A test method for accurately obtaining the cohesion of proppant packing layer

By testing the maximum friction coefficient and shear stress of the proppant, and using the least squares method to fit a straight line, the problem of difficulty in accurately obtaining the cohesion of the proppant filling layer in the existing technology is solved, and accurate cohesion measurement and Low cost operation.

CN115046920BActive Publication Date: 2024-10-25SOUTHWEST PETROLEUM UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210654901.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-10
Publication Date
2024-10-25
Estimated Expiration
2042-06-10

AI Technical Summary

Technical Problem

It is difficult to accurately test the cohesion of the proppant filling layer with existing technology, which affects the laying and filling effect of proppant in fractures, thereby affecting the effect of hydraulic fracturing modification.

Method used

By preparing proppant samples of different types and particle sizes, testing their maximum friction coefficient and shear stress, using the least squares method to fit a straight line to obtain the proppant cohesion until the determination coefficient r2 is greater than 0.85 to determine the fitting result. .

Benefits of technology

It achieves accurate acquisition of the cohesion of the proppant filling layer, has low operating cost, is suitable for a variety of proppant and wetting particles, and has wide applicability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115046920B_ABST
    Figure CN115046920B_ABST
Patent Text Reader

Abstract

The present invention discloses a test method for accurately obtaining the cohesion of a proppant filling layer, including: preparing multiple proppant samples; testing the maximum friction coefficient of each proppant sample, taking the average of multiple groups of maximum friction coefficients as the friction coefficient of the proppant sample; testing the shear stress of the proppant sample under different normal stresses, and then plotting the test data in a rectangular coordinate system with the normal stress as the horizontal coordinate and the shear stress as the vertical coordinate; taking the friction coefficient as the slope of the test data fitting line, increasing the intercept of the fitting line, taking the maximum intercept that does not change the slope as the intercept of the fitting line; back-calculating the determination coefficient; and finally determining the final intercept of the fitting line as the cohesion of the proppant sample. The present invention can accurately obtain the cohesion of the proppant filling layer; has low operating cost, strong feasibility, and does not require complex test equipment; has wide applicability, and is suitable for obtaining the cohesion of wet particles with low cohesion in addition to the proppant filling layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a testing method for accurately obtaining the cohesion of a proppant filling layer, and belongs to the technical field of oil and gas production increase and transformation. Background Art

[0002] Large-scale horizontal well multi-cluster hydraulic fracturing is a key technology for the effective exploitation of unconventional oil and gas reservoirs. During the hydraulic fracturing process, a large amount of proppant is injected into the underground fractures along with the fracturing fluid, and moves, settles and accumulates under the action of liquid carrying, proppant-proppant / fracture wall collision and proppant self-weight. Finally, it is unevenly laid and filled in the fractures and supports the fractures, delaying the closure time of the fractures after fracturing, and providing sufficient conductivity for the flow of oil and gas. The mechanical properties of the filling layer formed by the accumulation of proppant particles wetted by the fracturing fluid (hereinafter collectively referred to as the "proppant filling layer") determine the laying and filling effect of the proppant in the fracture, and ultimately affect the fracturing transformation effect.

[0003] Cohesion is one of the important indicators of the mechanical properties of proppant filling layers. Therefore, it is necessary to test the cohesion of liquids with different viscosities and proppant filling layers of different types and particle sizes to provide data support for evaluating the stability of proppant filling layers and conducting numerical simulations of proppant transport. Summary of the invention

[0004] In order to overcome the problems in the prior art, the present invention provides a testing method for accurately obtaining the cohesion of a proppant packing layer.

[0005] The technical solution provided by the present invention to solve the above technical problems is: a test method for accurately obtaining the cohesion of a proppant filling layer, comprising the following steps:

[0006] S1. Prepare multiple proppant samples;

[0007] S2. testing the maximum friction coefficient of each proppant sample, and taking the average value of multiple groups of maximum friction coefficients as the friction coefficient of the proppant sample;

[0008] S3, testing the shear stress of the proppant sample under different normal stresses, and then plotting the test data in a rectangular coordinate system with the normal stress as the abscissa and the shear stress as the ordinate;

[0009] S4, using the friction coefficient in step S2 as the slope of the test data fitting line in step S3, increasing the intercept of the fitting line, and taking the maximum intercept that does not change the slope as the intercept of the fitting line;

[0010] S5, back-calculate the determination coefficient r based on the test data in step S3 and the fitting straight line in step S4 2 , if the determination coefficient r 2If the determination coefficient is greater than 0.85, the slope and intercept obtained in step S4 are determined to be the final slope and intercept of the fitted line; if the determination coefficient is less than 0.85, steps S1-S5 are repeated until the determination coefficient r 2 Greater than 0.85;

[0011] S6. Finally, the final intercept of the fitting straight line is determined as the cohesion of the proppant sample.

[0012] A further technical solution is that the water content of each proppant sample in step S1 is the same.

[0013] A further technical solution is that the number of proppant samples in step S1 is 4 or 5.

[0014] A further technical solution is that in step S3, the shear stress of the proppant sample is tested by a rapid shear test method.

[0015] A further technical solution is that in step S4, the intercept of the fitting line is increased based on the least squares method.

[0016] A further technical solution is that the maximum intercept in step S4 is accurate to 3 decimal places.

[0017] A further technical solution is that the determination coefficient r in step S5 is 2 The calculation formula is:

[0018]

[0019] Where: n is the number of proppant samples; y i is the corresponding shear stress under the i-th normal stress tested based on the quick shear test in step B, kPa; is the corresponding shear stress under the i-th normal stress predicted based on the fitting line in step E, kPa; is the average shear stress, kPa.

[0020] The present invention has the following beneficial effects:

[0021] 1. Ability to accurately obtain the cohesion of the proppant filling layer;

[0022] 2. Low operating cost, strong feasibility, and no need for complex test equipment;

[0023] 3. It has wide applicability. In addition to the proppant filling layer, it is also suitable for obtaining the cohesion of wetted particles with low cohesion. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the result of the quick shear test of the proppant sample;

[0025] Figure 2 The cohesion diagram of different types of proppant-filled samples obtained by testing based on the method of the present invention is shown in FIG. DETAILED DESCRIPTION

[0026] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] A testing method for accurately obtaining the cohesion of a proppant packing layer of the present invention comprises the following steps:

[0028] A. Prepare proppant filling samples with different proppant types, different particle sizes, and different fracturing fluid viscosities at a certain water content. Prepare 4 or 5 samples with the same water content, proppant type, different particle sizes, and different fracturing fluid viscosities, among which the same water content, proppant type, different particle sizes, and different fracturing fluid viscosities are regarded as one group;

[0029] B. Test the maximum friction coefficient of each sample in each group of samples, and take the average value as the friction coefficient of each group of samples;

[0030] C. Based on the quick shear test process, the shear stress of each group of specimens under different normal stresses is tested, and the test data points are plotted in a rectangular coordinate system with normal stress as the abscissa and shear stress as the ordinate;

[0031] D. Take the coefficient of friction of each set of samples as the slope of the fitted straight line of the test data points in step C, increase the intercept of the fitted straight line based on the least squares method, and take the maximum intercept (accurate to 3 decimal places) that does not change the slope as the intercept of the fitted straight line temporarily;

[0032] E. Back-calculate the determination coefficient r using the fitting line obtained in step D and the test data in step C 2 If the determination coefficient is greater than 0.85, the slope and intercept obtained in step D are considered to be the final slope and intercept of the fitted straight line; if the determination coefficient is less than 0.85, the data that deviates greatly from the existing fitted straight line are tested repeatedly based on steps A and B. If the repeated test results (more than twice) are not much different, steps A, B, C, D, and E are repeated until the determination coefficient is greater than 0.85.

[0033] Coefficient of determination r 2 The calculation formula is:

[0034]

[0035] Where: n is the number of proppant samples; y iis the corresponding shear stress under the i-th normal stress tested based on the quick shear test in step B, kPa; is the corresponding shear stress under the i-th normal stress predicted based on the fitting line in step E, kPa; is the average shear stress, kPa.

[0036] Example

[0037] Step 1: After peeling the 250ml beaker, measure 150ml of proppant and pour it into the beaker to weigh it. After calculating the mass of fracturing fluid that needs to be added at a certain moisture content according to the moisture content calculation formula, use a 100ml graduated cylinder to add it into the beaker containing the proppant, and stir with a glass rod while adding to ensure that all the proppant is in full contact with the liquid; repeat this process 4 or 5 times to prepare a set of samples required for the test;

[0038] According to the above steps, 8 groups of proppant filling samples were prepared, and the sample preparation parameters are shown in Table 1;

[0039] Table 1 Proppant filling sample preparation parameters

[0040]

[0041]

[0042] Step 2: Test the maximum friction coefficient of each sample in each group of samples, and take the average value as the friction coefficient of each group of samples. The results are shown in Table 2.

[0043] Table 2 Friction coefficient test results

[0044] Sample No. Proppant type and particle size Average friction coefficient 1 20 / 40 mesh quartz sand 0.4961 2 30 / 50 mesh quartz sand 0.5229 3 40 / 70 mesh quartz sand 0.5475 4 70 / 140 mesh quartz sand 0.5176 5 20 / 40 mesh ceramsite 0.4842 6 30 / 50 mesh ceramsite 0.4915 7 40 / 70 mesh ceramsite 0.5126 8 70 / 140 mesh ceramsite 0.5004

[0045] Step 3: Based on the rapid shear test method, test the shear stress of each group of samples under different normal stresses, and plot the test data points in a rectangular coordinate system with normal stress as the horizontal coordinate and shear stress as the vertical coordinate. The results are as follows: Figure 1 As shown;

[0046] Each group of samples is subjected to 4 or 5 shear tests, and the normal stress is loaded in sequence: 50kPa (0.765kg hanging plate, which can be omitted), 100kPa (adding 0.765kg weight), 200kPa (adding 1.53kg weight), 300kPa (adding 1.53kg weight);

[0047] The rapid shear test method also includes the following improvements:

[0048] (1) During the sample filling process, the filling surface should be kept flat, no gaps should be allowed, the filling height should be appropriate, and the top cover of the shear box should be firmly pressed on the surface of the proppant filling layer;

[0049] (2) When the reading of the dynamometer dial indicator remains unchanged (maintained for 1 minute or more) or obviously retreats, record the reading; when the pointer swings back and forth near the peak value, shearing stops when the shear displacement reaches 4 mm; when there is no peak value on the dynamometer during the shearing process, shearing stops when the shear displacement reaches 6 mm;

[0050] (3) After each shearing operation, the shear stress and normal stress are released, the pressure frame is moved, the proppant particles and liquid in the shear box and on the upper and lower surfaces of the shear box are cleaned, and the sample in the next beaker is refilled into the shear box.

[0051] Step 4: Take the friction coefficient of each set of samples as Figure 1 The slope of the fitted line of the test data point is calculated. Based on the least square method, the intercept of the fitted line is increased. The maximum intercept (accurate to 3 decimal places) that does not change the slope is temporarily taken as the intercept of the fitted line.

[0052] Step 5: According to the determination coefficient r 2 The linear fitting determination coefficient and cohesion of the eight groups of samples were obtained by the calculation formula. The results are shown in Figure 2 As shown;

[0053] Step 6: If the linear fitting determination coefficients of the eight groups of samples are all greater than 0.85, then the maximum intercept in step 4 is the cohesion of each group of samples.

[0054] The above description is not intended to impose any form of limitation on the present invention. Although the present invention has been disclosed through the above embodiments, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A test method for accurately obtaining the cohesion of a proppant packing layer, characterized in that: The following steps are involved: S1. Prepare multiple proppant samples; The water content of each proppant sample was the same; S2. testing the maximum friction coefficient of each proppant sample, and taking the average value of multiple groups of maximum friction coefficients as the friction coefficient of the proppant sample; S3, testing the shear stress of the proppant sample under different normal stresses, and then plotting the test data in a rectangular coordinate system with the normal stress as the abscissa and the shear stress as the ordinate; S4, using the friction coefficient in step S2 as the slope of the test data fitting line in step S3, increasing the intercept of the fitting line, and taking the maximum intercept that does not change the slope as the intercept of the fitting line; S5, back-calculate the determination coefficient r based on the test data in step S3 and the fitting straight line in step S4 2 , if the determination coefficient r 2 If the determination coefficient is greater than 0.85, the slope and intercept obtained in step S4 are determined to be the final slope and intercept of the fitted line; if the determination coefficient is less than 0.85, steps S1-S5 are repeated until the determination coefficient r 2 Greater than 0.85; Where: n is the number of proppant samples; y i is the corresponding shear stress under the i-th normal stress tested based on the quick shear test in step S3, kPa; is the corresponding shear stress under the i-th normal stress predicted based on the fitting straight line in step S4, kPa; is the average shear stress, kPa; S6. Finally, the final intercept of the fitting straight line is determined as the cohesion of the proppant sample.

2. A testing method for accurately obtaining the cohesion of a proppant packing layer according to claim 1, characterized in that: The number of proppant samples in step S1 is 4 or 5.

3. A testing method for accurately obtaining the cohesion of a proppant packing layer according to claim 1, characterized in that: In step S4, the intercept of the fitting line is increased based on the least square method.

4. A testing method for accurately obtaining the cohesion of a proppant packing layer according to claim 1, characterized in that: The maximum intercept in step S4 is accurate to 3 decimal places.