A method to avoid wall damage in ultrafast laser processing of cavities
By using a step-by-step drilling method of black alumina ceramic particles and sodium thiosulfate in ultrafast laser processing, combined with the absorption effect of the filler, the problem of cavity-to-wall damage is solved, the processing efficiency and quality are improved, and the Effective protection against walls.
Patent Information
- Application Number
- CN202210638885.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-07
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-06-07
AI Technical Summary
During ultrafast laser processing, it is difficult to effectively protect the wall damage of the cavity structure. The existing technology has insufficient accessibility and removal of filling materials, and the control technology is immature, which affects the processing efficiency and quality of the parts.
Black alumina ceramic particles and sodium thiosulfate are used as filling materials. Through the step-by-step drilling method and the combination of fillers, high-power drilling is performed first and then low-power trimming is used. The fillers are used to absorb laser energy to prevent damage to the wall, and The filler is removed after processing by heating and washing with water.
It effectively avoids damage to the opposite wall of the cavity, improves the processing efficiency and quality of the parts, significantly reduces the ablation of the opposite wall material, solves the problem of insufficient process control timeliness, and ensures the reuse and removal of the filler sex.
Smart Images

Figure CN115026420B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ultrafast laser processing, and in particular to a wall damage protection strategy for ultrafast laser processing of cavity-containing parts. Background Art
[0002] Ultrafast laser refers to laser pulse width in the picosecond or femtosecond range. Ultrafast laser processing is an important part of the field of precision processing. As a non-contact processing method, ultrafast laser processing is fast, flexible, and widely applicable to difficult-to-process materials. Due to its extremely short pulse time and ultra-high peak power, it can achieve "cold processing" of materials. With reasonable processing technology, it can achieve precision processing of materials without heat-affected zones, recast layers, and microcracks.
[0003] It is inevitable that there will be cavity structures inside parts processed by ultrafast lasers, and the distance between cavities is generally small. However, during the ultrafast laser processing process, the energy at the center of the laser beam spot is higher and the heat accumulates faster, resulting in sufficient laser energy within a certain range in the processing direction, making the material removal rate at the center of the spot much greater than that at the edge. For processing methods such as drilling, this uneven processing depth will cause the microholes to be opened preferentially from the center of the spot. At this time, the edges of the microholes are uneven. In order to make the edges of the microhole outlets smooth, the laser processing time needs to be extended to trim the microholes. During the trimming process, the center of the high-energy laser beam spot will pass through the cavity and directly irradiate the surface of the opposite wall of the cavity, which is very likely to cause the removal of the opposite wall material, thereby causing damage to the wall, and in severe cases, the entire part will be scrapped. Therefore, damage-free processing of the opposite wall at a small cavity distance is one of the problems that need to be urgently solved in the application and promotion of ultrafast laser technology in this scenario.
[0004] At present, there are usually two strategies for protecting the wall of ultrafast laser processing cavities: one is to use filling materials, that is, to fill the cavity with appropriate materials to block the laser from removing the opposite wall material; the other strategy is to achieve it through penetration sensing technology, that is, to control the laser energy to decrease rapidly at the moment of microhole penetration to avoid the removal of the opposite wall material. However, the research on the above two methods has its limitations. Usually, when selecting the filling material in the cavity, only the melting point, thermal conductivity and other characteristics of the material itself are considered, and its accessibility during filling and removability after processing are rarely considered. The filling performance of the filler will directly affect the protection effect of wall damage. In addition, the removal of the material after processing is an important factor affecting the overall processing efficiency of the parts. In terms of process control, in theory, controlling the laser energy through software is low-cost and effective, but this technology requires extremely high real-time requirements for the system, and the current control technology is not yet mature. And because the ultrafast laser action time is extremely short, it is very easy to cause damage to the opposite wall material in the process of controlling the laser power reduction. Summary of the invention
[0005] The present invention aims to solve the current technical problem of wall damage in ultrafast laser processing of cavity-containing parts and provide a method for avoiding wall damage in ultrafast laser processing of cavities.
[0006] The method of the present invention for avoiding damage to the wall in ultrafast laser processing of the cavity is carried out according to the following steps:
[0007] 1. First, process the part to keep only one opening, and seal the rest of the openings; then heat the filler black alumina ceramic particles and the base material sodium thiosulfate together to 60°C~70°C to completely melt the sodium thiosulfate into liquid, and then fill the heated filler black alumina ceramic particles into the cavity of the part from the opening of the part and fill the cavity; then fill the liquid sodium thiosulfate into the cavity of the part to fill the remaining space in the cavity, place the open end of the part vertically upward, cool the part naturally to room temperature to solidify the sodium thiosulfate, and then seal the open end of the part;
[0008] The part is a hollow metal part having at least one opening;
[0009] The particle size of the black alumina ceramic particles is smaller than the opening size of the part;
[0010] 2. Perform ultrafast laser drilling on the cooled parts. First, select 10W~20W high-power high-efficiency drilling to 100μm~200μm from the bottom, then reduce the laser power and use 2W~8W low-power fine drilling to continue to remove the material at the bottom of the microhole until it is opened. Maintain 2W~8W low-power fine drilling to trim the edge of the hole (trimming is a prior art, for the purpose of removing burrs, etc., and is not a feature of this application) until the drilling process is completed;
[0011] 3. Open the seal of one end of the drilled part, raise the temperature to 60℃~70℃, melt the solid sodium thiosulfate into liquid again, pour out the filling material in the inner cavity of the part, and wash with water or ultrasonically clean it with water to completely remove the filling material remaining in the inner cavity of the part.
[0012] The reason why black alumina is selected as the filling material of the present invention is:
[0013] 1. Alumina ceramic materials have a high damage threshold and are difficult to process materials with high melting points. They will not react or bond with the matrix of metal parts and can be removed only by water flow or ultrasonic vibration.
[0014] 2. Compared with traditional white or transparent alumina ceramics, the use of black alumina ceramic particles can increase its absorption rate of lasers, and further reduce laser damage under the dual effects of diffuse reflection and absorption;
[0015] 3. Select alumina ceramic particles with a diameter in the range of 0.045mm~1mm to ensure the filling is as compact as possible when filling the inner cavity of the parts and strengthen the protection of the opposite wall.
[0016] The present invention selects the reason of sodium thiosulfate:
[0017] 1. Sodium thiosulfate has a low melting point of only 48°C. Considering the filling performance, it is only necessary to raise the overall temperature to above 48°C (60°C~70°C) and melt it into liquid state for filling. Liquid sodium thiosulfate has good fluidity and can be smoothly filled into the cavity gap, reducing the difficulty of filling.
[0018] 2. Sodium thiosulfate is soluble in water. If there is a small amount of filler remaining inside the part after laser processing, it can be removed by flushing with water or ultrasonic vibration;
[0019] 3. The fillers sodium thiosulfate and black alumina ceramic particles can be reused after being taken out from the inner cavity of the part, which is economical.
[0020] Advantages of the present invention:
[0021] The step-by-step drilling method (high power first, then low power) in the present invention can reduce the laser energy passing through the microhole when trimming the hole edge while maintaining the drilling efficiency. Adding fillers can further absorb the laser energy passing through the bottom of the microhole, effectively blocking the laser from irradiating the opposite wall material of the cavity, thereby preventing damage to the wall. After the laser drilling is completed, the internal filling material can be removed by simply heating the entire part. The filling material can be reused, and because the base material sodium thiosulfate is soluble in water, it is not easy to cause filler residue inside the cavity.
[0022] The present invention can effectively avoid damage to the opposite wall of the cavity during ultrafast laser processing of parts containing cavities, solves the problem of insufficient timeliness of controlling damage to the wall by a single process method and immature control technology, and improves the shortcomings of low accessibility and poor removability of existing cavity filling materials. The combination of the step-by-step drilling mode and the added filler can significantly reduce the ablation of the opposite wall material while ensuring the processing efficiency and quality of the parts. The combination of process and filler not only retains the advantages of the existing method, but also further enhances the protective effect of the cavity on the opposite wall, while also ensuring the processing efficiency and quality of the parts. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a schematic diagram of the black alumina ceramic particles and the base material sodium thiosulfate after filling in step 1 of experiment 1;
[0024] Figure 2 This is a schematic diagram of high-power and high-efficiency processing in step 2 of experiment 1;
[0025] Figure 3 This is a schematic diagram of power fine processing in step 2 of experiment 1;
[0026] Figure 4 This is a schematic diagram of the internal structure of the part after laser processing is completed in step 3 of experiment 1 and the filling inside the cavity is removed;
[0027] Figure 5 This is the macroscopic morphology of the opposite wall of the part containing the cavity after ultrafast laser processing in Experiment 1;
[0028] Figure 6 This is the macroscopic morphology of the opposite wall after the ultrafast laser processing of the cavity-containing part in Experiment 2;
[0029] Explanation of the reference numerals: 1. Drilling side of the part, 2. Wall protection side, 3. Black aluminum oxide particles, 4. Sodium thiosulfate, 5. High-power laser beam, 6. Low-power laser beam, 7. Processed through hole, 8. Cavity after removing the filler. DETAILED DESCRIPTION
[0030] Specific implementation method 1: This implementation method is a method for avoiding damage to the wall in ultrafast laser processing of the cavity, which is specifically carried out in the following steps:
[0031] 1. First, process the part to keep only one opening, and seal the rest of the openings; then heat the filler black alumina ceramic particles and the base material sodium thiosulfate together to 60°C~70°C to completely melt the sodium thiosulfate into liquid, and then fill the heated filler black alumina ceramic particles into the cavity of the part from the opening of the part and fill the cavity; then fill the liquid sodium thiosulfate into the cavity of the part to fill the remaining space in the cavity, place the open end of the part vertically upward, cool the part naturally to room temperature to solidify the sodium thiosulfate, and then seal the open end of the part;
[0032] The part is a hollow metal part having at least one opening;
[0033] The particle size of the black alumina ceramic particles is smaller than the opening size of the part;
[0034] Second, perform ultrafast laser drilling on the cooled parts. First, select 10W~20W high-power high-efficiency drilling to 100μm~200μm from the bottom, then reduce the laser power and use 2W~8W low-power fine drilling to continue removing the material at the bottom of the microhole until it is opened. Then maintain 2W~8W low-power fine drilling to trim the edge of the hole until the drilling process is completed.
[0035] 3. Open the seal of one end of the drilled part, raise the temperature to 60℃~70℃, melt the solid sodium thiosulfate into liquid again, pour out the filling material in the inner cavity of the part, and wash with water or ultrasonically clean it with water to completely remove the filling material remaining in the inner cavity of the part.
[0036] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that the particle size of the black alumina ceramic particles described in step 1 is 0.045 mm to 1 mm. Other aspects are the same as those of specific implementation method 1.
[0037] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that in step 1, the filler black alumina ceramic particles and the base material sodium thiosulfate are heated to 65° C. so that the sodium thiosulfate is completely melted into liquid. The rest is the same as specific implementation method 1 or 2.
[0038] Specific implementation method 4: This implementation method is different from the specific implementation methods 1 to 3 in that the hollow metal part described in step 1 is a nickel-based high-temperature alloy. The rest is the same as the specific implementation methods 1 to 3.
[0039] Specific implementation method 5: This implementation method is different from specific implementation method 4 in that the hollow metal part described in step 1 is made of stainless steel. The rest is the same as specific implementation method 4.
[0040] Specific implementation example 6: This implementation example is different from specific implementation example 5 in that the pulse width of the ultrafast laser in step 2 is 200 fs to 20 ps. The rest is the same as specific implementation example 5.
[0041] Specific implementation example 7: This implementation example is different from specific implementation example 6 in that: in step 2, a 14W high-power high-efficiency drilling is first selected to drill a hole to a distance of 150 μm from the bottom. The rest is the same as specific implementation example 6.
[0042] Specific implementation eight: This implementation differs from specific implementation seven in that in step two, the laser power is then reduced and a 4W low-power fine drilling method is used to continue removing the material at the bottom of the microhole until it is opened. The rest is the same as specific implementation seven.
[0043] Specific implementation method 9: This implementation method is different from specific implementation method 8 in that in step 2, the hole edge is trimmed by fine drilling with a low power of 4W until the drilling process is completed. The rest is the same as specific implementation method 7.
[0044] Specific embodiment 10: This embodiment is different from specific embodiment 7 in that: in step 3, the temperature of the drilled part is raised to 65° C. The rest is the same as specific embodiment 7.
[0045] The present invention is verified by the following tests:
[0046] Experiment 1: This experiment is a method to avoid wall damage in ultrafast laser processing cavity, and is specifically carried out in the following steps:
[0047] 1. Heat the filler black alumina ceramic particles and the base material sodium thiosulfate to 65°C to make the sodium thiosulfate completely melted into liquid, and then fill the heated filler black alumina ceramic particles into the cavity of the part from the opening of the part and fill the cavity; then fill the liquid sodium thiosulfate into the cavity of the part to fill the remaining space in the cavity, place the open end of the part vertically upward, and let the part cool naturally to room temperature to solidify the sodium thiosulfate, and then seal the open end of the part (such as Figure 1 The closing method is to glue a metal plate to the open end with glue;
[0048] The part is a hollow metal cube with one end open and the other end closed, made of nickel-based high-temperature alloy GH3230, with a wall thickness of 1.5 mm and a distance between opposite surfaces in the inner cavity of 0.5 mm;
[0049] The particle size of the black alumina ceramic particles is 0.045 mm;
[0050] 2. Perform ultrafast laser drilling on the cooled parts. First, select 14W high-power and efficient drilling to 150μm from the bottom (such as Figure 2 Then reduce the laser power and use 4W low-power fine drilling to continue removing the bottom material of the microhole until it is opened. Then keep 4W low-power fine drilling to trim the edge of the hole until the drilling process is completed (as shown in the figure). Figure 3 status shown);
[0051] 3. Open the seal of one end of the drilled part, raise the temperature to 65°C, melt the solid sodium thiosulfate into liquid again, pour out the filling material in the inner cavity of the part, and wash it with water or ultrasonically clean it with water to remove all the filling materials remaining in the inner cavity of the part (such as Figure 4 status shown).
[0052] Figure 5 This is a macroscopic morphology image (optical microscope) of the opposite wall of the hole in the cavity part processed in Experiment 1. It can be clearly seen from the figure that by using fillers in combination with step-by-step drilling, there is no trace of laser ablation on the inner surface of the nickel-based high-temperature alloy sample, indicating that this method can effectively prevent laser damage to the opposite wall material.
[0053] Experiment 2: This experiment is different from Experiment 1 in that:
[0054] The part described in step 1 is a hollow metal cube with one end open and the other end closed, made of 304 stainless steel, with a wall thickness of 1 mm, and a distance between opposite surfaces in the inner cavity of 2 mm; the particle size of the black alumina ceramic particles is 0.6 mm;
[0055] In step 2, first select 16W high-power high-efficiency drilling to 150μm from the bottom, then reduce the laser power and use 6W low-power fine drilling to continue removing the material at the bottom of the microhole until it is opened, and maintain 6W low-power fine drilling to trim the edge of the hole until the drilling process is completed.
[0056] The rest are different from Experiment 2.
[0057] Figure 6 This is the macroscopic morphology of the opposite wall of the hole in the cavity part processed in Experiment 2 (optical microscope). It can be clearly seen from the figure that by using fillers in combination with step-by-step drilling, there is no trace of laser ablation on the inner surface of the stainless steel sample, indicating that this method can effectively prevent laser damage to the opposite wall material.
Claims
1. A method for avoiding wall damage in ultrafast laser processing of a cavity, characterized in that The method to avoid wall damage in ultrafast laser processing of cavities is to proceed as follows: Step 1: First, process the part to keep only one opening, and close the other openings; then heat the filler black alumina ceramic particles and the base material sodium thiosulfate together to 60°C~70°C to make the sodium thiosulfate completely melt into liquid, and then fill the heated filler black alumina ceramic particles into the cavity of the part from the opening of the part and fill the cavity; then fill the liquid sodium thiosulfate into the cavity of the part to fill the remaining space in the cavity, place the open end of the part vertically upward, cool the part naturally to room temperature to solidify the sodium thiosulfate, and then close the open end of the part; The part is a hollow metal part having at least one opening; The particle size of the black alumina ceramic particles is smaller than the opening size of the part; Step 2: Perform ultrafast laser drilling on the cooled parts. First, select 10W~20W high-power high-efficiency drilling to 100μm~200μm from the bottom, then reduce the laser power and use 2W~8W low-power fine drilling to continue removing the material at the bottom of the microhole until it is opened. Then maintain 2W~8W low-power fine drilling to trim the edge of the hole until the drilling process is completed. Step 3: Open the seal of one end of the drilled part, raise the temperature to 60℃~70℃, melt the solid sodium thiosulfate into liquid again, pour out the filling material in the inner cavity of the part, and wash the remaining filling material in the inner cavity of the part with water or ultrasonically clean it with water to remove it completely.
2. A method for avoiding wall damage in ultrafast laser processing of a cavity according to claim 1, characterized in that The particle size of the black alumina ceramic particles described in step 1 is 0.045 mm to 1 mm.
3. A method for avoiding wall damage in ultrafast laser processing of a cavity according to claim 1, characterized in that In step 1, the filler black alumina ceramic particles and the base material sodium thiosulfate are heated together to 65° C. so that the sodium thiosulfate is completely melted into a liquid.
4. A method for avoiding wall damage in ultrafast laser processing of a cavity according to claim 1, characterized in that The hollow metal part described in step 1 is a nickel-based high-temperature alloy.
5. A method for avoiding wall damage in ultrafast laser processing of a cavity according to claim 1, characterized in that The hollow metal part described in step 1 is stainless steel.
6. A method for avoiding wall damage in ultrafast laser processing of a cavity according to claim 1, characterized in that The pulse width of the ultrafast laser in step 2 is 200fs~20ps.
7. A method for avoiding wall damage in ultrafast laser processing of a cavity according to claim 1, characterized in that In step 2, first select 14W high-power and high-efficiency drilling to 150μm from the bottom.
8. A method for avoiding wall damage in ultrafast laser processing of a cavity according to claim 1, characterized in that In step 2, the laser power is then reduced and a 4W low-power fine drilling method is used to continue removing the material at the bottom of the microhole until it is opened.
9. A method for avoiding wall damage in ultrafast laser processing of a cavity according to claim 8, characterized in that In step 2, maintain 4W low power fine drilling to trim the hole edge until the drilling process is completed.
10. A method for avoiding wall damage in ultrafast laser processing of a cavity according to claim 1, characterized in that In step 3, the temperature of the drilled parts is raised to 65°C.