Preparation method of petroleum coke raw material and petroleum coke raw material
Through the thermal mixing and granulation process of self-made organic binder and carbon-containing fine powder, the problem of difficulty in granulating fine petroleum coke and low yield is solved, and the green ball strength and crushing yield of petroleum coke raw material are improved. Efficient petroleum coke raw material preparation is achieved, reducing costs and energy consumption.
Patent Information
- Application Number
- CN202210695328.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-20
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-06-20
AI Technical Summary
In the existing technology, the granulation of finely powdered petroleum coke is difficult, the yield is low, the green ball strength is low, and the cost of using binders is high, resulting in waste problems in industrial silicon smelting and steel smelting.
The self-made organic binder and carbon-containing fine powder are thermally mixed, granulated and calcined and then crushed to prepare petroleum coke raw material with high yield. The asphalt and coke materials are used in the process of preparing graphite electrodes. The by-product acts as a binder, reducing energy consumption and costs.
The strength of green balls and the yield after crushing are improved. The prepared petroleum coke raw material can be used in electric furnaces and chlorination furnaces, with a yield of more than 93%, reducing the purchase cost of binders and energy consumption.
Smart Images

Figure BDA0003702058800000111 
Figure BDA0003702058800000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of recovery and utilization of carbonaceous fine powder, in particular to a preparation method of a petroleum coke raw material and the petroleum coke raw material. Background Art
[0002] Charcoal, washed coal, petroleum coke, and semi-coke are currently commonly used carbonaceous reducing agents in industrial production. Charcoal is a dark brown or black porous solid fuel left after incomplete combustion of wood raw materials or pyrolysis under air-tight conditions. Since charcoal comes from wood raw materials, excessive use will cause serious damage to forest resources. With the enhancement of people's environmental awareness, the carbon-based reducing agents currently used are mostly washed coal and petroleum coke, which are rich in resources and widely available. Petroleum coke is widely used in the production of industrial silicon and the smelting of steel due to its ultra-high fixed carbon content, low ash content, good reducibility and low price. As a reducing agent, petroleum coke has specific requirements for particle size in different industrial production fields. Too fine petroleum coke powder cannot be added to electric furnace smelting, so it is undoubtedly a waste of fine powder petroleum coke.
[0003] The most common method of utilizing fine powdered petroleum coke is granulation. However, due to its fine particle size, the granulation process is difficult and the finished product is easily affected by production. The specific defects include: (1) the coke powder is extremely difficult to granulate and the yield is low; (2) the raw ball strength is low and the pulverization rate increases during transportation; (3) impurities are easily introduced when selecting the binder; (4) the calcination temperature is high, resulting in energy waste.
[0004] Patent CN105329897A discloses a method for preparing a composite reducing agent used in industrial silicon smelting production. The raw materials used include petroleum coke materials, anthracite / bituminous coal materials, charcoal powder, and carbon powder mixtures such as biomass charcoal / semi-coke, which are mixed evenly in a mass ratio of 30-50:30-50:20-40 to obtain a mixture, and 2-4% of organic binder by mass, 1-3% of additives by mass of the mixture, and 8-15% of water by mass of the mixture are added, mixed and stirred, and then pressed into balls, and dried to obtain a composite reducing agent that can be used in industrial silicon smelting production. Binders, additives, water, and a variety of carbon-based raw materials are required, and there will be a problem of cumbersome feeding in actual industrial production.
[0005] Patent application CN103874745A discloses a method for granulating and calcining raw coke, wherein raw coke with a particle size distribution of 0.1 mm to 50 mm is divided into undersized and oversized parts, the undersized coke is granulated with a binder such as starch, lignin sulfonate, sugar, carboxymethyl cellulose, asphalt, etc., and the oversized coke is mixed with the granulated coke to form a feed mixture and calcined to form calcined coke. The granulation method adopted in this method may cause problems such as poor strength of the pelletized material and high-temperature pulverization, and asphalt as a binder is also a waste of cost.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] An object of the present invention is to provide a method for preparing petroleum coke raw materials to solve the technical problems in the prior art of difficulty in granulating carbon-containing fine powder, low yield and low green ball strength.
[0008] Another object of the present invention is to provide a petroleum coke raw material prepared by the method for preparing a petroleum coke raw material, wherein the petroleum coke raw material has a high yield.
[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0010] The method for preparing petroleum coke raw material comprises the following steps:
[0011] The carbonaceous fine powder and the organic binder are hot mixed, the obtained mixed system is granulated to obtain green balls, and the green balls are calcined and crushed;
[0012] The organic binder is mainly prepared by the following method:
[0013] In a reducing atmosphere, a mixture of asphalt and coke is calcined from room temperature to 550-650° C., and volatiles at different temperatures are collected and condensed to obtain the organic binder.
[0014] In one embodiment, the carbonaceous fines include sorted coke fines.
[0015] In one embodiment, at least 85% of the carbonaceous fine powder has a particle size less than 0.045 mm.
[0016] In one embodiment, the mass content of water in the carbonaceous fine powder is less than or equal to 22%.
[0017] In one embodiment, the carbonaceous fine powder has an ash content of less than 18%, a volatile matter of less than 7%, and a fixed carbon content of more than 75%, by mass percentage.
[0018] In one embodiment, the thermal mixing comprises hot melt spraying.
[0019] In one embodiment, the mass of the organic binder is 15% to 23% of the mass of the carbonaceous fine powder.
[0020] In one embodiment, the mass ratio of the asphalt to the coke material is (20-30):(70-80).
[0021] In one embodiment, the volatile matter in the char material is 5% to 15% by mass.
[0022] In one embodiment, the volatile matter in the asphalt is 45% to 55% by mass.
[0023] In one embodiment, the room temperature is 15 to 25°C;
[0024] In one embodiment, the binder is a by-product of the pitch and the coke material in the process of preparing a graphite electrode.
[0025] In one embodiment, the temperature of the heat mixing is 105-120° C., and the time of the heat mixing is 40-90 min.
[0026] In one embodiment, the pressure used for granulation is 5-8t.
[0027] In one embodiment, the calcination temperature of the green balls is 250-350° C., and the calcination time of the green balls is 60-150 min.
[0028] In one embodiment, during the calcination process, 2 to 3 mm dry basis coke powder is spread between the green balls.
[0029] In one embodiment, the petroleum coke raw material is prepared using an electric furnace and / or a chlorination furnace.
[0030] In one embodiment, after the crushing process, a petroleum coke raw material with a particle size of 5 to 15 mm is obtained and used in an electric furnace.
[0031] In one embodiment, after the crushing process, a petroleum coke raw material with a particle size of 0.25 to 3 mm is obtained and used in a chlorination furnace.
[0032] The petroleum coke raw material is prepared by the method for preparing the petroleum coke raw material.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] (1) The method for preparing a petroleum coke raw material of the present invention comprises the following steps: heat-mixing a homemade organic binder with a carbonaceous fine powder, and then granulating the mixture. The obtained green balls have a relatively high green ball strength, which is more than 11 times per ball. The green balls are further calcined and crushed to obtain a petroleum coke raw material with a particle size of 5 to 15 mm and a yield of more than 93%, which can be used in an electric furnace. The prepared petroleum coke raw material with a particle size of 0.25 to 3 mm can be used in a chlorination furnace.
[0035] (2) The petroleum coke raw material prepared by the method for preparing the petroleum coke raw material of the present invention has a higher yield. DETAILED DESCRIPTION
[0036] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0037] In one aspect, the present invention relates to a method for preparing a petroleum coke raw material of the present invention, comprising the following steps:
[0038] The carbonaceous fine powder and the organic binder are hot mixed, the obtained mixed system is granulated to obtain green balls, and the green balls are calcined and crushed;
[0039] The organic binder is mainly prepared by the following method:
[0040] In a reducing atmosphere, a mixture of asphalt and coke is calcined from room temperature to 550-650° C., and volatiles at different temperatures are collected and condensed to obtain the organic binder.
[0041] The invention adopts a self-made organic binder and carbon-containing fine powder for hot mixing and then granulation to obtain green balls with higher green ball strength; the green balls are further calcined and crushed to obtain petroleum coke raw materials with a particle size of 5 to 15 mm and a higher yield.
[0042] In one embodiment, the organic binder component is a complex mixture of hydrocarbons, aromatic hydrocarbons and heterocyclic organic compounds.
[0043] In one embodiment, the organic binder is first kept in liquid state and has fluidity, and is combined with the coke powder by spraying. At this time, the organic binder will be tightly wrapped by the coke powder to form small pellets, and the distribution is uneven. At this time, the small pellets will have different degrees of bursting phenomenon when directly pressed into tablets, and will adhere to the pelletizing machine mold. Therefore, a hot mixing method is required. The purpose of hot mixing includes: ensuring that the melting of the organic binder can infiltrate the surface of the coke powder, and completely mix with the fine material to form a strong bonding force, and can be tightly bonded with the fine powder after polycondensation and solidification. Stirring can be added during hot mixing to ensure that the coke and binder are evenly mixed and to reduce the hot mixing time.
[0044] In one embodiment, the reducing atmosphere comprises CO and / or CO2.
[0045] In one embodiment, the carbonaceous fines include sorted coke fines.
[0046] In one embodiment, at least 85% of the carbonaceous fine powder has a particle size less than 0.045 mm. That is, in the carbonaceous fine powder of the present invention, the proportion of particles with a particle size less than 0.045 mm includes but is not limited to 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99% or 100%. That is, the present invention is mainly aimed at recycling the fine powder of sorted coke with a smaller particle size to prepare petroleum coke raw materials.
[0047] In one embodiment, the mass content of water in the carbonaceous fine powder is less than or equal to 22%. In one embodiment, the mass content of water in the carbonaceous fine powder includes but is not limited to 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%.
[0048] When there is a lot of moisture in the carbonaceous fine powder, the granulation process generally requires drying before granulation. In the present invention, the main function of the hot mixing method is to melt the homemade binder and fuse it with the coke powder particles, accompanied by the evaporation of a certain amount of moisture, thereby avoiding the drying process of petroleum coke with ultra-high water content. In addition, when the ultrafine petroleum coke is calcined in a drying kiln at a temperature greater than 400°C, there is a risk of fire and explosion.
[0049] In one embodiment, the carbonaceous fine powder is obtained by flotation of inert waste slag (upper slag). The collector mainly acts on the surface of the coke powder, making it hydrophobic, and can also easily adhere to the surface of the bubbles, thereby increasing its floatability. Therefore, during hot mixing, the melted coal tar can be fused with the coke powder, and the molded product has a certain strength after cooling.
[0050] In one embodiment, the ash content of the carbonaceous fine powder is less than 18%, the volatile matter is less than 7%, and the fixed carbon is greater than 75% by mass percentage. The main components of the inert waste slag are carbon concentrate, titanium concentrate and a portion of quartz silicon. The ash content of the carbonaceous fine powder includes but is not limited to 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16% or 17%. The volatile matter includes but is not limited to 1%, 2%, 3%, 4%, 5%, 6%. The fixed carbon includes but is not limited to 76%, 77%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90% or 95%, etc.
[0051] In one embodiment, the mass of the organic binder is 15% to 23% of the mass of the carbonaceous fine powder. In one embodiment, the mass of the organic binder is 16%, 17%, 18%, 19%, 20%, 21%, 22% or 23% of the mass of the carbonaceous fine powder. The present invention ensures the green ball strength of the carbonaceous fine powder by using an appropriate amount of organic binder, which is beneficial to improving the yield of the crushed material. If the amount of binder is too low, it will affect the strength of the green ball; if the amount of binder is too high, it will increase the hot mixing time, and the temperature and time during calcination will also increase, resulting in a waste of energy.
[0052] In one embodiment, the mass ratio of the asphalt to the coke material is (20-30):(70-80), for example, 20:80, 25:75, 30:70, etc.
[0053] In one embodiment, the volatile matter in the coke material is 5% to 15% by mass, for example, 6%, 7%, 8%, 10%, 11%, 12%, 14% or 15%.
[0054] In one embodiment, the volatile matter in the asphalt is 45% to 55% by mass, for example, 46%, 48%, 50%, 51%, 52%, 54% or 55%.
[0055] In one embodiment, the room temperature is 15-25° C. For example, it can be 15° C., 16° C., 17° C., 18° C., 19° C., 20° C., 21° C., 22° C., 23° C., 24° C. or 25° C.
[0056] In one embodiment, the binder is a byproduct of the asphalt and the coke in the process of preparing the graphite electrode. The binder is the volatile matter collected in the calcination and roasting processes of preparing the graphite electrode, which is basically a waste material. Using it as a binder can realize waste material utilization.
[0057] During the calcination process of the asphalt and coke materials in the preparation of the electrode, the volatiles in the asphalt and coke materials can basically be completely volatilized at a temperature of 200 to 650°C, and are collected by flue condensation to obtain the above-mentioned binder. The heating rate and the insulation time are mainly set according to the electrode product. In one embodiment, calcination from room temperature to 550 to 650°C specifically includes: the heating rate from room temperature to 350°C is 35 to 45°C / h, the heating rate from 350°C to 550°C is 2 to 3.5°C / h, and the heating rate from 550°C to 650°C is 2 to 2.5°C / h.
[0058] The organic binder obtained by the method of the present invention has a low softening point and a low calcination temperature, thereby reducing the purchase cost.
[0059] In one embodiment, the temperature of the heat mixing is 105-120°C, and the time of the heat mixing is 40-90 minutes. In one embodiment, the temperature of the heat mixing includes but is not limited to 105°C, 106°C, 107°C, 108°C, 109°C, 110°C, 110°C, 111°C, 112°C, 113°C, 114°C, 115°C, 116°C, 117°C, 118°C, 119°C or 120°C.
[0060] In one embodiment, the pressure used for granulation is 5-8t. In one embodiment, the pressure used for granulation includes but is not limited to 5t, 6t, 7t or 8t. The present invention uses a suitable pressure to facilitate the molding of coke powder, thereby facilitating the drop strength of green balls.
[0061] The equipment used for granulation includes a wet pelletizer and / or a dry pelletizer. The effect of fully mixing the materials is achieved, thereby improving the yield. The wet pelletizer is preferred.
[0062] In one embodiment, the calcination temperature of the green balls is 250-350° C., and the calcination time of the green balls is 60-150 min.
[0063] The green balls of the present invention can be calcined at a relatively low temperature, which can further save energy. During calcination, the organic binder is heated to partially volatilize and analyze, and bubbles are generated between the coke powders. The pyrolysis products gather together to form a mixture of gas, liquid and solid phases, forming a colloid, and forming a carbonaceous skeleton between the coke powders. After solidification, it is tightly combined with the coke powders, thereby greatly improving the strength.
[0064] In one embodiment, the calcination temperature of the green ball includes but is not limited to 250° C., 260° C., 270° C., 290° C., 300° C., 310° C., 320° C., 330° C., 340° C. or 350° C. The calcination time of the green ball includes but is not limited to 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min or 150 min.
[0065] During calcination in the present invention, 2-3 mm dry coke powder needs to be spread between the green balls to avoid the green balls from sticking together during the calcination process, which is not conducive to crushing. The dry coke powder is dry petroleum coke with a carbon grade of more than 95%, and the mass proportion of the particles below -160 mesh is more than 85%.
[0066] In one embodiment, the petroleum coke raw material is prepared using an electric furnace and / or a chlorination furnace.
[0067] In one embodiment, a roller crusher is used, and after the crushing process, a petroleum coke raw material with a particle size of 5 to 15 mm is obtained for use in an electric furnace.
[0068] In one embodiment, after the crushing process, a petroleum coke raw material with a particle size of 0.25 to 3 mm is obtained and used in a chlorination furnace.
[0069] On the other hand, the present invention relates to a petroleum coke raw material prepared by the method for preparing the petroleum coke raw material.
[0070] In a preferred embodiment, the method for preparing petroleum coke raw material comprises the following steps:
[0071] The carbon-containing fine powder and the organic binder are hot mixed, and the obtained mixed system is granulated to obtain green balls, and the green balls are calcined and crushed; the organic binder is mainly prepared by the following method: a mixture of asphalt and coke is roasted from 15 to 25°C to 550 to 650°C under a reducing atmosphere, and volatiles at different temperatures are collected and condensed to obtain the organic binder; the carbon-containing fine powder is selected coke fine powder, and at least 85% of the carbon-containing fine powder has a particle size of less than 0.045mm, and the mass content of water in the carbon-containing fine powder is less than or equal to 22%; the ash content of the carbon-containing fine powder is less than 18%, the volatile matter is less than 7%, and the fixed carbon is greater than 7 5%; the mass of the organic binder is 15% to 25% of the mass of the carbonaceous fine powder; in the raw materials for preparing the organic binder, the mass ratio of asphalt and coke is (20 to 30): (70 to 80); the temperature of the hot mixing is 105 to 120°C, and the time of the hot mixing is 40 to 90 minutes; the pressure used for granulation is 5 to 8 tons; the calcination temperature of the green ball is 250 to 350°C, and the calcination time of the green ball is 60 to 150 minutes; after the crushing treatment, a petroleum coke raw material with a particle size of 5 to 15 mm is obtained, which is used in an electric furnace; or, after the crushing treatment, a petroleum coke raw material with a particle size of 0.25 to 3 mm is obtained, which is used in a chlorination furnace.
[0072] The present invention will be further described below in conjunction with specific embodiments and comparative examples.
[0073] Example 1
[0074] The method for preparing petroleum coke raw material comprises the following steps:
[0075] (a) taking a carbonaceous fine powder having a particle size of less than 0.045 mm and a moisture content of 20%, adding a liquid organic binder having a mass ratio of 15%, and uniformly mixing at 105° C. for 90 minutes until the liquid organic binder is substantially completely melted;
[0076] The preparation method of the above-mentioned liquid organic binder includes: roasting a mixture of asphalt and coke from room temperature to 650°C, collecting volatiles at different temperatures and condensing them to obtain the organic binder; wherein the mass ratio of asphalt to coke is 25:75; in terms of mass percentage, the volatile matter in the coke is 10%; in terms of mass percentage, the volatile matter in the asphalt is 50%.
[0077] (b) taking the hot mixed material and pelletizing it on a pelletizing machine at a pressure of 8t;
[0078] (c) The green balls are calcined at 350°C for 60 minutes and crushed to a qualified particle size using a double-roll crusher after cooling.
[0079] Example 2
[0080] The method for preparing petroleum coke raw material comprises the following steps:
[0081] (a) taking a carbonaceous fine powder having a particle size of less than 0.045 mm and a moisture content of 22%, adding a liquid organic binder having a mass ratio of 23%, and uniformly mixing at 120° C. for 40 minutes until the liquid organic binder is substantially completely melted;
[0082] The preparation method of the above liquid organic binder is the same as that of Example 1;
[0083] (b) taking the hot mixed material and pelletizing it on a pelletizing machine at a pressure of 8t;
[0084] (c) Calcine the green balls at 300°C for 150 min, and after cooling, crush them to a qualified particle size using a double-roll crusher.
[0085] Example 3
[0086] The method for preparing petroleum coke raw material comprises the following steps:
[0087] (a) taking a carbonaceous fine powder having a particle size of less than 0.045 mm and a moisture content of 18%, adding a liquid organic binder having a mass ratio of 20%, and uniformly mixing at 105° C. for 70 minutes until the liquid organic binder is substantially completely melted;
[0088] The preparation method of the above liquid organic binder is the same as that of Example 1;
[0089] (b) taking the hot mixed material and pelletizing it on a pelletizing machine at a pressure of 8t;
[0090] (c) Calcine the green balls at 300°C for 100 min, and after cooling, crush them to a qualified particle size using a double-roll crusher.
[0091] Example 4
[0092] The method for preparing petroleum coke raw material comprises the following steps:
[0093] (a) taking a carbonaceous fine powder having a particle size of less than 0.045 mm and a moisture content of 5%, adding a liquid organic binder having a mass ratio of 20%, and uniformly mixing at 110° C. for 60 minutes until the liquid organic binder is substantially completely melted;
[0094] The preparation method of the liquid organic binder is the same as that of Example 1;
[0095] (b) taking the hot mixed material and pelletizing it on a pelletizing machine at a pressure of 5t;
[0096] (c) The green balls are calcined at 250°C for 90 minutes and crushed to a qualified particle size using a double-roll crusher after cooling.
[0097] Example 5
[0098] The method for preparing petroleum coke raw material comprises the following steps:
[0099] (a) Take selected coke fine powder with a particle size of less than 0.045 mm, wherein the fixed carbon content is more than 90%, the ash content is not more than 5%, the volatile matter is not more than 5%, and the moisture content is 20%, add 15% by mass of liquid organic binder, and mix uniformly at 115° C. for 50 minutes until the liquid organic binder is basically completely melted;
[0100] The preparation method of the above-mentioned liquid organic binder includes: roasting a mixture of asphalt and coke from room temperature to 600°C, collecting volatiles at different temperatures and condensing them to obtain the organic binder; wherein the mass ratio of asphalt to coke is 20:80; in terms of mass percentage, the volatile matter in the coke is 15%; in terms of mass percentage, the volatile matter in the asphalt is 45%.
[0101] (b) taking the hot mixed material and pelletizing it on a pelletizing machine at a pressure of 7t;
[0102] (c) The green balls are calcined at 310°C for 75 minutes, and after cooling, they are crushed with a double-roll crusher to a particle size of 0.25 to 3 mm for use in a chlorination furnace.
[0103] Comparative Example 1
[0104] The method for preparing petroleum coke raw material comprises the following steps:
[0105] (a) taking a carbonaceous fine powder having a particle size of less than 0.045 mm and a moisture content of 5%, adding a liquid organic binder having a mass ratio of 10%, and uniformly mixing at 110° C. for 60 minutes until the liquid organic binder is substantially completely melted;
[0106] (b) taking the hot mixed material and pelletizing it on a pelletizing machine at a pressure of 5t;
[0107] (c) The green balls are calcined at 250°C for 90 minutes, and after cooling, they are crushed into acceptable particle sizes using a double-roll crusher, preferably 5 to 15 mm.
[0108] Test example
[0109] 1. Raw ball strength test
[0110] The green balls obtained in each embodiment were subjected to strength tests, and the results are shown in Table 1.
[0111] Table 1 Test results of green ball strength
[0112]
[0113]
[0114] As shown in Table 1, the green balls obtained by the present invention have a high green ball strength of more than 11 times / piece by using a homemade organic binder and hot mixing with carbonaceous fine powder, using appropriate dosage ratio and other parameter conditions, and then granulating. However, the addition ratio of the liquid organic binder in Comparative Example 1 is relatively low, which will affect the green ball strength.
[0115] 2. Yield Results
[0116] The results of crushing to particle size of 5-15 mm and 0.25-3 mm are shown in Table 2.
[0117] Table 2 Yield
[0118] Example Yield (%) Example 1 95.3 Example 2 96.6 Example 3 95.5 Example 4 93.3 Example 5 94.8 Comparative Example 1 88.3
[0119] As shown in Table 2, the petroleum coke raw material obtained by crushing to a particle size of 5 to 15 mm or 0.25 to 3 mm by the method of the present invention has a higher yield, while the yield of the method in Comparative Example 1 is relatively low.
[0120] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a petroleum coke raw material, characterized in that: The following steps are involved: The carbonaceous fine powder and the organic binder are hot mixed, the obtained mixed system is granulated to obtain green balls, and the green balls are calcined and crushed; The organic binder is mainly prepared by the following method: In a reducing atmosphere, a mixture of asphalt and coke is calcined from room temperature to 550-650° C., volatiles at different temperatures are collected and condensed to obtain the organic binder; the mass ratio of the asphalt to the coke is (20-30): (70-80); The hot mixing includes hot melt spraying; the temperature of the hot mixing is 105-120° C., and the time of the hot mixing is 40-90 minutes; After the crushing process, a petroleum coke raw material with a particle size of 5 to 15 mm is obtained and used in an electric furnace; After the crushing process, a petroleum coke raw material with a particle size of 0.25-3 mm is obtained, which is used in a chlorination furnace.
2. The method for preparing petroleum coke raw material according to claim 1, characterized in that: Contains at least one of the following characteristics (1) to (4): (1) The carbonaceous fine powder includes sorted coke fine powder; (2) At least 85% of the carbonaceous fine powder has a particle size of less than 0.045 mm; (3) The mass content of water in the carbonaceous fine powder is less than or equal to 22%; (4) In terms of mass percentage, the ash content of the carbonaceous fine powder is less than 18%, the volatile matter is less than 7%, and the fixed carbon is greater than 75%.
3. The method for preparing a petroleum coke raw material according to claim 1 or 2, wherein the mass of the organic binder is 15% to 23% of the mass of the carbonaceous fine powder.
4. The method for preparing petroleum coke raw material according to claim 1, characterized in that: Contains at least one of the following characteristics (1) to (2): (1) The volatile matter in the coke material is 5% to 15% by mass; (2) The volatile matter in the asphalt is 45% to 55% by mass.
5. The method for preparing a petroleum coke raw material according to claim 1 or 4, characterized in that: Contains at least one of the following characteristics (1) to (2): (1) The room temperature is 15-25°C; (2) The organic binder is a by-product of the asphalt and the coke material in the process of preparing the graphite electrode.
6. The method for preparing petroleum coke raw material according to claim 1, characterized in that: The pressure used in the granulation is 5~8t.
7. The method for preparing petroleum coke raw material according to claim 1, characterized in that: Contains at least one of the following characteristics (1) to (2): (1) The calcination temperature of the green ball is 250-350°C, and the calcination time of the green ball is 60-150 minutes; (2) During the calcination process, 2 to 3 mm of dry coke powder is spread between the green balls.
8. The petroleum coke raw material prepared by the method for preparing a petroleum coke raw material according to any one of claims 1 to 7.
Citation Information
Patent Citations
Pelletization and calcination of green coke
CN103874745A
Preparation method of compound reducing agent applied to industrial silicon smelting production
CN105329897A
Method for using petroleum coke fine powder in preparation of prebaked anode used for aluminum electrolysis
CN102839393A
Petroleum tar fine powder balling method
CN108975299A
process for obtaining volatile products from solid bituminous materials
FR826967A