Titanium alloy workpiece, housing, titanium alloy workpiece preparation method and etching solution

By forming a constriction-like and spike-like surface treatment on the titanium alloy workpiece, the problem of titanium alloy surface treatment is solved, the bonding strength with the material body is improved, and its application potential in electronic product casings is enhanced.

CN115110139BActive Publication Date: 2024-10-29SHENZHENSHI YUZHAN PRECISION TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202110298354.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-19
Publication Date
2024-10-29
Estimated Expiration
2041-03-19

AI Technical Summary

Technical Problem

The good corrosion resistance of titanium alloys makes surface treatment difficult, limiting its application in consumer electronics housing materials, especially when preventing antenna signal shielding and connecting non-metallic parts to metal housings.

Method used

A titanium alloy workpiece is used, and its surface is sandblasted and electrochemically etched to form neck-shaped holes. It is combined with aluminum elements and acidic or alkaline additives to form a radial or coral-like spike structure to enhance the bonding force with the material body.

Benefits of technology

It improves the bonding strength and drawing force between the titanium alloy workpiece and the material body, solves the problem of titanium alloy surface treatment, and enhances its application potential in electronic product casings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115110139B_ABST
    Figure CN115110139B_ABST
Patent Text Reader

Abstract

A titanium alloy workpiece includes a titanium alloy substrate and a first hole arranged on the titanium alloy substrate, wherein at least one of the first holes has an inner diameter greater than the diameter of the hole mouth, and the first hole is in a necked shape. The present application also provides a shell including a titanium alloy workpiece, a method for preparing a titanium alloy workpiece, and an etching liquid for etching a titanium alloy to form a titanium alloy workpiece.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of metal materials, and in particular to a titanium alloy workpiece, a housing, a method for preparing a titanium alloy workpiece, and an etching solution. Background Art

[0002] Portable consumer electronic products are increasingly used in people's lives. Consumers have higher and higher requirements for the appearance and performance of electronic products. Titanium alloy has the advantages of high strength, low density, good mechanical properties, good toughness and good corrosion resistance, and is a good choice as the substrate of electronic product shells.

[0003] In order to prevent antenna signal shielding and avoid signal shielding by the entire metal shell, the main body of the metal shell needs to be provided with a non-metallic part, and the connection between the non-metallic part and the main body needs to be processed and holed on the main body of the metal shell. However, it is precisely because of the good corrosion resistance of titanium alloy that the surface treatment of titanium alloy becomes difficult, thus limiting the application of titanium alloy as a shell material for consumer electronic products. Summary of the invention

[0004] In view of this, it is necessary to provide a titanium alloy workpiece that can be effectively combined with other materials and a method for preparing the same, as well as a shell including the titanium alloy workpiece and an etching solution for preparing the titanium alloy workpiece.

[0005] A titanium alloy workpiece comprises a titanium alloy substrate and a first hole arranged on the titanium alloy substrate; wherein at least one inner diameter of the first hole is larger than the diameter of the hole mouth, and the first hole is in a necked shape.

[0006] In some embodiments, a second hole is further provided on the titanium alloy substrate, the second hole is located on the inner wall of the first hole, and the second hole is a radial spike structure.

[0007] In some embodiments, a second hole is further provided on the titanium alloy substrate, the second hole is located on the inner wall of the first hole, and the second hole has a coral-like structure.

[0008] In some embodiments, the titanium alloy matrix includes aluminum elements.

[0009] In some embodiments, the first pores have a pore depth ranging from 20 μm to 70 μm.

[0010] In some embodiments, the median depth of the first pores ranges from 35 μm to 60 μm.

[0011] In some embodiments, the porosity of the first pores ranges from 30% to 60%.

[0012] In some embodiments, the titanium alloy workpiece further includes an aluminum alloy substrate, wherein the aluminum alloy substrate is connected to the titanium alloy substrate, and a third hole is disposed on the surface of the aluminum alloy substrate, and the third hole is coral-shaped.

[0013] A shell for electronic equipment, comprising: a titanium alloy workpiece and a material body; wherein the titanium alloy workpiece comprises a titanium alloy substrate and a first hole arranged on the titanium alloy substrate, the first hole has at least one inner diameter larger than the hole mouth diameter, the first hole is necked, and the material body is arranged in the first hole.

[0014] In some embodiments, a second hole is further provided on the titanium alloy substrate, the second hole is located on the inner wall of the first hole, the second hole is a radial spike structure, and the material body is provided in the second hole.

[0015] In some embodiments, a second hole is further provided on the titanium alloy substrate, the second hole is located on the inner wall of the first hole, the second hole is a coral-like structure, and the material body is provided in the second hole.

[0016] In some embodiments, the titanium alloy matrix includes aluminum elements.

[0017] In some embodiments, the material of the material body is selected from at least one of metal, polymer, ceramic, and glass.

[0018] In some embodiments, the first pores have a pore depth ranging from 20 μm to 70 μm.

[0019] In some embodiments, the porosity of the first pores ranges from 30% to 60%.

[0020] In some embodiments, the titanium alloy workpiece further includes an aluminum alloy substrate, wherein the aluminum alloy substrate is connected to the titanium alloy substrate, a third hole is disposed on the surface of the aluminum alloy substrate, the third hole has a coral-like structure, and the material body is disposed in the third hole.

[0021] A method for preparing a titanium alloy workpiece, comprising sandblasting a titanium alloy product; placing the sandblasted titanium alloy product in an etching solution, using the titanium alloy product as an anode, applying a voltage, and forming a first hole on the surface of a titanium alloy component in the titanium alloy product to form a titanium alloy workpiece; wherein the etching solution comprises an organic liquid, a co-solvent, and a chloride; the chloride can dissociate into Cl in the co-solvent - , the organic liquid is miscible with the co-solvent; at least one of the first holes has an inner diameter larger than the hole diameter, and the first hole is in a necked shape.

[0022] In some embodiments, a second hole is further formed on the surface of the titanium alloy component, the second hole is located on the inner wall of the first hole, and the second hole is a radial spike structure.

[0023] In some embodiments, a second hole is further formed on the surface of the titanium alloy component, the second hole is located on the inner wall of the first hole, and the second hole has a coral-like structure.

[0024] In some embodiments, the titanium alloy component further includes aluminum, and the etching solution further includes an alkaline additive or an acidic additive; the alkaline additive or the acidic additive reacts with the aluminum element, and the Cl in the chloride - The first pore and the second pore are formed on the surface of the titanium alloy component by reacting with the titanium element in the titanium alloy component.

[0025] In some embodiments, when a voltage is applied, a current density in the range of 2 A / dm 2 -15A / dm 2 .

[0026] In some embodiments, the titanium alloy product also includes an aluminum alloy component. Before placing the titanium alloy product into the etching solution, the preparation method also includes placing the titanium alloy product into an electrolyte, using the titanium alloy product as an anode, and applying voltage to form an anodic oxide film on the aluminum alloy component of the titanium alloy product; wherein the electrolyte includes at least one of phosphoric acid, sulfuric acid, and oxalic acid, and the voltage ranges from 10V to 30V.

[0027] In some embodiments, the titanium alloy product also includes an aluminum alloy component. After placing the titanium alloy product into the etching solution, the preparation method further includes: placing the titanium alloy product into the etching solution to form a third hole in the aluminum alloy component of the titanium alloy product; wherein the third hole is coral-shaped, and the etching solution includes water, chloride and inorganic acid, the chloride concentration range is 10g / L-50g / L, and the inorganic acid concentration range is 10g / L-100g / L.

[0028] An etching solution for etching titanium alloy, comprising an organic liquid, a solvent and a chloride; wherein the chloride can dissociate into Cl in the solvent - To etch titanium alloy, the organic liquid is miscible with the flux.

[0029] In some embodiments, the co-solvent is water.

[0030] In some embodiments, the volume ratio of the organic liquid to the co-solvent ranges from 2:1 to 10:1.

[0031] In some embodiments, the dielectric constant of the organic liquid is in the range of 20-50.

[0032] In some embodiments, the organic liquid is selected from at least one of propylene glycol, glycerol, ethylene glycol, diethylene glycol, lactic acid and triethanolamine.

[0033] In some embodiments, the conductivity of the etching solution is in the range of 0.3 μS / cm-30 μS / cm.

[0034] In some embodiments, the chloride is selected from at least one of sodium chloride, ferric chloride, copper chloride and potassium chloride.

[0035] In some embodiments, the etching solution further includes a basic additive or an acidic additive, wherein the basic additive includes at least one of an inorganic base and an organic base; and the acidic additive includes at least one of an inorganic acid and an organic acid.

[0036] In some embodiments, the acidic additive includes oxalic acid, and the chloride dissociated in the co-solvent is Cl - The molar ratio of the oxalic acid is in the range of 1:1-5:1.

[0037] The surface of the titanium alloy workpiece provided in the present application has a first hole in a necked shape, which can increase the pulling force between the titanium alloy workpiece and the material body filled in the first hole, thereby increasing the bonding strength between the titanium alloy workpiece and the material body. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a cross-sectional picture taken with a Keyence laser microscope after a material body is formed in the first hole and the second hole on the surface of the titanium alloy substrate provided in one embodiment of the present application, magnified 200 times.

[0039] Figure 2A for Figure 1 The cross-sectional picture magnified 500 times is shown after a material body is formed in the first hole and the second hole on the surface of the titanium alloy substrate.

[0040] Figure 2B for Figure 1 The cross-sectional picture magnified 1000 times is shown after a material body is formed in the first hole and the second hole on the surface of the titanium alloy substrate.

[0041] Figure 3 A flow chart of a method for preparing a titanium alloy workpiece provided in some embodiments of the present application.

[0042] Figure 4This is a picture taken using a KEYENCE laser microscope, showing an embodiment of the present application in which a material body is formed in a first hole and a second hole, and then the material body is separated from a titanium alloy substrate, with the material body remaining in the hole.

[0043] Figure 5 for Figure 4 A magnified image of a certain area.

[0044] Figure 6 This is a tensile test diagram for testing the separation of the material body and the titanium alloy matrix.

[0045] Figure 7 This is a morphology test image of the first hole of corrosion on the titanium alloy surface according to an embodiment of the present application, taken using a white light interferometer.

[0046] Figure 8 For Figure 7 The depth diagram of the first hole tested along line segment AA in the test diagram shown is shown.

[0047] Fig. 9 For Figure 7 The depth diagram of the first hole tested along line segment BB in the test diagram shown is shown.

[0048] Fig.10 Based on Figure 8 and Fig. 9 The hole depth distribution map of the first hole is obtained by calculating the depth of the tested holes.

[0049] Fig.11 These are pictures of titanium alloy workpieces according to some embodiments of the present application taken using a KEYENCE laser microscope.

[0050] Fig.12 for Fig.11 An enlarged view of the titanium alloy substrate and the first hole formed on the surface of the titanium alloy substrate.

[0051] Fig.13 for Fig.11 An enlarged view of the aluminum alloy matrix and the third hole formed on the surface of the aluminum alloy matrix.

[0052] Fig.14 This is a picture of the first hole formed on the titanium alloy surface in Example 4-3 of the present application, taken using a Keyence laser microscope.

[0053] Fig.15 for Fig.14 A magnified image of a certain area.

[0054] Fig.16 This image was taken using a KEYENCE laser microscope. Fig.14 The picture shows a titanium alloy substrate and a material body being formed in a first hole of the titanium alloy substrate, followed by separation of the titanium alloy substrate and a material body remaining in the first hole.

[0055] Fig.17 This is a picture of the first hole formed on the titanium alloy surface in Example 5-2 of the present application, taken using a Keyence laser microscope.

[0056] Fig.18 for Fig.17 A magnified image of a certain area.

[0057] Fig.19 This image was taken using a KEYENCE laser microscope. Fig.17 The picture shows a titanium alloy substrate and a material body being formed in a first hole of the titanium alloy substrate, followed by separation of the titanium alloy substrate and a material body remaining in the first hole.

[0058] Main component symbols

[0059] Titanium alloy workpiece 100 Titanium alloy substrate 10 First hole 22 Second hole 24 Aluminum alloy substrate 30 The third hole 32 shell 200 material body 210 DETAILED DESCRIPTION

[0060] In order to more clearly understand the above-mentioned purposes, features and advantages of the present application, the present application is described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that, in the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other. In the following description, many specific details are set forth to facilitate a full understanding of the present application, and the described embodiments are only a part of the embodiments of the present application, rather than all of the embodiments.

[0061] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes all and any combination of one or more related listed items.

[0062] The present application provides an etching solution, which is used to etch titanium alloy during the process of applying voltage to form micropores of a certain shape on the surface of the titanium alloy.

[0063] The etching solution includes organic liquid, solvent and chloride.

[0064] The organic liquid is selected from substances that are miscible with the co-solvent. In some embodiments, the organic liquid can be selected from at least one of propylene glycol, glycerol, ethylene glycol, diethylene glycol, lactic acid, and triethanolamine. The organic liquid and the co-solvent are miscible, so that the etching solution is a uniform solution, so that the ions in the etching solution used to corrode the titanium alloy can be uniformly loaded on the surface of the titanium alloy.

[0065] The dielectric constant of the organic liquid is in the range of 20-50, so as to reduce the conductivity of the etching solution, thereby providing a stable environment for the formation of micropores on the surface of the titanium alloy during the etching process.

[0066] The auxiliary solvent is water, which is used to dissolve chloride so that chloride dissociates into Cl - , thereby etching the titanium alloy during the application of voltage.

[0067] Water can be water added to the etching solution alone, including ordinary water or deionized water; it can also be water produced by adding compounds containing crystal water to the etching solution. Water is used to dissociate chloride to produce Cl - .

[0068] The volume ratio of organic liquid to solvent is in the range of 2:1-10:1. The mass fraction of organic liquid to solvent has a great influence on the formation of pores. Among them, the appropriate volume ratio is conducive to the formation of pores with suitable pore diameter, pore depth and porosity. When the volume ratio is too large, that is, there is more organic liquid and less solvent, more chlorides used for corrosion cannot be dissolved; when the volume ratio is too small, that is, there is less organic liquid and more solvent, surface corrosion is caused on the surface of titanium alloy and pores of reasonable size cannot be formed.

[0069] Chloride is a compound that can dissociate into Cl in the cosolvent. - The substance can be selected from at least one of sodium chloride, ferric chloride, copper chloride and potassium chloride.

[0070] The conductivity range of the etching solution is 0.3μS / cm-30μS / cm. The conductivity range of the etching solution is small, that is, the resistance is large, which can generate a small current density during the application of voltage, so that the etching solution slowly corrodes the titanium alloy, preventing the current density from being too large, causing the reaction to be uncontrollable, and thus forming holes that do not meet production requirements.

[0071] The titanium alloy is electrochemically corroded in an organic environment. The organic environment system can provide a high-voltage and low-current corrosion environment, in which the Ti-O bond in the titanium alloy can be polarized, making it easy for the Cl - The chemical bonds are destroyed to form micropores of specific shapes. Figure 1 , Figure 2A and Figure 2B, a housing 200 is shown in the figure. The housing 200 is used for consumer electronic devices, including but not limited to consumer electronic products, power tools, drones, energy storage devices, power devices, etc. The housing 200 includes a titanium alloy workpiece 100 and a material body 210. The titanium alloy workpiece 100 is corroded to obtain a titanium alloy substrate 10 and a first hole 22 formed on the surface of the titanium alloy substrate 10. At least one of the first holes 22 has an inner diameter greater than the diameter of the hole mouth. The first hole 22 is necked, that is, the diameter of the first hole 22 gradually increases and then gradually decreases from the bottom of the hole to the hole mouth, thereby improving the pull-out force between the titanium alloy and the material body 210 subsequently formed in the first hole 22.

[0072] A second hole 24 is also formed on the surface of the titanium alloy. The second hole 24 is located on the inner wall of the first hole 22. The second hole 24 has a radial spike structure, that is, the second hole 24 is formed in a radial direction from the hole wall of the first hole 22 to the main body of the titanium alloy. The inner wall of the second hole 24 has an uneven spike structure, and the inner wall of the second hole 24 is a non-smooth inner wall. Under the dual effect of the necking structure of the first hole 22 and the radial spike structure of the inner wall of the second hole 24, the bonding between the titanium alloy and the material body 210 is stronger, and the pulling force between the titanium alloy and the material body 210 is further enhanced.

[0073] In some embodiments, the second hole 24 may also be in a coral-like structure, and the surface of the coral-like structure also has an uneven spike structure, which can enhance the bonding force between the titanium alloy and the material body 210.

[0074] In some embodiments, the titanium alloy further includes aluminum, and the etching solution further includes an alkaline additive or an acidic additive to make the titanium alloy - ) or acidic (H + ) environment. In the process of applying voltage, on the one hand, OH - or H + It can react with the aluminum oxide on the surface of the titanium alloy, which is beneficial to the formation of local small positive and negative areas on the surface of the titanium alloy and improve the morphological difference of the titanium alloy surface; on the other hand, during the electrochemical corrosion process, OH - or H + It will corrode the titanium-aluminum grain boundary and accelerate the etching reaction.

[0075] The alkaline additive may include at least one of an inorganic base and an organic base. The inorganic base may be sodium hydroxide, potassium hydroxide, etc., and the organic base may be sodium methoxide, potassium ethoxide, potassium tert-butoxide, etc.

[0076] The acidic additive may include at least one of an inorganic acid and an organic acid. The inorganic acid may be hydrochloric acid, sulfuric acid, phosphoric acid, etc., and the organic acid may be citric acid, oxalic acid, etc.

[0077] In some embodiments, the acidic additive is oxalic acid, which can be an oxalic acid compound added to the etching solution, or can be provided by oxalate and inorganic acid, such as adding sodium oxalate and sulfuric acid to the etching solution to form oxalic acid. - The molar ratio of oxalic acid to oxalic acid is in the range of 1:1-5:1. This is because oxalic acid dissociates into oxalate ions in the etching solution, and the oxalate ions react with titanium in the titanium alloy to generate titanium oxalate that is soluble in water, thereby further accelerating the reaction between the etching solution and the titanium element in the titanium alloy, thereby helping to form the first hole 22 with a larger hole depth.

[0078] See also Figure 3 The present application also provides a method for preparing a titanium alloy workpiece 100, comprising the following steps:

[0079] Step S1: sandblasting the titanium alloy product to remove the oxide film on the surface of the titanium alloy product and to form micropores on the surface of the titanium alloy product to increase the surface roughness of the titanium alloy product.

[0080] The material for sandblasting can be selected from aluminum oxide, zirconium oxide, iron oxide, etc.

[0081] In some embodiments, the particle size of the material is 80 μm-120 μm, the pressure is 0.15 MPa-0.3 MPa, and the time is 20 s-60 s. It is understandable that the above-mentioned sandblasting parameters can be adjusted as needed and are not limited thereto.

[0082] The size of the micropores formed during the sandblasting process is related to the parameters during the sandblasting process, and the sandblasting parameters can be adjusted as needed.

[0083] After the sandblasting process, the titanium alloy is cleaned to remove impurities such as oil, oxides, etc. on the surface of the titanium alloy, which is conducive to the smooth progress of the etching reaction.

[0084] Step S2: Put the titanium alloy product after sandblasting into the etching solution, use the titanium alloy product as the anode, apply voltage, and form the first hole 22 on the surface of the titanium alloy part in the titanium alloy product to form the titanium alloy workpiece 100, and the remaining titanium alloy is the titanium alloy matrix 10. The etching solution includes an organic liquid, a solvent and a chloride. The chloride can dissociate into Cl in the solvent. - , the organic liquid and the co-solvent are miscible.

[0085] During the voltage application process, the etching liquid etches the micropores formed during the sandblasting process to form the first hole 22. The first hole 22 has at least one hole with an inner diameter larger than the hole opening diameter, and the first hole 22 is in a necked shape.

[0086] In some embodiments, when a voltage is applied, a current density in the range of 2 A / dm 2 -15A / dm 2 Avoid too high current density, which will cause uncontrollable etching reaction; also avoid too low current density, which will cause too slow etching rate and reduce production efficiency.

[0087] In some embodiments, the applied voltage ranges from 15V to 40V; the temperature range of the etching solution ranges from 40°C to 80°C; and the voltage application time ranges from 5min to 60min. The above is only an example, but not a limitation.

[0088] Furthermore, in some embodiments, by increasing the time of applying voltage (for example, more than 10 minutes), a second hole 24 can be formed on the surface of the first hole 22, and the second hole 24 is located on the inner wall of the first hole 22, and the second hole 24 is a radial spike structure or a coral-like structure. The shapes of the first hole 22 and the second hole 24 are related to the elements in the titanium alloy, the composition of the etching solution, and the etching parameters. The second hole 24 is a small hole, which is mainly caused by the composition and structure of the titanium alloy part itself, and involves the metastable form of the corrosion hole. Since the inner wall of the first hole 22 is not smooth, when the etching time is increased, the oxygen content in the inner wall part of the first hole 22 is low, which is conducive to the anodic dissolution of titanium. In addition, Cl in the inner wall part of the first hole 22 - Will aggregate, resulting in Cl - The increase in concentration further facilitates corrosion, thereby forming radial or coral-shaped second holes 24 .

[0089] The type of titanium alloy is not limited and can be selected from Ti-6Al-4V, Ti-5Al-2.5Sn, Ti-2Al-2.5Zr, etc. The type of titanium alloy can be selected according to the use environment of the titanium alloy workpiece 100. Taking the titanium alloy type Ti-6Al-4V as an example, the titanium alloy also includes aluminum elements.

[0090] In some embodiments, the titanium alloy component further includes aluminum, and the etching solution further includes an alkaline additive or an acidic additive; the alkaline additive or the acidic additive reacts with the aluminum element, and the Cl in the chloride - The titanium alloy component reacts with the titanium element in the titanium alloy component to form the first pores 22 and the second pores 24 on the surface of the titanium alloy component.

[0091] In some embodiments, the titanium alloy product further includes an aluminum alloy component, the aluminum alloy component is connected to the titanium alloy component, and before the titanium alloy product is sandblasted, the preparation method further includes:

[0092] Step S0: placing the titanium alloy product into an electrolyte, using the titanium alloy product as an anode, and applying voltage to form an anodic oxide film on the aluminum alloy component of the titanium alloy product.

[0093] In some embodiments, the electrolyte includes at least one of phosphoric acid, sulfuric acid, and oxalic acid, the concentration of the electrolyte ranges from 100 g / L to 200 g / L, the voltage ranges from 10 V to 30 V, and the treatment time is from 5 min to 30 min. The thickness of the anodized film on the surface of the aluminum alloy part is from 15 μm to 20 μm.

[0094] In the step of forming an anodic oxide film on the surface of the aluminum alloy part, an anodic oxide film will also be formed on the surface of the titanium alloy part. Since the chemical stability of the titanium alloy is better than that of the aluminum alloy, the anodic oxide film formed on the surface of the titanium alloy part is thinner than the anodic oxide film on the surface of the aluminum alloy part. Before the subsequent sandblasting process, the anodic oxide film on the surface of the aluminum alloy part will be shielded to prevent the anodic oxide film on the surface of the aluminum alloy part from being damaged during the sandblasting process. It should be noted that during the sandblasting process, the anodic oxide film formed on the surface of the titanium alloy will be destroyed, so as to facilitate the titanium alloy part to form the first hole 22 in the etching step.

[0095] In some embodiments, after the anodizing step and before the sandblasting step, the anodized film formed on the surface of the aluminum alloy component is shielded with a rubber plug to prevent the anodized film formed on the surface of the aluminum alloy component from being damaged during the sandblasting process. After the sandblasting, the rubber plug is removed.

[0096] In some embodiments, after placing the titanium alloy product into the etching solution, the preparation method further comprises:

[0097] Step S3: placing the titanium alloy product in a corrosive solution to form a third hole in the aluminum alloy component of the titanium alloy product, wherein the third hole is coral-shaped, the corrosive solution comprises water, chloride and inorganic acid, the concentration range of the chloride is 10g / L-50g / L, and the concentration range of the inorganic acid is 10g / L-100g / L.

[0098] It should be noted that, after the titanium alloy component is etched, a titanium alloy matrix is ​​formed, and after the aluminum alloy component is etched, an aluminum alloy matrix is ​​formed.

[0099] Please refer again Figure 1 , Figure 2A and Figure 2B , is a cross-sectional schematic diagram of forming a material body 210 in a first hole 22 of an etched titanium alloy (i.e., a titanium alloy substrate 10) according to an embodiment of the present application. The first hole 22 has at least one hole inner diameter greater than the hole opening diameter, and the first hole 22 is in a necked shape.

[0100] In some embodiments, Figure 1 As shown, the titanium alloy substrate 10 also has a second hole 24, which is located on the inner wall of the first hole 22 (large hole). The second hole 24 (small hole) is a radial spike structure or a coral shape, that is, a large hole covers a small hole, which can increase the contact area between the titanium alloy substrate 10 and the material body 210 subsequently formed in the first hole 22, and increase the pull-out force between the titanium alloy substrate 10 and the material body 210; and the second hole 24 is radial, that is, the direction of the second hole 24 is anisotropic, which further increases the pull-out force between the titanium alloy substrate 10 and the material body 210. It should be noted that Figure 1 , Figure 2A and Figure 2B It is a cross-sectional view of the titanium alloy after etching. Although in the cross-sectional view, the first hole 22 and part of the second hole 24 form a straight hole from top to bottom, due to the different positions of the cross-section, the actual projection of the first hole 22 opening does not necessarily fall on the opening of part of the second hole 24. Therefore, when the white light interferometer tests the hole depth of the first hole 22, it will not be affected by the depth of the second hole 24.

[0101] See also Figures 4 to 5 , which is a test diagram of an embodiment of the present application in which the material body 210 is formed in the first hole 22 and then separated from the titanium alloy substrate 10, and the material body 210 remains in the first hole 22. Figure 5 It can be seen that a large amount of material body 210 remains in the first hole 22 , which proves that the bonding force between the material body 210 and the titanium alloy substrate 10 is strong. Figure 6 The tensile force data used to separate the material body 210 from the titanium alloy substrate 10. It can be seen from the tensile force data that, compared with the conventional 20 MPa, the tensile force data in this embodiment is much higher than 20 MPa. Figure 5 and Figure 6 It can be seen that during the tensile test, due to the neck-shaped structure of the first hole 22 on the titanium alloy substrate 10, the bonding force between the material body 210 and the titanium alloy substrate 10 is relatively strong, and the tensile force value when the material body 210 and the titanium alloy substrate 10 are separated is close to the fracture strength of the material body 210 itself, resulting in the tensile force data between the material body 210 and the titanium alloy substrate 10 being much higher than 20 MPa. In addition, due to the neck-shaped structure of the first hole 22, most of the material body 210 in the first hole 22 can remain in the first hole 22 when the main body of the material body 210 is separated from the titanium alloy substrate 10.

[0102] The hole depth of the first hole 22 ranges from 20μm to 70μm; the median range of the hole depth of the first hole 22 ranges from 35μm to 60μm; the porosity of the first hole 22 ranges from 30% to 60%. Compared with conventional methods, the hole depth, the hole diameter and the moderate porosity formed on the titanium alloy surface by the above preparation method are deeper, larger and more moderate, which is conducive to forming a PA glue (a single-component nylon special glue with a polyethylene polymer as the main body) with low fluidity and high strength in the first hole 22, thereby improving the application range of the titanium alloy substrate 10. In addition, the etching solution used in the above preparation method does not contain fluorine components, and the etching environment is mild and green and environmentally friendly.

[0103] See also Figures 7 to 10 , is a titanium alloy workpiece 100 after the titanium alloy is etched by the above preparation method in some embodiments of the present application, and a white light interferometer is used to test the hole depth distribution of the first hole 22 of the titanium alloy surface corrosion, wherein, from Fig.10 It can be seen that uniformly distributed first holes 22 are formed on the surface of the titanium alloy. From the test results of the hole depth, it can be seen that the hole depths of the first holes 22 in this embodiment are mostly distributed in the range of 30 μm-60 μm. It should be noted here that the white light interferometer can only measure straight holes, so the depth of the first hole 22 is mainly measured, rather than the depth of the first hole 22 plus the second hole 24.

[0104] See also Figure 11-13 In some embodiments, the titanium alloy workpiece further comprises an aluminum alloy substrate 30, and the aluminum alloy substrate 30 is connected to the titanium alloy substrate 10 (see Figure 11). The surface of the titanium alloy substrate 10 is provided with a first hole 22 (see Figure 12). Fig.12 ), the aluminum alloy substrate 30 is provided with a third hole 32 on its surface (see Fig.13 ), the third hole 32 is a coral-like structure, and the third hole 32 is used to set the material body 210.

[0105] The embodiment of the present application provides a titanium alloy workpiece 100, which includes a titanium alloy substrate 10 and a first hole 22 disposed on the titanium alloy substrate 10. The first hole 22 has at least one inner diameter that is larger than the hole diameter, and the first hole 22 is in a necked shape.

[0106] The titanium alloy substrate 10 is formed by etching the titanium alloy.

[0107] See also Figure 1 , Figure 2A and Figure 2B The present application also provides a housing 200, which is used for electronic devices, including but not limited to consumer electronic products (such as mobile communication devices, tablet computers, laptop computers, wearable devices, etc.), power tools, drones, energy storage devices, power devices, etc.

[0108] The housing 200 includes the titanium alloy workpiece 100 and a material body 210, and the material body 210 is disposed in the first hole 22. The material body 210 may be selected from at least one of metal, polymer, ceramic and glass.

[0109] The present application is described below through specific examples and comparative examples. It should be noted that the titanium alloy is first subjected to a cleaning step before electrochemical etching to remove impurities such as oil stains and oxides on the surface of the titanium alloy.

[0110] The specific cleaning steps include: placing the titanium alloy in a degreasing agent R100 with a temperature of 55°C and a concentration of 50g / L for degreasing treatment for 5 minutes, then washing with water and drying; then spraying aluminum oxide with a particle size of 100μm for sandblasting, wherein the pressure of the spray gun is 0.2MPa and the time is 60s; after ultrasonic water washing at 80Hz for 5 minutes, soaking in sulfuric acid at room temperature for 5 minutes; then washing with water and drying, thereby completing the cleaning steps.

[0111] The cleaned titanium alloy is etched, and the etching steps include: providing a cleaned titanium alloy, placing it in an etching solution, using the titanium alloy as an anode, applying voltage, and forming a first hole 22 on the surface of the titanium alloy to form a titanium alloy workpiece 100.

[0112] The titanium alloy workpiece 100 formed after etching is tested, including tests on hole depth, hole diameter and porosity. In addition, a tensile test is also included. The tensile test step includes forming a material body 210 (PA glue) in the first hole 22 of the titanium alloy workpiece 100, and testing the tensile force required to separate the titanium alloy substrate 10 and the material body 210, thereby detecting the pull-out force between the titanium alloy substrate 10 and the material body 210.

[0113] Example 1-1

[0114] The etching solution includes 85% ethylene glycol (organic liquid), 3% sodium chloride (chloride), 10% deionized water (solvent) and 2% oxalic acid (additive) by mass; the current density is 10A / dm 2 , etching temperature is 60min, and etching time is 40min.

[0115] Example 1-2

[0116] The difference from Example 1-1 is that the organic liquid in the etching solution is diethylene glycol.

[0117] Examples 1-3

[0118] The difference from Example 1-1 is that the organic liquid in the etching solution is propylene glycol.

[0119] Examples 1-4

[0120] The difference from Example 1-1 is that the organic liquid in the etching solution is propylene glycol.

[0121] Examples 1-5

[0122] The difference from Example 1-1 is that the organic liquid in the etching solution is lactic acid.

[0123] Examples 1-6

[0124] The difference from Example 1-1 is that the organic liquid in the etching solution is triethanolamine.

[0125] Comparative Example 1-1

[0126] The difference from Example 1-1 is that the etching solution contains 95% deionized water, 3% sodium chloride and 2% oxalic acid, that is, Comparative Example 1 does not contain an organic liquid.

[0127] Please refer to Table 1 for the main differences in conditions and corresponding test results between Examples 1-1 to 1-6 and Comparative Example 1-1.

[0128] Table 1

[0129]

[0130] From the data in Table 1, it can be seen that the etching solutions of Examples 1-1 to 1-6 all contain organic liquids compared to Comparative Example 1-1, while the etching solution provided in Comparative Example 1-1 does not contain organic liquids, resulting in that Comparative Example 1-1 cannot form the first hole 22 on the titanium alloy surface under the same etching conditions as Examples 1-1 to 1-6, indicating that the organic liquid can provide a stable environment for etching the titanium alloy. Compared with Examples 1-1 to 1-6, the pore diameter, pore depth and porosity of the first pore 22 formed by etching solutions containing different types of organic liquids have certain differences.

[0131] Example 2-1

[0132] The etching solution includes 85% propylene glycol (organic liquid), 4% sodium chloride (chloride), 10% deionized water (solvent) and 1% oxalic acid (additive) by mass fraction; the current density is 5A / dm 2 , etching temperature is 80min, and etching time is 20min.

[0133] Example 2-2

[0134] The difference from Example 2-1 is that the organic liquid in the etching solution is 75% propylene glycol, and the co-solvent is 20% deionized water.

[0135] Example 2-3

[0136] The difference from Example 2-1 is that the organic liquid in the etching solution is 65% propylene glycol, and the co-solvent is 30% deionized water.

[0137] Comparative Example 2-1

[0138] The difference from Example 2-1 is that the organic liquid in the etching solution is 55% propylene glycol, and the co-solvent is 40% deionized water.

[0139] Comparative Example 2-2

[0140] The difference from Example 2-1 is that the organic liquid in the etching solution is 95% propylene glycol and does not contain a solvent.

[0141] Please refer to Table 2, which shows the main differences between Examples 2-1 to 2-3 and Comparative Examples 2-1 to 2-2 and the corresponding test results.

[0142] Table 2

[0143]

[0144] From the data in Table 2, it can be seen that by comparing Examples 2-1 to 2-3 with Comparative Examples 2-1 to 2-2, the mass fractions of the organic liquid and the co-solvent have a great influence on the formation of the first pore 22. Among them, the greater the mass fraction of the organic liquid and the smaller the mass fraction of the co-solvent, the smaller the pore size, the greater the pore depth, and the greater the porosity, and thus the greater the pulling force separating the titanium alloy substrate 10 and the material body 210. This is because the co-solvent is conducive to the dissolution of chloride used for corrosion. When the mass fraction of the co-solvent is too large (Comparative Example 2-1), it causes surface corrosion on the titanium alloy surface and fails to form the first pore 22 of reasonable size. When there is no co-solvent, since the chloride cannot dissociate in the co-solvent to produce a large amount of Cl for corrosion of the titanium alloy, the first pore 22 of reasonable size cannot be formed. - In Comparative Example 2, since the etching solution contains a large amount of organic solvent but no co-solvent, the movement speed of ions in the organic system is too slow, resulting in a decrease in the corrosiveness of the etching solution, and no pores can be formed on the titanium alloy, that is, the surface of the titanium alloy does not change significantly.

[0145] Example 3-1

[0146] The etching solution includes 80% by mass of diethylene glycol (organic liquid), 10% of deionized water (cosolvent), and 10% of sodium chloride (chloride) and oxalic acid (additive), wherein the molar ratio of sodium chloride to oxalic acid is 3:1; the current density is 12A / dm 2 , etching temperature is 50min, and etching time is 10min.

[0147] Example 3-2

[0148] The difference from Example 3-1 is that the molar ratio of sodium chloride to oxalic acid is 2:1.

[0149] Example 3-3

[0150] The difference from Example 3-1 is that the molar ratio of sodium chloride to oxalic acid is 1:1.

[0151] Comparative Example 3-1

[0152] The difference from Example 3-1 is that the molar ratio of sodium chloride to oxalic acid is 1:2.

[0153] Please refer to Table 3 for the main differences in conditions and corresponding test results between Examples 3-1 to 3-3 and Comparative Example 3-1.

[0154] Table 3

[0155]

[0156] It can be seen from the data in Table 3 that an appropriate molar ratio of chloride to additive is conducive to adjusting the pore size, pore depth and porosity of the first pores 22 formed, so as to improve the pulling force between the titanium alloy substrate 10 and the material body 210. If the molar ratio of chloride to additive is too small, that is, the content of chloride is too small, Cl - The corrosion ability of the reaction tank is reduced, and the number of effective first holes 22 formed is reduced; the molar ratio of chloride to additive is too large, that is, the chloride content is too much, which will cause surface corrosion. The presence of oxalic acid can control the acidity of the reaction tank solution, and at the same time can complex free titanium to stabilize the reaction tank solution and promote the progress of the etching reaction.

[0157] Example 4-1

[0158] The etching solution includes 85% lactic acid (organic liquid), 10% deionized water (solvent) and 5% ferric chloride (chloride); the current density is 15A / dm 2 , etching temperature is 40min, and etching time is 30min.

[0159] Example 4-2

[0160] The difference from Example 4-1 is that citric acid (acidic additive) is further added to the etching solution, so that the mass fraction of citric acid in the etching solution is 1%, and the mass fraction of deionized water in the etching solution is 10%.

[0161] Example 4-3

[0162] The difference from Example 4-1 is that citric acid is further added to the etching solution, so that the mass fraction of citric acid in the etching solution is 2%, and the mass fraction of deionized water in the etching solution is 10%.

[0163] Please refer to Table 4 for the main differences in conditions between Examples 4-1 to 4-3 and the corresponding test results.

[0164] Table 4

[0165]

[0166] It can be seen from the data in Table 4 that adding a certain amount of acidic additives to the etching solution is beneficial to increasing the hole depth of the first hole 22, thereby increasing the pulling force between the titanium alloy substrate 10 and the material body 210; but too much acidic additive will cause the local pore size to be too large, the porosity to decrease, and the pulling force to decrease.

[0167] See also Fig.14 and Fig.15 , is a picture of the first hole 22 formed on the titanium alloy surface in Example 4-3 of the present application taken using a Keyence laser microscope, wherein: Fig.14 For the picture magnified 30 times, Fig.15 The image is magnified 200 times. Fig.16 , for Fig.14 The picture shows a titanium alloy substrate 10 and a material body 210 being separated after a material body 210 is formed in the first hole 22 of the titanium alloy, and a material body 210 remaining in the first hole 22 .

[0168] Example 5-1

[0169] The etching solution includes 75% triethanolamine (organic liquid), 20% deionized water (solvent) and 5% sodium chloride (chloride); the current density is 15A / dm 2 , etching temperature is 45min, and etching time is 30min.

[0170] Example 5-2

[0171] The difference from Example 5-1 is that sodium hydroxide (alkaline additive) is further added to the etching solution, so that the mass fraction of sodium hydroxide in the etching solution is 4%, and the mass fraction of deionized water in the etching solution is 20%.

[0172] Example 5-3

[0173] The difference from Example 5-1 is that sodium hydroxide (alkaline additive) is further added to the etching solution, so that the mass fraction of sodium hydroxide in the etching solution is 8%, and the mass fraction of deionized water in the etching solution is 20%.

[0174] Please refer to Table 5 for the main differences in conditions between Examples 5-1 to 5-3 and the corresponding test results.

[0175] Table 5

[0176]

[0177] It can be seen from the data in Table 5 that adding a certain amount of alkaline additives to the etching solution is beneficial to increasing the hole depth of the first hole 22, thereby increasing the pulling force between the titanium alloy substrate 10 and the material body 210; but too much acidic additives will cause the local pore size to be too large, the porosity to decrease, and the pulling force to decrease.

[0178] See also Fig.17 and Fig.18 , is a picture of the first hole 22 formed on the titanium alloy surface in Example 5-2 of the present application taken using a Keyence laser microscope, wherein: Fig.17 For the picture magnified 30 times, Fig.18 The image is magnified 200 times. Fig.19 , for Fig.17 The picture shows that after the material body 210 is formed in the first hole 22 of the titanium alloy, the titanium alloy substrate 10 and the material body 210 are separated, and the material body 210 remains in the first hole 22 .

[0179] The surface of the titanium alloy workpiece 100 provided in the present application has a first hole 22 in a necked shape, which can increase the pulling force between the titanium alloy workpiece 100 and the material body 210 filled in the first hole 22 , thereby increasing the bonding strength between the titanium alloy workpiece 100 and the material body 210 .

[0180] The above implementation modes are only used to illustrate the technical solutions of the present application and are not intended to limit the present application. Although the present application has been described in detail with reference to the above preferred implementation modes, a person skilled in the art should understand that the technical solutions of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present application.

Claims

1. A method for preparing a titanium alloy workpiece, comprising: Providing a titanium alloy product, wherein the titanium alloy product comprises a titanium alloy component and an aluminum alloy component; placing the titanium alloy product in an electrolyte, using the titanium alloy product as an anode, and applying voltage to form an anodic oxide film on the aluminum alloy part of the titanium alloy product; Sandblasting titanium alloy products; The titanium alloy product subjected to sandblasting is placed in an etching solution, and a voltage is applied with the titanium alloy product as an anode to form a first hole on the surface of the titanium alloy component in the titanium alloy product. The etching solution includes an organic liquid, a cosolvent and a chloride; the chloride can dissociate into Cl in the cosolvent. - , the organic liquid is miscible with the co-solvent, and the organic liquid is selected from at least one of propylene glycol, glycerol, ethylene glycol, diethylene glycol, lactic acid and triethanolamine; the first hole has at least one hole with an inner diameter larger than the hole diameter, and the first hole is in a necked shape; and The titanium alloy product is placed in a corrosive solution to form a third hole on the surface of the aluminum alloy component.

2. The preparation method according to claim 1, wherein A second hole is also formed on the surface of the titanium alloy component. The second hole is located on the inner wall of the first hole, and the second hole is a radial spike structure.

3. The preparation method according to claim 1, wherein A second hole is also formed on the surface of the titanium alloy component. The second hole is located on the inner wall of the first hole and has a coral-like structure.

4. The preparation method according to claim 2 or 3, wherein The titanium alloy component also includes aluminum, and the etching solution also includes an alkaline additive or an acidic additive; the alkaline additive or the acidic additive reacts with the aluminum, and Cl in the chloride - The first pore and the second pore are formed on the surface of the titanium alloy component by reacting with the titanium element in the titanium alloy component.

5. The preparation method according to claim 1, wherein When voltage is applied, the current density generated is in the range of 2A / dm 2 -15A / dm 2 .

6. The preparation method according to claim 1, wherein The electrolyte includes at least one of phosphoric acid, sulfuric acid, and oxalic acid, and the voltage ranges from 10V to 30V.

7. The preparation method according to claim 1, wherein The third hole is coral-shaped, and the corrosive liquid includes water, chloride and inorganic acid. The concentration range of the chloride is 10g / L-50g / L, and the concentration range of the inorganic acid is 10g / L-100g / L.

8. The preparation method according to claim 1, wherein The co-solvent is water.

9. The preparation method according to claim 1, wherein The volume ratio of the organic liquid to the co-solvent is in the range of 2:1-10:

1.

10. The preparation method according to claim 1, wherein: The dielectric constant of the organic liquid is in the range of 20-50.

11. The preparation method according to claim 1, wherein: The conductivity of the etching solution ranges from 0.3 μS / cm to 30 μS / cm.

12. The preparation method according to claim 1, wherein: The chloride is selected from at least one of sodium chloride, ferric chloride, copper chloride and potassium chloride.

13. The preparation method according to claim 1, wherein The etching solution further includes an alkaline additive or an acidic additive. The alkaline additive includes at least one of an inorganic base and an organic base; the acidic additive includes at least one of an inorganic acid and an organic acid.

14. The preparation method according to claim 13, wherein: The acidic additive includes oxalic acid, and the chloride dissociated in the co-solvent - The molar ratio of the oxalic acid is in the range of 1:1-5:

1.

15. A titanium alloy workpiece prepared by the method for preparing a titanium alloy workpiece according to any one of claims 1 to 14, the titanium alloy workpiece comprising: A titanium alloy substrate and a first hole disposed on the titanium alloy substrate; as well as An aluminum alloy substrate, the aluminum alloy substrate is connected to the titanium alloy substrate, and a third hole is arranged on the surface of the aluminum alloy substrate; Among them, at least one of the first holes has an inner diameter that is larger than the hole opening diameter, and the first hole is in a necked shape.

16. The titanium alloy workpiece according to claim 15, wherein: A second hole is also arranged on the titanium alloy substrate. The second hole is located on the inner wall of the first hole and has a radial spike structure.

17. The titanium alloy workpiece according to claim 15, wherein: A second hole is also arranged on the titanium alloy substrate. The second hole is located on the inner wall of the first hole and has a coral-like structure.

18. The titanium alloy workpiece according to claim 15, wherein: The titanium alloy matrix includes aluminum elements.

19. The titanium alloy workpiece according to claim 15, wherein: The first holes have a hole depth ranging from 20 μm to 70 μm.

20. The titanium alloy workpiece according to claim 15, wherein: The median value of the pore depth of the first pores ranges from 35 μm to 60 μm.

21. The titanium alloy workpiece according to claim 15, wherein: The porosity of the first pores is in the range of 30%-60%.

22. The titanium alloy workpiece according to claim 15, wherein: The third hole is coral-shaped.

23. A housing for an electronic device, comprising: The titanium alloy workpiece according to claim 15; as well as material body; The material body is disposed in the first hole and the third hole.

24. The housing of claim 23, wherein: A second hole is also arranged on the titanium alloy substrate. The second hole is located on the inner wall of the first hole. The second hole is in a radial spike structure. The material body is arranged in the second hole.

25. The housing of claim 23, wherein: A second hole is also arranged on the titanium alloy substrate. The second hole is located on the inner wall of the first hole. The second hole is in a coral-like structure. The material body is arranged in the second hole.

26. The housing of claim 23, wherein: The titanium alloy matrix includes aluminum elements.

27. The housing of claim 23, wherein: The material of the material body is selected from at least one of metal, polymer, ceramic and glass.

28. The housing of claim 23, wherein: The first holes have a hole depth ranging from 20 μm to 70 μm.

29. The housing of claim 23, wherein: The porosity of the first pores is in the range of 30%-60%.

30. The housing of claim 23, wherein: The third hole has a coral-like structure.

Citation Information

Patent Citations

  • Compositions and methods for selective removal of metal or metal alloy after metal silicide formation

    CN101233601A

  • Metal part, metal product and method for manufacturing metal part

    CN111188081A

  • Metal product, preparation method for metal product, metal complex and preparation method for metal complex

    CN112342604A