Method for producing and filling a container designed for holding food
Using high-power laser radiation to form a weakened portion at the connecting edge of the PET sheet solves the problems of high maintenance costs and inflexibility caused by the use of cutting tools in the existing technology, achieves flexible container design and high productivity, and ensures the safety of the container Reliability and cost-effectiveness.
Patent Information
- Application Number
- CN202180009271.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-01-17
- Filing Date
- 2021-01-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-01-12
AI Technical Summary
In the existing technology, when producing and filling food containers, the use of blades or knives results in high equipment maintenance costs, inflexibility and difficulty in changing the size of the container set. Especially when using PET materials, the tool life is shortened, the cost is increased, and it is difficult to produce by bending. Weakened part.
High-power laser radiation is used to locally reduce the joint edges of the PET sheets, reducing the crystallinity and forming weakened parts, avoiding the use of tools and allowing flexible changes in container shape and size.
It reduces equipment maintenance costs, improves production flexibility and industrial productivity, ensures the reliability and competitiveness of containers, avoids the use of cutting tools, and does not affect the transparency and recyclability of PET materials.
Smart Images

Figure CN115003601B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for producing and filling a container designed to contain food. Background Art
[0002] Typically, the method of producing and filling food provides the following steps:
[0003] - shaping the sheet (usually made of PS or polystyrene) to provide a plurality of accommodation receptacles provided with at least one access inlet;
[0004] - filling the container with at least one food through the access opening;
[0005] - Sealing the access opening by means of a closing film or sheet unrolled from a roll;
[0006] - cutting into groups of containers by means of a blade or knife;
[0007] - providing respective weakened and separating portions at the edges for connection between at least two adjacent containing containers in the same group.
[0008] The step of providing a weakened portion is also performed using a blade or knife, which is typically operated to provide a cut at the connecting edge.
[0009] This method and the equipment used have two disadvantages:
[0010] The use of cutting blades or knives for grouping is not particularly flexible, and varying the size of the group or the extension of the weakened section at the equipment level is rather complicated.
[0011] These problems are compounded by other issues, particularly if one wishes to use PET instead of PS to provide the containment receptacle.
[0012] In fact, in this case, the life of the blade or tool can be significantly shortened and the cost can be significantly increased.
[0013] Furthermore, when transparent or colored PET having a relatively high toughness is used as the material, it is practically impossible to produce a weakened portion capable of allowing separation between containers by bending them mutually without using scissors or a knife.
[0014] In particular, PET in layered form (i.e. sheets with a thickness greater than 250 μm) with an initial crystallinity of up to 10% is a resilient and tough material, and therefore, in order to produce a weakened portion at the connecting edge between at least two different containing containers by scoring with a knife, a system must be used in which the knives are closer to each other and must score through almost the entire material thickness; despite this, there is no guarantee that the intended purpose will be achieved.
[0015] This, among other things, leads to a shorter tool life in PET applications and thus to higher costs.
[0016] Finally, the process becomes difficult to replicate.
[0017] Conventionally (see patent GB 2543495), the possibility of increasing the brittleness of PET by a local increase in crystallinity induced by the action of laser radiation is known: the thermal effect, an inevitable consequence of the action of laser radiation on the material it attacks, is in fact responsible for the increase in crystallinity.
[0018] It is also known from the literature that crystallization is a process that requires sufficient time and temperature and is induced by prolonged exposure to low-power laser radiation. In this way, the heating effect caused by the laser radiation is maximized so that the crystallization temperature range of PET is reached without the action of the laser causing ablation of the sample, or if it is reached, it is obtained at low speeds [MF Sonnenschein and CM Roland, Appl. Phys. Lett. 57 (5), 1990].
[0019] While it is true that crystallinity and therefore brittleness can be increased in PET by prolonged exposure to low-power lasers, this approach is also not suitable for industrial requirements, which increasingly demand increased productivity by reducing production times. Summary of the invention
[0020] It is an object of the present invention to provide a method for producing and filling a container designed to contain food, which method improves the prior art in one or more of the above-mentioned aspects.
[0021] Within this aim, an object of the invention is to provide a method for producing and filling containers designed to contain food which allows reducing the maintenance costs of the plant.
[0022] Another object of the invention is to devise a method for producing and filling containers designed to contain food which is very flexible and allows to easily vary the shape of the sets of interconnected containers and of the weakened portions.
[0023] Another object of the present invention is to provide a method for producing and filling containers designed to contain food which is highly reliable, relatively easy to provide and at a competitive cost, and which maintains the high industrial productivity that is a characteristic of current container manufacturing made of PS.
[0024] This object, as well as these and other objects which will become more apparent hereinafter, are achieved by a method for producing and filling a container designed for containing food according to claim 1 , optionally having one or more of the features of the dependent claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Further features and advantages of the invention become more apparent from the description of a preferred but not exclusive embodiment of a method according to the invention for producing and filling a container designed to contain food, shown by way of non-limiting example in the accompanying drawings, in which:
[0026] Figure 1 is a schematic diagram of an apparatus for producing and filling containers designed to hold food;
[0027] Figure 2 is a top view of a container provided by the method according to the present invention;
[0028] Figure 3 The 3D texture (relief, pattern, relief) of the surface opposite to the one acted on by the laser is shown, obtained using a Zygo high-definition optical instrument: The texture obtained in three areas of the sample shows that there are tension variations in the weakened parts (caused by the laser emitting step) that lead to surface depressions;
[0029] Figure 4 The 3D texture of the surface opposite to the laser-acted surface is shown, obtained using a Zygo high-definition optical instrument; the texture obtained in three areas of the sample shows that there are tension variations in the weakened parts (caused by the laser emitting step) that lead to surface misalignment;
[0030] Figure 5 View of a sample with a continuous weakened section on the left and a weakened section with through openings on the right; the sample is viewed with polarized light; the tension state changes significantly in the immediate vicinity of the laser action, where only heat, not the laser beam, reaches;
[0031] Figure 6 The three images of the weakened part on the surface are shown in Figure 1. The image with 3.5x magnification clearly shows the entire cutout; the image with 16x magnification shows the edge of the cutout, as well as the cutout groove in the middle (the object of analysis); the image with 56x magnification shows only the cutout groove to be analyzed.
[0032] Figure 7 The following are three images of a weakened section on the surface: the 3.5x magnified image clearly shows the entire cut; the 16x magnified image shows the through opening and the "bridge"; the 32x magnified image highlights the "bridge" of the weakened section to be analyzed.
[0033] Figure 8 is an image view of surface defects of a sample with a known thermal history;
[0034] Fig. 9 Overlay of Raman microscopy spectra is shown; the spectrum designated by A is between 1000-2050 cm -1 There is a clear fluorescence signal within the range, so it must be excluded;
[0035] Fig.10 Showing 1800-2050cm -1 Superposition of Raman microscopy spectra with maximum intensity variation within the range. The spectrum designated by B is an example of an acceptable spectrum, with a maximum intensity variation below 150; in contrast, spectrum C is unacceptable because its maximum intensity variation is greater than 150;
[0036] Fig.11 This is a magnified image of the holes created in the sample after analysis using Raman microscopy;
[0037] Fig.12 is an example of the treatment of the cold crystallization peak in the second scan of the calorimetric analysis;
[0038] Fig.13 This is an example of processing the melting peak in the second scan of a calorimetric analysis.
[0039] Fig.14 An example of a cross-sectional analysis of a sample with a known thermal history is shown;
[0040] Fig.15 and Fig.16 and Fig.17 The analysis conditions set in the Omnic software for obtaining Raman spectra are shown, which are further detailed in the detailed description;
[0041] Fig.18 An example of analyzing Raman spectra by using the Peak Resolve function according to the method detailed in the specific embodiment is shown;
[0042] Fig.19 The straight line calibration line for the tank 1 treatment is shown, including the equation of the line and R 2 value;
[0043] Fig. 20 The straight line calibration line for the tank 2 treatment is shown, including the equation of the line and R 2 value;
[0044] Fig.21 The straight line calibration line for 1-mm PET sheet processing is shown, including the line equation and R 2 value. DETAILED DESCRIPTION
[0045] With reference to the accompanying drawings, the method for producing and filling a container for holding food according to the present invention comprises the following steps:
[0046] - forming a sheet 10 made of PET (polyethylene terephthalate) so as to provide a plurality of containment containers 11 provided with at least one access opening 12; the initial crystallinity of the sheet made of PET is less than or equal to 10%;
[0047] - filling said container with at least one food through said access opening;
[0048] - Sealing the access opening 12 by means of a closing membrane 13;
[0049] A weakened portion 21 is provided at a connecting edge 22 between at least two adjacent receiving containers 11 .
[0050] In particular, the step of providing the weakened portion 21 comprises the step of emitting laser radiation 40 at at least a portion of the connecting edge 22 to provide a local reduction in the cross section of the connecting edge 22 along the weakened portion 21 .
[0051] For example, the local reduction in cross section is at least equal to 50%, preferably at least equal to 70% and even more preferably at least equal to 80% relative to the initial cross section.
[0052] According to the present invention, after the step of emitting laser radiation 40, the final crystallinity at the weakened portion 21 is lower than, equal to or greater than a percentage of the crystallinity of the portions (regions) of the connecting edge 22 that are not affected by the changes caused by the laser radiation 40 emission step and the sealing step, which is at most equal to 3%.
[0053] In fact, as will become clear from the tests described below, the crystallinity of the portion of the connecting edge 22 that is not affected by the modifications due to the step of emitting laser radiation 40 and the step of sealing corresponds substantially to that of the sheet 10 .
[0054] In practice, the emission step is performed at a speed and laser power such that at the end of the step, at the edge of the connection:
[0055] - Reduction in crystallinity;
[0056] - maintenance of the same degree of crystallinity; or
[0057] - Increase in crystallinity, at most equal to 3%.
[0058] The crystallinity after the emission step is evaluated at the substantially weakened portion 21 .
[0059] In particular, the step of providing the weakened portion 21 comprises a step of emitting laser radiation 40 originating from a laser having a power at least equal to 250W.
[0060] Advantageously, the laser emits at a wavelength absorbed by PET: for example, a CO2 laser with a wavelength equal to 10.6 microns, 10.2 microns or 9.3 microns can be used.
[0061] Laser irradiation occurs at least at a portion of the connecting edge 22 to provide a localized reduction in the cross-section of the connecting edge 22 along the weakened portion 21 .
[0062] A local reduction in cross section is to be understood as meaning a reduction in the cross section of the connecting edge 22 which is substantially constant along the longitudinal extension of the weakened portion 21 and as meaning the provision of a plurality of through openings which pass through the connecting edge and are spaced apart from one another to provide the weakened portion 21 .
[0063] The reduction in cross section along the connecting edge 22 can also provide through-openings which are staggered by a constant reduction in thickness or by a sequence of different reductions in thickness.
[0064] It has surprisingly been found that, although the emitting step does not lead to an increase in the crystallinity (more than 3%), the weakened portion 21 is able to ensure extremely effective rupture along the connecting edge 22 between two adjacent receiving containers 11 .
[0065] Conveniently, the thickness of the connecting edge 22 to which the step of providing the weakened portion 21 is performed is from 300 microns to 1800 microns, and more preferably from 700 microns to 1300 microns.
[0066] Advantageously, between the sealing step and the step for providing the weakened portion 21 , there is a step for separating the receiving containers 11 of the group 31 of receiving containers 11 .
[0067] Preferably, this separation step is performed by means of a laser beam designed to perform a cut 30 at the connecting edges between the containing containers 11 .
[0068] At the end of the method according to the present invention, a group (called a multi-pack) 31 of storage containers 11 is obtained; corresponding weakened portions 21 are formed between adjacent storage containers 11 of the same group 31 and are suitable for allowing each storage container 11 to be separated from other storage containers 11 of the same group 31.
[0069] The use of a laser to provide the weakened portion 21 makes the method according to the invention very flexible, since it can easily be programmed if the size of the receiving container 11 or the shape of the group 31 changes.
[0070] The providing step comprises the following steps: emitting laser radiation with a power greater than 250 W and preferably less than 1500 W at a speed of 15 m / min to 170 m / min, more preferably emitting laser radiation with a power of 300 W to 1200 W at a speed of 20 m / min to 144 m / min.
[0071] In this regard, an attempt has been made to verify whether the control of the operating conditions using the laser (in terms of power and speed) affects the final crystallinity in an experimentally controllable way (by determining a decrease, no change or an increase of up to 3%) and, therefore, a reduction in the toughness of the joined edges, in order to determine the optimal operating conditions and parameters for obtaining both an extremely favorable rupture and the implementation of a process capable of ensuring sufficient productivity.
[0072] To this end, a series of experimental tests were conducted.
[0073] First, the changes in crystallinity of samples subjected to laser irradiation were studied.
[0074] The use of laser radiation with a power greater than 250 W, although not significantly increasing the crystallinity, allows to modify the tension distribution inside the PET, thus obtaining an increase in its brittleness.
[0075] The extremely fast action of the intense laser light acting in a localized manner minimizes thermal effects and does not alter the area adjacent to the weakened portion 21, thus causing a change in the tension of the polymer chains, which makes the PET fragile at the weakened portion, without even causing a significant increase in crystallinity.
[0076] The laser acts on the side of the connecting edge 22 that points upward, ie, on the side opposite to the receiving container 11 .
[0077] Furthermore, the method according to the invention provides for a sterilization step to be carried out upstream or downstream of the thermoforming step.
[0078] The method further provides for performing a step of extracting the gas and the volatile matter during the emitting step.
[0079] Said extraction step allows to eliminate gases and volatile substances from the emission zone, but at the same time makes the action of the laser more efficient.
[0080] According to the invention, it is possible to provide for the use of a high amount of dye or a high amount of pigment which reduces, ie decreases, the transparency of the finished PET sheet.
[0081] Furthermore, no issues arise that would prevent the use of recycled or partially recycled PET.
[0082] The present invention thus describes an alternative method of making PET fragile without resorting to the usual crystallization methods: in fact it is observed that at the weakened portions 21 there is a local variation in the degree of crystallinity which does not increase by more than 3% relative to the areas where the laser has not acted.
[0083] As mentioned previously, this change in material tension can be assessed indirectly by using appropriate techniques for surface analysis and observing the sample with polarized light.
[0084] In the literature, it is known that the occurrence of sample deformation is related to the change of the tensile state. Using the Zygo high-definition optical instrument for detecting 3D surfaces to collect the surface profile, it can be observed that in the sample surface that is not directly exposed to the laser action but is opposite to it, deformation can be generated in the weakened part, such as dents or dislocations on the surface.
[0085] Furthermore, observation of a sample provided with a weakened portion under polarized light can highlight changes in the tension state of the material in the immediate vicinity of the action of the laser beam, where only the radiated heat has reached.
[0086] In this regard, it has been found experimentally that, on the opposite side relative to the laser action, the material that has undergone the thermal effect of the laser attempts to reorganize itself, remaining coupled to the "cold" material.
[0087] The determination of crystallinity in polymers is the subject of much discussion, and there are many techniques for determining it.
[0088] X-ray diffraction and calorimetric analysis techniques based on differential scanning calorimetry (hereinafter also referred to as "DSC") are the most widely used techniques for determining the crystallinity of polymer samples, but there are problems such as sample preparation, analysis time, accuracy and complexity of data analysis, and in the case of X-ray diffraction, the cost of the technique is high, so it is more advantageous to use Raman microscopy, which also allows faster analysis and is non-destructive.
[0089] However, Raman spectroscopy is not a self-sufficient technique, but needs to be correlated with other methods of measuring crystallinity by constructing calibration curves [V. Shabafrooz et al. SPE ANTECTM Indianapolis 2016].
[0090] In the analysis reported below, microscopic-scale Raman spectroscopy (hereinafter referred to as “Raman microscopy”) was used because it is an effective technique for sample point analysis and, moreover, it can be localized at weakened portions.
[0091] Raman microscopy was then correlated to the DSC calorimetric technique by constructing an appropriate calibration curve having on the abscissa axis the degree of crystallinity calculated by DSC (Xc (%)) and on the ordinate axis the values obtained by Raman microscopy.
[0092] Specific samples with known thermal history were prepared for this purpose.
[0093] Whenever materials with different properties are to be investigated (different intrinsic viscosity (IV), different thickness, different additives, ...), calibration curves should be prepared as well as samples with known thermal history.
[0094] Calorimetric analysis was performed using a Perkin Elmer DSC 8500 differential scanning calorimeter with a CLN2 liquid nitrogen cooling system, Pyris processing software, and the direction of the endothermic transition was toward the positive value of the ordinate axis. For each analysis, a sample amount of 7-15 mg was weighed in a manually closed non-sealed sample holder. The samples were not pre-treated before analysis, all of which were performed in a nitrogen flow (20 mL / min).
[0095] The purpose of using this instrument is twofold:
[0096] 1) Preparation of samples with known thermal history for later analysis by Raman microscopy;
[0097] 2) Prepare samples with known thermal history similar to the previous samples and calculate their crystallinity by DSC calorimetric analysis.
[0098] In both cases, areas not affected by thermoforming of the finished container were sampled to prepare specimens with a known thermal history.
[0099] With reference to the dual purpose of using the DSC tool, the analytical conditions are divided into:
[0100] 1) To prepare a sample with known thermal history for analysis by Raman microscopy:
[0101] a. First scan (1 scan): at 20°C / min, from 30°C to 300°C;
[0102] b. Isotherm: 1 min at 300 °C;
[0103] c. Cooling: from 300°C to 0°C at X°C / min, X=20; 50; 100; quenching obtained by selecting the "Ballistic Cool to Temperature" setting; 200.
[0104] 2) To prepare a similar sample with a known thermal history to be processed to obtain crystallinity from DSC:
[0105] a. First scan (1 scan): 20°C / min, from 30°C to 300°C;
[0106] b. Isotherm: 1 min at 300 °C;
[0107] c. Cooling: from 300°C to 0°C at X°C / min, X = 20; 50; 100; Quenching obtained by selecting the "Ballistic Cooling to Temperature" setting; 200;
[0108] d. Second scan (2nd scan): at 20°C / min, from 0°C to 300°C.
[0109] The analysis conditions thus set allow to eliminate the thermal history of the melting of the sample due to the first scan. By cooling at a controlled and defined rate (20; 50; 100; quenching; 200 ° C / min), samples with increasing crystallinity are obtained with decreasing cooling rate. Therefore, the sample used for the subsequent Raman analysis and the sample also subjected to a second heating are considered similar for the same cooling rate. The former is directly analyzed by Raman microscopy, while the latter, which also undergoes a second heating from processing under the analysis conditions, obtains by DSC the crystallinity developed during cooling. This value must be correlated with the Raman microscopy value calculated for its similar samples.
[0110] Since the processing operation for calculating crystallinity is carried out on the second heating, the instrument has been calibrated to heat and cool at a rate of 20°C / min according to the recommendations for PET analysis [A. Hammer, Thermal analysis of polymers. Part 1: DSC of thermoplastics, Mettler Toledo UserCom 31].
[0111] Determination of crystallinity by DSC for samples with known thermal history was performed by processing the second scan (2 scan). The melting and cold crystallization peaks were processed to derive heat of fusion and crystallization values. Processing was performed in such a way that the integrated baseline coincided with the baseline of the specific thermogram by subtracting the absolute value of the heat of crystallization (cold crystallization in 2 scan) normalized for sample mass (ΔHcc) from the heat of fusion normalized for sample mass (ΔHf), and matching the result with the tabulated value of ΔHf° for PET (140 J / g), which is the theoretical value of the heat of fusion normalized for 100% crystalline PET mass, which was determined by an indirect method using the Flory equation described below:
[0112] XC 冷却后 (%) = (ΔH f -│ΔH cc │)*100 / 140
[0113] [“Polymer Heat of Fusion”, Thermal applications note, RL Blaine, G. Ellis et al., Spectrochimica Acta Part A, 1995, vol. 51, 2139-2145. The equations used follow those of V. Shabafrooz et al. SPE ANTECTM Indianapolis 2016].
[0114] For spectral analysis, Raman microscopy was used by using a Thermo Fisher DXR Raman microscope.
[0115] Regarding Raman spectroscopy applied to PET, it is known that molecular vibrations are active at specific Raman shifts, and the intensity or shape of their signals depends on the crystallinity of the sample [SG Kazarian, NH Brantley, CA Eckert, Vibrational Spectroscopy 19, 1999, 277-283 A Study of Polymer Crystallinity Using the Raman Station 400F, www.perkinelmer.com; JS Rossier et al., Langmuir 15, 1999, 5173-5178, G. Ellis et al., Spectrochimica Acta Part A, 1995, vol. 51, 2139-2145; JC Rodriguez-Cabello et al., Journal of Raman spectroscopy, vol. 25, 1994, 335-34].
[0116] In the tests performed, the vibrations corresponding to carbonyl stretching were analyzed, the bandwidth of which decreases as the crystallinity of the analyzed samples increases.
[0117] The full width at half maximum (FWHH) of the band associated with this vibrational motion was calculated and it is at 1700 cm -1 -1760cm -1 Developed within the Raman shift range [JCRodriguez-Cabello et al., Journal of Ramanspectroscopy, vol.25, 1994, 335-34].
[0118] For samples analyzed by Raman microscopy, a distinction was made between samples with known thermal history (prepared in DSC as described previously) and samples with unknown crystallinity to be determined by interpolation from the calibration curve.
[0119] In fact, samples with unknown crystallinity were analyzed on the surface exposed to the action of the laser, acquiring spectra in at least 3 points of the region of interest: in particular, 3 points in the lower part of the cut ("groove") were analyzed in the case of continuous weakening, and 3 points equidistant from the through opening ("bridge") in the case of weakening with through openings were analyzed in the solid region (solid region). Samples with known thermal history prepared in DSC were instead analyzed in cross section by Raman microscopy, by fixing each sample in a specific holder (kit provided by ThermoFisher) for cross section analysis to fix the flat surface of the sample to the clamping element. The sample was then cleanly cut using a blade (supplied by ThermoFisher) to obtain a rectangular section centered on the circular sample, on which spectra were acquired at at least 10 points.
[0120] The contents of the spectrum acquisition and processing report are valid for all samples.
[0121] Record Raman spectra by setting the following acquisition mode in the "Omnic for Dispersive Raman" software:
[0122] 1) In the acquisition window of the experimental settings, select the "Auto Exposure" option, "Required S / N" equals 500, "Maximum acquisition time (min)" equals 5, and "Preview exposure time (s)" equals 1;
[0123] 2) In the same acquisition window, the final format of the displayed spectrum is also set, especially the "Shifted spectrum (cm -1 )", in "Calibration", select the "Fluorescence" option from the drop-down menu, in the sub-window opened by clicking the word "Fluorescence", select "Use polynomial order: 6", and select "Cosmic ray threshold: Low"; In addition, in the present invention, the spectrum is acquired by selecting the optional "Use smart background" option in the same window;
[0124] 3) In the Bench window of the experimental setup, select 532 nm as the "Laser Wavelength" (for lasers of this wavelength, the instrument must be properly calibrated), set the "Laser Power" equal to 10 mW (the maximum value that can be set for the instrument used), set the "Aperture" equal to a 25 μm pinhole, and set the minimum and maximum acquisition ranges in the present invention to 200 to 3500 cm -1Finally, a 10x lens is selected in the workbench window and a lens with this magnification is used in the optical module to focus the optical image of the area of interest and to properly analyze the selected point. The "Grating", "Estimated Resolution", "Estimated Spot Size" and "Allowed Range" parameters cannot be modified manually by the operator but depend on the characteristics of the instrument or other parameter settings described here.
[0125] 4) To have better control over the spectral acquisition, it is also recommended to set all acquisition controls, which can be selected in the Quality window of the experimental setup.
[0126] In the Atlμs window, using the "Sampling Point Tool" function for each sample, several points are selected for the acquisition of spectra (at least 10 points for samples with known thermal history and at least 3 points for unknown samples). These points must be selected so that the image of each point is in focus and care is taken to avoid surface defects; in addition, for samples with known thermal history, the distance between the points must be almost constant, the sequence must cover the entire length of the longitudinal direction of the previously obtained rectangular cross section, and care must be taken to avoid bubbles or roughness. Once the points of interest have been selected, the spectral acquisition can be continued through the "Acquisition Plot" function.
[0127] If it is not possible to use the Sample Point Tool function, or if there are problems with sequential acquisition of selected points, it is possible to acquire spectra manually one at a time, understanding that the general criteria for point acquisition given above apply.
[0128] The spectrum acquisition mode is set to interrupt the analysis after five minutes of acquisition, regardless of whether the required S / N ratio has been achieved. Therefore, it is necessary to pay attention to the acquired spectra and take into account that the spectrum cannot be considered acceptable if:
[0129] -1000-2050cm -1 In the Raman shift range, it has a signal (peak) or a baseline shift (linear to curve) due to fluorescence;
[0130] - In the Raman shift range where there are no peaks associated with the sample (e.g., 1800-2050 cm -1 ), it has a maximum intensity (Raman intensity) variation, defined as the difference between the absolute maximum and minimum values in the selected range, greater than 150 units.
[0131] If this happens, the advice is to:
[0132] - Check if the analysis area is in focus;
[0133] - Check that the sample is clean and free of dust or grease that may interfere with the analysis;
[0134] -Change analysis point.
[0135] It is also possible that a hole is created at the analysis point after Raman microscopy analysis. This phenomenon can be observed through the Atlμs window and in any case the software reports it as "Sample burning" in the "Acquisition Status" window. In this case, the analysis point needs to be changed.
[0136] For the processing of the spectra obtained by Raman, we proceed as follows:
[0137] 1) In the spectrum, 1820-1640cm -1 The peak resolution function was selected in the analysis.
[0138] 2) In the analysis window opened by the peak resolution function, analyze by Gaussian / Lorentzian function [JC Rodriguez-Cabello et al., Journal of Raman spectroscopy, vol. 25, 1994, 335-344; S. Yang, S. Michielsen, Macromolecules 36, 2003, 6484-6492, using "high sensitivity", "noise target" of 0.5 and linear "baseline"];
[0139] 3) Once you select 1780-1680cm -1 Range, calculate the FWHH value by clicking the corresponding button.
[0140] For all samples, the average of the FWHH values obtained was then calculated (for samples with unknown crystallinity, 3 points were averaged and for samples with known thermal history, at least 10 points were averaged) and used in a consistent manner for each sample:
[0141] 1) Use the average value of the FWHH of samples with known thermal history to construct a calibration curve;
[0142] 2) Interpolate the FWHH averages of samples with unknown crystallinity on the calibration curve to derive their crystallinity.
[0143] The development of the proposed analytical method allows analyzing a targeted point of the sample to verify that the step of emitting laser radiation in the weakened portion determines the crystallinity with respect to the reference, with a local variation of the crystallinity not exceeding 3%.
[0144] The crystallinity of a reference is:
[0145] Case A) Crystallinity of non-thermoformed PET sheets;
[0146] Case B) The crystallinity of the semicircular part of the finished container is indicated as follows:
[0147] 1) At least 0.6mm from the through incision;
[0148] 2) At least 0.3mm away from the weakened part;
[0149] 3) At least 0.3mm away from heat seal;
[0150] Case C) is less preferred, the crystallinity at the heat seal ring of the finished container.
[0151] The heat seal ring was included in the reference because it has been shown to be representative of the non-thermoformed area of the PET container, as the sealing operation does not alter the crystallinity of the PET.
[0152] Example 1
[0153] Can 1 – Thickness 1.2mm
[0154] Using can 1 , with a thickness of 1.2 mm in the areas not directly subjected to the thermoforming action, a calibration curve was established which applies only to the inspection case by preparing samples with a known thermal history, obtained from the non-thermoformed and non-heat-sealed parts of can 1 .
[0155] Samples with known thermal history were prepared by DSC according to the method described below:
[0156] I. To prepare a sample with a known thermal history for analysis by Raman microscopy:
[0157] a. The first scan (1 scan) was from 30°C to 300°C at 20°C / min;
[0158] b. Isotherm: 1 min at 300 °C;
[0159] c. Cooling: 300°C to 0°C at X°C / min, X=20; quenching obtained by selecting the "Ballistic Cool to Temperature" setting; 200.
[0160] II. To prepare similar samples with known thermal history to be processed for crystallinity by DSC:
[0161] a. First scan (1 scan): from 30°C to 300°C at 20°C / min;
[0162] b. Isotherm: 1 min at 300 °C;
[0163] c. Cooling: 300°C to 0°C at X°C / min, X = 20; Quenching obtained by selecting the "Ballistic Cooling to Temperature" setting; 200;
[0164] a. Second scan (2nd scan): from 0°C to 300°C at 20°C / min.
[0165] The crystallinity of a sample with a known thermal history is determined by DSC by processing the second scan (2 scans) to calculate the crystallinity due to the cooling step at a specified rate. The treatment takes into account the thermogram of the second scan. By setting a "standard" linear integration baseline, the melting heat value (ΔHf) and cold crystallization value (ΔHcc) normalized for the sample mass are obtained by integrating the exothermic peaks generated by cold crystallization and the endothermic peaks generated by melting. The melting peak and the cold crystallization peak are processed so that the integral baseline is consistent with the baseline of the specific thermogram. According to this principle, only for the case proposed in this embodiment, the melting peak is processed in the temperature range of 210°C-262°C, and the cold crystallization peak is processed in the temperature range of 137°C-183°C. In the case where the sample is cooled at 20°C / min, the thermogram does not show the peak caused by cold crystallization in the second heating.
[0166] Fig.12 and Fig.13 A typical processed thermogram showing the cold crystallization peak and the melting peak.
[0167] In particular, Fig.12 is an example of the treatment of cold crystallization peaks in the second scan of a calorimetric analysis, while Fig.13 is an example of the processing of melting peaks in the second scan of a calorimetric analysis.
[0168] For each calorimetric analysis considered, the following formula applies:
[0169] XC 冷却后 (%) = (ΔH f -│ΔH cc │)*100 / 140
[0170] The crystallinity of samples with known thermal history can thus be inferred from thermal analysis (DSC).
[0171] Samples with known thermal history prepared for Raman microscopy analysis were appropriately sliced and inserted into appropriate sample holders to obtain at least 10 spectra in the longitudinal direction of the slice ( Fig.14 ).
[0172] Fig.15 , Fig.16 and Fig.17 Images showing the set analysis conditions reported descriptively in the previous sections.
[0173] Fig.18 An example of processing acquired spectra in the manner described in the previous sections is shown.
[0174] After processing each spectrum, the mean of the FWHH values obtained for each sample was calculated. These values were used to construct the ordinate axis of the calibration curve, which was specific to tank 1, and the crystallinity of the homologous sample obtained by processing the corresponding thermogram and used to construct the abscissa axis.
[0175] The points of the graph were then processed by a linear trend line, the equation of which was used for subsequent interpolation of the FWHH values of the unknown crystallinity samples from Can 1 (but not from the others).
[0176] Fig.19 The straight calibration line for tank 1 is shown, including Eq.
[0177]
[0178] Table 1 - Values calculated by DSC and Raman microscopy used to construct calibration curves.
[0179] Since the initial PET sheet was not available, in the Can 1 sample the reference area was located in a semicircular section of the finished can:
[0180] - At least 0.6mm from the through cut;
[0181] - At least 0.3mm away from the weakened part;
[0182] - At least 0.3mm from the heat seal area.
[0183] In the portion thus determined, 3 spectra were acquired using Raman microscopy (the method of acquiring the spectra and the corresponding processing were carried out as described above for Raman microscopy) and the average of the FWHH values was calculated. The average FWHH value was then inserted into the straight calibration line constructed for Can 1. This operation allowed the crystallinity of the Can 1 reference to be calculated.
[0184]
[0185] Table 2 - Reference portion of Can 1. Xc (%) was calculated using the straight calibration line equation associated with Can 1.
[0186] Continuous weakening part
[0187] a) Use a laser with a power of 300W and a speed equal to 21m / min.
[0188] Spectra were obtained by Raman microscopy, analyzing the sample surface below the weakened portion (called the "groove").
[0189]
[0190] Table 3 - Raman microscopy of the grooves of the continuous weakened section. The data refer to a laser firing step with a power of 300 W and a speed of 21 m / min. For the calculation of Xc (%), the equation of the straight calibration line associated with tank 1 was used.
[0191] The average Xc value (%) at the slot of the weakened portion was compared with the average Xc value (%) of the reference by setting the formula ΔXc (%) = weakened portion Xc (%) - "reference" Xc (%)
[0192] Table 4 - Change in crystallinity between Xc(%) in the weakened portion and Xc(%) of the previously defined "reference".
[0193] b) Use a laser with a power of 750 W and a speed of 77 m / min.
[0194] Spectra were obtained by Raman microscopy, analyzing the sample surface below the weakened portion (called the "groove").
[0195]
[0196] Table 5 - Raman microscopy of the grooves of the continuous weakened section. The data refer to a laser firing step with a power of 750 W and a speed of 77 m / min. For the calculation of Xc (%), the equation of the straight calibration line associated with tank 1 was used.
[0197] The average Xc value (%) of the weakened portion grooves was compared to the average Xc value (%) of the reference by setting the formula ΔXc(%) = weakened portion Xc(%) - "reference" Xc(%).
[0198]
[0199] Table 6 - Change in crystallinity between Xc(%) in the weakened portion and Xc(%) of the previously defined "reference".
[0200] c) Use a laser with a power of 1200 W and a speed of 124 m / min.
[0201] Spectra were obtained by Raman microscopy, analyzing the sample surface below the weakened portion (called the "groove").
[0202]
[0203] Table 7 - Raman microscopy of the grooves of the continuous weakened section. The data refer to a laser firing step with a power of 1200 W and a speed of 124 m / min. For the calculation of Xc (%) the equation of the straight calibration line associated with Can 1 was used.
[0204] The Xc average (%) of the grooves of the weakened portion is compared to the Xc average (%) of the reference by setting the formula ΔXc (%) = weakened portion Xc (%) - "reference" Xc (%).
[0205]
[0206] Table 8 - Change in crystallinity between Xc(%) in the weakened portion and Xc(%) of the previously defined "reference".
[0207] Weakened section with through opening
[0208] a) Use a laser with a power of 300 W and a speed of 20 m / min.
[0209] Spectra were obtained by Raman microscopy, analyzing the sample surface of three solid regions of the weakened portion (called "bridges") at points substantially equidistant from the through-opening.
[0210]
[0211]
[0212] Table 9 - Raman microscopy of bridges provided with weakened portions with through openings. The data refer to laser shot steps with a power of 300 W and a speed of 20 m / min. For the calculation of Xc (%) the equation for the straight calibration line associated with Can 1 was used.
[0213] The Xc average (%) of the grooves of the weakened portion is compared to the Xc average (%) of the reference by setting the formula ΔXc (%) = weakened portion Xc (%) - "reference" Xc (%).
[0214]
[0215] Table 10 - Change in crystallinity between Xc(%) in the weakened portion and Xc(%) of the previously defined "reference".
[0216] b) Use a laser with a power of 750 W and a speed of 45 m / min.
[0217] Spectra were obtained by Raman microscopy, analyzing the sample surface of three solid regions of the weakened portion (called "bridges") at points substantially equidistant from the through-opening.
[0218]
[0219] Table 11 - Raman microscopy of bridges with weakened portions provided with through openings. The data refer to a laser shot step with a power of 750 W and a speed of 45 m / min. For the calculation of Xc (%) the straight calibration line equation associated with Can 1 was used.
[0220] The Xc average (%) of the grooves of the weakened portion was compared to the Xc average (%) of the reference by setting the formula ΔXc(%) = weakened portion Xc(%) - "reference" Xc(%).
[0221]
[0222] Table 12 - Change in crystallinity between Xc(%) in the weakened portion and Xc(%) of the previously defined "reference".
[0223] c) Use a laser with a power of 1200 W and a speed of 72 m / min.
[0224] Spectra were obtained by Raman microscopy, analyzing the sample surface of three solid regions of the weakened portion (called "bridges") at points substantially equidistant from the through-opening.
[0225]
[0226] Table 13 - Raman microscopy of bridges provided with weakened portions with through openings. Data refer to laser shot steps with a power of 1200 W and a speed of 72 m / min. For the calculation of Xc (%) the straight calibration line equation associated with Can 1 was used.
[0227] The Xc average (%) of the grooves of the weakened portion was compared to the Xc average (%) of the reference by setting the formula ΔXc(%) = weakened portion Xc(%) - "reference" Xc(%).
[0228]
[0229] Table 14 - Change in crystallinity between Xc(%) in the weakened portion and Xc(%) of the previously defined "reference".
[0230] Research on heat sealing ring
[0231] In order to correctly define the reference for the subsequent measurements of the crystallinity variations associated with the laser firing steps, the heat seal ring in can 1 was studied. In particular, by Raman microscopy, the FWHH values of the upper and lower non-thermoformed areas of the can at the heat seal ring were calculated and interpolated on a straight calibration line to calculate the crystallinity in said points and compare them with that of the reference.
[0232] In this case, three points at the upper and lower parts of the heat seal ring were also analyzed.
[0233]
[0234] Table 15 - Study of heat seal rings. The term "upper" is understood to mean the upper part of the can, while the term "lower" is understood to mean the lower part. For the calculation of Xc (%), the equation of the straight calibration line associated with can 1 was used.
[0235]
[0236] Table 16 - Change in crystallinity between Xc(%) of the upper and lower regions of the heat seal ring and the Xc(%) of the previously defined "reference".
[0237] Example 2
[0238] Can 2 - Thickness 1.27mm
[0239] Using can 2, 1.27 mm thick in the areas not directly subjected to the action of thermoforming, a calibration curve was constructed by preparing samples with known thermal history obtained from non-thermoformed and non-heat-sealed parts of can 2, valid only for the case examined.
[0240] Since the various steps for constructing the calibration curve have been described in detail in Example 1 related to Tank 1 and there are no changes in Example 2 for Tank 2, they will be omitted below and the focus will be on the differences made for Tank 2.
[0241] Similar samples with known thermal history were prepared by cooling from 300°C to 0°C at X°C / min, where X = 20, 100, quenching obtained by selecting the "Ballistic Cool to Temperature" setting.
[0242] To analyze samples with known thermal history, in particular to determine the degree of crystallinity by DSC calorimetry, the melting peak in the temperature range 210°C-266°C and the cold crystallization peak in the temperature range 120°C-165°C were processed.
[0243] Raman analysis was performed following the procedures already given without significant modifications.
[0244] For Tank 2, the FWHH average from Raman microscopy and the crystallinity average from DSC were processed by a linear trend line, and this equation was used to interpolate samples from the same Tank 2 (and not others) with unknown crystallinity.
[0245] Fig. 20 The straight calibration line for tank 2 is shown, including Eq.
[0246]
[0247]
[0248] Table 17 - Values calculated by DSC and Raman microscopy used to construct calibration curves.
[0249] Since the initial PET sheet was not available, in the Can 2 sample the reference area was located in a semicircular section of the finished can:
[0250] - At least 0.6mm from the through cut;
[0251] - At least 0.3mm away from the weakened part;
[0252] - At least 0.3mm from the heat seal area.
[0253] In the portion thus determined, 3 spectra were obtained using Raman microscopy (the method of obtaining the spectra and the corresponding processing were performed as described above for Raman microscopy) and the average of the FWHH values was calculated. The average FWHH value was then interpolated into the straight calibration line constructed for Tank 2. This operation allowed the calculation of the crystallinity of the Tank 2 reference.
[0254]
[0255] Table 18 - Reference portion of tank 2. For the calculation of Xc (%), the equation for the straight calibration line associated with tank 2 was used.
[0256] Continuous weakening part
[0257] a) Use a laser with a power of 300W and a speed equal to 22m / min.
[0258] Spectra were obtained by Raman microscopy, analyzing the sample surface below the weakened portion (called the "groove").
[0259]
[0260] Table 19 - Raman microscopy of the grooves of the continuous weakened section. The data refer to a laser firing step with a power of 300 W and a speed of 22 m / min. For the calculation of Xc (%), the equation of the straight calibration line associated with tank 2 was used.
[0261] The Xc average (%) of the grooves of the weakened portion was compared to the Xc average (%) of the reference by setting the formula ΔXc(%)=weakened portion Xc(%)-"reference" Xc(%).
[0262]
[0263] Table 20 - Change in crystallinity between Xc(%) in the weakened portion and Xc(%) of the previously defined "reference".
[0264] b) Use a laser with a power of 750 W and a speed equal to 68 m / min.
[0265] Spectra were obtained by Raman microscopy, analyzing the sample surface below the weakened portion (called the "groove").
[0266]
[0267] Table 21 - Raman microscopy of the grooves of the continuous weakened section. The data refer to a laser firing step with a power of 750 W and a speed of 68 m / min. For the calculation of Xc (%), the equation of the straight calibration line associated with tank 2 was used.
[0268] The Xc average (%) of the grooves of the weakened portion was compared to the Xc average (%) of the reference by setting the formula ΔXc(%)=weakened portion Xc(%)-"reference" Xc(%).
[0269]
[0270] Table 22 - Change in crystallinity between Xc(%) in the weakened portion and Xc(%) of the previously defined "reference".
[0271] c) Use a laser with a power of 1200 W and a speed equal to 109 m / min.
[0272] Spectra were obtained by Raman microscopy, analyzing the sample surface below the weakened portion (called the "groove").
[0273]
[0274]
[0275] Table 23 - Raman microscopy of the grooves of the continuous weakened section. The data refer to a laser firing step with a power of 1200 W and a speed of 109 m / min. For the calculation of Xc (%), the equation of the straight calibration line associated with tank 2 was used.
[0276] The Xc average (%) of the grooves of the weakened portion was compared to the Xc average (%) of the reference by setting the formula ΔXc(%)=weakened portion Xc(%)-"reference" Xc(%).
[0277]
[0278] Table 24 - Change in crystallinity between Xc(%) in the weakened portion and Xc(%) of the previously defined "reference".
[0279] Weakened section with through opening
[0280] a) Use a laser with a power of 300 W and a speed of 21 m / min.
[0281] Spectra were obtained by Raman microscopy, analyzing the sample surface of three solid regions of the weakened portion (called "bridges") at points substantially equidistant from the through-opening.
[0282]
[0283] Table 25 - Raman microscopy of bridges provided with weakened portions with through openings. Data refer to laser firing steps with a power of 300 W and a speed of 21 m / min. For the calculation of Xc (%) the equation for the straight calibration line associated with tank 2 was used.
[0284] The Xc average (%) of the grooves of the weakened portion was compared to the Xc average (%) of the reference by setting the formula ΔXc(%)=weakened portion Xc(%)-"reference" Xc(%).
[0285]
[0286] Table 26 - Change in crystallinity between Xc in the weakened portion and Xc of the previously defined "reference".
[0287] b) Use a laser with a power of 750 W and a speed of 55 m / min.
[0288] Spectra were obtained by Raman microscopy, analyzing the sample surface of three solid regions of the weakened portion (called "bridges") at points substantially equidistant from the through-opening.
[0289]
[0290] Table 27 - Raman microscopy of bridges provided with weakened portions with through openings. Data refer to laser firing steps with a power of 750 W and a speed of 55 m / min. For the calculation of Xc (%) the equation for the straight calibration line associated with Can 2 was used.
[0291] The Xc average (%) of the grooves of the weakened portion was compared to the Xc average (%) of the reference by setting the formula ΔXc(%)=weakened portion Xc(%)-"reference" Xc(%).
[0292]
[0293] Table 28 - Change in crystallinity between Xc in the weakened portion and Xc of the previously defined "reference".
[0294] c) Use a laser with a power of 1200 W and a speed of 88 m / min.
[0295] Spectra were obtained by Raman microscopy, analyzing the sample surface at three solid areas (called "bridges") in the weakened portion at points substantially equidistant from the through-opening.
[0296]
[0297] Table 29 - Raman microscopy of bridges provided with weakened portions with through openings. Data refer to laser firing steps with a power of 1200 W and a speed of 88 m / min. For the calculation of Xc (%) the equation for the straight calibration line associated with tank 2 was used.
[0298] The Xc average (%) of the grooves of the weakened portion was compared to the Xc average (%) of the reference by setting the formula ΔXc(%)=weakened portion Xc(%)-"reference" Xc(%).
[0299]
[0300] Table 30 - Change in crystallinity between Xc(%) in the weakened portion and Xc(%) of the previously defined "reference".
[0301] Research on heat sealing ring
[0302] In order to correctly define the reference for the subsequent measurements of the crystallinity variations associated with the laser firing steps, the heat seal ring in can 2 was studied. In particular, by Raman microscopy, the FWHH values of the upper and lower non-thermoformed areas of the can at the heat seal ring were calculated and interpolated on a straight calibration line to calculate the crystallinity in said points and compare them with the crystallinity of the can.
[0303] In this case, three points at the upper and lower parts of the heat seal ring were also analyzed.
[0304]
[0305] Table 31 - Study of heat seal rings. The term "upper" is understood to mean the upper part of the can and the term "lower" is understood to mean the lower part. For the calculation of Xc (%), the equation of the straight calibration line associated with can 2 was used.
[0306]
[0307] Table 32 - Change in crystallinity between Xc(%) of the upper and lower regions of the heat seal ring and the Xc(%) of the previously defined "reference".
[0308] Example 3
[0309] Sheet made of PET, 1mm thick.
[0310] Using a sheet made of PET with a thickness of 1 mm, a calibration curve was constructed by preparing samples with a known thermal history (obtained on a portion of the sheet not exposed to the laser), which calibration curve applies only to the case examined.
[0311] Since the various steps for constructing the calibration curve have been described in detail in Example 1 with reference to Can 1 and are unchanged for the PET sheet, they will be omitted hereinafter and attention will be focused on the differences made for the PET sheet.
[0312] Similar specimens with known thermal history were prepared by cooling from 300°C to 0°C at X°C / min, X = 20, 50, 100, 200, quenching obtained by selecting the "Ballistic Cool to Temperature" setting.
[0313] For the analysis of samples with known thermal history, in particular for the determination of the degree of crystallinity by DSC calorimetric analysis, melting peaks in the temperature range 210°C-263°C and cold crystallization peaks in the temperature range 118°C-185°C were processed.
[0314] Raman analysis was performed according to the already specified procedures without significant modifications.
[0315] For sheets with a thickness of 1 mm, the FWHH averages from Raman microscopy and the crystallinity averages from DSC were processed by a linear trend line, whose equation was used to interpolate samples of unknown crystallinity originating from the same 1 mm sheet (but not others).
[0316] Fig.21 A straight calibration line for a 1 mm sheet made of PET is shown, including the equation.
[0317]
[0318] Table 33 - Values calculated by DSC and Raman microscopy used to construct the calibration curve.
[0319] The equation thus constructed relating the straight calibration line was used to derive the crystallinity of the reference and weakened sections to verify that the variation between the two crystallinities was less than 3%.
[0320] On the surface of a sheet made of PET not subjected to the action of the laser, 3 spectra were obtained by Raman microscopy (the mode of spectral acquisition and the associated processing were performed as described previously) and the average of the calculated FWHH values was calculated. The average FWHH value was then inserted into a straight calibration line constructed for a 1 mm PET sheet. This operation allows the calculation of the crystallinity of the sheet not subjected to the action of the laser.
[0321]
[0322] Table 34 - Part of the sheet surface analysed which was not exposed to the laser. For the calculation of Xc (%) the straight calibration line constructed for this sample was used.
[0323] Continuous weakening part
[0324] a) Use a laser with a power of 300 W and a speed of 22 m / min.
[0325] Spectra were obtained by Raman microscopy, analyzing the sample surface below the weakened portion (called the "groove").
[0326]
[0327] Table 35 - Raman microscopy of grooves of continuous weakened sections. Data refer to a laser firing step with a power of 300 W and a rate of 22 m / min. Xc (%) was calculated using the equation of the straight calibration line associated with a 1-mm PET sheet.
[0328] The Xc average (%) of the grooves of the weakened portion was compared to the Xc average (%) of the reference by setting the formula ΔXc(%)=weakened portion Xc(%)-"reference" Xc(%).
[0329]
[0330] Table 36 - Change in crystallinity between Xc(%) in the weakened portion and Xc(%) of the previously defined "reference".
[0331] b) Use a laser with a power of 750 W and a speed of 32 m / min.
[0332] Spectra were obtained by Raman microscopy, analyzing the sample surface below the weakened portion (called the "groove").
[0333]
[0334] Table 37 - Raman microscopy of the grooves of the continuous weakened portion. Data refer to a laser firing step with a power of 750 W and a speed of 32 m / min. Xc (%) was calculated using the equation of the straight calibration line associated with a 1-mm PET sheet.
[0335] The Xc average (%) of the grooves of the weakened portion was compared to the Xc average (%) of the reference by setting the formula ΔXc(%)=weakened portion Xc(%)-"reference" Xc(%).
[0336]
[0337] Table 38 - Change in crystallinity between Xc(%) in the weakened portion and Xc(%) of the previously defined "reference".
[0338] c) Use a laser with a power of 1200 W and a speed of 92 m / min.
[0339] Spectra were obtained by Raman microscopy, analyzing the sample surface below the weakened portion (called the "groove").
[0340]
[0341] Table 39 - Raman microscopy of the grooves of the continuous weakened portion. Data refer to a laser firing step with a power of 1200 W and a speed of 92 m / min. Xc (%) was calculated using the equation of the straight calibration line associated with a 1-mm PET sheet.
[0342] The Xc average (%) of the grooves of the weakened portion was compared to the Xc average (%) of the reference by setting the formula ΔXc(%)=weakened portion Xc(%)-"reference" Xc(%).
[0343]
[0344]
[0345] Table 40 - Change in crystallinity between Xc(%) in the weakened portion and Xc(%) of the previously defined "reference".
[0346] Weakened section with through opening
[0347] a) Use a laser with a power of 300 W and a speed of 20 m / min.
[0348] Spectra were obtained by Raman microscopy, analyzing the sample surface of three solid regions of the weakened portion (called "bridges") at points substantially equidistant from the through-opening.
[0349]
[0350] Table 41 - Raman microscopy of bridges with weakened portions having through openings. Data refer to laser firing steps with a power of 300 W and a speed of 20 m / min. Xc (%) was calculated using the equation for the straight calibration line associated with a 1-mm PET sheet.
[0351] The Xc average (%) of the grooves of the weakened portion was compared to the Xc average (%) of the reference by setting the formula ΔXc(%)=weakened portion Xc(%)-"reference" Xc(%).
[0352]
[0353] Table 42 - Change in crystallinity between Xc(%) in the weakened portion and Xc(%) of the previously defined "reference".
[0354] b) Use a laser with a power of 750 W and a speed of 25 m / min.
[0355] Spectra were obtained by Raman microscopy, analyzing the sample surface of three solid regions of the weakened portion (called "bridges") at points substantially equidistant from the through-opening.
[0356]
[0357] Table 43 - Raman microscopy of bridges with weakened portions provided with through openings. Data refer to a laser firing step with a power of 750 W and a speed of 25 m / min. Xc (%) was calculated using the equation for the straight calibration line associated with a 1-mm PET sheet.
[0358] The Xc average (%) of the grooves of the weakened portion was compared to the Xc average (%) of the reference by setting the formula ΔXc(%)=weakened portion Xc(%)-"reference" Xc(%).
[0359]
[0360] Table 44 - Change in crystallinity between Xc(%) in the weakened portion and Xc(%) of the previously defined "reference".
[0361] c) Use a laser with a power of 1200 W and a speed of 58 / min.
[0362] Spectra were obtained by Raman microscopy, analyzing the sample surface of three solid regions of the weakened portion (called "bridges") at points substantially equidistant from the through-opening.
[0363]
[0364] Table 45 - Raman microscopy of bridges with weakened portions having through openings. Data refer to laser firing steps with a power of 1200 W and a speed of 58 m / min. Xc (%) was calculated using the straight calibration line equation associated with a 1-mm PET sheet.
[0365] The Xc average (%) of the grooves of the weakened portion was compared to the Xc average (%) of the reference by setting the formula ΔXc(%)=weakened portion Xc(%)-"reference" Xc(%).
[0366]
[0367] Table 46 - Change in crystallinity between Xc(%) in the weakened portion and Xc(%) of the previously defined "reference".
[0368] Example 4
[0369] Sheet made of PET, 1mm thick.
[0370] Low power and low speed testing.
[0371] In order to verify the effect of low-power laser (power less than 250 W) acting on PET sheet at low speed (speed less than 15 m / min), the following test was conducted.
[0372] The samples tested were similar to those in the previous Example 3: the straight calibration line constructed and displayed for the samples of Example 3 is therefore also valid for the Example 4 under consideration and is used in the calculations reported below to verify that the variation between the crystallinity of the reference area and the weakened portion is less than 3%.
[0373] On the surface of the PET sheet not exposed to the laser, three spectra were acquired by Raman microscopy (spectral acquisition mode and related processing were performed as described above) and the average of the calculated FWHH values was calculated. The average FWHH value was then inserted into the straight calibration line constructed for the 1-mm PET sheet. This operation allowed the calculation of the crystallinity of the sheet not exposed to the laser.
[0374]
[0375] Table 47 - Part of the sheet surface analysed which was not exposed to the laser. For the calculation of Xc (%) the straight calibration line constructed for this sample was used.
[0376] Low power and low speed testing.
[0377] a) Use a laser with a power of 150 W and a speed of 13 m / min.
[0378] Spectra were obtained by Raman microscopy, analyzing the sample surface below the weakened portion (called the "groove").
[0379]
[0380] Table 48 - Raman microscopy of the grooves of the continuous weakened portion. Data refer to laser firing steps with a power of 150 W and a speed of 13 m / min. Xc (%) was calculated using the equation of the straight calibration line associated with a 1-mm PET sheet.
[0381] The Xc average (%) of the grooves of the weakened portion was compared to the Xc average (%) of the reference by setting the formula ΔXc(%)=weakened portion Xc(%)-"reference" Xc(%).
[0382]
[0383] Table 49 - Change in crystallinity between Xc(%) in the weakened portion and Xc(%) of the previously defined "reference".
[0384] b) Use a laser with a power of 75 W and a speed of 8 m / min.
[0385] Spectra were obtained by Raman microscopy, analyzing the sample surface below the weakened portion (called the "groove").
[0386]
[0387] Table 50 - Raman microscopy of the grooves of the continuous weakened portion. Data refer to a laser firing step with a power of 75 W and a speed of 8 m / min. Xc (%) was calculated using the equation of the straight calibration line associated with a 1-mm PET sheet.
[0388] The Xc average (%) of the grooves of the weakened portion was compared to the Xc average (%) of the reference by setting the formula ΔXc(%)=weakened portion Xc(%)-"reference" Xc(%).
[0389]
[0390] Table 51 - Change in crystallinity between Xc(%) in the weakened portion and Xc(%) of the previously defined "reference".
[0391] In the tests carried out on this Example 4 at low power and low speed, it was observed that even with the use of low power laser shot steps acting at low speed, it was possible to provide a continuous weakening with a reduced cross section suitable for facilitating the separation of the can at the weakening thus provided. However, from the subsequent analysis, it has been observed that working under these conditions, an increase in crystallinity is obtained in the weakened portion, so that the variation in crystallinity between the weakened portion and the reference is greater than the +3% value previously indicated.
[0392] On the one hand, this finding is consistent with what has been reported in the literature, according to which an increase in the crystallinity is associated with an increase in the brittleness of the sample; on the other hand, it confirms that the effect of the laser radiation has an impact on the material that is more than just a reduction in the cross section. The application of heat associated with the laser radiation and transferred to the material actually confers a change in the local properties of the material, ranging from a mere change in the state of tension of the material (high power and high speed laser radiation) to an increase in the crystallinity (low power and low speed laser radiation).
[0393] The low action speed of the laser (equal to 13 m / min for the 150-W laser and 8 m / min for the 75-W laser), still leads to the desired result of separation of the cans from each other, however, also corresponds to a longer production time of the weakened parts, thus outlining a situation that is incompatible with high industrial productivity requirements.
[0394] In practice it has been found that the invention achieves the intended aim and objects by providing a method which is very flexible and which enables the provision of weakened portions, even on containers made of PET, which allow practical and simple separation of the containers from one another.
[0395] In practice it has been found that the invention achieves the intended aim and objects, providing an extremely flexible method capable of allowing the provision of weakened portions even on containers made of PET, which allow practical and simple separation of the containers from one another.
[0396] The advantages of the method described in the present invention can be traced back to the possibility of operating with a particularly powerful laser radiation emission system, which in particular allows solving the problem of producing PET containers, avoiding the use of blades or knives and reducing the costs related to system maintenance, allowing containers of different shapes and sizes to be provided with an extremely flexible method and allowing having a system that maintains industrial production high speeds.
[0397] The invention thus conceived is susceptible of numerous modifications and variations, all of which are within the scope of the appended claims; moreover, all the details may be replaced by other technically equivalent elements.
[0398] In practice, the materials used, as long as they are compatible with the specific use, as well as the possible shapes and dimensions, may be any according to requirements and the state of the art.
[0399] The disclosures in Italian Patent Application No. 102020000000787 from which this application claims priority are incorporated herein by reference.
[0400] In case reference signs are attached to the technical features mentioned in any claim, the sole purpose of these reference signs is to increase the intelligibility of the claim and therefore these reference signs have no limiting effect on the interpretation of each element exemplarily identified by these reference signs.
Claims
1. A method for producing and filling a container designed to contain food, characterized in that The method comprises the following steps: - shaping a sheet (10) made of PET (polyethylene terephthalate) to provide a plurality of containment containers (11), the containment containers (11) being provided with at least one access opening (12), the initial crystallinity of the PET sheet being lower than or equal to 10%; - filling the receiving container (11) with at least one food through the access opening (12); - sealing the access opening (12) by means of a closing membrane (13); - providing a weakened portion (21) at a connecting edge (22) between at least two adjacent containing containers (11), the providing step comprising the steps of: emitting laser radiation (40) at at least a portion of the connecting edge (22) to provide a local reduction in the cross section of the connecting edge (22) along the weakened portion (21); - after the laser radiation emission step, the final crystallinity at the weakened portion (21) is lower than, equal to or greater than the crystallinity of the portion of the connecting edge (22) not affected by the changes caused by the laser radiation (40) emission step and the sealing step by a percentage of at most 3%.
2. The method according to claim 1, characterized in that The thickness of the connecting edge is 300 micrometers to 1800 micrometers.
3. The method according to claim 1 or 2, characterized in that: The sheet (10) made of PET includes a sheet made of transparent PET.
4. The method according to claim 1 or 2, characterized in that: The providing step includes the step of emitting laser radiation with a power of 250 W to 1500 W at a speed of 15 m / min to 170 m / min.
5. The method according to claim 1 or 2, characterized in that: The providing step comprises the step of emitting laser radiation with a power greater than 500 W and a speed greater than 60 m / min and more preferably greater than 80 m / min.
6. The method according to claim 1 or 2, characterized in that: The providing step is adapted to provide a local reduction of the connecting edge, the local reduction being substantially constant along the longitudinal extension of the weakened portion.
7. The method according to claim 1 or 2, characterized in that: The providing step is adapted to provide a plurality of through openings through the connecting edge, the plurality of through openings being spaced apart from each other to provide the weakened portion.
8. The method according to claim 1 or 2, characterized in that: The crystallinity of the area subjected to the laser radiation emission step is calculated by Raman microscopy analysis on at least three points of the sample and by measuring the crystallinity of the area under the coverage of 1700-1760 cm -1 The Raman shift gap signal is calculated by interpolating the FWHH of the average value obtained on the calibration curve.
9. The method according to claim 1 or 2, characterized in that: If the weakened portion comprises a local reduction of the connecting edge (22) of constant longitudinal extension, or if the weakened portion is formed in a solid area which is equidistant from the through opening in the weakened portion (21) provided with the through opening, the area of interest on which at least three points of the sample are identified in order to calculate the crystallinity of the area subjected to the emission step is defined in the lower part ("groove") of the weakened portion (21).
10. The method according to claim 1 or 2, characterized in that: The step of providing a weakened portion (21) is performed after the sealing step.
11. The method according to claim 1 or 2, characterized in that: The method comprises a sterilization step carried out upstream or downstream of the thermoforming step.
12. The method according to claim 1 or 2, characterized in that: The method essentially comprises during the emitting step a step of extracting gases and volatile substances.
Citation Information
Patent Citations
Forming apparatus and method and object thus made
CN104411476A
Method for removing brittle-hard material by means of laser radiation
CN105377500A
Container with frangible weakened portion and manufacture thereof
CN108495793A
Weakening apparatus and method for weakening packaging materials
CN110139746A
Apparatus for heating preforms made of thermoplastic material
CN110177671A