A method for rapidly preparing gel

Through the thiol-disulfide bond exchange reaction between Ellman's reagent and thiol-modified polymer, the problem of complex and long organic reactions in gel preparation is solved, and fast and simplified gel preparation is achieved, which is universal and fast self-healing. Combined functions.

CN115093579BActive Publication Date: 2024-10-15SHANDONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210645152.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-09
Publication Date
2024-10-15
Estimated Expiration
2042-06-09

AI Technical Summary

Technical Problem

Existing gel preparation methods have problems such as complex organic reactions, many precursor molecules, high costs, and long preparation times. They also lack universality and cannot prepare a variety of polymer gels quickly and effectively.

Method used

The thiol-disulfide bond exchange reaction between Ellman's reagent and thiol-modified polymer is used. By dissolving Ellman's reagent in deionized water or an alkaline buffer solution and mixing it with the thiol-modified polymer, hydrogels can be quickly prepared, simplifying the organic synthesis steps and Shorten gel formation time.

Benefits of technology

This method greatly simplifies the gel preparation process, involves only the synthesis of one precursor molecule, shortens the gel formation time, is universal, and can quickly prepare synthetic polymer, natural polymer and biopolymer gels, and Give the gel rapid self-healing and secondary modification functions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115093579B_ABST
    Figure CN115093579B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of polymer materials, and in particular to a method for rapid preparation of gel, the preparation method comprising the following steps: dissolving Ellman reagent (DTNB) in deionized water or an alkaline buffer solution; dissolving a thiol-modified polymer in deionized water or an alkaline buffer solution; mixing the two solutions evenly and standing to obtain a hydrogel. The method for rapid preparation of gel at most involves the synthesis of a precursor molecule, which simplifies the required organic synthesis process, and the method for rapid preparation of gel based on thiol-disulfide exchange reaction can not only effectively reduce the synthesis of precursor molecules in the gel preparation process, simplify organic reactions, but also achieve rapid preparation of gel; and the method can be applied to more polymers (synthetic polymers, natural polymers, biopolymers) to synthesize gels, and the gel synthesized by the method has the performance of rapid self-healing and secondary modification, and has a wide range of biomedical application potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a method for rapidly preparing gel. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Gel is a three-dimensional network structure. Due to its wide application in biomedicine, including diagnosis, tissue framework, drug delivery, etc., gel preparation methods have received more and more attention. Generally, gels can be synthesized from synthetic polymers (such as polyethylene glycol) or natural polymers (such as carboxymethyl chitosan, hyaluronic acid) based on hydrophobic interactions, hydrogen bonds, click chemistry, amination reactions, etc. For example, block polymers of polyethylene glycol and polycaprolactone can form gels through the strong hydrophobic effect of polycaprolactone; polyethylene glycol molecules terminated with cyclopropane cyclooctyne and azide groups can prepare gels through azide-alkyne cycloaddition reactions between the two molecules; gels can also be quickly prepared by reacting N-hydroxysuccinimide activated molecules with other amino-containing molecules. Although the above-mentioned gel preparation method can achieve rapid preparation of gels, it usually requires the synthesis of two or more precursor molecules before preparing the gel, and the organic synthesis process involved is relatively complicated and costly. At the same time, the above-mentioned gel preparation method lacks universality, and one method cannot be applied to the preparation of more polymer gels. Thiol is a highly reactive group that can react with maleimide and olefin / alkyne through click chemistry or Michael addition reaction, and molecules containing thiol can be used to synthesize gels through the above reactions. The use of thiol-modified molecules to prepare gels has similar disadvantages to the method described above, that is, the organic reaction process involved is relatively complicated. By using an oxidation method, molecules containing thiol groups are oxidatively cross-linked, so that gels can be prepared using one molecule. This method of preparing gels by oxidative cross-linking overcomes the problems of complex organic reactions and more precursor molecules involved in the gel preparation process of the aforementioned method. However, the reaction rate of the thiol oxidation reaction is low, so it takes a long time to prepare gels by oxidative cross-linking. Summary of the invention

[0004] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for rapidly preparing gel based on thiol-disulfide bond exchange reaction, which can not only effectively reduce the synthesis of precursor molecules in the gel preparation process and simplify organic reactions, but also realize the rapid preparation of gel.

[0005] The thiol-disulfide bond exchange reaction between Ellman's reagent [5,5-dithio-bis-(2-nitrobenzoic acid)] (DTNB) and thiol groups has a high reaction coefficient, a fast reaction rate and high reaction activity. This principle can be used to achieve rapid preparation of hydrogels.

[0006] In order to achieve the above object, the technical solution of the present invention is as follows:

[0007] In a first aspect of the present invention, a method for rapidly preparing a gel is provided, comprising the following steps:

[0008] The Ellman reagent (DTNB) is dissolved in deionized water or an alkaline buffer solution; the thiol-modified polymer is dissolved in deionized water or an alkaline buffer solution; the two solutions are mixed evenly and allowed to stand to obtain a hydrogel.

[0009] In a second aspect of the present invention, a gel prepared by the above-mentioned rapid gel preparation method is provided.

[0010] In a third aspect of the present invention, a use of the above gel in the biomedical field is provided.

[0011] The specific embodiments of the present invention have the following beneficial effects:

[0012] (1) The rapid preparation method of the gel provided by the present invention uses a thiol-modified polymer as a substrate, and the entire gel preparation process involves the synthesis of at most one precursor molecule, which greatly simplifies the organic synthesis steps;

[0013] (2) The rapid preparation method of the gel provided by the present invention can use a synthetic polymer, a natural polymer, or a biological polymer, and has universal applicability;

[0014] (3) Compared with the method of oxidative thiol cross-linking, the gel preparation method disclosed in the present invention can greatly shorten the gel formation time.

[0015] (4) The polymer mass concentration of the hydrogel prepared by the gel preparation method disclosed in the present invention can be as low as 1%;

[0016] (5) The gel synthesized by the preparation method of the gel disclosed in the present invention has the function of rapid secondary modification; in the formed gel, there will be a small amount of uncross-linked thiol-nitrobenzoic acid; after the gel is formed, a functional molecule containing a thiol group is added to the gel again, which can achieve rapid secondary modification and functionalization of the gel.

[0017] (6) The gel prepared by the method of the present invention contains a small amount of converted thiol groups that have not reacted with thiol groups, which gives the prepared gel the property of rapid self-healing.

[0018] (7) The gel preparation method disclosed in the present invention is universal; thiol groups can be modified on synthetic or natural polymers, and this method can be used to achieve rapid preparation of functional hydrogels; for example, hyaluronic acid can target cells with high expression of surface CD44 protein, such as MDA-MB-231 cells and immune cells; hyaluronic acid gel can be synthesized using this method to achieve cell screening. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0020] Figure 1 These are photographs of 8-arm-PEG-SH gels with a mass concentration of 1% prepared in Example 1 and Comparative Example 1 after being allowed to stand for 400 minutes; wherein a is a photograph of the gel prepared in Example 1 after being allowed to stand for 400 minutes, and b is a photograph of the gel prepared in Comparative Example 1 after being allowed to stand for 400 minutes.

[0021] Figure 2 These are SEM images of 8-arm-PEG-SH gels with a mass concentration of 1% prepared in Example 1 and Comparative Example 1; wherein a is the SEM image of Example 1, and b is the SEM image of Comparative Example 1.

[0022] Figure 3 It is a comparison chart of the gelation time of Example 1 and Comparative Example 1.

[0023] Figure 4 It is a comparison chart of the gelation time of Example 2 and Comparative Example 2.

[0024] Figure 5 This is the gelling time of polyethylene glycol with different molecular weights used in Example 3.

[0025] Figure 6 It is the gelation time of Example 4 and Comparative Example 4.

[0026] Figure 7 Schematic diagram of the self-healing performance of the gel in Example 5.

[0027] Figure 8 It is a comparison chart of the secondary modification performance of Example 1 and Comparative Example 1.

[0028] Fig. 9 These are pictures of MDA-MB-231 (a) and HeLa (b) cells cultured on gel in Example 5. DETAILED DESCRIPTION

[0029] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used in the present application have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0030] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0031] In one embodiment of the present invention, a method for rapidly preparing a gel is provided, comprising the following steps:

[0032] The Ellman reagent (DTNB) is dissolved in deionized water or an alkaline buffer solution; the thiol-modified polymer is dissolved in deionized water or an alkaline buffer solution; the two solutions are mixed evenly and allowed to stand to obtain a hydrogel.

[0033] In one or more embodiments, the polymer is a combination of one or more of a synthetic polymer, a natural polymer, and a biopolymer;

[0034] Preferably, the synthetic polymer is selected from polyethylene glycol, polymethacrylic acid, polyacrylic acid; the natural polymer is selected from carboxymethyl chitosan, sodium alginate, hyaluronic acid; the biopolymer is selected from fetal bovine serum albumin;

[0035] In one or more embodiments, the thiol-modified polymer is thiol polyethylene glycol; or a combination of one or more of Traut's reagent, cysteamine, and mercaptopropionic acid to modify the above polymer;

[0036] More preferably, the molecular weight of the mercapto polyethylene glycol used is 5K-40K.

[0037] Preferably, the thiol modification rate is 5% to 40%.

[0038] In one or more embodiments, the pH value of the deionized water is 6.0-7.0, and the pH value of the alkaline buffer solution is 7.0-10.0;

[0039] Preferably, the alkaline buffer solution is selected from tris(hydroxymethylaminomethane) hydrochloride aqueous solution, 3-morpholinepropanesulfonic acid-sodium hydroxide buffer aqueous solution, disodium hydrogen phosphate-sodium dihydrogen phosphate buffer aqueous solution, sodium hydroxide aqueous solution, potassium hydroxide aqueous solution or ammonia solution; further preferably, the alkaline buffer solution is selected from disodium hydrogen phosphate-sodium dihydrogen phosphate buffer aqueous solution, sodium hydroxide aqueous solution, potassium hydroxide aqueous solution or ammonia solution.

[0040] In one or more embodiments, the mass concentration of the thiol-modified polymer in the mixed solution is 1% to 50%.

[0041] In one or more embodiments, the amount of DTNB in ​​the mixed solution is 10% to 80% of the amount of thiol in the thiol-modified polymer.

[0042] The method for rapidly preparing gel disclosed in the present invention involves the synthesis of at most one precursor molecule, which simplifies the required organic synthesis process, and the method can be applied to synthesizing gels of a large number of polymers (synthetic polymers, natural polymers, and biological polymers). At the same time, the gel synthesized by this method has the properties of rapid self-healing and secondary modification, and has the potential for broad biomedical applications.

[0043] In one embodiment of the present invention, a gel prepared by the above-mentioned rapid gel preparation method is provided.

[0044] In one embodiment of the present invention, a use of the above-mentioned gel in the biomedical field is provided.

[0045] The present invention will be further explained and illustrated below in conjunction with specific embodiments.

[0046] Example 1

[0047] 8-arm-PEG-SH

[0048] Add DTNB to prepare 8-arm-PEG-SH gel with a mass concentration of 1%:

[0049] Prepare 200 μL of 25 mg / mL 8-arm-PEG-SH (10 KDa) solution, prepare 300 μL of 2.64 mg / mL DTNB solution, add the DTNB solution dropwise to the 8-arm-PEG-SH solution under vortexing, and let it stand for 400 minutes to obtain 8-arm-PEG-SH gel with a mass concentration of 1%. Figure 1 As shown in a, the SEM photo Figure 2 As shown in a.

[0050] Comparative Example 1

[0051] 8-arm-PEG-SH gel with a mass concentration of 1% was prepared by oxidation method.

[0052] Dissolve 5 mg of 8-arm-PEG-SH (10 KDa) in 500 μl of PB buffer at pH 8.0 and place for 120 h to obtain a gel with a mass concentration of 1%. Figure 1 As shown in b, after 400 minutes, it is still in liquid state and has not formed a gel. This proves that adding DTNB can effectively increase the gelation rate. The SEM results after gelation are as follows Figure 2 As shown in b.

[0053] The comparison of gelation time between Example 1 and Comparative Example 1 is shown in the figure below: Figure 3 shown.

[0054] Example 2

[0055] DTNB was added to prepare 8-arm-PEG-SH gel with a mass concentration of 10%.

[0056] Prepare 200 μL of 250 mg / mL 8-arm-PEG-SH (10 KDa) and 300 μL of 26.4 mg / mL DTNB solution. Add the DTNB solution dropwise to the 8-arm-PEG-SH solution under vortexing and let stand for 20 minutes to obtain a 10% 8-arm-PEG-SH gel. The gelation time is as follows: Figure 4 shown.

[0057] Comparative Example 2

[0058] 8-arm-PEG-SH gel with a mass concentration of 10% was prepared by oxidation method.

[0059] 50 mg of 8-arm-PEG-SH (10 KDa) was dissolved in 500 μl of PB buffer (pH 8.0) and allowed to stand for 14 h to obtain a 10% 8-arm-PEG-SH gel. The gelation time was as follows: Figure 4 shown.

[0060] Example 3

[0061] The same gel preparation method as in Example 1 was adopted, using 8-arm-PEG-SH with molecular weights of 10KDa, 20KDa, and 40KDa, respectively, and a gel with a mass concentration of 5% was prepared by oxidation method and adding DTNB. The gelation time is shown in 5.

[0062] Example 4

[0063] Add DTNB to prepare carboxymethyl chitosan gel, hyaluronic acid gel, sodium alginate gel and polyacrylic acid gel respectively:

[0064] Synthesis of mercaptocarboxymethyl chitosan molecules: Weigh 200 mg of carboxymethyl chitosan and place it in a round-bottom flask. Dissolve it in 10 mL of PB buffer with a pH of 7.4, add 12 mg of sodium ethylenediaminetetraacetate (EDTA) and stir until completely dissolved. Then add 41.2 mg of Traut's reagent and stir at room temperature for 4 hours. Then, dialyze and freeze-dry the reaction solution to obtain mercaptocarboxymethyl chitosan.

[0065] Synthetic mercapto hyaluronic acid, mercapto sodium alginate, mercapto polyacrylic acid:

[0066] 500 mg of hyaluronic acid was weighed and placed in a round-bottom flask, dissolved with 20 mL of PB buffer at pH 8.5, and then 10 mL of 4-(4,6-dimethoxytriazine-2-yl)-4-methylmorpholine hydrochloride (DMTMM) solution with a mass concentration of 40 mg / mL was added, and then 10 mL of 2-(2-pyridyldisulfide)ethylamine hydrochloride solution with a mass concentration of 25 mg / mL was added, and the solution was stirred at room temperature for 12 hours and then dialyzed. Excess dithiothreitol was added to the dialyzed solution, and the thiol-modified hyaluronic acid was obtained after dialyzation and freeze-drying.

[0067] Weigh 500 mg of sodium alginate and place it in a round-bottom flask, dissolve it with 20 mL of PB buffer with a pH of 8.5, then add 10 mL of DMTMM solution with a mass concentration of 40 mg / mL, and then add 10 mL of 2-(2-pyridyldisulfide)ethylamine hydrochloride solution with a mass concentration of 25 mg / mL, and stir at room temperature for 12 hours before dialyzing. Add excess dithiothreitol to the dialyzed solution, dialyze, and freeze-dry to obtain sodium thioalginate.

[0068] The preparation method of mercapto polyacrylic acid is consistent with the above method, the mass of added DMTMM is 150 mg, and the mass of added 2-(2-pyridyldisulfide)ethylamine hydrochloride is 80 mg.

[0069] Weigh 25 mg of mercaptocarboxymethyl chitosan, stir and dissolve it with 400 μl of water, then add 100 μl of 33 mg / mL DTNB solution under vortexing, and let it react for a while to obtain a mercaptocarboxymethyl chitosan gel with a mass concentration of 5%; adopt the same method, weigh 15 mg of mercapto hyaluronic acid, mercapto sodium alginate, and mercapto polyacrylic acid, add a certain concentration of DTNB solution to obtain the corresponding gel; the gelation time is as follows Figure 6 shown.

[0070] Comparative Example 4

[0071] Carboxymethyl chitosan, hyaluronic acid, sodium alginate and polyacrylic acid gel were prepared by oxidation method.

[0072] Weigh 25 mg of mercaptocarboxymethyl chitosan and dissolve it in 500 μl of tertiary water. After standing for 120 hours, a gel with a mass concentration of 5% is obtained. Weigh 15 mg of mercaptohyaluronic acid, sodium alginate, polyacrylic acid, and polymethacrylic acid, respectively, and dissolve them in 500 μl of tertiary water. After standing for a period of time, a gel with a mass concentration of 3% is obtained. Figure 6 As shown, adding DTNB can reduce the gelation time. At the same time, it shows that this method has good universality.

[0073] Example 5

[0074] The cut hydrogel of Example 1 and the hydrogel of Comparative Example 1 were placed together. Figure 7 As shown, it shows that the hydrogel has good self-healing properties.

[0075] Secondary modification performance of gel: Gels were prepared in 24-well plates based on DTNB triggering (DPEG hydrogel) and oxidation method (PEG hydrogel). The gel was rinsed with DPBS several times. A 1 mg / mL linear polyethylene glycol solution with a thiol end and a 1 mg / mL cRGDfc solution were added and rinsed after 10 seconds. U87 cells and HeLa cells were cultured on the secondary modified gel. The cell density difference was as follows: Figure 8 As shown, the gel prepared by oxidation of 8-arm-PEG-SH is PEG, and the gel formed by adding DTNB is DPEG. After modification with linear polyethylene glycol, the cell density on the surface of DPEG hydrogel was significantly reduced; after modification with cRGDfc, the U87 cell density on the surface of DPEG hydrogel was significantly increased; the above experiments show that the hydrogel has rapid modification performance.

[0076] Functionalized gel: MDA-MB-231 and HeLa cells were cultured using the hyaluronic acid gel in Example 3. Figure 8 As shown in the figure, a is MDA-MB-231 and b is HeLa cells. The density of MDA-MB-231 cells on the surface of hyaluronic acid gel is higher, indicating that this method can quickly prepare functional hydrogels and be used for cell screening.

[0077] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for rapid preparation of gel, characterized in that: The preparation method comprises the following steps: Dissolve Ellman's reagent (DTNB) in deionized water or an alkaline buffer solution; dissolve the thiol-modified polymer in deionized water or an alkaline buffer solution; mix the two solutions evenly and let them stand to obtain a hydrogel; The amount of DTNB in ​​the mixed solution is 10% to 80% of the amount of thiol in the thiol-modified polymer.

2. The method for rapid preparation of gel according to claim 1, characterized in that: The polymer is a combination of one or more of synthetic polymers and natural polymers.

3. The method for rapid preparation of gel according to claim 2, characterized in that: The synthetic polymer is selected from polyethylene glycol, polymethacrylic acid, and polyacrylic acid; the natural polymer is selected from carboxymethyl chitosan, sodium alginate, hyaluronic acid, and fetal bovine serum albumin.

4. The method for rapid preparation of gel according to claim 1, characterized in that: The thiol-modified polymer is thiol polyethylene glycol; the molecular weight of thiol polyethylene glycol is 5K-40K; and the thiol modification rate is 5%-40%.

5. The method for rapid preparation of gel according to claim 2, characterized in that: The thiol-modified polymer is obtained by modifying the polymer according to claim 2 by a combination of one or more of Traut's reagent, cysteamine, and mercaptopropionic acid.

6. The method for rapid preparation of gel according to claim 1, characterized in that: The pH value of the deionized water is 6.0-7.0, and the pH value of the alkaline buffer solution is 7.0-10.

0.

7. The method for rapid preparation of gel according to claim 6, characterized in that: The alkaline buffer solution is selected from tris(hydroxymethylaminomethane) hydrochloride aqueous solution, 3-morpholinepropanesulfonic acid-sodium hydroxide buffer aqueous solution, disodium hydrogen phosphate-sodium dihydrogen phosphate buffer aqueous solution, sodium hydroxide aqueous solution, potassium hydroxide aqueous solution or ammonia aqueous solution.

8. The method for rapid preparation of gel according to claim 7, characterized in that: The alkaline buffer solution is selected from a sodium hydrogen phosphate-sodium dihydrogen phosphate buffer aqueous solution, a sodium hydroxide aqueous solution, a potassium hydroxide aqueous solution or an ammonia aqueous solution.

9. The method for rapid preparation of gel according to claim 1, characterized in that: The mass concentration of the thiol-modified polymer in the mixed solution is 1%~50%.

10. The gel prepared according to any one of claims 1 to 9.