Glass fiber manufacturing device and manufacturing method
By controlling the height difference of molten glass and nozzle hole design, combined with temperature adjustment, the glass deformation and bushing load in the manufacturing of special-shaped cross-section glass fibers is solved, and fiber manufacturing with high flatness is achieved.
Patent Information
- Application Number
- CN202180013112.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-06
- Filing Date
- 2021-01-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-01-05
AI Technical Summary
In the prior art, when producing special-shaped cross-section glass fibers, molten glass is prone to deform to a perfect circle due to surface tension, making it difficult to form a high flatness, and to prevent deformation, it is necessary to increase the viscosity, which makes it difficult for the glass to flow out and exert excessive load on the bushing.
By setting nozzle holes between the feeder and the bushing, the height difference between the molten glass liquid level is 0.3m~1.5m, using a flat cross-section nozzle hole design and dumbbell-shaped nozzle hole, combined with the heating unit to adjust the glass temperature to ensure the glass Have sufficient viscosity upon flow and reduce load on the bushing.
It is realized that molten glass is easy to flow out and not easily deform, avoiding excessive load on the bushing, and can produce high flat rate special-shaped cross-section glass fibers, which can adapt to a variety of glass fiber manufacturing conditions.
Smart Images

Figure CN115066403B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a device and a method for manufacturing glass fibers, and more particularly to a device and a method for manufacturing glass fibers with flat cross-sections and special cross-sections. Background Art
[0002] As one type of glass fiber, a flat cross-sectional shape of a special-shaped cross-section glass fiber is known (see Patent Document 1). The strength of a fiber-reinforced plastic (FRP) obtained by kneading and compounding the special-shaped cross-section glass fiber with a resin is high, so the special-shaped cross-section glass fiber is used in various fields such as fibers for FRP.
[0003] Here, the profiled cross-section glass fiber can be produced, for example, by the following method.
[0004] The irregular cross-section glass fiber is manufactured using a device having a feeder and a bushing, the feeder being used to circulate molten glass generated in a glass melting furnace, etc., and the bushing being arranged at a position lower than the feeder. The bushing has a plurality of nozzles, and the nozzle hole provided in each nozzle is formed into a flat shape (long round, elliptical, etc.). The irregular cross-section glass fiber is manufactured by causing the molten glass to flow out from the nozzle hole of each nozzle while the entire flow path from the inside of the feeder to the nozzle hole of the bushing is filled with molten glass, and the molten glass that has flowed out is drawn out and cooled.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2018 / 020743 Summary of the invention
[0008] Technical problem that the invention aims to solve
[0009] However, the above method has the following problems.
[0010] When the molten glass flows out from the nozzle hole, due to the influence of surface tension, the molten glass will deform in the direction in which its surface area becomes smaller. That is, the molten glass deforms in a way that the cross section becomes a perfect circle. Therefore, it is not easy to form a special-shaped cross-section glass fiber with a high flatness. As a countermeasure, in order to increase the viscosity of the molten glass and suppress the deformation caused by surface tension, it is considered to make the temperature of the molten glass flowing out of the nozzle hole low temperature. However, due to this countermeasure, the viscosity of the molten glass becomes high, so it is easy to make it difficult for the molten glass to flow out from the nozzle hole. Therefore, when manufacturing a special-shaped cross-section glass fiber, it is necessary to make improvements so that the molten glass can easily flow out from the nozzle hole. However, due to this improvement, a load will be applied to the bushing. Therefore, it is desired to manufacture a special-shaped cross-section glass fiber with a high flatness without increasing the load on the bushing.
[0011] The present invention has been made in view of the above circumstances and has as its technical object to enable molten glass to flow out easily from a nozzle hole and to avoid excessive load on a bushing when producing a deformed cross-section glass fiber.
[0012] Technical solutions to the problem
[0013] The present invention for solving the above-mentioned problems is constructed as follows: it comprises: a feeder, which allows molten glass to flow; and a bushing, which is provided with a nozzle hole with a flat cross-section and is arranged at a position lower than the feeder, and in a state where the entire flow path from the inside of the feeder to the nozzle hole of the bushing is filled with molten glass, the molten glass supplied from the feeder to the bushing flows out from the nozzle hole to manufacture special-shaped cross-section glass fibers, and in the glass fiber manufacturing device, the height difference between the nozzle hole and the liquid level of the molten glass in the feeder is 0.3m to 1.5m.
[0014] In the present device, by making the height difference between the nozzle hole and the liquid level of the molten glass in the feeder less than 1.5m, the pressure acting on the bushing from the molten glass can be made to fall within the range where the load applied to the bushing is not excessive. Furthermore, by making the above-mentioned height difference more than 0.3m, it is possible to ensure a sufficiently large pressure (head pressure) so that the molten glass can easily flow out of the nozzle hole. Based on the above content, according to the present device, when manufacturing special-shaped cross-section glass fibers, the molten glass can be easily made to flow out from the nozzle hole, and excessive load on the bushing can be suppressed. In addition, according to the present device, the following effects can also be obtained. That is, it is possible to avoid excessive load on the bushing. Therefore, compared with the past, it is possible to achieve a design change that can reduce the strength of the bushing, such as increasing the number of nozzle holes provided on the bushing or enlarging the opening area of each nozzle hole, and can widely cope with a variety of glass fiber manufacturing conditions.
[0015] The glass fiber production apparatus of the present invention preferably includes a pipe connecting the feeder and the bushing.
[0016] In this way, by adjusting the length of the tube in the vertical direction, the height difference between the nozzle hole and the liquid level of the molten glass in the feeder can be easily changed. Therefore, the pressure acting on the bushing from the molten glass can be easily changed. As a result, it is possible to avoid excessive load on the bushing while ensuring the head pressure of the flat nozzle hole suitable for making the molten glass flow out easily from the nozzle hole.
[0017] In the glass fiber manufacturing device of the present invention, it is preferred that the nozzle hole has a pair of short wall surfaces opposing each other in the long diameter direction of the flat cross-section and a pair of long wall surfaces opposing each other in the short diameter direction of the flat cross-section, the pair of short wall surfaces are straight and parallel to each other, and the distance between the pair of long wall surfaces decreases in the long diameter direction from the side of each short wall surface in the pair of short wall surfaces toward the center between the pair of short wall surfaces.
[0018] Thus, the area of the two end sides of the flat cross section of the nozzle hole is larger than the area of the central side. Therefore, the amount of molten glass flowing out from the central side of the flat cross section of the nozzle hole is less than the amount of molten glass flowing out from the two end sides of the flat cross section of the nozzle hole, so the molten glass on the central side is quickly cooled and solidified, and as a result, it is not easy to deform in the direction in which the surface area of the molten glass becomes smaller. Therefore, it is possible to manufacture a high flatness fiber. In addition, by adjusting the distance between the pair of long wall surfaces at the central part and the two end sides, the height difference between the nozzle hole corresponding to the distance and the liquid level of the molten glass in the feeder can be easily set.
[0019] In the glass fiber manufacturing device of the present invention, it is preferred that the flat cross-section of the nozzle hole is a dumbbell shape including a central wall portion and a pair of end wall portions located at both ends of the central wall portion, the central wall portion has a pair of straight and mutually parallel central wall portions, and the pair of end wall portions respectively have: a pair of vertical end wall portions, which are connected to the central wall portion and are perpendicular to the central wall portion when viewed from above; a pair of parallel end wall portions, which are connected to the vertical end wall portions and are parallel to the central wall portion when viewed from above; and terminal end wall portions, which are connected to the parallel end wall portions and are parallel to the pair of vertical end wall portions.
[0020] Thus, the molten glass flowing out from the two ends of the dumbbell shape is surrounded by multiple wall surfaces, so the molten glass is subject to greater resistance. As a result, the overall rounding of the cross section of the glass fiber can be avoided, and high flatness fiber can be manufactured. By adjusting the dumbbell shape, the height difference between the nozzle hole and the liquid level of the molten glass in the feeder can be adjusted.
[0021] The glass fiber production apparatus of the present invention preferably includes a heating means for providing a temperature difference between the bushing and the tube.
[0022] Thereby, the temperature of the molten glass before flowing into the bushing can be maintained higher than the temperature of the molten glass when flowing out from the nozzle hole (temperature suitable for forming glass fibers).
[0023] In the glass fiber production apparatus of the present invention, it is preferred that the temperature of the tube be adjusted to be higher than the temperature of the bushing by the heating means.
[0024] In this way, the temperature of the tube can be adjusted to be higher than the temperature of the bushing, so the viscosity of the molten glass can be maintained at a low state until it is about to flow into the bushing from the tube. On the other hand, the temperature of the molten glass is lowered after it flows into the bushing, and the viscosity of the molten glass can be increased to a viscosity suitable for manufacturing fibers with a high flatness. In this way, the viscosity of the molten glass can be made as low as possible until it is about to flow into the bushing, and the pressure loss of the molten glass when it flows in the tube can be reduced. Therefore, the height difference between the nozzle hole and the liquid level of the molten glass in the feeder can be reduced.
[0025] In the glass fiber production apparatus of the present invention, it is preferable that the ratio of the opening area of the nozzle hole to the unit area of the surface of the bushing on which the nozzle hole is provided is 5% to 15%.
[0026] Thereby, glass fibers can be produced efficiently.
[0027] In addition, in order to solve the above-mentioned problem, the manufacturing method of the glass fiber of the present invention uses a feeder for circulating molten glass and a bushing provided with a nozzle hole with a flat cross-section and arranged at a position lower than the feeder. When the entire flow path from the inside of the feeder to the nozzle hole of the bushing is filled with molten glass, the molten glass supplied from the feeder to the bushing flows out from the nozzle hole to manufacture special-shaped cross-section glass fibers. In the manufacturing method of the glass fiber, the height difference between the nozzle hole and the liquid level of the molten glass in the feeder is set to 0.3m to 1.5m.
[0028] According to this method, the above-mentioned operation and effects obtained by the above-mentioned glass fiber production apparatus of the present invention can be obtained in the same manner.
[0029] In the method for producing glass fibers of the present invention, it is preferred that a heating unit is used to adjust the temperature of a tube connecting the feeder and the bushing to be higher than the temperature of the bushing.
[0030] According to this method, the above-mentioned operation and effects obtained by the above-mentioned glass fiber production apparatus of the present invention can be obtained in the same manner.
[0031] Effects of the Invention
[0032] According to the present invention, when producing a deformed cross-section glass fiber, molten glass can be easily flowed out from the nozzle hole, and excessive load on the bushing can be avoided. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a cross-sectional view of the glass fiber production apparatus according to the first embodiment.
[0034] Figure 2It is a cross-sectional view showing the periphery of the nozzle for deformed-cross-section glass fibers included in the glass fiber production apparatus according to the first embodiment.
[0035] Figure 3 It is a bottom view showing the periphery of the nozzle for deformed-cross-section glass fibers included in the glass fiber production apparatus according to the first embodiment.
[0036] Figure 4 The figures are figures showing a nozzle for irregular-section glass fibers provided in a glass fiber manufacturing device according to a first embodiment, wherein (a) is a side view of the nozzle, (b) is a 4b-4b sectional view of (a), (c) is a 4c-4c sectional view of (a), and (d) is a 4d-4d sectional view of (a).
[0037] Figure 5 It is a cross-sectional view showing a glass fiber with a special cross section.
[0038] Figure 6 The figures are figures showing a nozzle for irregular-section glass fibers provided in a glass fiber manufacturing apparatus according to a second embodiment, wherein (a) is a side view of the nozzle, (b) is a 9b-9b sectional view of (a), and (c) is a 9c-9c sectional view of (a).
[0039] Figure 7 The drawings show a nozzle for irregular-cross-section glass fibers provided in a glass fiber production apparatus according to a third embodiment, wherein (a) is a side view of the nozzle and (b) is a top view.
[0040] Figure 8 It is a cross-sectional view of a glass fiber production apparatus according to a fourth embodiment.
[0041] Fig. 9 It is a bottom view schematically showing the periphery of the nozzle for irregular-cross-section glass fibers included in the glass fiber production apparatus according to the fifth embodiment.
[0042] Explanation of symbols
[0043] 1 Glass fiber manufacturing device
[0044] 2 Molten Glass
[0045] 2a Liquid level
[0046] 2f Special-section glass fiber
[0047] 3 feeder
[0048] 4 Bushing
[0049] 5 Tubes
[0050] 6 Nozzle hole
[0051] H Height difference DETAILED DESCRIPTION
[0052] Hereinafter, a glass fiber manufacturing apparatus and a glass fiber manufacturing method according to embodiments of the present invention will be described with reference to the drawings.
[0053] In the present specification, a numerical range expressed using “to” means a range including the numerical values described before and after “to” as the minimum value and the maximum value, respectively.
[0054] <First Embodiment>
[0055] In the execution of the method for producing glass fiber according to the first embodiment, Figure 1 The manufacturing device 1 of glass fiber shown in the figure (hereinafter referred to as manufacturing device 1). The manufacturing device 1 includes a feeder 3 for circulating molten glass 2, a bushing 4 arranged at a position lower than the feeder 3, and a tube 5 connecting the feeder 3 and the bushing 4. The manufacturing device 1 is configured to supply molten glass 2 from the feeder 3 to the bushing 4 via the tube 5, and to draw out and cool the molten glass 2 flowing out of the nozzle hole 6 of the bushing 4 to manufacture a special-shaped cross-section glass fiber 2f (hereinafter referred to as glass fiber 2f).
[0056] In the present embodiment, the molten glass 2 is made of E glass, but the present invention is not limited thereto, and the molten glass 2 may be made of other glass such as D glass, S glass, AR glass, or C glass.
[0057] The feeder 3 is connected to a glass melting furnace (not shown) and can flow molten glass 2 generated by continuously melting glass raw materials in the melting furnace. A liquid level 2a of the molten glass 2 is formed inside the feeder 3. The height of the liquid level 2a of the molten glass 2 is adjusted by the amount of glass raw materials supplied to the melting furnace per unit time, etc.
[0058] The bushing 4 has a base plate 7 at the bottom. The base plate 7 has a plurality of nozzles 8 for irregular cross-section glass fibers (hereinafter referred to as nozzles 8) having the same structure as each other, and a cooling pipe 9 disposed near the nozzles 8. In addition, a nozzle hole 6 is formed in each nozzle 8. The nozzle hole 6 provided in each nozzle 8 is formed flat, and the details will be described later.
[0059] The cross-sectional shape of the tube 5 is formed into a cylindrical shape, and is arranged in a manner that the tube axis extends in the vertical direction. The upper end of the tube 5 is connected to the bottom of the feeder 3, and the lower end of the tube 5 is connected to the upper end of the bushing 4. It should be noted that as long as the tube 5 can connect the feeder 3 located relatively above and the bushing 4 located relatively below, the cross-sectional shape of the tube 5 and the direction in which the tube axis extends may be different from those in the present embodiment. In addition, the feeder 3 and the tube 5 may also be connected by a flow block and a bushing block that are omitted from the figure.
[0060] Part or the entirety of each of the bushing 4 , the tube 5 , the nozzle 8 , and the cooling tube 9 is made of platinum or a platinum alloy (for example, a platinum-rhodium alloy).
[0061] The entire flow path from the connection between the bottom of the feeder 3 and the upper end of the tube 5 to the nozzle hole 6 of the bushing 4 is filled with the molten glass 2. Thus, the pressure (head pressure) for causing the molten glass 2 to flow out of the nozzle hole 6 is determined by the height difference H between the nozzle hole 6 and the liquid level 2a of the molten glass 2 in the feeder 3. Here, the height difference H can be adjusted mainly by changing the length of the tube 5, for example.
[0062] The height difference H is adjusted to 0.3m to 1.5m. This is because if the height difference H is less than 0.3m, the head pressure becomes too small, and it may be difficult to make the molten glass 2 flow out from the nozzle hole 6 with a flat cross section. On the other hand, if the height difference H exceeds 1.5m, the head pressure becomes too large, which will apply excessive load to the bushing 4 (substrate 7). It should be noted that it is preferred to adjust the height difference H to 0.5m to 1.2m, and it is more preferred to adjust the height difference H to 0.5m to 1m.
[0063] The temperature and viscosity of the molten glass 2 when forming the glass fibers 2f are set to 1100°C to 1250°C (preferably 1150°C to 1200°C), 10 2.6 dPa·s~10 3·8 dPa·s (preferably 10 2.9 dPa·s~10 3·3 dPa·s). The "temperature and viscosity of the molten glass 2" mentioned here refers to the temperature and viscosity of the molten glass 2 at the position where it flows into the nozzle 8. In addition, the temperature and viscosity of the molten glass 2 are adjusted by, for example, heating both the bushing 4 and the tube 5. In addition, the temperature and viscosity of the molten glass 2 can also be adjusted by heating the molten glass 2 and the feeder 3 in the glass melting furnace by electric heating.
[0064] On the surface of the glass fiber 2f, a sizing agent is applied by an applicator (not shown), and hundreds to thousands of glass fibers 2f are spun into a strand 2s. The spun strand 2s is wound around a bobbin 10 as a winding device as a fiber bundle 2r. The strand 2s is cut into a length of about 1 mm to 20 mm, for example, and used as a chopped strand.
[0065] like Figure 2 and Figure 3As shown, the nozzle 8 has a pair of relatively long long wall portions 11 and a pair of relatively short short wall portions 12 at the front end portion for flowing out the molten glass 2. The nozzle hole 6 having a flat cross section is formed by being surrounded by these long wall portions 11 and short wall portions 12. A notch portion 13 is provided in each of the pair of long wall portions 11, 11, and the nozzle hole 6 is connected to the external space of the nozzle 8 through the notch portion 13.
[0066] The cooling pipe 9 cools the molten glass 2 by circulating cooling water 14 therein. The outer shape of the cooling pipe 9 is formed in a plate shape, and is arranged in a manner such that the plate surface is parallel to the long wall portion 11. Here, the cooling pipe 9 is provided integrally with the substrate 7, but may also be provided at a position away from the substrate 7. In addition, the cooling pipe 9 may also be formed in a circular tube shape.
[0067] The height position of the cooling pipe 9 is adjusted according to the cooling conditions of the molten glass 2. As an example, the cooling pipe 9 can be arranged at a position above the front end of the nozzle 8 in a manner that the molten glass 2 drawn from the nozzle 8 does not face the plate surface of the cooling pipe 9. On the other hand, the cooling pipe 9 can also be arranged across the top and bottom of the front end of the nozzle 8 in a manner that both the nozzle 8 and the molten glass 2 drawn from the nozzle 8 face the plate surface of the cooling pipe 9. In addition, in the cooling of the molten glass 2, in addition to using the cooling pipe 9, cooling fins or the like that cool the molten glass 2 by air flow can also be used. In addition, the cooling pipe 9 is not a necessary structure and can also be omitted.
[0068] like Figure 3 As shown in FIG. 1 , a plurality of nozzle rows P are arranged in parallel at intervals on a substrate 7. Each nozzle row P includes a plurality of nozzles 8. The plurality of nozzles 8 included in the same nozzle row P are arranged so that the nozzle holes 6 formed in the plurality of nozzles 8 are located on the same straight line. The number of the nozzle holes 6 is, for example, 100 or more, preferably 300 or more, and more preferably 800 or more. In addition, the number of the nozzle holes 6 is, for example, 5000 or less, preferably 3000 or less, and more preferably 1500 or less.
[0069] The cooling pipe 9 is arranged between two adjacent nozzle rows P and P so as to extend parallel to the nozzle row P. Thus, the molten glass 2 in the nozzle hole 6 is cooled by the notch 13 facing the cooling pipe 9. Specifically, at the front end of the nozzle 8, the molten glass 2 is rapidly cooled by the cooling pipe 9 from a temperature of more than 1000°C. Here, the cooling pipe 9 also has a function of improving durability by cooling the bushing 4 (substrate 7) and the nozzle 8 to suppress the deterioration of these components caused by heat.
[0070] like Figure 4As shown in (a) to (d), the notch 13 provided in the long wall portion 11 of each nozzle 8 is formed into an isosceles trapezoid whose upper base is shorter than the lower base. Thus, the opening width of the notch 13 gradually increases as it moves toward the front end of the nozzle 8. In addition, in the present embodiment, the lower base of the trapezoid is substantially the same length as the long wall portion 11. In addition, the depth D (length along the up and down direction) of the notch 13 is set to 0.1 mm to 2 mm. This is because, in the case where the depth D exceeds 2 mm, in the cross section of the manufactured glass fiber 2f, the two ends in the length direction are too thin, and the glass fiber 2f is easily damaged.
[0071] The shape of the notch 13 is not limited to a trapezoid, and may be other shapes. For example, it may be a triangle or a semicircle. However, even in the case of adopting these other shapes, the notch 13 preferably has an opening width that gradually expands as it goes toward the front end side of the nozzle 8. In addition, the notch 13 is not a necessary structure and may be omitted.
[0072] The nozzle hole 6 has: an inlet for the molten glass 2 formed on the base end side of the nozzle 8; and an outlet for the molten glass 2 formed on the front end side, and the cross section of the nozzle hole 6 is a uniform shape from the inlet to the outlet. Here, each nozzle hole 6 formed in the plurality of nozzles 8 has the same structure (specifically, shape, size, surface roughness of the inner peripheral surface 15). In addition, the cross-sectional shape of the nozzle hole 6 may be different between the inlet and the outlet. That is, the shape of the nozzle hole 6 may change from the inlet to the outlet.
[0073] The nozzle hole 6 has an inner circumferential surface 15 made of platinum or a platinum alloy. The inner circumferential surface 15 has: a pair of short wall surfaces 15a, 15a, which are opposite to each other in the long diameter direction of the flat cross section of the nozzle hole 6; and a pair of long wall surfaces 15b, 15b, which are opposite to each other in the short diameter direction of the flat cross section of the nozzle hole 6. In the present embodiment, the pair of short wall surfaces 15a, 15a are arc-shaped, and the pair of long wall surfaces 15b, 15b are parallel to each other. Therefore, the nozzle hole 6 is an oblong shape. Here, when the length of the short wall surface 15a along the short diameter direction is X and the length of the long wall surface 15b along the long diameter direction is Y, the value of (Y / X) is set to 2 to 5. In addition, when the cross-sectional shape of the nozzle hole 6 changes from the inlet to the outlet, the value of (Y / X) before and after the change is in the range of 2 to 5. In this case, the value of (Y / X) before and after the change may also be different.
[0074] In addition, the average value of the surface roughness Ra of the short wall surface 15a is greater than the average value of the surface roughness Ra of the long wall surface 15b. Specifically, the average value of the surface roughness Ra of the short wall surface 15a is within the range of 2 μm or more and 10 μm or less, and the average value of the surface roughness Ra of the long wall surface 15b is within the range of 1 μm or more and less than 10 μm.
[0075] The average value of the surface roughness Ra can be adjusted by changing the shape of the drill used or vibrating the drill when forming the nozzle hole 6 by drilling. In addition, the average value of the surface roughness Ra can also be adjusted by bringing the drill into contact with the formed nozzle hole 6 again or performing annealing.
[0076] Here, the average value of the surface roughness Ra is a value in an unused state (i.e., a state before the molten glass 2 is circulated). The specific method for measuring the average value of the surface roughness Ra is as follows (1) to (4). (1) After a plurality of nozzles 8 that can be assembled into the present manufacturing apparatus are manufactured under the same manufacturing conditions, the nozzle 8 to be measured is extracted from these nozzles 8 as a sample. (2) The extracted sample is oriented along the direction in which the hole axis of the nozzle hole 6 extends (i.e., when the sample is assembled into the present manufacturing apparatus, it becomes Figure 1 , 2 (in the vertical direction). (3) For the inner circumferential surface 15 (short wall surface 15a and long wall surface 15b) of the nozzle hole 6, the measurement is performed in the direction along which the hole axis of the nozzle hole 6 extends in accordance with JIS B0601:2001. It should be noted that a surface roughness meter (product name: ET4000) manufactured by Kosaka Laboratory Co., Ltd. is used in the measurement, and the measurement distance is set to 1 mm. Here, the measurement is carried out on six locations with different positions (specifically, three locations for the short wall surface 15a and three locations for the long wall surface 15b). (4) The average value of the surface roughness Ra values measured at each of the six locations is taken as the average value of the surface roughness Ra of the inner circumferential surface 15. Furthermore, the average values of the three surface roughness Ra values measured by the short wall surface 15a and the long wall surface 15b are taken as the average values of the surface roughness Ra of the short wall surface 15a and the long wall surface 15b, respectively. On this basis, the average value of the surface roughness Ra of the inner peripheral surface 15 , the short wall surface 15 a , and the long wall surface 15 b of the nozzle 8 other than the sample is regarded as the same value as the average value of the surface roughness Ra measured for the sample.
[0077] The average value of the kurtosis Rku (pointiness) of the inner peripheral surface 15 of the nozzle hole 6 is greater than or equal to 2 (preferably within the range of 4 to 10). The magnitude relationship of the kurtosis Rku between the short wall surface 15a and the long wall surface 15b is the same as the surface roughness Ra.
[0078] like Figure 5As shown, the glass fibers 2f manufactured by the manufacturing device constructed as described above each become irregular cross-section glass fibers having a flat cross-section shape (i.e., the shape in the cross section perpendicular to the lead-out direction). According to the manufacturing device, the contact resistance between the molten glass 2 at the short wall surface 15a and the inner peripheral surface 15 is greater than the contact resistance between the molten glass 2 at the long wall surface 15b and the inner peripheral surface 15. Therefore, the rounding of the entire cross section of the glass fiber 2f can be avoided, and a high flatness fiber can be manufactured.
[0079] Therefore, according to the manufacturing apparatus 1 configured as described above, by making the height difference H less than 1.5 m, it is possible to avoid excessive load on the bushing 4 (substrate 7). In addition, according to the manufacturing apparatus 1 configured as described above, by making the height difference H more than 0.3 m, it is possible to make the molten glass 2 flow out from the nozzle hole 6 easily. Therefore, it is possible to avoid damage to the bushing 4 (substrate 7) caused by high pressure, and obtain a glass having Figure 5 The glass fiber 2f has a high flattening ratio cross-sectional shape (that is, a cross-sectional shape perpendicular to the drawing direction of the glass fiber 2f) as shown. Specifically, the cross-sectional shape of the glass fiber 2f is formed into a shape close to an oval.
[0080] In the description of the other embodiments, the same reference numerals are used for elements substantially the same as those described in the first embodiment, and duplicate descriptions are omitted, and only differences from the first embodiment are described.
[0081] <Second Embodiment>
[0082] like Figure 6 As shown in (a) to (c), the second embodiment is different from the first embodiment described above in that: when viewed from the direction along the axis of the nozzle hole 6, the pair of short wall surfaces 15a are linear, and the pair of short wall surfaces 15a are parallel to each other; in the long diameter direction of the flat cross section of the nozzle hole 6, the distance between the pair of long wall surfaces 15b decreases as the distance from each short wall surface side of the pair of short wall surfaces 15a toward the center between the pair of short wall surfaces 15a. As a result, the area of the two end sides of the flat cross section of the nozzle hole 6 is larger than the area of the center side. As a result, the amount of molten glass 2 flowing out from the center side of the flat cross section of the nozzle hole 6 is less than the amount of molten glass 2 flowing out from the two end sides of the flat cross section of the nozzle hole 6, so the molten glass 2 on the center side is quickly cooled and solidified, and as a result, it is difficult to deform in the direction in which the surface area of the molten glass 2 decreases. Therefore, a high flatness fiber can be manufactured. In addition, by adjusting the distance between the pair of long wall surfaces 15b in the center and on the two end sides, it can be set to a height difference H corresponding to the distance.
[0083] In addition, the surface roughness Ra of the short wall surface 15 a and the long wall surface 15 b is preferably the same as that of the first embodiment.
[0084] <Third Embodiment>
[0085] like Figure 7 As shown in (a) and (b) of the third embodiment, the difference between the third embodiment and the first embodiment is that the nozzle hole 6 is formed into a dumbbell shape, and the flat cross section of the nozzle hole 6 includes a central wall surface and a pair of end wall surfaces located at both ends of the central wall surface. Figure 7 As shown in (b), the nozzle 8 includes: a pair of straight and mutually parallel central wall surfaces 15c, 15c constituting the central wall surface; and a pair of end wall surfaces 15d, 15d. In addition, the pair of end wall surfaces 15d, 15d respectively include: a pair of vertical end wall surfaces 15d1, 15d1 connected to the central wall surface 15c and perpendicular to the central wall surface 15c when viewed from above; a pair of parallel end wall surfaces 15d2, 15d2 connected to the vertical end wall surface 15d1 and parallel to the central wall surface 15c when viewed from above; and terminal end wall surfaces 15d3 connected to the pair of parallel end wall surfaces 15d2 and parallel to the vertical end wall surface 15d1. As a result, the molten glass 2 flowing out of the end wall surface 15d is surrounded by the vertical end wall surface 15d1, the parallel end wall surface 15d2 and the terminal end wall surface 15d3, so that the molten glass 2 is subject to a large resistance from the end wall surface 15d. As a result, the entire cross section of the glass fiber 2f can be prevented from being rounded, and a high-flatness fiber can be produced. The height difference H can be adjusted by adjusting the shape of the wall surface portions 15d at both ends.
[0086] In addition, it is preferable that the average value of the surface roughness Ra of the end wall surface portions 15 d is larger than the average value of the surface roughness Ra of the central wall surface 15 c .
[0087] <Fourth Embodiment>
[0088] exist Figure 8 In the fourth embodiment shown, the manufacturing apparatus 1 is provided with a heating unit 18 for providing a temperature difference between the bushing 4 and the tube 5, and the temperature of the tube 5 is adjusted to be higher than the temperature of the bushing 4 by the heating unit 18. Thus, the temperature of the molten glass 2 before flowing into the bushing 4 is maintained higher than the temperature of the molten glass 2 when flowing out of the nozzle hole 6 (a temperature suitable for forming the glass fiber 2f). And, by adjusting the temperature of the molten glass 2 before flowing into the bushing 4 and the temperature of the molten glass 2 when flowing out of the nozzle hole 6 as described below, it is possible to set a height difference H corresponding to the temperature.
[0089] The heating unit 18 includes a first heater 19 for electrically heating the liner 4 and a second heater 20 for electrically heating the tube 5. The first heater 19 and the second heater 20 can independently adjust the magnitude of the current flowing in the liner 4 and the tube 5, respectively, thereby independently heating the liner 4 and the tube 5. In addition, a heater including an electromagnetic induction heating coil surrounding the tube 5 may be provided instead of the second heater 20.
[0090] In this device, the temperature of the tube 5 can be adjusted to be higher than the temperature of the bushing 4, so the temperature of the molten glass 2 can be kept high until just before it flows from the tube 5 into the bushing 4, and the viscosity of the molten glass 2 can be maintained at a low state at the upstream side of the bushing 4. Furthermore, after flowing into the bushing 4, the temperature of the molten glass 2 is lowered, and the viscosity of the molten glass 2 can be increased to a viscosity suitable for manufacturing fibers with a high flatness. In this way, the viscosity of the molten glass 2 can be made as low as possible until just before it flows into the bushing 4, thereby reducing the pressure loss when the molten glass 2 flows in the tube 5. Therefore, the height difference between the nozzle hole 6 and the liquid level of the molten glass 2 in the feeder 3 can be reduced.
[0091] Here, in order to avoid devitrification in the molten glass 2, the temperature of the bushing 4 is preferably set to 1100° C. or higher. The temperature of the bushing 4 is, for example, 1130° C. to 1280° C. On the other hand, the temperature of the tube 5 is, for example, 1180° C. to 1350° C. In addition, in the present embodiment, the temperature difference between the bushing 4 and the tube 5 is set to 50° C. to 200° C.
[0092] <Fifth Embodiment>
[0093] exist Fig. 9 In the fifth embodiment shown (illustration other than the nozzle hole 6 and the substrate 7 is omitted), the nozzle hole 6 is formed into an oblong shape, and the ratio of the opening area of the nozzle hole 6 to the unit area of the substrate 7 is adjusted to 5% to 15%. The reason for adjusting within this range is that if the ratio is less than 5%, it may be difficult to make the molten glass 2 flow out of the nozzle hole 6, and if the ratio exceeds 15%, there is a possibility that the strength of the bushing 4 (substrate 7) becomes insufficient. By adjusting the ratio of the opening area of the nozzle hole 6 to the unit area of the substrate 7 to 5% to 15%, glass fibers can be efficiently manufactured.
[0094] In this embodiment, the above ratio is expressed by {( Fig. 9The above ratio can be calculated by increasing or decreasing the number of nozzle holes 6 while keeping the opening area of each nozzle hole 6 fixed, or by increasing or decreasing the opening area of each nozzle hole 6 while keeping the number of nozzle holes 6 fixed. However, it is preferred that the opening area of each nozzle hole 6 is 3 mm 2 ~15mm 2 In addition, regarding the nozzle hole 6 , the value of (Y / X) is preferably 2 to 8.
[0095] Here, the manufacturing device and manufacturing method of glass fiber involved in the present invention are not limited to the structure and mode described in the above-mentioned embodiment. For example, in the above-mentioned embodiment, the bottom of the feeder 3 is connected to the upper end of the bushing 4 by the tube 5, but it is not limited to this. It is also possible to remove the tube 5 and directly attach the upper end of the bushing 4 to the bottom of the feeder 3. Even in this case, the height difference H between the nozzle hole 6 and the liquid level 2a of the molten glass 2 in the feeder 3 is set to 0.3m to 1.5m.
Claims
1. A glass fiber manufacturing device, characterized in that: The manufacturing device comprises: a feeder that circulates molten glass; a bushing that is provided with a nozzle hole having a flat cross section and is arranged below the feeder; and a pipe that connects the feeder and the bushing. and a heating unit for setting a temperature difference between the bushing and the pipe, In a state where the entire flow path from the inside of the feeder to the nozzle hole of the bushing is filled with molten glass, the molten glass supplied from the feeder to the bushing is made to flow out from the nozzle hole to produce a deformed cross-section glass fiber. The glass fiber manufacturing apparatus is configured such that the temperature of the tube is adjusted to be higher than the temperature of the bushing by the heating means, and the height difference between the nozzle hole and the liquid level of the molten glass in the feeder is 0.3 m to 1.5 m.
2. The glass fiber manufacturing device according to claim 1, characterized in that: The temperature difference between the bushing and the tube is 50°C to 200°C.
3. The glass fiber manufacturing device according to claim 1 or 2, characterized in that: The nozzle hole has: a pair of short wall surfaces, the pair of short wall surfaces are opposite to each other in the long diameter direction of the flat cross section; and a pair of long wall surfaces, the pair of long wall surfaces are opposite to each other in the short diameter direction of the flat cross section, The pair of short wall surfaces are straight and parallel to each other, The distance between the pair of long wall surfaces decreases in the major diameter direction from the respective short wall surfaces of the pair of short wall surfaces toward the center between the pair of short wall surfaces.
4. The glass fiber manufacturing device according to claim 1 or 2, characterized in that: The flat cross section of the nozzle hole is a dumbbell shape including a central wall portion and a pair of end wall portions located at both ends of the central wall portion. The central wall portion has a pair of straight central wall surfaces that are parallel to each other. The pair of end wall portions respectively include: a pair of vertical end wall surfaces, which are connected to the central wall surface and are perpendicular to the central wall surface when viewed from above; a pair of parallel end wall surfaces, which are connected to the vertical end wall surfaces and are parallel to the central wall surface when viewed from above; and terminal end wall surfaces, which are connected to the parallel end wall surfaces and are parallel to the pair of vertical end wall surfaces.
5. The glass fiber manufacturing device according to claim 1 or 2, characterized in that: The ratio of the opening area of the nozzle hole to a unit area of the surface of the bushing on which the nozzle hole is provided is 5% to 15%.
6. A method for producing glass fiber, characterized in that: A feeder for circulating molten glass, a bushing provided with a nozzle hole having a flat cross section and arranged below the feeder, a pipe connecting the feeder and the bushing, and a heating unit for providing a temperature difference between the bushing and the pipe, In a state where the entire flow path from the feeder to the nozzle hole of the bushing is filled with molten glass, the molten glass supplied from the feeder to the bushing flows out from the nozzle hole to produce a deformed cross-section glass fiber, In the method for producing glass fiber, The temperature of the tube is adjusted to be higher than the temperature of the bushing using the heating means, and the height difference between the nozzle hole and the liquid level of the molten glass in the feeder is set to 0.3 m to 1.5 m.
7. The method for producing glass fiber according to claim 6, characterized in that: The temperature difference between the bushing and the tube is 50°C to 200°C.
Citation Information
Patent Citations
Manufacturing apparatus and manufacturing method for modified cross-section glass fiber
WO2018020743A1
Nozzle for producing glass fibers having modified cross-section, and modified cross-section glass fiber production device and production method therefor
CN109071313A
Nozzle tip for producing glass fibers and method for producing glass fibers
CN110337422A
Production glass fiber wire drawing smelting pot
CN208200748U