A method for regenerating positive electrode material of ternary lithium battery and positive electrode material of ternary lithium battery

By obtaining the precursor of the ternary lithium battery cathode material from the malic acid leaching solution of the spent lithium battery cathode material through the oxidation precipitation method, and calcining it with the lithium source, the problem of high recycling cost and complex operation is solved, and an efficient and low-cost ternary lithium battery is achieved. The cathode material of the lithium-ion battery is regenerated and has excellent charge and discharge performance.

CN115084697BActive Publication Date: 2024-10-22KUNMING UNIV OF SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210504593.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-10
Publication Date
2024-10-22
Estimated Expiration
2042-05-10

AI Technical Summary

Technical Problem

In the existing technology, the recycling cost of lithium battery cathode materials is high and can easily lead to organic pollution. Moreover, the coprecipitation method is complex and time-consuming, resulting in low product purity.

Method used

A nickel source, a cobalt source, and a manganese source are added to the malic acid leaching solution of the spent lithium battery cathode material, and the ternary lithium battery cathode material precursor is obtained through the oxidation precipitation method, and is mixed with the lithium source for calcination treatment to obtain a regenerated ternary lithium battery. Cathode material. This method performs oxidation precipitation at a pH value of 6 to 11, an oxygen pressure of 0.2 to 1.2 MPa, a temperature of 60 to 140°C, and a time of 1 to 6 hours. The calcination temperature is 700 to 1000°C and the time is 8 to 14 hours.

Benefits of technology

It achieves short precipitation time, simple operation, low cost, high precipitation rate, and excellent charge and discharge performance of the regenerated cathode material, avoiding the energy consumption and pollution problems of traditional recycling methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115084697B_ABST
    Figure CN115084697B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for regenerating positive electrode materials of ternary lithium batteries and positive electrode materials of ternary lithium batteries, wherein the method comprises the following steps: providing a malic acid leachate of waste lithium battery positive electrode materials; adding a nickel source, a cobalt source, and a manganese source to the malic acid leachate of the waste lithium battery positive electrode materials to obtain a mixed nickel-cobalt-manganese-rich leachate; performing oxidation precipitation on the mixed nickel-cobalt-manganese-rich leachate to obtain a precursor of positive electrode materials of ternary lithium batteries; mixing the precursor of positive electrode materials of ternary lithium batteries with a lithium source, and performing calcination treatment to obtain the positive electrode materials of ternary lithium batteries. The present invention aims at the deficiencies of the existing coprecipitation method and the extraction and separation method, and coprecipitates nickel, cobalt, and manganese by oxidation precipitation, which not only has a short precipitation time, simple operation, high precipitation rate, and low cost, but also has excellent charge and discharge performance of the precursor after lithium supplementation and regeneration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of recycling and reuse of waste lithium batteries, and in particular to a method for regenerating anode materials of ternary lithium batteries and anode materials of ternary lithium batteries. Background Art

[0002] Lithium-ion battery positive electrode materials have the advantages of good cycle stability, high energy density, and stable electrochemical platform, which makes them widely used in new energy electric vehicles and large and small energy storage fields. The extensive use of lithium-ion batteries will inevitably produce a large number of waste lithium-ion batteries. Although they are solid waste pollutants, they have high utilization value. With the increasing use of lithium-ion batteries, the demand for metals such as nickel, cobalt, manganese, and lithium required in lithium-ion batteries has also increased dramatically, while my country has serious resource shortages of cobalt, nickel, and lithium. Therefore, the recycling of waste lithium-ion battery positive electrode materials is a way to solve the country's resource shortage problem and will also play a certain role in environmental protection.

[0003] At present, acid leaching is mainly used for the recovery of waste lithium battery positive electrode materials, and extraction and step-by-step precipitation are often used for the separation of metal ions in the leachate. Organic reagents will be introduced during the extraction process, which not only increases the recovery cost, but also causes organic pollution. During the step-by-step precipitation process, since each valuable metal element must be extracted and separated one by one, this will increase the amount of chemical reagents used, resulting in an increase in the recovery cost, and in the step-by-step precipitation process, the co-precipitation of nickel, cobalt, and manganese will also result in a low purity of the product. Therefore, using the leachate of waste lithium battery positive electrode materials directly as a raw material for regenerating ternary positive electrode materials can not only avoid the problems of energy consumption and pollution caused by traditional recycling methods, but also achieve the closed-loop utilization of lithium battery positive electrode materials in the industry and reduce the preparation cost of positive electrode materials.

[0004] When synthesizing ternary positive electrode materials from the leachate of waste lithium battery positive electrode materials, the traditional sodium carbonate and sodium hydroxide coprecipitation method is often used. However, these two methods need to maintain a certain pH value during the coprecipitation process, and the coprecipitation time is usually more than 12 hours. In the patent with publication number CN111252814A, 3 mol / L sodium carbonate solution, 0.5 mol / L ammonium bicarbonate solution and 0.2 mol / L ammonia water are added to the sulfuric acid leachate at a feeding rate of 20 mL / h, the solution pH is maintained at 8, and then the temperature is raised to 65 ° C, stirred at 300 rpm for 24 hours, and solid-liquid separation is performed to obtain a nickel-cobalt-manganese carbonate coprecipitation precursor. Therefore, the traditional coprecipitation method has the disadvantages of complex operation and long coprecipitation time when coprecipitating nickel, cobalt and manganese.

[0005] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0006] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a method for regenerating a ternary lithium battery positive electrode material and a ternary lithium battery positive electrode material, aiming to solve the problems in the prior art of recycling lithium battery positive electrode materials that the extraction separation method has high recovery cost and easily causes organic pollution, and the co-precipitation method has complex operation and long co-precipitation time.

[0007] The technical solution adopted by the present invention to solve the above technical problems is as follows:

[0008] A method for regenerating positive electrode materials of a ternary lithium battery, comprising the steps of:

[0009] Provide malic acid leaching solution of waste lithium battery positive electrode materials;

[0010] Adding a nickel source, a cobalt source and a manganese source to the malic acid leachate of the waste lithium battery positive electrode material to obtain a mixed nickel-cobalt-manganese-rich leachate;

[0011] The mixed nickel-cobalt-manganese-rich leaching solution is subjected to oxidation precipitation to obtain a precursor of a positive electrode material for a ternary lithium battery;

[0012] The precursor of the positive electrode material of the ternary lithium battery is mixed with a lithium source and calcined to obtain the positive electrode material of the ternary lithium battery.

[0013] The method for regenerating positive electrode materials of a ternary lithium battery, wherein the nickel source is nickel carbonate or nickel sulfate, the cobalt source is cobalt carbonate or cobalt sulfate, and the manganese source is manganese carbonate or manganese sulfate.

[0014] The method for regenerating positive electrode materials for ternary lithium batteries, wherein the step of oxidatively precipitating the mixed nickel-cobalt-manganese-rich leachate specifically comprises the steps of: adjusting the pH of the mixed nickel-cobalt-manganese-rich leachate, introducing pressurized oxygen, raising the temperature, and performing oxidative precipitation.

[0015] The method for regenerating positive electrode materials for ternary lithium batteries, wherein the conditions for the oxidation precipitation are: pH value of 6 to 11, oxygen pressure of 0.2 to 1.2 MPa, temperature of 60 to 140° C., and time of 1 to 6 hours.

[0016] The method for regenerating positive electrode materials of a ternary lithium battery, wherein the lithium source is lithium carbonate.

[0017] The method for regenerating the positive electrode material of a ternary lithium battery, wherein the steps of mixing the positive electrode material precursor of the ternary lithium battery with a lithium source and calcining the mixture to obtain the positive electrode material of the ternary lithium battery are specifically as follows:

[0018] The precursor of the positive electrode material of the ternary lithium battery is mixed with a lithium source, ground, calcined, crushed and then sieved to obtain the positive electrode material of the ternary lithium battery.

[0019] The method for regenerating the positive electrode material of a ternary lithium battery, wherein the lithium source is mixed with the positive electrode material precursor of the ternary lithium battery in a molar ratio of Li / M=1.02-1.10:1, wherein M=Ni+Co+Mn.

[0020] The method for regenerating positive electrode materials of ternary lithium batteries, wherein the calcination temperature is 700-1000° C. and the calcination time is 8-14 hours.

[0021] A positive electrode material for a ternary lithium battery, wherein the positive electrode material is prepared by the method described in the above scheme of the present invention.

[0022] Beneficial effect: The present invention discloses a method for regenerating positive electrode materials of a ternary lithium battery and a positive electrode material of a ternary lithium battery, wherein the method comprises the steps of: providing a malic acid leachate of a waste lithium battery positive electrode material; adding a nickel source, a cobalt source and a manganese source to the malic acid leachate of the waste lithium battery positive electrode material to obtain a mixed nickel-cobalt-manganese-rich leachate; oxidizing and precipitating the mixed nickel-cobalt-manganese-rich leachate to obtain a precursor of a positive electrode material of a ternary lithium battery; mixing the precursor of the positive electrode material of a ternary lithium battery with a lithium source and treating it by a high-temperature solid phase method to obtain the positive electrode material of a ternary lithium battery. The invention aims at the disadvantages of long separation process, complicated operation, high recovery cost and low product purity when separating various valuable metal elements by the existing step-by-step precipitation method and solvent extraction method, and the problem that sodium hydroxide and sodium carbonate co-precipitation method are often used when precipitating nickel, cobalt and manganese by the co-precipitation method, and these methods usually take more than 12 hours and have a long precipitation time. The invention proposes a new method for regenerating ternary positive electrode materials from malic acid leachate of waste lithium battery positive electrode materials, co-precipitating nickel, cobalt and manganese by oxidation precipitation, and the precipitation time of the co-precipitation does not exceed 6 hours. Not only is the precipitation time short, the operation is simple, the precipitation rate is high and the cost is low, but the regenerated positive electrode material has excellent charge and discharge performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 A flow chart of a preferred embodiment of a method for regenerating positive electrode materials of a ternary lithium battery provided by the present invention.

[0024] Figure 2 This is a curve showing the effect of temperature on the precipitation rate of Ni, Co and Mn during oxygen oxidation precipitation in an embodiment of the present invention.

[0025] Figure 3 The oxygen oxidation precipitation of Ni in the embodiment of the present invention 2+ 、Co 2+ , Mn 2+ When E and a M2+ Relationship diagram (120℃, pH=10, P O2 =0.8Mpa).

[0026] Figure 4 A process flow chart of a specific implementation method of the ternary lithium battery positive electrode material regeneration method provided by the present invention.

[0027] Figure 5 Example 1-LiNi of the present invention 0.5 Co 0.2 Mn 0.3 O 2 (523 type) and Example 3-LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 XRD pattern of (333 type) regenerated positive electrode material.

[0028] Figure 6 Regeneration of LiNi in Example 1 of the present invention 0.5 Co 0.2 Mn 0.3 O 2 First charge and discharge curve of (523 type) positive electrode material.

[0029] Figure 7 Regeneration of LiNi in Example 2 of the present invention 0.6 Co 0.2 Mn 0.2 O 2 (Type 622) XRD pattern of positive electrode material.

[0030] Figure 8 Regeneration of LiNi in Example 2 of the present invention 0.6 Co 0.2 Mn 0.2 O 2 (Type 622) Rate performance of positive electrode materials.

[0031] Fig. 9 Regeneration of LiNi in Example 3 of the present invention 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 (Type 333) Cyclic performance of positive electrode materials. DETAILED DESCRIPTION

[0032] The present invention provides a ternary lithium battery positive electrode material regeneration method and a ternary lithium battery positive electrode material. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0033] With the development of electric vehicles, the energy density requirements for lithium-ion batteries are also increasing. In order to ensure that the battery has a longer cycle life, ternary cathode material lithium-ion batteries are also constantly developing in the direction of high nickel. In the actual production process of high nickel cathode material lithium-ion batteries, many problems have arisen. The higher the nickel content of the ternary material, the easier it is to react with H in the air. 2 O and CO 2 Reaction, forming LiOH and Li on the surface of the material 2 CO 3 , thereby increasing its alkalinity. Polyvinylidene fluoride (PVDF) is the most commonly used binder in China. Its alkali resistance is poor. When the molecular chain is affected by alkaline substances, hydrogen fluoride (HF) elimination reaction will occur to generate double bonds, causing cross-linking reactions between PVDF molecular chains, resulting in gelation of the slurry, which ultimately affects the coating process and reduces the cycle efficiency of lithium-ion batteries.

[0034] Based on this, the present invention provides a method for regenerating positive electrode materials of ternary lithium batteries, see Figure 1 , which comprises the steps of:

[0035] S10. Provide malic acid leaching solution of waste lithium battery positive electrode materials;

[0036] S20, adding a nickel source, a cobalt source, and a manganese source to the malic acid leachate of the waste lithium battery positive electrode material to obtain a mixed nickel-cobalt-manganese-rich leachate;

[0037] S30, performing oxidation precipitation on the mixed nickel-cobalt-manganese-rich leaching solution to obtain a precursor of a positive electrode material for a ternary lithium battery;

[0038] S40, mixing the precursor of the positive electrode material of the ternary lithium battery with a lithium source, and performing calcination treatment to obtain the positive electrode material of the ternary lithium battery.

[0039] Specifically, the present invention aims at the disadvantages of long separation process, complicated operation, high recovery cost and low product purity when separating each valuable metal element by the existing step-by-step precipitation method and solvent extraction method, and the problem that the sodium hydroxide and sodium carbonate co-precipitation method is often used when precipitating nickel, cobalt and manganese by the co-precipitation method, and these methods usually take more than 12 hours and have a long precipitation time. A new method for regenerating ternary positive electrode materials from malic acid leachate of waste lithium battery positive electrode materials is proposed. Nickel, cobalt and manganese are co-precipitated by oxidation precipitation. The precipitation time of the co-precipitation does not exceed 6 hours. Not only is the precipitation time short, the operation is simple, the precipitation rate is high and the cost is low, but the regenerated positive electrode material has excellent charge and discharge performance.

[0040] In some embodiments, the nickel source is nickel carbonate or nickel sulfate, the cobalt source is cobalt carbonate or cobalt sulfate, and the manganese source is manganese carbonate or manganese sulfate.

[0041] Specifically, the present invention regenerates a ternary lithium battery positive electrode material from a malic acid leachate of a waste lithium battery high manganese positive electrode material. Therefore, in the step S20, a nickel source, a cobalt source, and a manganese source are added to the malic acid leachate of the waste lithium battery positive electrode material to achieve the required ratio of the ternary lithium battery positive electrode material. Specifically, the adjusted molar ratio of nickel, cobalt, and manganese ions is 1:1:1, 5:2:3, 6:2:2, or 8:1:1, but is not limited thereto.

[0042] In some embodiments, malic acid leaching of the positive electrode material of waste NCM523, NCM622 or NCM111 lithium ion batteries can obtain a leachate with a corresponding molar ratio, which can be directly oxidized and precipitated to obtain a precursor material with a corresponding molar ratio. Therefore, the ion concentration can be adjusted accordingly according to the molar ratio of each element of the positive electrode material to be prepared.

[0043] In some preferred embodiments, the nickel source is nickel carbonate, the cobalt source is cobalt carbonate, and the manganese source is manganese carbonate.

[0044] In this embodiment, the oxidative precipitation is oxygen oxidative precipitation, and the step of performing oxidative precipitation on the mixed nickel-cobalt-manganese-rich leachate specifically includes the steps of adjusting the pH of the mixed nickel-cobalt-manganese-rich leachate, introducing oxygen, pressurizing it, and then heating it to perform oxidative precipitation.

[0045] Specifically, since it is impossible to use oxygen oxidation precipitation method to deposit Ni 2+ 、Co 2+ , Mn 2+ Oxidized to NiOOH, CoOOH, MnOOH, so in this embodiment, Ni 2+ 、Co 2+ , Mn 2+ The oxidation precipitation is carried out. The specific precipitation reaction of each metal ion present in the malic acid leachate of the high manganese positive electrode material of the waste lithium battery during the oxygen oxidation precipitation is as follows:

[0046] 4Mn 2+ +O 2 +6H 2 O→4MnOOH+8H +

[0047] 4Co 2+ +O 2 +6H 2 O→4CoOOH+8H +

[0048] 4Ni 2+ +O 2 +6H 2 O→4NiOOH+8H +

[0049] Therefore, in this embodiment, the conditions of the oxygen oxidation precipitation are: pH value is 6-11, oxygen pressure is 0.2-1.2 MPa, temperature is 60-140° C., and time is 1-6 h.

[0050] In some preferred embodiments, the pH value of the oxygen oxidation precipitation is 7-10, the oxygen pressure is 0.8-1.0 MPa, the temperature is 100-120° C., and the time is 3-4 hours.

[0051] In order to determine the optimal oxygen pressure, oxygen oxidation precipitation was carried out at 60, 80, 100, and 120 °C under the conditions of 400 mL malic acid leaching solution of high manganese cathode material of waste lithium battery, precipitation time of 3 h, pH = 10, and oxygen pressure of 0.8 MPa, respectively, to study the effect of temperature on the precipitation rate of Ni, Co, and Mn. The experimental results are shown in Figure 2 As shown by Figure 2 It can be seen that when the temperature is 60-120°C, the precipitation rate of manganese increases from 96.4% to 99.9%, and the precipitation rate of manganese remains almost unchanged, which shows that temperature has little effect on the precipitation rate of manganese. The precipitation rate of cobalt increases from 31.6% to 96.8%, and the precipitation rate of nickel increases from 0.7% to 94.4%, which shows that the precipitation temperature has a great influence on the precipitation rates of nickel and cobalt. Therefore, the optimal precipitation temperature is selected as 120°C. At this time, the precipitation rates of nickel, cobalt, and manganese are 94.4%, 96.8%, and 99.9%, respectively. Since the leaching rate of each valuable metal is significantly improved at 120°C, the oxygen oxidation precipitation of Ni under the conditions of pH = 10, T = 120°C, and oxygen pressure of 0.8MPa is calculated and plotted. 2+ 、Co 2+ , Mn 2+ The relationship between the potential and ion concentration at Figure 3 As shown by Figure 3 It can be seen that at pH = 10, T = 120 ° C, P O2 =0.8MPa, Ni 2+ 、Co 2+ , Mn 2+ All of them can be oxidized and precipitated by oxygen. Finally, it was determined that the optimal temperature for oxygen oxidation precipitation was 120℃ and the optimal oxygen pressure was 0.8MPa.

[0052] The above experiments can also prove that under pressurized and high-temperature conditions, the oxygen oxidation precipitation method has a higher precipitation rate for nickel, cobalt, and manganese ions. Therefore, this embodiment preferably adopts the method of oxygen oxidation precipitation to precipitate the nickel, cobalt, and manganese ions in the malic acid leachate of the high-manganese positive electrode material of the waste lithium battery, so that the nickel, cobalt, and manganese ions can be precipitated as much as possible, thereby maximizing the recovery of the high-manganese positive electrode material of the waste lithium battery, and can also ensure that the final regenerated positive electrode material can meet the nickel-cobalt-manganese molar ratio requirement, further reducing the regeneration cost of the positive electrode material of the ternary lithium battery.

[0053] In some embodiments, the lithium source is lithium carbonate.

[0054] In some embodiments, the method for preparing the malic acid leachate of high manganese positive electrode material of waste lithium battery comprises the steps of:

[0055] The positive electrode materials separated from the waste lithium batteries are placed in water, ball-milled or sand-milled, and then sieved;

[0056] The screened positive electrode material is added into a malic acid solution, and a reducing agent is added at the same time, and the waste lithium battery positive electrode material malic acid leaching solution is obtained by filtering.

[0057] Specifically, the waste lithium battery is discharged by using a salt solution to ensure that the open circuit voltage is lower than 1.0V; the discharged lithium battery is disassembled, the outer shell is separated to obtain a battery core, the battery core is immersed in a solvent for cleaning, the cleaned battery core is obtained, and the electrolyte is recovered and processed; the cleaned battery core is separated by a reverse rolling process to obtain a positive electrode sheet, a diaphragm and a negative electrode sheet, the positive electrode sheet is roasted, crushed and sieved, the positive electrode material is separated from the aluminum foil, the separated positive electrode material is placed in water, ball milled or sand milled and then sieved, the sieved positive electrode material is added to a malic acid solution, and a reducing agent is added at the same time, and the malic acid leachate of the waste lithium battery positive electrode material is obtained by filtering, specifically, the reducing agent is hydrogen peroxide, ascorbic acid, glucose, sodium thiosulfate, NaHSO 3 , vitamin C or more in any proportion.

[0058] In some embodiments, the step of mixing the precursor of the positive electrode material of the ternary lithium battery with a lithium source and calcining the mixture to obtain the positive electrode material of the ternary lithium battery is specifically as follows:

[0059] The precursor of the positive electrode material of the ternary lithium battery is mixed with a lithium source in proportion, ground, calcined, crushed and then sieved to obtain the positive electrode material of the ternary lithium battery.

[0060] In this embodiment, the lithium source is mixed with the ternary lithium battery positive electrode material precursor in a molar ratio of Li / M=1.02-1.10:1, wherein M=Ni+Co+Mn, preferably, Li / M=1.05-1.08:1.

[0061] Specifically, the amount of lithium source added is slightly more than the theoretical molar ratio of 1:1 in order to prevent lithium loss during the calcination process, which would result in an insufficient proportion of the final ternary lithium battery positive electrode material and affect its use.

[0062] In this embodiment, the calcination temperature is 700-1000° C., and the calcination time is 8-14 hours. Preferably, the calcination temperature is 800-900° C., and the calcination time is 10-12 hours.

[0063] In some specific embodiments, Figure 4 As shown, it is a process flow chart of a specific implementation method of the regeneration method of the positive electrode material of a ternary lithium battery provided by the present invention, which is specifically: taking malic acid leachate of waste lithium battery positive electrode material, adding nickel carbonate, cobalt carbonate and manganese carbonate to the leachate to make the molar ratio of nickel: cobalt: manganese reach the required ratio, adjusting the pH value of the configured solution, and then sending it into an autoclave and installing a cover, turning on the oxygen switch to adjust the oxygen pressure, and turning on the heating switch to adjust the reaction temperature to react to obtain precipitated residue, adding lithium carbonate to the precipitated residue obtained by oxygen oxidation according to a preset molar ratio and grinding it in an agate mortar, and then putting it into a muffle furnace for calcination to obtain a regenerated positive electrode material for a ternary lithium battery.

[0064] The present invention also provides a ternary lithium battery positive electrode material, which is prepared by the method described in the above scheme of the present invention.

[0065] The present invention also provides an application of the nickel-cobalt-lithium manganese oxide ternary positive electrode material prepared by the above scheme and method of the present invention in the preparation of lithium ion batteries, and synthesizing the regenerated ternary lithium battery positive electrode material into a button battery.

[0066] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments, and are only used to illustrate the present invention but not to limit the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0067] The molar ratio of nickel:cobalt:manganese in the malic acid leachate of the waste lithium battery positive electrode material selected in Examples 1-3 is 1.3:1:14. Therefore, in Examples 1-3, only the nickel source and the cobalt source need to be supplemented. However, in actual use, the ion concentration can be adjusted according to the actual molar ratio of nickel, cobalt and manganese in the malic acid leachate of the waste lithium battery positive electrode material to meet the molar ratio of nickel, cobalt and manganese in the product to be prepared.

[0068] Example 1 Regeneration of LiNi from waste lithium battery positive electrode material malic acid leaching solution0.5 Co 0.2 Mn 0.3 O 2 Cathode Materials

[0069] Take 300mL of malic acid leaching solution of waste lithium battery positive electrode material, add nickel carbonate and cobalt carbonate to the leaching solution, so that the molar ratio of nickel: cobalt: manganese is 5:2:3, adjust the pH value of the prepared solution to 10, then send it into the autoclave and cover it, turn on the oxygen switch to adjust the oxygen pressure to 0.8MPa, and turn on the heating switch to set the reaction temperature to 120℃, and react under this reaction condition for 4h. At this time, the precipitation rates of nickel, cobalt, and manganese are 96.28%, 97.37%, and 99.47%, respectively. Add lithium carbonate to the precipitate obtained by oxygen oxidation at a molar ratio of Li:M=1.05:1 and grind it in an agate mortar for 15min, then put it into a muffle furnace and calcine it at 850℃ for 10h to obtain lithium battery regeneration LiNi 0.5 Co 0.2 Mn 0.3 O 2 Positive electrode material, the lithium battery regeneration LiNi 0.5 Co 0.2 Mn 0.3 O 2 The XRD pattern of the positive electrode material is as follows Figure 5 As shown. Regenerated LiNi 0.5 Co 0.2 Mn 0.3 O 2 The first charge and discharge curve of the positive electrode material is as follows Figure 6 As shown, the first discharge capacity is 184 mAh g -1 .

[0070] Example 2 Regeneration of LiNi from waste lithium battery positive electrode material malic acid leaching solution 0.6 Co 0.2 Mn 0.2 O 2 Cathode Materials

[0071] Take 300ml of malic acid leaching solution of waste lithium battery positive electrode material, add nickel carbonate and cobalt carbonate to the leaching solution to make the molar ratio of nickel: cobalt: manganese 6:2:2, adjust the pH value of the prepared solution to 10.5, then send it into the autoclave and cover it, turn on the oxygen switch to adjust the oxygen pressure to 1MPa, turn on the heating switch to set the reaction temperature to 120℃, and react under this reaction condition for 3h. At this time, the precipitation rates of nickel, cobalt, and manganese are 95.3%, 96.3%, and 99.4%, respectively. Add lithium carbonate to the precipitate obtained by oxygen oxidation at a molar ratio of Li:M=1.06:1 and grind it in an agate mortar for 15min, then put it into a muffle furnace and calcine it at 850℃ for 12h to obtain regenerated LiNi0.6 Co 0.2 Mn 0.2 O 2 Positive electrode material, the regenerated LiNi 0.6 Co 0.2 Mn 0.2 O 2 The XRD pattern of the positive electrode material is as follows Figure 7 As shown. Regenerated LiNi 0.6 Co 0.2 Mn 0.2 O 2 The rate performance of the cathode material is Figure 8 As shown, the discharge capacity retention rate after high rate cycling is 99.2%.

[0072] Example 3 Regeneration of LiNi from waste lithium battery positive electrode material malic acid leaching solution 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 Cathode Materials

[0073] Take 300ml of malic acid leaching solution of waste lithium battery positive electrode material, add nickel carbonate and cobalt carbonate to the leaching solution to make the molar ratio of nickel: cobalt: manganese 1:1:1, adjust the pH value of the prepared solution to 9.5, then send it into the autoclave and cover it, turn on the oxygen switch to adjust the oxygen pressure to 0.8MPa, turn on the heating switch to set the reaction temperature to 100℃, and react for 3h under this reaction condition. At this time, the precipitation rates of nickel, cobalt, and manganese are 93.2%, 95.7%, and 99.1%, respectively. . The precipitate obtained by oxygen oxidation is added with lithium carbonate in a molar ratio of Li:M=1.08:1 and ground in an agate mortar for 15min, and then placed in a muffle furnace and calcined at 800℃ for 12h to obtain the regenerated LiNi for ternary lithium battery 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 Positive electrode material, the ternary lithium battery regeneration LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 The XRD pattern of the positive electrode material is as follows Figure 5 As shown. Regenerated LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 The cycling performance of the positive electrode material is Fig. 9 As shown, the discharge capacity retention rate after 100 charge and discharge cycles is 86.1%.

[0074] In summary, the present invention discloses a method for regenerating positive electrode materials of ternary lithium batteries and positive electrode materials of ternary lithium batteries, wherein the method comprises the steps of: providing a malic acid leachate of waste lithium battery positive electrode materials; adding a nickel source, a cobalt source, and a manganese source to the malic acid leachate of the waste lithium battery positive electrode materials to obtain a mixed nickel-cobalt-manganese-rich leachate; subjecting the mixed nickel-cobalt-manganese-rich leachate to oxidation precipitation to obtain a precursor of positive electrode materials of ternary lithium batteries; mixing the precursor of positive electrode materials of ternary lithium batteries with a lithium source, and subjecting the precursor to calcination treatment to obtain the positive electrode materials of ternary lithium batteries. In view of the shortcomings of the existing coprecipitation method and extraction and separation method, the present invention proposes a new method for regenerating ternary positive electrode materials from malic acid leachate of waste lithium battery positive electrode materials, wherein nickel, cobalt, and manganese are coprecipitated by oxidation precipitation, which not only has a short precipitation time, simple operation, high precipitation rate, and low cost, but also has excellent charge and discharge performance of the precursor after lithium supplementation and regeneration.

[0075] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for regenerating positive electrode materials of a ternary lithium battery, characterized in that: Includes steps: The positive electrode materials separated from the waste lithium batteries are placed in water, ball-milled or sand-milled, and then sieved; The screened positive electrode material is added into a malic acid solution, and a reducing agent is added at the same time, and filtered to obtain a malic acid leachate of the waste lithium battery positive electrode material; Adding a nickel source, a cobalt source and a manganese source to the malic acid leachate of the waste lithium battery positive electrode material to obtain a mixed nickel-cobalt-manganese-rich leachate; The pH of the mixed nickel-cobalt-manganese-rich leaching solution is adjusted, oxygen is introduced, pressurized and heated, and oxidation precipitation is performed, wherein the oxidation precipitation conditions are: pH value is 6-11, oxygen pressure is 0.2-1.2 MPa, temperature is 60-140° C., and time is 1-6 hours; a precursor of a positive electrode material for a ternary lithium battery is obtained; The precursor of the positive electrode material of the ternary lithium battery is mixed with a lithium source and calcined to obtain the positive electrode material of the ternary lithium battery.

2. The method for regenerating positive electrode materials of a ternary lithium battery according to claim 1, characterized in that: The nickel source is nickel carbonate or nickel sulfate, the cobalt source is cobalt carbonate or cobalt sulfate, and the manganese source is manganese carbonate or manganese sulfate.

3. The method for regenerating positive electrode materials of a ternary lithium battery according to claim 1, characterized in that: The lithium source is lithium carbonate.

4. The method for regenerating positive electrode materials of a ternary lithium battery according to claim 1, characterized in that: The steps of mixing the precursor of the positive electrode material of the ternary lithium battery with a lithium source and calcining the mixture to obtain the positive electrode material of the ternary lithium battery are specifically as follows: The precursor of the positive electrode material of the ternary lithium battery is mixed with a lithium source, ground, calcined, crushed and then sieved to obtain the positive electrode material of the ternary lithium battery.

5. The method for regenerating positive electrode materials of a ternary lithium battery according to claim 1 or 4, characterized in that: The lithium source is mixed with the precursor of the positive electrode material of the ternary lithium battery in a molar ratio of Li / M=1.02-1.10:1, wherein M=Ni+Co+Mn.

6. The method for regenerating positive electrode materials of a ternary lithium battery according to claim 1 or 4, characterized in that: The calcination temperature is 700-1000° C., and the calcination time is 8-14 hours.

7. A ternary lithium battery positive electrode material, characterized in that: The method is prepared by any one of claims 1 to 6.

Citation Information

Patent Citations

  • Recovery method of positive electrode material of waste ternary lithium ion battery

    CN111252814A

  • Method for preparing spherical aluminum-doped nickel lithium carbonate for lithium ion battery positive electrode material

    CN102074679A

  • High-nickel cathode material and preparation method thereof, and lithium ion battery

    CN110336004A