surface of the gold-tin solder frame after welding, so as to avoid the gold layer and oxides affecting the secondary welding.

[0026] (6) The gold-tin soldering frame and the upper cover are welded together in a eutectic furnace, which is a closed furnace chamber that needs to be evacuated to remove oxygen in the furnace chamber to prevent high-temperature oxidation. In addition, the furnace chamber is filled with formic acid because formic acid is reducing. The surfaces of the upper cover and the gold-tin soldering frame are more or less oxidized. Filling with formic acid can reduce the welding surface and increase the reliability of welding.

[0027] (7) The weight content of gold in the existing gold-tin eutectic material is 80%, and the balance is tin. However, as the gold content increases, the melting point of the eutectic material will also rise sharply. The gold content of the gold-tin solder frame in the present invention is 78%-79.5%. This is because in order to increase the wettability during welding, the surface of the upper cover has been plated with a 0.01-0.02μm gold layer. After the gold-tin solder frame is welded, the gold in the gold-plated layer will also migrate to the gold-tin solder frame. The gold content of 78%-79.5% can effectively avoid affecting the melting point temperature of the gold-tin solder frame during secondary welding, so that the melting point temperature of the gold-tin solder frame during secondary welding is maintained at 280℃-300℃. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of the cross-sectional structure of the present invention.

[0029] Figure 2 for Figure 1 A partial enlarged schematic diagram of the medium-sized kovable substrate.

[0030] Figure 3 This is a top view after secondary grinding treatment of the present invention.

[0031] Figure 4 It is a schematic diagram of the cross-sectional structure of the unfused gold-tin solder frame of the present invention.

[0032] Figure 5 for Figure 4 A partial enlarged schematic diagram of the medium-sized kovable substrate.

[0033] The meanings of the symbols in the figure are as follows:

[0034] 1- Kovar substrate, 2- Nickel layer, 3- Gold layer, 4- Gold soldering frame, 5- Laser etching area. DETAILED DESCRIPTION

[0035] like Figure 1-5 As shown, a method for manufacturing a gold-tin solder preformed upper cover of a quartz crystal resonator comprises the following steps:

[0036] S1, performing a grinding process on the surface of the kovar substrate 1;

[0037] Specifically, the Kovar substrate 1 and the gold-tin solder frame 4 need to be stamped before the first grinding treatment; the melting point of the Kovar substrate 1 is 200-310 degrees, which is close to the thermal expansion coefficient of the ceramic base; the grinder is a planetary centrifugal grinder (the grinder has high grinding efficiency, good consistency and uniformity, and the speed and abrasive can be adjusted to control the surface state of the product); the surface roughness Ra of the Kovar substrate 1 after grinding is less than 0.05μm; the grinding drum capacity of the grinder is 6L, the grinding speed is 450 rpm, the grinding time is 20 minutes, the volume ratio of brown corundum abrasive to product is 20:1, the total volume is 2L, and 50mL of LC-100 grinding liquid produced by Japan TIPION Company and 2L of water are added.

[0038] S2. The surface of the kovar substrate 1 is subjected to nickel plating and gold plating in sequence, so that a nickel layer 2 and a gold layer 3 are formed in sequence on the surface of the kovar substrate 1; the thickness of the nickel layer 2 is 3-5 μm, and the thickness of the gold layer 3 is 0.01-0.02 μm; the nickel layer 2 and the gold layer 3 are both made by a roll plating process.

[0039] S3. Perform etching pretreatment on one side of the kovar substrate 1 welded to the gold-tin solder frame 4 in step S2 (the purpose is to make its surface hydrophobic so that the gold-tin solder frame 4 will not spread out on the kovar substrate 1 after melting, so that the gold-tin solder frame 4 can maintain the status quo of the solder frame), so that the outer size of the etched part of the kovar substrate 1 is consistent with the inner size of the gold-tin solder frame 4; the etching width of the laser etched part is 0.2mm-0.4mm, and the etching depth is 0.02-0.05μm.

[0040] S4. The gold-tin soldering frame 4 is welded onto the outer surface of the etched portion of the kovar substrate 1, that is, the outer periphery of the gold-tin soldering frame 4 is consistent with the outer periphery of the kovar substrate 1, and the inner periphery of the gold-tin soldering frame 4 is consistent with the outer periphery of the etched portion, to obtain a preformed upper cover, and the welded kovar substrate 1 and the gold-tin soldering frame 4 are both subjected to secondary grinding treatment.

[0041] The secondary grinding treatment is, on the one hand, to remove the excess gold layer 3 on the surface and side wall of the Kovar substrate 1 to prevent the gold-tin solder frame 4 from spreading along the Kovar substrate 1 during the subsequent welding of the base; on the other hand, to remove the oxides generated on the surface of the gold-tin solder frame 4 during welding, thereby ensuring the reliability of the secondary welding (i.e., when the preformed upper cover is connected to the base, the gold-tin solder frame 4 on the Kovar substrate 1 is first melted so that the gold-tin solder frame 4 is welded to the metal welding ring on the base).

[0042] Furthermore, the welding equipment in the above step 4 is a gold-tin eutectic furnace; the process route is to evacuate the furnace of the gold-tin eutectic furnace, heat it to 250°C, fill the furnace with formic acid for 3-5 minutes, and then heat it to 310°C-320°C at a rate of 1-2°C per second, keep it warm for 30 seconds, and then cool it to 100°C at a rate of 2-4°C per second before taking it out of the furnace. The grinding drum capacity of the grinder is 6L, the grinding speed is 200 rpm, the time is 30 minutes, the volume ratio of the cylindrical high-aluminum porcelain abrasive to the Kovar substrate 1 is 30:1, the total volume is 3L, and 50 ml of LC-100 grinding liquid produced by Japan TIPION Company and 2L of water are added.

[0043] The material of the gold-tin soldering frame 4 is a tin-rich gold-tin eutectic material, that is, the tin content in the gold-tin eutectic material is relatively high, and the gold content of the gold-tin soldering frame 4 is 78%-79.5%.

[0044] It should be noted that the present invention also provides a method for connecting the base and the upper cover, that is, firstly welding the gold-tin soldering frame 4 to the metal soldering ring on the base, and then welding the other side of the gold-tin soldering frame 4 to the upper cover.

[0045] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for manufacturing a gold-tin solder preformed upper cover of a quartz crystal resonator, characterized in that: The steps include: S1, performing a grinding process on the surface of the kovar substrate (1); S2, sequentially performing nickel plating and gold plating on the surface of the kovar substrate (1), so that a nickel layer (2) and a gold layer (3) are formed on the surface of the kovar substrate (1); S3, performing etching pretreatment on the side of the Kovar substrate (1) welded to the gold-tin solder frame (4) in step S2, so that the outer dimensions of the etched portion of the Kovar substrate (1) are consistent with the inner dimensions of the gold-tin solder frame (4); S4, welding a gold-tin solder frame (4) onto the outer peripheral surface of the etched portion of the Kovar substrate (1) to obtain a preformed upper cover.

2. The method for manufacturing a gold-tin solder preformed upper cover of a quartz crystal resonator according to claim 1, characterized in that: In the step S1, the surface roughness Ra of the kovar substrate (1) after grinding is less than 0.05 μm.

3. The method for manufacturing a gold-tin solder preformed upper cover of a quartz crystal resonator according to claim 1, characterized in that: In step S2, the thickness of the nickel layer (2) is 3-5 μm, and the thickness of the gold layer (3) is 0.01-0.02 μm; the nickel layer (2) and the gold layer (3) are both produced by a roll plating process.

4. The method for manufacturing a gold-tin solder preformed upper cover of a quartz crystal resonator according to claim 1, characterized in that: The etching width of the etching part in step S3 is 0.2 mm-0.4 mm, and the etching depth is 0.02-0.05 μm.

5. The method for manufacturing a gold-tin solder preformed upper cover of a quartz crystal resonator according to claim 1, characterized in that: After the gold-tin soldering frame (4) is welded to the Kovar substrate (1), the gold-plated layer at other locations on the surface of the Kovar substrate (1) is subjected to secondary grinding treatment; the thickness of the gold-tin soldering frame (4) is 10-15 um.

6. The method for manufacturing a gold-tin solder preformed upper cover of a quartz crystal resonator according to claim 5, characterized in that: The grinding machines for the primary grinding process and the secondary grinding process are both planetary centrifugal grinding machines; the grinding speed of the primary grinding process is 450 rpm, the grinding time is 20 minutes, the volume ratio of the brown corundum abrasive of the grinding machine to the Kovar substrate (1) is 20:1, and the total volume is 2L; the grinding speed of the secondary grinding process is 200 rpm, the grinding time is 30 minutes, the volume ratio of the cylindrical high-alumina porcelain abrasive of the grinding machine to the Kovar substrate (1) after the gold-tin solder frame (4) is fused is 30:1, and the total volume is 3L.

7. The method for manufacturing a gold-tin solder preformed upper cover of a quartz crystal resonator according to claim 1, characterized in that: The welding equipment in step S4 is a gold-tin eutectic furnace; the process route is to evacuate the furnace of the gold-tin eutectic furnace, heat it to 250°C, fill the furnace with formic acid for 3-5 minutes, and then heat it to 310°C-320°C at a rate of 1-2°C per second, keep it warm for 30 seconds, then cool it down to 100°C at a rate of 2-4°C per second and take it out of the furnace.

8. The method for manufacturing a gold-tin solder preformed upper cover of a quartz crystal resonator according to claim 1, characterized in that: The material of the gold-tin soldering frame (4) is a tin-rich gold-tin eutectic material, and the weight content of gold in the gold-tin soldering frame (4) is 78%-79.5%.

9. The method for manufacturing a gold-tin solder preformed upper cover of a quartz crystal resonator according to claim 1, characterized in that: Before the primary grinding process of the Kovar substrate (1), the Kovar substrate (1) and the gold-tin soldering frame (4) need to be stamped.