A method for evaluating the anti-skid performance of the wearing layer of steel slag asphalt mixture pavement

By establishing a correlation model of friction factor and texture parameters and friction coefficient decay law on the road surface of steel slag asphalt mixture, combined with three-dimensional laser scanning technology, the problems of poor universality and low repetition of anti-slip performance evaluation in the existing technology are solved. The rapid and accurate evaluation and targeted treatment of the anti-slip properties of steel slag asphalt pavement are achieved.

CN115081813BActive Publication Date: 2024-11-15TONGJI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210557396.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-20
Publication Date
2024-11-15
Estimated Expiration
2042-05-20

AI Technical Summary

Technical Problem

The prior art has poor universality, poor repeatability, low test efficiency, and great influence on human factors when evaluating the anti-slip properties of steel slag asphalt pavements, which leads to inaccurate evaluation of anti-slip properties.

Method used

By abrading the steel slag asphalt mixture under an indoor accelerated loading wear meter, recording the friction factor and texture parameters, establishing a correlation model between the friction factor and texture parameters and a friction coefficient decay law prediction model, and formulating anti-slip performance status evaluation standards , three-dimensional laser scanning technology is used to collect pavement texture data and calculate friction coefficient to evaluate anti-slip performance.

Benefits of technology

It realizes a fast, accurate and objective evaluation of the anti-slip properties of steel slag asphalt mixture pavement, overcomes the problems of poor universality and low repetition of traditional methods, provides targeted repair or treatment measures, and improves the accuracy and practicality of evaluation. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115081813B_ABST
    Figure CN115081813B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for evaluating the anti-skid performance of a wearing layer of a steel slag asphalt mixture pavement, comprising: obtaining a modeling sample of a steel slag asphalt mixture pavement, and performing abrasion at different times under a set load to obtain modeling samples with different wear degrees; recording a friction factor μ, a macro texture parameter, and a micro texture parameter under each set number of times; establishing a correlation model between the friction factor and the macro texture and the micro texture, and establishing a friction coefficient decay law prediction model that associates the friction coefficient with the number of load actions; drawing a curve, and selecting a critical value μ according to the curve law. a ; Obtain the road sample to be evaluated, test its macro texture parameters and micro texture parameters, and substitute them into the correlation model to obtain the test friction factor μ ce ; According to the friction factor μ ce Compared with the prior art, the present invention has the advantages of fast measurement speed, complete information, intuitive image, and accurate reflection of surface three-dimensional morphology information.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of anti-skid performance of highway asphalt pavement, and in particular to an anti-skid performance evaluation method for a wearing layer of a steel slag asphalt mixture pavement. Background Art

[0002] Good pavement anti-skid performance is an important guarantee for driving safety. At present, steel slag asphalt pavement has not been systematically and large-scaled. Although there are many physical projects, the overall scale is small and most of them are test sections of 1 km. The survey found that although most of the research at home and abroad is about improving the material properties of steel slag asphalt mixtures, the road performance of pavement in terms of anti-deformation, anti-rutting, and anti-cracking has been sufficiently guaranteed, but the research on the durability of steel slag pavement anti-skid function is scarce, and the effective evaluation of anti-skid performance has not been studied in depth.

[0003] The friction mechanism of asphalt pavement is mainly related to the macro-texture and micro-texture of the road surface. At present, the commonly used evaluation and characterization indicators in the "Highway Engineering Quality Inspection and Evaluation Standard" (JTG F80 / 1-2017, Volume 1, Civil Engineering) are mainly structural depth MTD, swing value BPN, lateral force coefficient SFC and longitudinal force coefficient BFC. Among them, MTD and BPN are simple to operate and have low equipment cost. They are fixed-point tests and require temporary traffic closure, which affects vehicle traffic. When operating, it is necessary to compete with the existing traffic on the road surface, resulting in poor repeatability, low test efficiency, great influence by human factors, and failure to reflect the actual anti-skid performance of the road surface. Although the lateral force coefficient SFC and the longitudinal force coefficient BFC are continuous tests, the biggest disadvantage of the test equipment is that they cannot be measured indoors, and the test equipment is expensive, with poor universality and economy. In addition, these commonly used detection methods and indicators cannot well reflect the morphological characteristics of surface objects, so that the rich morphological information of the road surface cannot be effectively expressed. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a method for evaluating the anti-skid performance of the wearing layer of a steel slag asphalt mixture pavement, which effectively solves the problem of poor universality of traditional anti-skid evaluation methods.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A method for evaluating the anti-skid performance of a wearing layer of a steel slag asphalt mixture pavement, comprising the following steps:

[0007] S1. Obtain a modeling sample of steel slag asphalt mixture pavement, and use an indoor accelerated loading abrasion tester to abrade it at different times under a set load to obtain modeling samples with different degrees of abrasion; at the same time, record the friction factor μ, macro texture parameters and micro texture parameters of the modeling sample at each set number of times, and the friction factor of the modeling sample before abrasion is μ0;

[0008] S2. Based on the recorded friction coefficient μ, macro texture parameters and micro texture parameters, a correlation model between the friction coefficient and the macro texture and micro texture is established, and a friction coefficient decay law prediction model is established that associates the friction coefficient with the number of load actions;

[0009] S3. Draw the relevant curve of the friction coefficient decay law prediction model and select the critical value μ according to the curve law. a ;

[0010] S4. Obtain the sample of steel slag asphalt mixture pavement to be evaluated, test its macro texture parameters and micro texture parameters, and substitute them into the correlation model to obtain the test friction factor μ ce ;

[0011] S5, according to the friction factor μ ce Make a judgment: When μ ce ≥μ0, the sample to be evaluated has excellent anti-skid condition; when μ0>μ ce ≥μ a When μ ce <μ a When , the sample to be evaluated has poor pavement skid resistance.

[0012] Furthermore, the macro texture parameters include the root mean square deviation of the cross-sectional profile R q , the micro texture parameters include the micro arithmetic mean height S a , peak density S pd and the average curvature of the crest S pc .

[0013] Furthermore, the expression of the correlation model is:

[0014] μ=k1R q +k2S a +k3S pd +k4S pc +C

[0015] Where k1, k2, k3, and k4 are coefficients obtained from regression analysis of test data, and C is a constant term.

[0016] Furthermore, the expression of the friction coefficient decay law prediction model is:

[0017] μ=a ln(N)+b

[0018] Where μ is the friction coefficient, a is the coefficient obtained by regression analysis of test data, b is the constant term, and N is the cumulative number of actions.

[0019] Furthermore, the modeling sample is a sample made in a laboratory and has the same gradation and aggregate as the road surface.

[0020] Furthermore, the number of modeling samples is at least three.

[0021] Furthermore, the correlation model and the friction coefficient decay law prediction model are both modeled using multivariate linear regression analysis.

[0022] Furthermore, modeling samples with different gradations and aggregates are selected to repeat steps S1 to S3, so as to improve the regression accuracy of the correlation model between the friction coefficient and the macro texture and micro texture, and the friction coefficient decay law prediction model.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The present invention establishes a correlation model between the friction factor and the macro-texture and micro-texture of the steel slag asphalt mixture pavement, and a prediction model for the decay law of the friction coefficient, so as to formulate a reference standard for the evaluation of the anti-skid performance status. This can effectively overcome the problems of various traditional evaluation methods such as ignoring the road surface morphology characteristics, poor repeatability, low test efficiency, and being greatly affected by human environmental factors. It has good universality and can accurately and objectively reflect the true anti-skid status of the road surface.

[0025] 2. The present invention can quickly evaluate the anti-skid performance of steel slag asphalt mixture pavement in engineering applications and provide targeted anti-skid performance repair or treatment measures, which is highly practical.

[0026] 3. The present invention can use modeling samples with different gradations and aggregates when establishing the model, thereby improving the accuracy and applicability of the model and improving the evaluation accuracy. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a schematic diagram of the process of the present invention.

[0028] Figure 2 These are the three preliminary grading curves of SMA-13.

[0029] Figure 3 R is the root mean square deviation of the cross-sectional profile q Schematic diagram.

[0030] Figure 4 is the arithmetic mean height S a Schematic diagram.

[0031] Figure 5 is the peak density S pd Schematic diagram.

[0032] Figure 6 Schematic diagram of friction coefficient decay curve. DETAILED DESCRIPTION

[0033] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0034] like Figure 1 As shown, this embodiment provides a method for evaluating the anti-skid performance of a wearing layer of a steel slag asphalt mixture pavement, which specifically includes the following steps:

[0035] Step S1, obtaining a modeling sample of a steel slag asphalt mixture pavement, and using an indoor accelerated loading abrasion tester to perform abrasion at different times under a set load to obtain modeling samples with different degrees of abrasion; at the same time, recording the friction coefficient μ, macro texture parameters and micro texture parameters of the modeling sample at each set number of times, and the friction coefficient of the modeling sample before abrasion is μ0.

[0036] Step S2: Based on the recorded friction coefficient μ, macro texture parameters and micro texture parameters, a correlation model between the friction coefficient and the macro texture and micro texture is established, and a friction coefficient decay law prediction model that associates the friction coefficient with the number of load actions is established.

[0037] Step S3: Draw the relevant curve of the friction coefficient decay law prediction model, and select the critical value μ according to the curve law and industry specification requirements. a .

[0038] Step S4: Obtain a sample of steel slag asphalt mixture pavement to be evaluated, test its macro texture parameters and micro texture parameters, and substitute them into the correlation model to obtain the test friction coefficient μ ce .

[0039] Step S5: According to the friction factor μ ce Make a judgment. ce ≥μ0, the sample to be evaluated has excellent pavement anti-skid condition; when μ0>μ ce ≥μ a When μ ce <μ a When , the sample to be evaluated has poor pavement skid resistance.

[0040] The specific development of each step is as follows:

[0041] 1. In step S1, a modeling sample of a steel slag asphalt mixture pavement is first obtained. The modeling sample is a sample made in a laboratory with the same gradation and aggregate as the pavement. The specific process is as follows:

[0042] ① Select steel slag that has been aged for more than 3 years. The original slag is processed by jaw crusher, hammer crusher and sand making machine. The specifications of steel slag are 10-15mm and 5-10mm. The various indicators of it as aggregate are tested. It must meet the technical requirements for coarse aggregate of pavement wearing layer in "Technical Specifications for Highway Asphalt Pavement Construction" (JTGF40-2004), as shown in Table 1.

[0043] Table 1 Test results of steel slag aggregate properties

[0044] Test indicators Steel slag Technical requirements Test procedures Apparent relative density 3.52 ≥2.6 T0304-2005 Crushing value / % 16.3 ≤26 T0316-2005 Los Angeles wear loss / % 12.1 <28 T0317-2005 Water absorption / % 1.5 ≤2 T0307-2005 Firmness / % 1.6 <12 T0314-2000 Content below 0.075mm / % 0.70 ≤1.0 T0310-2005 Polishing value 45 ≥36 T0321-2005 Adhesion grade 5 ≥4 T0326-2005

[0045] ② Set SMA-13 ​​steel slag asphalt mixture, use steel slag to replace the same volume of crushed stone, and adjust the reasonable gradation, such as Figure 2 After comparing various technical indicators, gradation 3 was selected, SBS modified asphalt was selected, and the oil-stone ratio was 6.2%. Steel slag asphalt mixture specimens were prepared according to the specifications. The specimens were in the form of rutting plates with a specification of 30cm×30cm×5cm, and three parallel specimens were prepared.

[0046] Second, in step S1, the friction coefficient μ, macro texture parameters and micro texture parameters of the modeling sample under each set number of action are recorded by laboratory indoor wear test, three-dimensional morphology feature acquisition test and dynamic friction coefficient experiment. The specific process is as follows:

[0047] ① Before the wear test, the macro texture, micro texture and dynamic friction coefficient of the surface of three parallel test pieces were measured. The test process is:

[0048] 1) Texture collection: Before the abrasion test, a laser scanner is used to test the macro texture and micro texture of the steel slag asphalt mixture surface. The wavelength range of the measurement is 0.5mm~20mm for macro texture and 0.001mm~0.5mm for micro texture. The macro texture is the root mean square deviation of the cross-sectional profile R q , the micro texture selects the micro arithmetic mean height S a , peak density S pd and the average curvature of the crest S pc :

[0049] like Figure 3 Shown is the root mean square deviation R of the cross-sectional profile q Schematic diagram; cross-sectional profile root mean square deviation R q Refers to the root mean square value of the surface profile deviation within the sampling range. qIt is equivalent to the concept of standard deviation in mathematical statistics, reflecting the standard deviation of the amplitude distribution of random surface topography. q It has a weighted effect on the contour amplitude. The larger the contour amplitude, the greater the weight of its influence on the result. This parameter is easy to statistically process, and since it is not significantly affected by scratches, contamination, and measurement noise, stable results can be obtained.

[0050] like Figure 4 Shown is the arithmetic mean height S a Schematic diagram, which can reflect the degree of deviation of the collected data from the reference surface in the height direction, that is, the average value of the average plane height difference, which represents the arithmetic mean of the absolute coordinates Z(x,y) in a defined area, S a The size represents the roughness of the surface of the object. The larger the value, the rougher the surface.

[0051] like Figure 5 Shown is the peak density S pd Schematic diagram, peak density S pd It reflects the density of contact points with the object in the surface topography. pd When it is larger, it means that the surface has more contact points when it comes into contact with other objects.

[0052] The average curvature of the crest S pc , reflects the arithmetic mean of the principal curvature of the crest on the surface. This parameter is derived from the arithmetic mean of the curvature within the defined area and is used to analyze the contact state between two objects. pc When the value is small, it indicates that the contact point is round. pc A large value indicates a sharper contact point.

[0053] The dynamic friction coefficient tester was used to obtain the pavement friction coefficient μ0 before wear. The principle of the dynamic friction coefficient test is similar to the principle of the friction coefficient measurement method tested by the dynamic rotary friction coefficient tester in JTG 3450-2019 Highway Roadbed and Pavement Field Test Procedure T0968. The dynamic friction force and dynamic friction coefficient are calculated by measuring the torque during the rotation process. The initial test values ​​of each index before wear are shown in Table 2.

[0054] Table 2 Texture and initial value of friction factor before test

[0055]

[0056] ② Under the specified load conditions, the specimen was worn with an accelerated loading abrasion tester. After each wear to a certain number of times, the three-dimensional laser surface texture acquisition was used to test the root mean square deviation R of the cross-sectional profile at different wear degrees. q , microscopic arithmetic mean height S a , peak density Spd , the average curvature of the wave crest S pc , and the friction factor u value, and record the data, as shown in Table 3. The wear number sequence is set to 10,000 times, 20,000 times, 30,000 times, 50,000 times, 100,000 times, 200,000 times, 500,000 times, and 1 million times.

[0057] Table 3 Texture and friction factor values ​​under different wheel load abrasion times

[0058]

[0059] 3. In step S2, a correlation model between the friction coefficient u of the steel slag asphalt mixture wearing layer and the macro-texture and micro-texture indicators is established through multivariate linear regression analysis:

[0060] μ=k1R q +k2S a +k3S pd +k4S pc +C

[0061] The coefficients k1, k2, k3, k4 and the constant term C are obtained as k1 = 0.09266, k2 = 0.0045, k3 = -0.00019, k4 = 7.29954 × 10 -6 , C = 0.33821, and then the friction coefficient calculation formula based on road surface texture is obtained:

[0062] μ=0.09266R q +0.0045S a -0.00019S pd +7.29954×10 -6 S pc +0.33821

[0063] Among them, R q , S a , S pd , S pc All of them are test values ​​measured by 3D laser scanning method.

[0064] The prediction model between the friction coefficient and the number of load actions (N) can also be obtained through the test data in Table 3:

[0065] μ=-0.01814ln(N)+0.58329

[0066] Therefore, the decay characteristic curve of friction coefficient with the number of load actions can be further drawn.

[0067] 4. Figure 6As shown in the figure, the friction coefficient critical line is established by comprehensively considering the characteristics of the decay curve and the requirements of industry specifications. In this case, it is set to 0.46. According to the curve change law, it is divided into three different stages, namely: stage I represents the early stage of load action, and the friction coefficient has a short rise within 10,000 to 20,000 times; stage II represents the process of gradual decrease of the friction coefficient after the cumulative number of load wear actions is within 10 million times. This stage is relatively long, the friction coefficient is generally above the critical line, and the pavement anti-skid performance is in a qualified and excellent state; stage III represents that with the continuous increase in the number of load actions, exceeding 10 million times, the friction coefficient drops below the critical line and maintains a relatively stable state. The pavement anti-skid performance at this stage is poor, and timely engineering treatment measures need to be taken. The evaluation standards for the pavement anti-skid performance status corresponding to each stage are shown in Table 4.

[0068] Table 4. Reference table for evaluation standards of pavement anti-skid performance status

[0069]

[0070]

[0071] Therefore, when evaluating the anti-slip state, first collect the sample to be evaluated and calculate the friction coefficient value, then Figure 6 By tracing the cumulative number of axle loads experienced by the road surface, it is possible to further determine the anti-skid performance status and service life stage of the steel slag asphalt pavement.

[0072] V. Inspection and evaluation in physical engineering

[0073] The established anti-skid performance evaluation formula is applied to actual projects to obtain road surfaces in different states or at different operating times, collect road surface morphology characteristics and data, and calculate the friction factor u based on the established evaluation formula. The characteristics of the friction factor decay of the wearing layer of the steel slag asphalt mixture pavement are then analyzed to quickly evaluate the actual state of the anti-skid performance, providing a basis for taking positive and effective engineering measures.

[0074] In summary, this method uses three-dimensional laser scanning technology to collect macro and micro texture data of the road surface, obtains the correlation with the friction coefficient, establishes a friction coefficient calculation formula based on morphological texture variables and a friction coefficient decay model based on the cumulative number of loading times, and formulates a reference standard for anti-skid performance status evaluation. It has the advantages of fast measurement speed, complete information, intuitive and vivid, and accurate reflection of the three-dimensional surface morphology information.

[0075] The anti-skid evaluation method based on texture indicators established in this way is expected to overcome the problems of traditional evaluation methods such as ignoring road surface morphology characteristics, poor repeatability, low test efficiency, being greatly affected by human environmental factors, poor universality, and being unable to objectively reflect the true anti-skid state of the road surface.

[0076] The present invention establishes a friction coefficient calculation formula based on morphological texture variables and a friction coefficient decay model based on the cumulative number of loading times, formulates a reference standard for anti-skid performance status evaluation, and then realizes a rapid evaluation of the anti-skid performance of steel slag asphalt pavement through engineering applications, and provides targeted anti-skid performance repair or treatment measures.

[0077] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A method for evaluating the anti-skid performance of the wearing layer of a steel slag asphalt mixture pavement, characterized in that: include: S1. Obtain a modeling sample of steel slag asphalt mixture pavement, and use an indoor accelerated loading abrasion tester to abrade it at different times under a set load to obtain modeling samples with different degrees of abrasion; at the same time, record the friction factor μ, macro texture parameters and micro texture parameters of the modeling sample at each set number of times, and the friction factor of the modeling sample before abrasion is μ0; S2. Based on the recorded friction coefficient μ, macro texture parameters and micro texture parameters, a correlation model between the friction coefficient and the macro texture and micro texture is established, and a friction coefficient decay law prediction model is established that associates the friction coefficient with the number of load actions; S3. Draw the relevant curve of the friction coefficient decay law prediction model and select the critical value μ according to the curve law. a ; S4. Obtain the sample of steel slag asphalt mixture pavement to be evaluated, test its macro texture parameters and micro texture parameters, and substitute them into the correlation model to obtain the test friction factor μ ce ; S5, according to the friction factor μ ce Make a judgment: When μ ce ≥μ0, the sample to be evaluated has excellent anti-skid condition; when μ0>μ ce ≥μ a When μ ce <μ a When , the sample to be evaluated has a poor pavement anti-skid condition; The macro texture parameters include the root mean square deviation of the cross-sectional profile R q , the micro texture parameters include the micro arithmetic mean height S a , peak density S pd and the average curvature of the crest S pc , where the root mean square deviation of the cross-sectional profile is R q , microscopic arithmetic mean height S a , peak density S pd and the average curvature of the crest S pc All obtained by laser scanning; The expression of the correlation model is: μ=k1R q +k2S a +k3S pd +k4S pc +C Where k1, k2, k3, and k4 are coefficients obtained from regression analysis of test data, and C is a constant term.

2. The method for evaluating the anti-skid performance of the wearing layer of a steel slag asphalt mixture pavement according to claim 1, characterized in that: The expression of the friction coefficient decay law prediction model is: μ=a ln(N)+b Where μ is the friction coefficient, a is the coefficient obtained by regression analysis of test data, b is the constant term, and N is the cumulative number of actions.

3. The method for evaluating the anti-skid performance of the wearing layer of a steel slag asphalt mixture pavement according to claim 1, characterized in that: The modeling samples are samples made in a laboratory and have the same gradation and aggregate as the road surface.

4. The method for evaluating the anti-skid performance of the wearing layer of a steel slag asphalt mixture pavement according to claim 1, characterized in that: The number of modeling samples is at least three.

5. The method for evaluating the anti-skid performance of the wearing layer of a steel slag asphalt mixture pavement according to claim 1, characterized in that: The correlation model and the friction coefficient decay law prediction model are both modeled using multivariate linear regression analysis.

6. The method for evaluating the anti-skid performance of the wearing layer of a steel slag asphalt mixture pavement according to claim 5, characterized in that: Select modeling samples with different gradations and aggregates and repeat steps S1 to S3 to improve the correlation model between the friction coefficient and the macro texture and micro texture, as well as the regression accuracy of the friction coefficient decay law prediction model.