Coated rare earth luminescent powder and preparation method thereof
By coating the surface of blue rare earth long afterglow luminescent materials with highly efficient light conversion inclusion compounds synthesized by metal organic frameworks and cyclodextrin-metal organic frameworks, the problem of limited colors of existing rare earth long afterglow luminescent materials has been solved, and the transition from blue to blue rare earth long afterglow luminescent materials has been solved. The color changes from green to orange, broadening the application range.
Patent Information
- Application Number
- CN202210525912.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-05-16
AI Technical Summary
Existing rare earth long afterglow luminescent materials have limited luminescent colors, making it difficult to achieve colors other than blue, green, sky blue, and yellow-green. Moreover, existing light color conversion methods are inefficient and cannot effectively broaden the scope of applications.
Metal organic frameworks (MOFs) and cyclodextrin-metal organic frameworks (CD-MOF) are used to synthesize high-efficiency light conversion inclusion complexes, and coat them on the surface of blue rare earth long afterglow luminescent materials. By regulating the inclusion complex formula and The concentration and coating thickness can achieve changes in luminous color, from blue to yellow-blue, yellow to orange.
It has successfully broadened the application scope of rare earth long-lasting luminescent materials and achieved controllable color changes from blue to orange, with simple operation and remarkable effects.
Smart Images

Figure CN115109581B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of luminescent materials, and in particular relates to a coated rare earth luminescent powder and a preparation method thereof. Background Art
[0002] Long afterglow luminescent materials refer to the phenomenon that after the material is excited by an external light source, it can continue to emit light for a period of time in a dark environment. This phenomenon of long-term continuous luminescence is due to its unique photoelectron storage and release mechanism. Long afterglow luminescent materials play a vital role in the fields of spectroscopy, photochemistry, photonics and material science. In recent years, more and more research has focused on the morphological manipulation, band operation and luminescence time of long afterglow. However, the luminescent colors of the relatively mature rare earth long afterglow materials that have been developed are only limited: blue, green, sky blue, yellow-green, and other colors are not yet mature. It is an effective technical method to achieve light color conversion by coating. This color conversion method mainly depends on two parameters, namely the light source of the luminescent material and the coated light conversion agent. The excitation spectrum of the light conversion agent must overlap or be close to the emission spectrum of the light source of the luminescent material to achieve effective light conversion.
[0003] Metal organic frameworks (MOFs) are framework materials composed of metals and organic ligands, and are a new type of porous material. Simply put, MOFs are framework materials composed of clusters composed of metal ions or metals and oxygen atoms, hydroxyls, carboxylic acids, etc. combined with organic ligands. The spatial isolation of fluorescent dye fluorophores is achieved by the inclusion reaction of MOFs and cyclodextrin-metal organic frameworks (CD-MOF), and efficient fluorescent materials are prepared as light converters. The present invention prepares coated rare earth luminescent powders by a two-step method. First, MOFs, cyclodextrin-metal organic frameworks (CD-MOF) and dyes are used to synthesize and prepare an efficient light converter; then the prepared efficient light converter is coated on the surface of a blue rare earth long afterglow luminescent material, thereby realizing its light color conversion, and developing a coated multicolor rare earth long afterglow luminescent material. Summary of the invention
[0004] In view of this, the technical problem to be solved by the present invention is to provide a coated rare earth luminescent powder and a preparation method thereof.
[0005] To achieve the above object, the present invention adopts the following technical solution:
[0006] A coated rare earth luminescent powder, characterized in that the coated rare earth luminescent powder is composed of the following components:
[0007] Component A: at least one of metal organic frameworks (MOFs), cyclodextrin-metal organic framework (CD-MOF) materials, wherein cyclodextrin-metal organic framework (CD-MOF) was purchased from Xi'an Ruixi Biotechnology Co., Ltd. and Beijing Beike New Materials Technology Co., Ltd.;
[0008] Component B: at least one of rhodamine 590, rhodamine 6G, rhodamine B, rhodamine B ethylenediamine, 5-carboxytetramethylrhodamine, anthocyanin Cy5, 6,7-dimethoxycoumarin, and fluorescein methotrexate triammonium salt;
[0009] Component C: rare earth long afterglow luminescent material;
[0010] Component D: one of silane coupling agent, aluminate coupling agent and titanate coupling agent;
[0011] Component E: one of silicone oil, acrylic acid and liquid paraffin;
[0012] Component F: at least one of water, toluene, m-xylene, n-pentanol and ethyl acetate.
[0013] Further, the MOFs is one of RE@MOF, Mn@MOF, Co@MOF, Cu@MOF, Zn@MOF, Mg@MOF, Ca@MOF, Sr@MOF, Pb@MOF, ZIF-8 MOF, ZIF-67 MOF, MOF-5, MOF-74, MOF-177 (wherein RE is La, Pr, Eu, Nd, Yb, Gd, Tb or Sm), purchased from Xi'an Qiyue Biotechnology Co., Ltd. ( ) and Beijing Beike New Materials Technology Co., Ltd. ( ).
[0014] Furthermore, the rare earth long afterglow luminescent material is CaAl2O4: Eu 2+ ,Nd 3+ Blue or Sr2MgSi2O7: Eu 2 + ,Dy 3+Blue, refer to [1]Mingxi Zhang, Fengfeng Li, Yongcheng Lin, Yan Li, YiShen.Enhanced afterglow performance of CaAl_2O_4:Eu~(2+),Nd~(3+) phosphors byco-doping Gd~(3+)[J].Journal of Rare Earths, 2021, 39(08):930-937. And [2] LiubinZheng, Yanan Zhu, Zengyuan Pang, Mingqiao Ge. Luminescence properties of composite material Sr_2MgSi_2O_7:Eu~(2+),Dy~(3+) / light conversion agent with multilayer structure[J].Journal of Rare Earths,2022,40(01):34-40. Preparation method.
[0015] The present invention also provides a method for preparing a coated rare earth luminescent powder, comprising the following steps:
[0016] (1) Prepare component A and component F into a dilute solution G, disperse by ultrasonic and let stand for 6-24 hours;
[0017] (2) Add component B to the static dilute solution of G, stir and react at 25-60°C and 400-1200 rpm for 1-12 hours to obtain H;
[0018] (3) Dry H at 70-140°C for 4-24h, take it out and grind it into powder to obtain photoconversion agent I;
[0019] (4) preparing solution J by mixing the photoconverter components I and C with component F;
[0020] (5) Stir solution J at 400-1200 rpm for 5-30 min at 25-60 °C, then heat to 70-100 °C, add components D and E, and continue stirring for 20-90 min. After separating the filtrate, freeze-dry the solid for 12-48 h, take it out, grind it, and sieve it to obtain the coated rare earth luminescent powder.
[0021] Furthermore, in step (1), the mass ratio of component A to component F is 1:100-500.
[0022] Furthermore, in step (1), the ultrasonic dispersion time is 15 to 90 minutes.
[0023] Furthermore, the mass ratio of component B in step (2) to component A in the dilute solution of G is 1:0.5-2.
[0024] Furthermore, in step (4), the mass ratio of the photoconverter I, component C and component F is 1:2-10:100-500.
[0025] Furthermore, in step (5), the mass ratio of component D to photoconverter I is 1:20-100; the mass ratio of component E to photoconverter I is 1:20-100.
[0026] Beneficial effects: The present invention first uses dyes and MOFs or dextrin-metal organic framework (CD-MOF) to synthesize a high-efficiency light conversion inclusion compound, and then coats it on the surface of a blue rare earth long afterglow luminescent material. By adjusting the formula and concentration of the high-efficiency light conversion inclusion compound, as well as the coating thickness of the inclusion compound on the surface of the blue rare earth long afterglow luminescent material, the blue light of the rare earth long afterglow luminescent material can be changed and adjusted to achieve the color of the complex changing between blue, yellow-blue, yellow and orange. Figure 1 The surface of the blue rare earth long afterglow luminescent material is coated with a high-efficiency light conversion inclusion compound to achieve luminescent color conversion, which has the characteristics of simple operation and significant effect, and can broaden the application range of rare earth long afterglow luminescent materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a color coordinate diagram; the color coordinate diagram is roughly divided into upper left, lower left, lower right, and middle according to the orientation, wherein the upper left is a greenish area, the lower left is a blueish and purple area, the lower right is a reddish area, and the middle is a yellowish area. From the upper left area to the lower left area, the color gradually changes from green to light green, light blue, and blue. From the lower left area to the lower right area, the color gradually changes from purple to light purple, pink, and red. From the upper left area to the lower right area, the color gradually changes from green to light green, yellow, orange, and red. The present invention mainly realizes controllable color adjustment from the middle left area to the middle right and lower right areas by coating the light-converting material on the surface of the blue long afterglow luminescent material, thereby preparing a coated colorful long afterglow luminescent material; Figure 1 The positions of the color coordinates corresponding to several embodiments and comparative examples; Embodiments 1-7 correspond to K1-K7, respectively, and Comparative Examples 1-3 correspond to K8-K 10 , K0 is a blank long afterglow luminescent material; K0-K 10The corresponding coordinates in the color scale system are K0 (0.14, 0.26), K1 (0.46, 0.43), K2 (0.39, 0.39), K3 (0.61, 0.36), K4 (0.51, 0.36), K5 (0.42, 0.38), K6 (0.53, 0.43), K7 (0.48, 0.39), K8 (0.34, 0.36), K9 (0.32, 0.35), K 10 (0.15, 0.25). DETAILED DESCRIPTION
[0028] Example 1
[0029] (1) Prepare a dilute solution G1 by mixing 1 g of Tb@MOF with 500 g of n-pentanol, disperse it by ultrasonic for 20 min, and let it stand for 24 h.
[0030] (2) Add 0.67 g of anthocyanin Cy5 to G1, stir the mixture at 60°C and 1000 rpm for 4 h to obtain H1.
[0031] (3) Dry H1 at 70°C for 24 h, take it out and grind it into powder to obtain the photoconverter I1.
[0032] (4) 1g I1 and 5g Sr2MgSi2O7: Eu 2+ ,Dy 3+ Prepare J1 solution with 400g of m-xylene.
[0033] (5) The J1 solution was stirred at 700 rpm at 60°C for 20 min and then heated to 80°C. 0.01 g of titanate coupling agent and 0.02 g of silicone oil were added and stirred for 30 min. The filtrate was separated and the solid was freeze-dried for 24 h. After that, it was taken out and ground and sieved to obtain the coated rare earth luminescent powder K1.
[0034] Example 2
[0035] (1) 1 g of cyclodextrin-metal organic framework (CD-MOF) was mixed with 150 g of water and 150 g of n-pentanol to prepare a dilute solution G2, which was then dispersed by ultrasonic for 15 min and allowed to stand for 6 h.
[0036] (2) Add 0.5 g of rhodamine 590 to G2 and stir the mixture at 45 °C and 900 rpm for 2 h to obtain H2.
[0037] (3) Dry H2 at 140°C for 4 h, take it out and grind it into powder to obtain the photoconverter I2.
[0038] (4) 1g I2 and 10g CaAl2O4: Eu 2+ ,Nd3+ Prepare J2 solution with 500g ethyl acetate.
[0039] (5) The J2 solution was stirred at 400 rpm for 30 min at 25 °C and then heated to 90 °C. 0.017 g of aluminate coupling agent and 0.05 g of acrylic acid were added and stirred for 60 min. The filtrate was separated and the solid was freeze-dried for 12 h. After that, it was taken out and ground and sieved to obtain the coated rare earth luminescent powder K2.
[0040] Example 3
[0041] (1) Prepare a dilute solution G3 by mixing 1 g ZIF-8 MOF with 100 g water, disperse by ultrasonic for 15 min, and let stand for 24 h.
[0042] (2) Add 0.5 g of rhodamine B and 0.5 g of 6,7-dimethoxycoumarin to G3, stir at 50°C and 1200 rpm for 12 h to obtain H3.
[0043] (3) Dry H3 at 80°C for 12 h, take it out and grind it into powder to obtain the photoconverter I3.
[0044] (4) 1g I3 and 2g CaAl2O4: Eu 2+ ,Nd 3+ Prepare J3 solution with 300g toluene.
[0045] (5) The J3 solution was stirred at 700 rpm at 35°C for 20 min and then heated to 85°C. 0.01 g of silane coupling agent and 0.01 g of acrylic acid were added and stirred for 60 min. The filtrate was separated and the solid was freeze-dried for 48 h. The solid was taken out and ground and sieved to obtain the coated rare earth luminescent powder K3.
[0046] Example 4
[0047] (1) Prepare a dilute solution G4 by mixing 1 g MOF-5 with 100 g toluene, disperse it by ultrasonic for 30 min, and let it stand for 24 h.
[0048] (2) Add 2 g of fluorescein methotrexate triammonium salt to G4 and stir the mixture at 25 °C and 800 rpm for 6 h to obtain H4.
[0049] (3) Dry H4 at 110°C for 4 h, take it out and grind it into powder to obtain the photoconverter I4.
[0050] (4) 1g I4 and 7g CaAl2O4: Eu 2+ ,Nd 3+ Prepare J4 solution with 100g toluene.
[0051] (5) The J4 solution was stirred at 800 rpm for 10 min at 35 °C and then heated to 70 °C. 0.05 g of silane coupling agent and 0.02 g of liquid paraffin were added and the stirring was continued for 60 min. The filtrate was separated and the solid was freeze-dried for 24 h. After that, it was taken out and ground and sieved to obtain the coated rare earth luminescent powder K4.
[0052] Example 5
[0053] (1) Prepare a dilute solution of G5 by mixing 1 g Eu@MOF with 200 g ethyl acetate, disperse by ultrasonic for 30 min, and let stand for 6 h.
[0054] (2) Add 0.55 g of rhodamine 590 to G5 and stir the mixture at 40 °C and 600 rpm for 2 h to obtain H5.
[0055] (3) Dry H5 at 100°C for 12 h, take it out and grind it into powder to obtain the photoconverter I5.
[0056] (4) 1g I5 and 6g Sr2MgSi2O7: Eu 2+ ,Dy 3+ Prepare J5 solution with 400g of m-xylene.
[0057] (5) The J5 solution was stirred at 400 rpm at 35 °C for 30 min and then heated to 90 °C. 0.03 g of titanate coupling agent and 0.02 g of silicone oil were added and stirred for 60 min. The filtrate was separated and the solid was freeze-dried for 48 h. After that, it was taken out and ground and sieved to obtain the coated rare earth luminescent powder K5.
[0058] Example 6
[0059] (1) Prepare a dilute G6 solution by mixing 1 g MOF-74 with 200 g water, disperse by ultrasonic for 30 min, and let stand for 12 h.
[0060] (2) Add 1.5 g of anthocyanin Cy5 to G6, stir the mixture at 40 °C and 600 rpm for 5 h to obtain H6.
[0061] (3) Dry H6 at 105°C for 10 h, take it out and grind it into powder to obtain the photoconverter I6.
[0062] (4) 1g I6 and 5g CaAl2O4: Eu 2+ ,Nd 3+ Prepare J6 solution with 200g of n-pentanol.
[0063] (5) The J6 solution was stirred at 600 rpm for 10 min at 40 °C and then heated to 75 °C. 0.02 g of silane coupling agent and 0.01 g of liquid paraffin were added and the stirring was continued for 40 min. The filtrate was separated and the solid was freeze-dried for 48 h. After that, it was taken out and ground and sieved to obtain the coated rare earth luminescent powder K6.
[0064] Example 7
[0065] (1) Prepare a dilute G7 solution by mixing 1 g of La@MOF with 200 g of water, disperse it by ultrasonic for 30 min, and let it stand for 12 h.
[0066] (2) Add 1 g of rhodamine 590 to G7 and stir the mixture at 40 °C and 600 rpm for 5 h to obtain H7.
[0067] (3) Dry H7 at 105°C for 10 h, take it out and grind it into powder to obtain the photoconverter I7.
[0068] (4) 1g I7 and 5g Sr2MgSi2O7: Eu 2+ ,Dy 3+ Prepare J7 solution with 200g of n-pentanol.
[0069] (5) The J7 solution was stirred at 600 rpm for 10 min at 40 °C and then heated to 75 °C. 0.02 g of silane coupling agent and 0.01 g of acrylic acid were added and stirred for another 40 min. The filtrate was separated and the solid was freeze-dried for 48 h. The solid was taken out and ground and sieved to obtain the coated rare earth luminescent powder K7.
[0070] Comparative Example 1
[0071] (1) Prepare a dilute solution of Rhodamine 590 (1 g) and water (200 g). Disperse the solution by ultrasonic for 30 min and allow to stand for 12 h.
[0072] (2) G8 was stirred at 40°C and 600 rpm for 5 h to obtain H8.
[0073] (3) Dry H8 at 105°C for 10 h, take it out and grind it into powder to obtain the photoconverter I8.
[0074] (4) 1g I8 and 5g Sr2MgSi2O7: Eu 2+ ,Dy 3+ Prepare J8 solution with 200g of n-pentanol.
[0075] (5) The J8 solution was stirred at 600 rpm for 10 min at 40 °C and then heated to 75 °C. 0.02 g of silane coupling agent and 0.01 g of acrylic acid were added and stirred for 40 min. The filtrate was separated and the solid was freeze-dried for 48 h. After that, it was taken out and ground and sieved to obtain the coated rare earth luminescent powder K8.
[0076] Comparative Example 2
[0077] (1) Prepare a dilute G9 solution by mixing 1 g La@MOF with 200 g water, disperse by ultrasonic for 30 min, and let stand for 12 h.
[0078] (2) G9 was stirred at 40°C and 600 rpm for 5 h to obtain H9.
[0079] (3) Dry H9 at 105°C for 10 h, take it out and grind it into powder to obtain the photoconverter I9.
[0080] (4) 1g I9 and 5g Sr2MgSi2O7: Eu 2+ ,Dy 3+ Prepare J9 solution with 200g of n-pentanol.
[0081] (5) After stirring at 600 rpm for 10 min at 40 °C, heat to 75 °C, add 0.02 g of silane coupling agent and 0.01 g of acrylic acid, and continue stirring for 40 min. After separating the filtrate, freeze-dry the solid for 48 h, take it out, grind it, and sieve it to obtain the coated rare earth luminescent powder K9.
[0082] Comparative Example 3
[0083] (1) 5g Sr2MgSi2O7: Eu 2+ ,Dy 3+ Prepare J10 solution with 200g of n-pentanol.
[0084] (2) The J10 solution was stirred at 600 rpm for 10 min at 40 °C and then heated to 75 °C. 0.02 g of silane coupling agent and 0.01 g of acrylic acid were added and stirred for 40 min. The filtrate was separated and the solid was freeze-dried for 48 h. After that, it was taken out and ground and sieved to obtain the coated rare earth luminescent powder K. 10 .
[0085] Sr2MgSi2O7: Eu 2+ ,Dy 3+ The color coordinates of the untreated blank sample K0, the coated rare earth luminescent powders K1-K10 obtained in Examples 1-7 and Comparative Examples 1-3 are shown in FIG. Figure 1 .
[0086] Combination Figure 1It can be seen that, compared with Example 7, Comparative Example 1 illustrates that rare earth MOFs and cyclodextrins can change the color of the dye after treatment and coating; compared with Example 7, Comparative Example 2 illustrates that the effect of only rare earth MOFs and cyclodextrin without dye on the color of the long afterglow luminescent material is different from that of Comparative Example 1; compared with Example 7, Comparative Example 3 illustrates that the treatment process has little effect on the color of the long afterglow luminescent material.
[0087] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and changes without departing from the principle of the present invention. These improvements and changes should also be regarded as the protection scope of the present invention.
Claims
1. A coated rare earth luminescent powder, Features: The coated rare earth luminescent powder is composed of the following components: Component A: at least one of metal organic frameworks (MOFs) and cyclodextrin-metal organic framework (CD-MOF) materials; Component B: at least one of rhodamine 590, rhodamine 6G, rhodamine B, rhodamine B ethylenediamine, 5-carboxytetramethylrhodamine, anthocyanin Cy5, 6,7-dimethoxycoumarin, and fluorescein methotrexate triammonium salt; Component C: Rare earth long afterglow luminescent material is CaAl 2 O 4 : Eu 2+ ,Nd 3+ Blue or Sr 2 MgSi 2 O 7 : Eu 2+ ,Dy 3+ One of the blue ones; Component D: one of silane coupling agent, aluminate coupling agent and titanate coupling agent; Component E: one of silicone oil, acrylic acid and liquid paraffin; Component F: at least one of water, toluene, m-xylene, n-pentanol and ethyl acetate.
2. The coated rare earth luminescent powder according to claim 1, Features: The MOFs are one of RE@MOF, Mn@MOF, Co@MOF, Cu@MOF, Zn@MOF, Mg@MOF, Ca@MOF, Sr@MOF, Pb@MOF, ZIF-8 MOF, ZIF-67MOF, MOF-5, MOF-74, and MOF-177, wherein RE is La, Pr, Eu, Nd, Yb, Gd, Tb, or Sm.
3. A method for preparing the coated rare earth luminescent powder according to any one of claims 1 to 2, Features: The following steps are involved: (1) Prepare component A and component F into a dilute solution G, disperse by ultrasonic and let stand for 6-24 hours; (2) Add component B to the static dilute solution of G, stir and react at 25-60°C and 400-1200 rpm for 1-12 hours to obtain H; (3) Dry H at 70-140°C for 4-24h, take it out and grind it into powder to obtain photoconversion agent I; (4) preparing solution J by mixing the photoconverter components I and C with component F; (5) Stir solution J at 400-1200 rpm for 5-30 min at 25-60 °C, then heat to 70-100 °C, add components D and E, and continue stirring for 20-90 min. After separating the filtrate, freeze-dry the solid for 12-48 h, take it out, grind it, and sieve it to obtain the coated rare earth luminescent powder.
4. The method for preparing the coated rare earth luminescent powder according to claim 3, Features: The mass ratio of component A to component F in step (1) is 1:100-500.
5. The method for preparing the coated rare earth luminescent powder according to claim 3, Features: The ultrasonic dispersion time in step (1) is 15 to 90 minutes.
6. The method for preparing the coated rare earth luminescent powder according to claim 3, Features: The mass ratio of component B in step (2) to component A in the dilute solution of G is 1:0.5-2.
7. The method for preparing the coated rare earth luminescent powder according to claim 3, Features: In step (4), the mass ratio of the photoconverter I, component C and component F is 1:2-10:100-500.
8. The method for preparing the coated rare earth luminescent powder according to claim 3, Features: In step (5), the mass ratio of component D to photoconverter I is 1:20-100; the mass ratio of component E to photoconverter I is 1:20-100.
Citation Information
Patent Citations
Rare earth long-persistence luminescent powder, preparation method and application thereof
CN102746845A
Skin core structure tombarthite strontium aluminate long afterglow luminescent fiber and preparation method thereof
CN106480525A
Rare earth long-afterglow light emitting powder, preparation method thereof, waterborne energy storage type rare earth long-afterglow light emitting coating and preparation method thereof
CN108865130A
Preparation method of composite color-changing nanofiber membrane
CN112626721A
Long-lasting phosphor material
WO2020199191A1