A label-free electrochemical immunosensor and its preparation method and application

Through the combination of reduced graphene oxide and gold nanoparticles by co-doping boron, sulfur and nitrogen, a markerless electrochemical immune sensor was constructed, which solved the problems of insufficient detection height limit and sensitivity in the prior art, and achieved the markers of chronic diseases efficient detection.

CN115060894BActive Publication Date: 2024-11-26HUBEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210630389.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-06
Publication Date
2024-11-26
Estimated Expiration
2042-06-06

AI Technical Summary

Technical Problem

Existing electrochemical immunosensors have high detection limits and low sensitivity in chronic disease marker detection, making it difficult to meet the needs of early diagnosis and system monitoring.

Method used

Graphene oxide, L-cysteine ​​and boric acid were used to carry out hydrothermal reaction to form boron, sulfur and nitrogen co-doped reducing graphene oxide, and combined with gold nanoparticles to prepare Au-B, S, N-rGO Nanocomposite materials, after modifying the electrode, antibodies were added to construct a label-free electrochemical immunosensor.

Benefits of technology

An electrochemical immunosensor with low detection limit and high sensitivity is realized, which can efficiently detect chronic disease markers and improve the specificity and sensitivity of the detection method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115060894B_ABST
    Figure CN115060894B_ABST
Patent Text Reader

Abstract

The present invention discloses a label-free electrochemical immunosensor and its preparation method and application, the method comprising: mixing graphene oxide, L-cysteine ​​and boric acid, adding deionized water for ultrasonic dispersion, adjusting pH to 8-9 for hydrothermal reaction, obtaining boron, sulfur and nitrogen co-doped reduced graphene oxide; obtaining a gold nanoparticle solution; dispersing the boron, sulfur and nitrogen co-doped reduced graphene oxide in the gold nanoparticle solution, washing and drying, obtaining Au-B, S, N-rGO nanocomposite materials; adding EDC and NHS solutions for activation and then dripping on the surface of a glassy carbon electrode to obtain an Au-B, S, N-rGO electrode; dripping an antibody solution on the electrode surface for incubation and washing, then dripping bovine serum albumin for washing, and then dripping a standard antigen solution to obtain a label-free electrochemical immunosensor. The label-free electrochemical immunosensor has a low detection limit, high sensitivity and high specificity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of novel nanocomposite materials and electrochemical immunosensor detection, and in particular to a label-free electrochemical immunosensor and a preparation method and application thereof. Background Art

[0002] In recent years, chronic diseases have affected the health of millions of people around the world due to their long incubation period, low cure rate and high lethality. Early diagnosis and systematic monitoring are the key to improving the survival rate of patients with chronic diseases. Therefore, it is imperative to develop a sensitive and reliable analytical method for detecting chronic disease markers. Electrochemical detection methods have become a research hotspot due to their high accuracy, convenient operation and low detection cost. However, existing electrochemical immunosensors have the disadvantages of high detection limit and low sensitivity when used in the detection of chronic disease markers.

[0003] Therefore, it is necessary to develop an electrochemical immunosensor with low detection limit and high sensitivity. Summary of the invention

[0004] The present invention aims to provide a label-free electrochemical immunosensor and a preparation method and application thereof. The label-free electrochemical immunosensor has a low detection limit, high sensitivity and high specificity.

[0005] In order to achieve the above object, the present invention adopts the following technical solution:

[0006] In a first aspect of the present invention, a method for preparing a label-free electrochemical immunosensor is provided, the method comprising:

[0007] The graphene oxide, L-cysteine ​​and boric acid are mixed, deionized water is added for ultrasonic dispersion, and the pH is adjusted to 8-9 for hydrothermal reaction, and then naturally cooled to room temperature, washed and dried to obtain boron, sulfur and nitrogen co-doped reduced graphene oxide;

[0008] The chloroauric acid solution was heated to 85-95° C., and then a sodium citrate solution was added for reflux reaction to obtain a wine red solution, which was naturally cooled to room temperature to obtain a gold nanoparticle solution;

[0009] Dispersing the boron, sulfur and nitrogen co-doped reduced graphene oxide in the gold nanoparticle solution, washing and drying, to obtain an Au-B, S, N-rGO nanocomposite material;

[0010] The Au-B, S, N-rGO nanocomposite material is added to EDC and NHS solution for activation to obtain a suspension; the suspension is then drop-coated on the surface of a glassy carbon electrode and dried naturally at room temperature to obtain an Au-B, S, N-rGO electrode;

[0011] Adding antibody solution to the surface of the Au-B, S, N-rGO electrode for incubation and then washing, and then adding bovine serum albumin and then washing to obtain an Au-B, S, N-rGO / Ab electrode;

[0012] The standard antigen solution was dropped on the surface of the Au-B,S,N-rGO / Ab electrode and incubated to obtain a label-free electrochemical immunosensor.

[0013] Furthermore, the mass ratio of the graphene oxide to the L-cysteine ​​is 1:(1-4), and the mass ratio of the graphene oxide to the boric acid is 1:(26.6-40).

[0014] Furthermore, the temperature of the hydrothermal reaction is 150-200° C., and the time of the high-temperature heating reaction is 8-12 hours.

[0015] Furthermore, the mass fraction of the chloroauric acid solution is 0.01%±0.005%; the mass fraction of the sodium citrate solution is 1%±0.5%; and the volume ratio of the chloroauric acid solution to the sodium citrate solution is 1:(0.01-0.03).

[0016] Furthermore, the temperature of the reflux reaction is 85 to 95° C., and the time of the reflux reaction is 10 to 45 minutes.

[0017] Furthermore, the mass volume ratio of the boron, sulfur and nitrogen co-doped reduced graphene oxide to the gold nanoparticle solution is 0.5 to 1.5 mg / ml.

[0018] Furthermore, the mass ratio of Au-B, S, N-rGO to EDC and NHS is 1:(1.5-5.8):(0.9-3.6).

[0019] Furthermore, the antibody incubation temperature is 4° C.; the bovine serum albumin incubation temperature is 37° C.; the antigen incubation temperature is 4-50° C.; and the antigen incubation time is 15-180 min.

[0020] Furthermore, the antibodies include: antibodies corresponding to protein biomarkers of various diseases such as cardiac troponin I, Aβ protein, pepsinogen, bladder tumor antigen, thyroglobulin, Golgi transmembrane glycoprotein 73, and human epididymis protein.

[0021] In a second aspect of the present invention, a label-free electrochemical immunosensor obtained by the method is provided.

[0022] In the third aspect of the present invention, there is provided the use of the label-free electrochemical immunosensor in the detection of antigen concentration in human serum.

[0023] In the application, a series of prepared standard antigen concentrations are dropped onto the working electrode, and the working electrode is immersed in 0.1 mol / L K3[Fe(CN)6] 3- / 4- / 0.1mol / L KCl solution, using an electrochemical workstation for differential pulse voltammetry detection. The peak current response signal changes with the change of antigen concentration, and a linear regression equation is established using the relationship between the peak current signal and the logarithmic change of the antigen; the diluted human serum is dripped onto the working electrode, and the differential pulse voltammetry method is used for detection. The antigen concentration in human serum can be measured according to the established linear regression equation.

[0024] The cyclic voltammetry test conditions are set as follows: the scanning range is -0.2 to 0.6 V, and the scanning rate is 50 mV / s. Electrochemical impedance spectroscopy conditions: frequency range: 10 -1 ~10 6 Hz, initial voltage: 0.30 V. DPV detection conditions: scanning range 0.7~0 V; pulse amplitude: 50 mV, pulse period: 500 ms.

[0025] One or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:

[0026] 1. The present invention provides a label-free electrochemical immunosensor and a preparation method thereof. After graphene oxide is doped with boron, sulfur and nitrogen atoms, the components play a synergistic role: some carbon atoms in the graphite structure are replaced by nitrogen, boron and sulfur atoms, thereby eliminating the restacking problem between graphene sheets. Boron, sulfur and nitrogen co-doped reduced graphene oxide not only increases the stability of graphene oxide but also enhances the conductivity of electrochemical performance. L-cysteine ​​can be used as a raw material to provide both a sulfur source and a nitrogen source. In addition, the carboxylic acid group of L-cysteine ​​can also couple antibodies with amide bonds, thereby increasing the binding rate of antibodies. Gold nanoparticles can be easily modified to boron, sulfur and nitrogen doped reduced graphene oxide materials through Au-S bonds to enhance the conductivity of the sensor.

[0027] 2. The present invention provides a label-free electrochemical immunosensor, which is constructed based on gold-modified boron, sulfur, and nitrogen-doped reduced graphene oxide composite materials. It has the advantages of low detection limit and high sensitivity in the detection of chronic disease markers, and can be further applied to the detection of various disease biomarkers. The immune reaction of antigens and antibodies is used to improve the specificity of the detection method. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0029] Figure 1 (A) is a transmission electron microscope image of GO. Figure 1 Middle (B) is a scanning electron microscope image of GO.

[0030] Figure 2 It is the scanning electron microscope image of B, S, N-rGO.

[0031] Figure 3 (A) is the transmission electron microscope image of Au-B, S, N-rGO. Figure 3 Middle (B) is the scanning electron microscope image of Au-B,S,N-rGO.

[0032] Figure 4 It is the XPS image of Au-B,S,N-rGO.

[0033] Figure 5 (A) is the cyclic voltammogram of electrodes modified with different materials. Figure 5 (B) is the electrochemical impedance spectrum of the electrode after modification with different materials. Figure 5 Among: (a)Bare GCE, (b) GO, (c) S,N-rGO, (d) B, S, N-rGO, (e) Au-B, S, N-rGO.

[0034] Figure 6 (A) is the DPV current signal diagram of Au-B,S,N-rGO / Ab / BSA / cTnI immunosensor. Figure 6 Middle (B) is the standard curve established between the logarithm of cTnI concentration and the response current.

[0035] Figure 7 (A) is the DPV current signal diagram of Au-B,S,N-rGO / Ab / BSA / Aβ(1-42) immunosensor. Figure 7 Middle (B) is a standard curve established between the logarithm of Aβ(1-42) concentration and the response current. DETAILED DESCRIPTION

[0036] The present invention will be described in detail below in conjunction with specific implementations and examples, and the advantages and various effects of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementations and examples are used to illustrate the present invention, rather than to limit the present invention.

[0037] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. In the event of a conflict, the present specification takes precedence.

[0038] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or obtained by existing methods. Steps S1, S2, S3, etc. of the present invention do not represent a strict order relationship, and the order can be adjusted appropriately as needed.

[0039] The technical solution of the embodiment of the present application is to solve the above technical problems, and the overall idea is as follows:

[0040] According to a typical embodiment of the present invention, a method for preparing a label-free electrochemical immunosensor is provided, the method comprising:

[0041] Step S1, mixing graphene oxide, L-cysteine ​​and boric acid, adding deionized water for ultrasonic dispersion, adjusting the pH to 8-9 for hydrothermal reaction, and then naturally cooling to room temperature, washing and drying to obtain boron, sulfur and nitrogen co-doped reduced graphene oxide;

[0042] In the step S1,

[0043] The mass ratio of the graphene oxide to the L-cysteine ​​is 1:(1-4), and the mass ratio of the graphene oxide to the boric acid is 1:(26.6-40). If the mass ratio is too small or too large, it is not conducive to complete reaction;

[0044] The temperature of the hydrothermal reaction is 150-200°C, and the high temperature heating reaction time is 8-12 hours. Such reaction temperature and reaction time are conducive to complete reaction;

[0045] The graphene oxide can be purchased directly or prepared in the following manner:

[0046] Weigh an appropriate amount of graphite and sodium nitrate, add concentrated sulfuric acid under ice bath conditions, stir for 0.5h, slowly add an appropriate amount of potassium permanganate, stir at room temperature for 1h, add a certain amount of deionized water after the solution turns dark green, stir at 37℃ for 1h, and then heat to 95℃ and reflux for 2h. After the reaction is over, add 30% hydrogen peroxide to terminate the reaction and cool to room temperature. Wash the prepared graphene oxide with 5% hydrochloric acid and deionized water several times and freeze-dry for 24h. The prepared graphene oxide sheets are ground into powder with a mortar for standby use. The mass ratio of graphite to sodium nitrate is 1:(0.3~2), and the optimal mass ratio is 1:(0.5~1). The mass ratio of graphite to sulfuric acid is 1:(36.8~73.6), and the better quality ratio is 1:(55~60). The mass ratio of graphite to potassium permanganate is 1:(1~5), and the better quality ratio is 1:(3~4). The mass ratio of graphite to 30% hydrogen peroxide is 1:(22.2-44.4), and the optimal mass ratio is 1:(30-35).

[0047] Step S2, heating the chloroauric acid solution to 85-95° C., adding the sodium citrate solution to carry out reflux reaction to obtain a wine red solution, and naturally cooling to room temperature to obtain a gold nanoparticle solution;

[0048] In the step S2,

[0049] The mass fraction of the chloroauric acid solution is 0.01%±0.005%; the mass fraction of the sodium citrate solution is 1%±0.5%; the volume ratio of the chloroauric acid solution to the sodium citrate solution is 1:(0.01-0.03). The mass fraction and volume ratio range is conducive to the preparation of gold nanoparticles within 20nm, so that nano-gold can be more evenly modified on the B, S, N-rGO nano-composite material to prevent nano-gold from agglomerating.

[0050] The temperature of the reflux reaction is 85-95° C., and the time of the reflux reaction is 10-45 min.

[0051] Step S3, dispersing the boron, sulfur, and nitrogen co-doped reduced graphene oxide in the gold nanoparticle solution, washing and drying, to obtain an Au-B, S, N-rGO nanocomposite material;

[0052] The mass volume ratio of the boron, sulfur and nitrogen co-doped reduced graphene oxide to the gold nanoparticle solution is 0.5 to

[0053] 1.5 mg / ml. Preferably 1 mg / ml.

[0054] Step S4, adding the Au-B, S, N-rGO nanocomposite material to EDC and NHS solution for activation to obtain a suspension; then drop-coating the suspension on the surface of a glassy carbon electrode and drying it naturally at room temperature to obtain an Au-B, S, N-rGO electrode;

[0055] The mass ratio of Au-B, S, N-rGO to EDC and NHS is 1:(1.5-5.8):(0.9-3.6).

[0056] Step S5, adding antibody solution to the surface of the Au-B, S, N-rGO electrode for incubation and then washing, and then adding bovine serum albumin and washing to obtain an Au-B, S, N-rGO / Ab electrode;

[0057] The antibodies include: antibodies corresponding to protein biomarkers of various diseases such as cardiac troponin I, Aβ protein, pepsinogen, bladder tumor antigen, thyroglobulin, Golgi transmembrane glycoprotein 73, and human epididymis protein.

[0058] The concentration range of the antibody solution is: (10ng / mL~100ng / mL)

[0059] The antibody incubation temperature is 4°C; the bovine serum albumin incubation temperature is 37°C; the antigen incubation temperature is 4-50°C;

[0060] Step S6, drop a standard antigen solution on the surface of the Au-B, S, N-rGO / Ab electrode and incubate to obtain a label-free electrochemical immunosensor.

[0061] The antigen incubation time is 15 to 180 minutes.

[0062] According to another typical embodiment of the present invention, a label-free electrochemical immunosensor prepared by the method is provided.

[0063] The present invention constructs a label-free electrochemical immunosensor, which has the advantages of low detection limit and high sensitivity in the detection of chronic disease markers, and can be further applied to the detection of various disease biomarkers. The immune reaction of antigen and antibody is used to improve the specificity of the detection method.

[0064] The following will describe in detail a label-free electrochemical immunosensor and its preparation method and application in combination with examples, comparative examples and experimental data.

[0065] Example 1. Gold-modified boron, sulfur, and nitrogen co-doped reduced graphene oxide and preparation method thereof

[0066] The embodiment of the present invention provides a method for preparing gold-modified boron, sulfur, and nitrogen co-doped reduced graphene oxide, comprising:

[0067] (1) Preparation of graphene oxide

[0068] Weigh 0.5g of graphite and 0.25g of sodium nitrate, mix them, add 15mL of concentrated sulfuric acid under ice bath conditions, stir for 0.5h, then slowly add 2g of potassium permanganate, stir at room temperature for 1h, and when the solution turns dark green, add 50mL of deionized water, stir at 37℃ for 1h, then heat to 95℃ and reflux for 2h. After the reaction is over, add 15mL of 30% hydrogen peroxide to terminate the reaction and cool to room temperature. Wash the prepared graphene oxide with 5% hydrochloric acid and deionized water several times and freeze-dry it for 24h. Grind the prepared graphene oxide sheets into powder in a mortar for later use. See the attached transmission electron microscope and scanning electron microscope images of the prepared GO. Figure 1 .

[0069] (2) Preparation of Boron, Sulfur and Nitrogen Co-doped Reduced Graphene Oxide

[0070] Weigh 15 mg of graphene oxide, 45 mg of L-cysteine ​​and 500 mg of boric acid, mix them, add 15 mL of purified water and sonicate for 15 min, add 150 μL of ammonia water to the suspension and sonicate for 30 min to mix. Transfer the evenly dispersed liquid to a polytetrafluoroethylene autoclave and hydrothermally react at 180 ° C for 10 hours. After the reaction is completed, cool to room temperature, wash three times with deionized water, wash twice with ethanol, and then vacuum dry for 12 hours to obtain dry B, S, N-rGO powder for use. SEM images of B, S, N-rGO are attached. Figure 2 .

[0071] (3) Preparation of gold nanoparticles

[0072] Take 100mL of 0.01% chloroauric acid solution and place it in a three-necked flask. After protecting from light, heat it to 90℃ and quickly add 2.0mL of 1% sodium citrate solution. After reflux at 90℃ for 15min, stop heating to obtain a wine red solution. After cooling to room temperature naturally, store it at 4℃ in the dark for later use.

[0073] (4) Preparation of gold-modified boron, sulfur, and nitrogen co-doped reduced graphene oxide

[0074] 100 mg B, S, N-rGO was dispersed in 100 mL Au NPs solution and stirred continuously at room temperature for 12 h. The solution was placed in a centrifuge tube, washed three times with purified water, and vacuum dried to obtain Au-B, S, N-rGO nanocomposites. The scanning electron microscopy and transmission electron microscopy images of Au-B, S, N-rGO are shown in the attached Figure 3 The XPS spectra of Au-B, S, N-rGO nanocomposites are shown in the attached Figure 4 .Depend on Figure 3 and Figure 4 It can be seen that the present invention successfully prepared gold-modified boron, sulfur, and nitrogen co-doped reduced graphene oxide.

[0075] Example 2: Preparation method and application of a label-free electrochemical immunosensor for cardiac troponin I

[0076] (1) Weigh 2 mg of the Au-B, S, N-rGO composite material prepared in Example 1, add 100 μL 0.03 mmol / L EDC and 100 μL 0.03 mmol / L NHS, and stir at 37° C. for 3 h to activate the carboxylic acid groups.

[0077] (2) 10 μL Au-B, S, N-rGO suspension was dropped onto the GCE surface and dried naturally at room temperature. Then 5 μL Ab (cardiac troponin I antibody) was dropped onto the Au-B, S, N-rGO electrode surface and incubated at 4 °C for 12 h. The unfixed antibody was washed with 0.1 mol / L PBS solution to remove the unfixed antibody. Then 3.0 μL 1% bovine serum albumin was dropped onto the Au-B, S, N-rGO / Ab electrode surface and incubated at 37 °C for 1 h to block nonspecific active sites. The solution was then washed with 0.1 mol / L PBS to remove excess BSA. Finally, 5 μL standard antigen solution (recombinant cardiac troponin I solution) was dropped onto the modified electrode surface and incubated at 37 °C for 2 h to construct the Au-B, S, N-rGO / Ab / BSA / cTnI electrochemical immunosensor.

[0078] Example 3: Preparation and application of an Aβ(1-42) label-free electrochemical immunosensor

[0079] (1) Weigh 2 mg of the Au-B, S, N-rGO composite material prepared in Example 1, add 100 μL 0.03 mmol / L EDC and 100 μL 0.03 mmol / L NHS, and stir at 37° C. for 3 h to activate the carboxylic acid groups.

[0080] (2) 10 μL of Au-B, S, N-rGO suspension was dropped onto the GCE surface and dried naturally at room temperature. Then 5 μL of Aβ(1-42) protein antibody was dropped onto the Au-B, S, N-rGO electrode surface and incubated at 4°C for 12 h. The unfixed antibody was washed with 0.1 mol / L PBS solution to remove the unfixed antibody. Then 3.0 μL of 1% bovine serum albumin was dropped onto the Au-B, S, N-rGO / Ab electrode surface and incubated at 37°C for 1 h to block nonspecific active sites. The solution was then washed with 0.1 mol / L PBS to remove excess BSA. Finally, 5 μL of standard antigen solution (recombinant Aβ(1-42) protein antibody solution) was dropped onto the modified electrode surface and incubated at 37°C for 2 h to construct the Au-B, S, N-rGO / Ab / BSA / Aβ(1-42) electrochemical immunosensor.

[0081] Comparative Example 1: GO modified electrode

[0082] (1) Glassy carbon electrode pretreatment

[0083] The glassy carbon electrode was continuously polished with aluminum oxide powder to remove the surface oxide layer, and then ultrasonically cleaned with ultrapure water and ethanol to remove any other physically adsorbed substances. The cleaned electrode was subjected to cyclic voltammetry in 0.1 mol / L PBS solution and 0.1 mol / L K3[Fe(CN)6] 3- / 4- The electrode is activated in the solution until the cyclic voltammetry current is stable. The activated electrode is washed again in ultrapure water and ethanol, and dried for later use.

[0084] (2) Preparation of GO-modified electrodes

[0085] 5 μL of GO suspension was added to the pretreated glassy carbon electrode and dried naturally at room temperature to prepare GO modified electrodes.

[0086] (1) Glassy carbon electrode pretreatment

[0087] The glassy carbon electrode was continuously polished with aluminum oxide powder to remove the surface oxide layer, and then ultrasonically cleaned with ultrapure water and ethanol to remove any other physically adsorbed substances. The cleaned electrode was subjected to cyclic voltammetry in 0.1 mol / L PBS solution and 0.1 mol / L K3[Fe(CN)6] 3- / 4- The electrode is activated in the solution until the cyclic voltammetry current is stable. The activated electrode is washed again in ultrapure water and ethanol, and dried for later use.

[0088] (2) Preparation of S,N-rGO suspension

[0089] Weigh 15 mg of graphene oxide and 45 mg of L-cysteine, mix them, add 15 mL of purified water and sonicate for 15 min, add 150 μL of ammonia water to the suspension and sonicate for 30 min to mix. Transfer the evenly dispersed liquid to a polytetrafluoroethylene autoclave and hydrothermally react at 180 ° C for 10 hours. After the reaction is completed, cool to room temperature, wash three times with deionized water, wash twice with ethanol, and vacuum dry for 12 hours to obtain dry, S, N-rGO powder for use.

[0090] (3) Preparation of S,N-rGO modified electrodes

[0091] The S, N-rGO suspension was dropped onto the dry glassy carbon electrode to prepare the S, N-rGO modified electrodes.

[0092] Comparative Example 3: B, S, N-rGO modified electrode

[0093] (1) Glassy carbon electrode pretreatment

[0094] The glassy carbon electrode was continuously polished with aluminum oxide powder to remove the surface oxide layer, and then ultrasonically cleaned with ultrapure water and ethanol to remove any other physically adsorbed substances. The cleaned electrode was subjected to cyclic voltammetry in 0.1 mol / L PBS solution and 0.1 mol / L K3[Fe(CN)6] 3- / 4- The electrode is activated in the solution until the cyclic voltammetry current is stable. The activated electrode is washed again in ultrapure water and ethanol, and dried for later use.

[0095] (2) Preparation of B, S, N-rGO suspension

[0096] Weigh 1 mg of B,S,N-rGO solid powder into a centrifuge tube, add 1 mL of DMF, and ultrasonically disperse for 15 min to obtain a B,S,N-rGO suspension.

[0097] (3) Preparation of B, S, N-rGO modified electrodes

[0098] The B,S,N-rGO suspension was dropped onto the dry glassy carbon electrode to prepare the B,S,N-rGO modified electrode.

[0099] Experimental Example 1: Evaluation of electrochemical performance of different electrodes

[0100] The modified electrodes prepared in Example 2, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were immersed in 0.1 mol / L K3[Fe(CN)6] 3- / 4- / 0.1mol / L KCl solution for electrochemical impedance spectroscopy detection. Cyclic voltammogram and electrochemical impedance spectrum are shown in Figure 5 shown.

[0101] Depend on Figure 5 It can be seen that the redox peak current signal of the Bare GCE modified electrode (Bare GCE is a bare glassy carbon electrode purchased from Tianjin Aida Hengsheng Technology Development Co., Ltd.), the GO modified electrode of Comparative Example 1, the S, N-rGO modified electrode of Comparative Example 2, the B, S, N-rGO modified electrode of Comparative Example 3 and the Au-B, S, N-rGO modified electrode of Example 1 gradually increases, and its impedance gradually decreases. This proves that Au-B, S, N-rGO can produce a synergistic effect due to the N, B, S atom doped reduced graphene oxide and gold nanoparticles, and its conductivity is much stronger than B, S, N-rGO and S, N-rGO.

[0102] Experimental Example 2: Detection limit and linear range determination

[0103] The label-free electrochemical immunosensor prepared in Example 2 was used to measure the content of cardiac troponin I (cTnI):

[0104] Establishment of standard curve: The prepared electrochemical immunosensor was used to detect cTnI antigens of different concentrations (50 ng / mL, 20 ng / mL, 5 ng / mL, 0.1 ng / mL, 0.01 ng / mL, 0.001 ng / mL and 0.0005 ng / mL) by differential pulse voltammetry, with a scanning range of 0.7 to 0 V; pulse amplitude: 50 mV, pulse period: 500 ms. The current peaks corresponding to different concentrations of cTnI antigen and the standard curves established between different concentrations of cTnI and the response current are shown in the attached Figure 6 .

[0105] Combination Figure 6 The linear range of the electrochemical immunosensor is 50 ng / mL-0.0005 ng / mL, and the linear regression equation is I=0.005lnCcTnI-0.478, (n=3R 2 =0.995) and the detection limit was 0.74 pg / mL. The comparison results of the electrochemical cTnI immunosensor with other detection methods are shown in Table 1.

[0106] Table 1 Comparison of electrochemical cTnI immunosensor with other detection methods.

[0107] Detection Methods <![CDATA[Linear range / ng·mL -1 > <![CDATA[Limit of detection / pg·mL -1 > References Electrochemistry 0.01-1 50 Liu, G, et al. 2016 Electrochemistry 0.1-10.0 70 Kazemi SH, et al. 2016 Fluorescence 0.02-40 20 B. Huang, et al. 2020 Electrochemiluminescence <![CDATA[5.0×10 -3 -20.0]]> 1.756 Tan Y, et al.2017 Electrochemistry <![CDATA[5.0×10 -4 -50.0]]> 0.74 Example 3

[0108] As shown in Table 1, the Au-B, S, N-rGO-based label-free electrochemical immunosensor provided in the embodiment of the present invention is more sensitive than other previously reported methods for detecting cTnI, and has a wider detection range and a lower detection limit. This is because the graphene lattice is doped with boron, sulfur, and nitrogen heteroatoms to improve the electrochemical activity. In addition, gold nanoparticles are modified to boron, sulfur, and nitrogen-doped reduced graphene oxide through Au-S bonds, thereby enhancing the conductivity of the composite material. The heteroatoms and Au NPs work synergistically to accelerate the electron transfer ability, thereby improving the sensitivity of the immunosensor.

[0109] Experimental Example 3: Detection limit and linear range determination

[0110] Determination of the content of amyloid β protein Aβ(1-42) by the label-free electrochemical immunosensor of Example 3:

[0111] Establishment of standard curve: The prepared electrochemical immunosensor was used to detect Aβ(1-42) antigen of different concentrations (10 ng / mL, 5 ng / mL, 1 ng / mL, 0.1 ng / mL, 0.01 ng / mL, 0.005 ng / mL, 0.001 ng / mL and 0.0001 ng / mL) by differential pulse voltammetry, with a scanning range of 0.7 to 0 V; pulse amplitude: 50 mV, pulse period: 500 ms.

[0112] The current peaks corresponding to different concentrations of Aβ(1-42) antigen and the standard curves established between different concentrations of Aβ(1-42) and the response current are shown in the attached Figure 7 . Combined Figure 7 The linear range of the electrochemical immunosensor is 10 ng / mL-0.0001 ng / mL, and the linear regression equation is I=0.0075lnCAβ(1-42)-0.3988(n=3, R 2 =0.994) with a detection limit of 0.072 pg / mL.

[0113] The comparison results of the electrochemical Aβ(1-42) immunosensor with other detection methods are shown in Table 2.

[0114] Table 2 Comparison of electrochemical Aβ(1-42) immunosensor with other detection methods.

[0115] Detection Methods <![CDATA[Linear range / ng·mL -1 > <![CDATA[Limit of detection / pg·mL -1 > References Electrochemistry <![CDATA[1.0×10 -3 -1.0]]> 1.4 Abbasi, et al. 2021 Electrochemistry <![CDATA[1.0×10 -3 -1.0]]> 3.0 Devi,et al.2020 Electrochemistry <![CDATA[2.3×10 -3 -0.45]]> 7.6 Tang M,et al.2018 Electrochemistry 2.25-36.0 0.9 Pi J,et al.2016 Electrochemistry <![CDATA[1.0×10 -4 -10.0]]> 0.072 Example 4

[0116] As shown in Table 2, the Au-B, S, N-rGO-based label-free electrochemical immunosensor provided by the present invention is more sensitive than other previously reported methods for detecting Aβ(1-42), and has a wider detection range and a lower detection limit. This is due to the increase in electrochemical activity by doping boron, sulfur, and nitrogen heteroatoms in the graphene lattice. In addition, gold nanoparticles are modified to boron, sulfur, and nitrogen-doped reduced graphene oxide through Au-S bonds, thereby enhancing the conductivity of the composite material. The heteroatoms and AuNPs work synergistically to accelerate the electron transfer ability, thereby improving the sensitivity of the immunosensor.

[0117] Finally, it should be noted that the terms "comprises," "includes," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements that are inherent to such process, method, article, or apparatus.

[0118] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0119] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a label-free electrochemical immunosensor, characterized in that: The method comprises: The graphene oxide, L-cysteine ​​and boric acid are mixed, deionized water is added for ultrasonic dispersion, and the pH is adjusted to 8-9 for hydrothermal reaction, and then naturally cooled to room temperature, washed and dried to obtain boron, sulfur and nitrogen co-doped reduced graphene oxide; The chloroauric acid solution was heated to 85-95° C., and then a sodium citrate solution was added for reflux reaction to obtain a wine red solution, which was naturally cooled to room temperature to obtain a gold nanoparticle solution; Dispersing the boron, sulfur and nitrogen co-doped reduced graphene oxide in the gold nanoparticle solution, washing and drying, to obtain an Au-B, S, N-rGO nanocomposite material; The Au-B, S, N-rGO nanocomposite material is added to EDC and NHS solution for activation to obtain a suspension; the suspension is then drop-coated on the surface of a glassy carbon electrode and dried naturally at room temperature to obtain an Au-B, S, N-rGO electrode; Adding antibody solution to the surface of the Au-B, S, N-rGO electrode for incubation and then washing, and then adding bovine serum albumin and then washing to obtain an Au-B, S, N-rGO / Ab electrode; The standard antigen solution was dropped on the surface of the Au-B,S,N-rGO / Ab electrode and incubated to obtain a label-free electrochemical immunosensor.

2. The method for preparing a label-free electrochemical immunosensor according to claim 1, characterized in that: The mass ratio of the graphene oxide to the L-cysteine ​​is 1:(1-4), and the mass ratio of the graphene oxide to the boric acid is 1:(26.6-40).

3. The method for preparing a label-free electrochemical immunosensor according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 150-200° C., and the time of the hydrothermal reaction is 8-12 h.

4. The method for preparing a label-free electrochemical immunosensor according to claim 1, characterized in that: The mass fraction of the chloroauric acid solution is 0.01%±0.005%; the mass fraction of the sodium citrate solution is 1%±0.5%; The volume ratio of the chloroauric acid solution to the sodium citrate solution is 1:(0.01-0.03).

5. The method for preparing a label-free electrochemical immunosensor according to claim 1, characterized in that: The temperature of the reflux reaction is 85 to 95° C., and the time of the reflux reaction is 10 to 45 min.

6. The method for preparing a label-free electrochemical immunosensor according to claim 1, characterized in that: The mass volume ratio of the boron, sulfur and nitrogen co-doped reduced graphene oxide to the gold nanoparticle solution is 0.5-1.5 mg / ml.

7. The method for preparing a label-free electrochemical immunosensor according to claim 1, characterized in that: The mass ratio of Au-B, S, N-rGO to EDC and NHS is 1:(1.5-5.8):(0.9-3.6).

8. The method for preparing a label-free electrochemical immunosensor according to claim 1, characterized in that: The antibody incubation temperature is 4°C; the bovine serum albumin incubation temperature is 37°C; the antigen incubation temperature is 4-50°C; and the antigen incubation time is 15-180 minutes.

9. A label-free electrochemical immunosensor prepared by the method according to any one of claims 1 to 8.