HP295 welding bottle steel and production method and application thereof

By optimizing the continuous casting and rolling process and cooling treatment of thin slabs, the carbon content and yield ratio of HP295 welding cylinder steel is controlled, and the problem of the strip structure affecting the deep drawing performance in the existing process is solved, achieving low cost and low emissions production effect.

CN118996261APending Publication Date: 2024-11-22HUNAN VALIN LIANYUAN IRON & STEEL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411395589.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When the existing thin slab continuous casting and rolling process produces HP295 welded cylinder steel, the high carbon content and fine grains lead to strip-like structure, which affects the deep drawing forming performance. The traditional process has high carbon dioxide emissions and high cost.

Method used

By optimizing the continuous casting and rolling process of thin slabs, the carbon content is controlled between 0.16% and 0.18%, and a short process process is adopted, combined with laminar flow cooling and winding steps, the yield ratio is controlled between 0.7~0.78, reducing carbon dioxide emissions and reducing production costs. .

Benefits of technology

The low yield-strength ratio and good deep drawing forming performance of HP295 welded cylinder steel are achieved, which reduces production costs and carbon dioxide emissions, and improves production efficiency and product welding performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996261A_ABST
    Figure CN118996261A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of HP295 welding bottle steel, in particular to HP295 welding bottle steel and a production method and application thereof. The HP295 welding bottle steel comprises iron and further comprises, by mass, 0.16% < = C < = 0.18%, 0.08% < = Si, 0.7% < = Mn < = 0.9%, 0.005% < = S, 0.015% < = P, 0.015% < = Als < = 0.045%, 0.01% < = Ti < = 0.03% and 0.006% < = N. The yield ratio of the HP295 welding bottle steel is 0.7-0.78, and the banded structure of the strip steel is below the level 1.5. According to the production method, a thin slab continuous casting and rolling process is adopted, the production time is greatly shortened, the carbon emission is reduced by about 40% compared with that of a traditional process, and the production cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of HP295 welding bottle steel, and in particular to a HP295 welding bottle steel and a production method and application thereof. Background Art

[0002] Welded gas cylinder steel is a special type of steel material, which is commonly used in gas cylinders in the ambient temperature range of -40℃ to 60℃. It is a special material for steel welded gas cylinders that can repeatedly contain liquefied petroleum gas. For welded gas cylinder steel, it is required to have a certain strength and good comprehensive mechanical properties (such as forming performance, welding performance and low cold brittle transition temperature, etc.). Therefore, during production, there are very strict requirements on the yield strength ratio, strength range, thickness and uniformity of welded gas cylinder steel.

[0003] Compared with the traditional production line process, the thin slab continuous casting and rolling process has the advantages of slight center segregation of the slab, high direct furnace temperature and short heating time (thin decarburization layer), good thickness uniformity, low carbon dioxide emissions, etc. However, due to the high carbon content (to ensure a low strength-to-yield ratio and avoid peritectic reaction, etc.) and metallurgical problems such as fine grains designed for HP295 welding bottle steel in the thin slab continuous casting and rolling process, it is easy to cause the banded structure and high strength-to-yield ratio of HP295 welding bottle steel, which affects the deep drawing performance. Summary of the invention

[0004] To solve the above problems, the present application proposes HP295 welding bottle steel and its production method and application. The composition design of the HP295 welding bottle steel is combined with the production conditions to control the production so that the strength-to-yield ratio of the HP295 welding bottle steel is 0.7 to 0.78.

[0005] This application is implemented through the following technical solutions:

[0006] One of the purposes of the present application is to provide an HP295 welding bottle steel, which includes iron and the following components in mass fraction: 0.16%≤C≤0.18%, Si≤0.08%, 0.7%≤Mn≤0.9%, S≤0.005%, P≤0.015%, 0.015%≤Als≤0.045%, 0.01%≤Ti≤0.03%, and N≤0.006%.

[0007] The HP295 welding bottle steel provided in the present application has a yield strength ratio of 0.7 to 0.78, and a strip structure of the strip steel of less than grade 1.5.

[0008] In some possible implementations, the HP295 welding bottle steel is composed of the following components in mass fractions: 0.16%≤C≤0.18%, Si≤0.08%, 0.7%≤Mn≤0.9%, S≤0.005%, P≤0.015%, 0.015%≤Als≤0.045%, 0.01%≤Ti≤0.03%, N≤0.006%, and the rest is iron and unavoidable impurities.

[0009] In some possible implementations, the HP295 welding bottle steel includes iron and also includes the following components in mass fractions: 0.165%≤C≤0.18%, 0.05%≤Si≤0.08%, 0.75%≤Mn≤0.9%, S≤0.003%, P≤0.012%, 0.015%≤Als≤0.025%, 0.01%≤Ti≤0.015%, and N≤0.0045%.

[0010] In some possible implementations, the HP295 welding bottle steel is composed of the following components in mass fractions: 0.165%≤C≤0.18%, 0.05%≤Si≤0.08%, 0.75%≤Mn≤0.9%, S≤0.003%, P≤0.012%, 0.015%≤Als≤0.025%, 0.01%≤Ti≤0.015%, N≤0.0045%, and the rest is iron and unavoidable impurities.

[0011] In some possible implementations, the thickness of the HP295 welding bottle steel is 2.5 mm to 6.0 mm.

[0012] In some possible implementations, the ferrite structure in the HP295 welding bottle steel accounts for 65% to 80% by area ratio, which enables the HP295 welding bottle steel to have a low yield strength ratio and good deep drawing processing performance and welding performance during user processing.

[0013] The second purpose of the present application is to provide a production method of the HP295 welding bottle steel provided in the present application, comprising the following steps:

[0014] The molten steel is subjected to thin slab continuous casting and rolling treatment to obtain a strip steel; in the thin slab continuous casting and rolling treatment step, the drawing speed of the thin slab is 3.5 m / min to 4.5 m / min;

[0015] The strip steel is subjected to laminar cooling and coiling steps to obtain HP295 welding bottle steel.

[0016] The production method of the HP295 welding bottle steel of the present application is a short-process process of continuous casting and rolling of thin slabs, which reduces carbon emissions by about 40% compared with traditional processes, thereby reducing production costs. At the drawing speed of the thin slab, the cooling rate of the thin slab is fast and the center segregation of the slab is slight. The high temperature directly entering the furnace makes the heating time short, thereby making the decarburization layer of the slab thinner, and the thickness uniformity of the short-process process is better controlled. The strip structure of the HP295 welding bottle steel produced by the production method is no more than level 1.5, and no cracking will occur during deep drawing and stretching. The short-process process of continuous casting and rolling of thin slabs adopted in the production method requires 110 minutes to 160 minutes from molten steel to steel coils, which speeds up the production rhythm.

[0017] In some possible implementations, the thin slab continuous casting and rolling processing steps include: continuously casting molten steel to obtain a thin slab, and then performing heating, descaling and finish rolling steps to obtain the strip steel.

[0018] In some possible implementations, the thin slab has a thickness of 55 mm to 70 mm. Thin slabs of this thickness are used in thin slab continuous casting and rolling processes.

[0019] In some possible implementations, the heating step includes: heating the continuous casting billet in a soaking furnace, the temperature of the furnace is 900° C. to 960° C., the time for heating the thin slab to the uniform temperature is 15 min to 30 min, and the heating rate is 5° C. / min to 12° C. / min;

[0020] The temperature of the soaking furnace is 1160° C. to 1210° C., and the soaking time is 21 min to 50 min.

[0021] The above-mentioned heating step, under the time and heating rate for heating to uniform temperature, makes the decarburization layer of the thin slab thinner, and the temperature difference between the head and tail of the slab is better controlled (≤15°C) during short-process heating and rolling; the thickness uniformity is better (±30μm).

[0022] In some possible implementations, in the descaling step, the inlet pressure is 18MPa-22MPa, and the outlet pressure is 28MPa-30MPa. In this case, the iron oxide scale generated on the surface of the slab during the heating process is removed cleanly to ensure the surface quality of the strip.

[0023] In some possible implementations, in the finishing rolling step, the outlet temperature of the finishing rolling stand is 830° C. to 900° C., and the rolling speed is 4.7 m / s to 8.8 m / s.

[0024] In some possible implementations, the rolling speed is uniform.

[0025] In some possible implementations, the finishing rolling is performed using a 7-stand finishing rolling mill.

[0026] In some possible implementations, the number of rolling passes in the finishing rolling step is 7. In some possible implementations, the total reduction rate in the finishing rolling step is 90% to 96.5%. In this case, sufficient total deformation ensures uniform product structure.

[0027] In some possible implementations, the laminar cooling step includes a first laminar cooling, air cooling and a second laminar cooling step. In this case, a two-stage laminar cooling mode is adopted to ensure a certain cooling rate to improve the banded structure of the strip steel. The air cooling time between the two laminar cooling stages can allow the ferrite grains to grow appropriately and the internal grains to be uniform, thereby obtaining a HP295 welding bottle steel with a low strength-to-yield ratio, a banded structure not greater than 1.5, and good formability and welding performance.

[0028] In some possible implementations, in the first laminar cooling step, the cooling temperature is 740°C to 800°C, the cooling rate is 70°C / s to 100°C / s, and the cooling time is 0.6s to 3.0s. In this case, the austenite after finish rolling begins to transform into ferrite, and at a higher cooling rate, the nucleation points are increased, which greatly improves the generation of banded structure.

[0029] In some possible implementations, the air cooling time is 2.0s to 4.5s. Within this air cooling time range, the ferrite grains after phase transformation have time to grow appropriately and uniform internal grains.

[0030] In some possible implementations, in the second laminar cooling step, the cooling temperature is 630°C to 690°C, the cooling rate is 30°C / s to 60°C / s, and the cooling time is 0.8s to 2.5s. In this case, the transformation of austenite to ferrite + pearlite is completed, forming a uniform ferrite and pearlite grain structure.

[0031] In some possible implementations, in the coiling step, the coiling temperature is 630° C. to 690° C. In this coiling temperature and speed range, while ensuring a low yield strength ratio, the microstructure grains can be refined and the strength and toughness of the material can be improved. Grain refinement can reduce stress concentration and improve the material's fatigue resistance and fracture resistance.

[0032] In some possible implementations, the steel coil obtained after the steps is naturally air-cooled. In this case, the steel coil does not enter the slow cooling pit but is naturally air-cooled, and the subsequent slow cooling process cost does not need to be increased.

[0033] The third object of the present application is to provide a welding bottle, the material of which includes the HP295 welding bottle steel produced by the production method of HP295 welding bottle steel provided in the present application.

[0034] The welding bottle provided in the present application is made of the HP295 welding bottle steel provided in the present application, and the scrap rate in the manufacturing process is less than 1.0‰ (ie ≤1.0‰). BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the embodiments of the present drawings or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present drawings. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.

[0036] Figure 1 This is the metallographic structure of the HP295 welding bottle steel in Example 1 of the present application.

[0037] Figure 2 This is the metallographic structure of the HP295 welding bottle steel in Comparative Example 1 of the present application.

[0038] The purpose, features and advantages of this figure will be further described in conjunction with the embodiments with reference to the accompanying drawings. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.

[0040] Obviously, the following descriptions are only some examples or embodiments of the present application. For ordinary technicians in this field, the present application can also be applied to other similar scenarios without creative work. In addition, it can also be understood that although the efforts made in this development process may be complicated and lengthy, for ordinary technicians in the field related to the content disclosed in this application, some changes in design, manufacturing or production based on the technical content disclosed in this application are just conventional technical means, and should not be understood as insufficient content disclosed in this application.

[0041] However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially the same structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the following description is provided for those skilled in the art to fully understand the present application and is not intended to limit the subject matter described in the claims.

[0042] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution, and all technical features and optional technical features of the present application can be combined with each other to form a new technical solution.

[0043] Example 1

[0044] Example 1 A HP295 welding bottle steel is proposed, which is composed of the following components by mass fraction: 0.168% C, 0.04% Si, 0.75% Mn, S≤0.003%, 0.012% P, 0.025% Als, 0.015% Ti, 0.0045% N, and the rest is iron and unavoidable impurities. The thickness of the HP295 welding bottle steel is 3.0 mm.

[0045] Example 1 also provides a production method for HP295 welding bottle steel of this embodiment, comprising the following steps:

[0046] (1) Heating: The ingot (thin slab) with a thickness of 70 mm is directly put into the furnace at a temperature of 950°C, the temperature of the soaking furnace is 1160°C to 1180°C, and the soaking time is 26 min.

[0047] (2) Descaling: The slabs are descaled after the heating step. The inlet descaling pressure is 19 MPa and the outlet descaling pressure is 29 MPa.

[0048] (3) Finish rolling: Finish rolling was performed using a 7-stand finishing mill with a final rolling temperature of 865°C, a rolling speed of 6.5 m / s, 7 rolling passes, and a total reduction ratio of 95.7%. Strip steel was obtained after finish rolling.

[0049] (4) The strip is cooled by the following two-stage laminar flow:

[0050] ① The first laminar cooling temperature is 770℃, the cooling rate is 90℃ / s, and the cooling time is 1.05s.

[0051] ②After the first laminar cooling, air cool for 3.5s.

[0052] ② The second stage laminar cooling temperature is 650℃, the cooling rate is 50℃ / s, and the cooling time is 1.7s.

[0053] (5) After laminar cooling, the strip is coiled at a temperature of 650°C.

[0054] (6) After coiling, bundle and store.

[0055] Example 2

[0056] Example 2 proposes an HP295 welding bottle steel, whose component content and thickness are the same as those of Example 1.

[0057] Example 2 also proposes a production method for the HP295 welding bottle steel of this embodiment, and the steps are basically the same as those of Example 1, except that:

[0058] In step (4):

[0059] ① The first laminar cooling temperature is 740℃, the cooling rate is 70℃ / s, and the cooling time is 1.9s.

[0060] ②After the first laminar cooling, air cool for 3.0s.

[0061] ② The second stage laminar cooling temperature is 630℃, the cooling rate is 30℃ / s, and the cooling time is 2.5s.

[0062] Example 3

[0063] Example 3 proposes an HP295 welding bottle steel, whose component content and thickness are the same as those in Example 1.

[0064] Example 3 also proposes a production method for HP295 welding bottle steel of this embodiment, and the steps are basically the same as those of Example 1, except that:

[0065] In step (4):

[0066] ① The first laminar cooling temperature is 790℃, the cooling rate is 80℃ / s, and the cooling time is 1.0s.

[0067] ②After the first laminar cooling, air cool for 4.0s.

[0068] ② The second stage laminar cooling temperature is 670℃, the cooling rate is 47℃ / s, and the cooling time is 1.7s.

[0069] Example 4

[0070] Example 4 proposes an HP295 welding bottle steel, whose component content and thickness are the same as those of Example 1.

[0071] Example 4 also proposes a production method for HP295 welding bottle steel of this embodiment, and the steps are basically the same as those of Example 1, except that:

[0072] In step (4),

[0073] ① The first laminar cooling temperature is 800℃, the cooling rate is 100℃ / s, and the cooling time is 0.6s.

[0074] ②After the first laminar cooling, air cool for 4.5s.

[0075] ② The second stage laminar cooling temperature is 690℃, the cooling rate is 60℃ / s, and the cooling time is 1.3s.

[0076] Example 5

[0077] Example 5 proposes a HP295 welding bottle steel, the composition of which is substantially the same as that of Example 1. The thickness of the HP295 welding bottle steel is 2.5 mm.

[0078] Example 4 also proposes a production method for HP295 welding bottle steel of this embodiment, and the steps are basically the same as those of Example 1, except that:

[0079] In step (3), the total reduction ratio of the finish rolling is 96.4%.

[0080] Example 6

[0081] Example 6 proposes a HP295 welding bottle steel, the composition of which is substantially the same as that of Example 1. The thickness of the HP295 welding bottle steel is 6 mm.

[0082] Example 6 also proposes a production method for HP295 welding bottle steel of this embodiment, and the steps are basically the same as those of Example 1, except that:

[0083] In step (3), the total reduction ratio of the finish rolling is 91.4%.

[0084] Example 7

[0085] Example 7 proposes an HP295 welding bottle steel, the composition and thickness of which are basically the same as those of Example 1, except that the C content is 0.17%.

[0086] Example 7 also proposes a production method for the HP295 welding bottle steel of this example, and the steps are basically the same as those of Example 1.

[0087] Example 8

[0088] Example 8 proposes an HP295 welding bottle steel, the composition and thickness of which are basically the same as those of Example 1, except that the C content is 0.18%.

[0089] Example 7 also proposes a production method of the HP295 welding bottle steel of this embodiment, and the steps are basically the same as those of Example 1.

[0090] Comparative Example 1

[0091] Comparative Example 1 proposes a HP295 welding bottle steel, which is composed of the following components by mass fraction: 0.168% C, 0.09% Si, 0.75% Mn, S≤0.006%, 0.015% P, 0.025% Als, 0.015% Ti, 0.0055% N, and the rest is iron and unavoidable impurities. The thickness of the HP295 welding bottle steel is 3.0 mm.

[0092] Comparative Example 1 also proposes a production method of HP295 welding bottle steel of this comparative example, comprising the following steps:

[0093] (1) Heating: The ingot (thin slab) with a thickness of 70 mm is directly put into the furnace at a temperature of 950°C, the temperature of the soaking furnace is 1170°C to 1200°C, and the soaking time is 30 min.

[0094] (2) Descaling: The slabs are descaled after the heating step. The inlet descaling pressure is 18 MPa and the outlet descaling pressure is 26 MPa.

[0095] (3) Finish rolling: Finish rolling was performed using a 7-stand finishing mill with a final rolling temperature of 865°C, a rolling speed of 6.0 m / s, 7 rolling passes, and a total reduction ratio of 95.7%. Strip steel was obtained after finish rolling.

[0096] (4) The strip is subjected to sparse laminar cooling in the latter stage: air cooling after finishing rolling, and then sparse cooling, with a cooling rate of 40°C / s and a cooling time of 5.5s.

[0097] (5) After laminar cooling, the coiling temperature of the strip is 630°C.

[0098] (6) After coiling, bundle and store.

[0099] Comparative Example 2

[0100] Comparative Example 2 proposes an HP295 welding bottle steel, whose component content and thickness are the same as those in Example 1.

[0101] Comparative Example 2 also proposes a production method for the HP295 welding bottle steel of this embodiment, and the steps are basically the same as those of Example 1, except that: in the laminar cooling step, air cooling is first performed after finishing rolling, and then primary cooling is adopted, the cooling temperature is 640°C, the cooling rate is 45°C / s, and the cooling time is 5.0s.

[0102] Comparative Example 3

[0103] Comparative Example 3 proposes an HP295 welding bottle steel, whose component content and thickness are the same as those in Example 1.

[0104] Comparative Example 3 also proposes a production method for the HP295 welding bottle steel of this embodiment, and the steps are basically the same as those of Example 1, except that in the laminar cooling step (4), after the finish rolling, the first stage of laminar cooling is performed without air cooling and directly enters the second stage of laminar cooling.

[0105] In order to verify the progress of the HP295 welding steel and the production method of HP295 welding steel provided in the examples of the present application, the HP295 welding steel provided in Examples 1 to 8 and Comparative Examples 1 to 3 were tested for tensile strength (R m ), yield strength (R el), strength-to-yield ratio, elongation at break and banded structure test, the results are shown in Table 1. In addition, the HP295 welding bottle steel of Example 1 and Comparative Example 1 was subjected to metallographic structure test, the results are shown in the attached specification Figure 1 and 2 shown.

[0106] Table 1

[0107]

[0108] According to Table 1 above and the instructions attached Figure 1 and 2 At least the following conclusions can be drawn:

[0109] (1) Appropriate C content and lower P and S content can adapt to the smooth production under short process continuous casting and high casting speed, as well as good inclusion control and performance.

[0110] (2) The short-process technology only takes about 2 hours from molten steel to steel coil products, which greatly improves the production rhythm and energy consumption cost by more than 40%.

[0111] (3) The mode of primary cooling + air cooling + secondary cooling after rolling ensures the mechanical properties and low yield strength ratio of the product at a higher cooling rate, while obtaining a more uniform structure and a low banded structure rating.

[0112] (4) By the attached Figure 1 and Figure 2 It can be seen that the ferrite grains of the HP295 welding bottle steel produced by the production method of the HP295 welding bottle steel provided in the embodiment of the present application are obvious and uniform, and the banded structure rating is low (significantly improved), which is below level 1.5. Figure 2 The HP295 welding bottle steel produced by the method of Comparative Example 1 has obvious banded structure, which may easily cause cracking during deep drawing of the strip steel.

[0113] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A HP295 welding bottle steel, the HP295 welding bottle steel comprising iron, characterized in that: It also includes the following components in mass fractions: 0.16%≤C≤0.18%, Si≤0.08%, 0.7%≤Mn≤0.9%, S≤0.005%, P≤0.015%, 0.015%≤Als≤0.045%, 0.01%≤Ti≤0.03%, and N≤0.006%.

2. The HP295 welding bottle steel according to claim 1, characterized in that: The HP295 welding bottle steel also includes the following components in mass fraction: 0.165%≤C≤0.18%, 0.05%≤Si≤0.08%, 0.75%≤Mn≤0.9%, S≤0.003%, P≤0.012%, 0.015%≤Als≤0.025%, 0.01%≤Ti≤0.015%, and N≤0.0045%.

3. The HP295 welding bottle steel according to claim 1 or 2, characterized in that: Calculated by area ratio, the ferrite structure in the HP295 welding bottle steel accounts for 65% to 80%.

4. A method for producing HP295 welding bottle steel as claimed in any one of claims 1 to 3, characterized in that: The steps include: The molten steel is subjected to thin slab continuous casting and rolling treatment to obtain a strip steel; in the thin slab continuous casting and rolling treatment step, the drawing speed of the thin slab is 3.5m / min to 4.5m / min, and the slab thickness is 60mm to 70mm; The strip steel is subjected to laminar cooling and coiling steps to obtain HP295 welding bottle steel.

5. The production method of HP295 welding bottle steel according to claim 4, characterized in that: The thin slab continuous casting and rolling treatment steps include: continuous casting of molten steel to obtain a thin slab, and then heating, descaling and finish rolling steps to obtain the strip steel; And / or, the laminar cooling step includes a first stage of laminar cooling, air cooling and a second stage of laminar cooling.

6. The production method of HP295 welding bottle steel according to claim 5, characterized in that: The heating step comprises: heating the continuous casting billet in a soaking furnace, wherein the temperature of the continuous casting billet in the furnace is 900° C. to 960° C., the time for heating the thin slab to the even temperature is 15 min to 30 min, and the heating rate is 5° C. / min to 12° C. / min; The temperature of the soaking furnace is 1160° C. to 1210° C., and the soaking time is 21 min to 50 min.

7. The production method of HP295 welding bottle steel according to claim 5, characterized in that: In the finishing rolling step, the outlet temperature of the finishing rolling stand is 830° C. to 900° C., and the rolling speed is 4.7 m / s to 8.8 m / s.

8. The method for producing HP295 welding bottle steel according to claim 7, characterized in that: In the finishing rolling step, the total reduction ratio is 90% to 96.5%.

9. The method for producing HP295 welding cylinder steel according to any one of claims 5 to 8, characterized in that: In the first laminar cooling step, the cooling temperature is 740°C to 800°C, the cooling rate is 70°C / s to 100°C / s, and the cooling time is 0.6s to 3.0s; And / or, the air cooling time is 2.0s to 4.5s; And / or, in the second laminar cooling step, the cooling temperature is 630°C to 690°C, the cooling rate is 30°C / s to 60°C / s, and the cooling time is 0.8s to 2.5s; And / or, in the coiling step, the coiling temperature is 630°C to 690°C.

10. A welding bottle, characterized in that: The material of the welding bottle includes HP295 welding bottle steel produced by the production method of HP295 welding bottle steel as described in any one of claims 4 to 9.