Deep blue photoelectroluminescent device based on gold-silver cluster complex and preparation method thereof
By using gold cluster complexes or gold-silver cluster complexes with diphenyl-2-pyridylphosphine as the ligand as the luminescent layer material, electroluminescent devices are prepared by vacuum evaporation method, which solves the difficulty of achieving deep blue in the existing technology. The problem of light emission achieves efficient deep blue light emitting performance.
Patent Information
- Application Number
- CN202210590579.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-05-27
AI Technical Summary
It is difficult for existing metal cluster compounds to achieve deep blue light emission, which limits their application in the OLED field.
Gold cluster complexes or gold-silver cluster complexes constructed with diphenyl-2-pyridylphosphine as ligands are used as the guest materials of the light-emitting layer, and electroluminescent devices are prepared by vacuum evaporation to achieve deep blue emission.
The electroluminescent device achieves deep blue luminescence with good thermal stability and comprehensive performance. The brightness can reach 80-88cd/m2, the current efficiency and power efficiency are excellent, and the external quantum efficiency reaches 0.34%-0.35%.
Smart Images

Figure CN115117264B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electroluminescence, and in particular relates to a deep blue light electroluminescent device based on a gold-silver cluster complex and a preparation method thereof. Background Art
[0002] Organic light-emitting diodes (OLEDs) are increasingly being used in people's lives, replacing traditional flat-panel displays. Moreover, the shift from rigid to flexible displays has accelerated the market shift from LCDs to OLEDs. However, in order to expand the use of OLEDs, some key issues must be addressed, among which the development of new luminescent materials for OLEDs is one of the most important issues.
[0003] As potential phosphorescent guest materials for OLEDs, metal cluster compounds show some favorable properties. Due to the presence of multiple heavy metal atoms, the spin-orbit coupling effect is significantly enhanced, and the intersystem crossing from the singlet state to the triplet state is very efficient. In addition, the intramolecular metal-metal interaction with energy comparable to that of hydrogen bonds not only enhances the molecular rigidity to improve the phosphorescence efficiency of the metal cluster species, but also improves the structural stability to resist energy loss from heat and radiation. Gold and silver clusters have been reported many times as the light-emitting layer of OLEDs, but the luminescent color is mainly concentrated in the yellow-green light region, and there is little research in the deep blue light region. For example, in 2015, Chen Zhongning's team reported a series of Au4Ag2 clusters and prepared electroluminescent devices using spin coating devices with an emission wavelength in the range of 482-550nm. They also reported a series of Au8Ag in 2020. 10 Clusters were also prepared by spin coating to prepare electroluminescent devices with emission wavelengths in the range of 520-556nm. Previous studies have shown that the luminescence properties of metal clusters have obvious structural dependence. The larger the metal core particle size, the smaller the band gap, causing the emission wavelength to red shift; conversely, the band gap of low-core metal clusters is larger and the emission wavelength is shorter. However, at present, it is still difficult for metal cluster compounds to achieve deep blue light emission, and new metal cluster compound luminescent materials need to be further developed to expand their application in the OLED field. Summary of the invention
[0004] In order to solve the above problems, the present invention provides an electroluminescent device prepared by using a metal cluster complex containing gold and silver as a guest material of a light-emitting layer. The metal cluster complex containing gold and silver is a gold cluster complex or a gold-silver cluster complex constructed with diphenyl-2-pyridylphosphine as a ligand. The metal cluster complex has good thermal stability. When used as a guest light-emitting material, the peak of the electroluminescent spectrum is 430-450nm, and the deep blue light emission of the electroluminescent device is achieved, thereby completing the present invention.
[0005] The object of the present invention is to provide a deep blue photoelectroluminescent device based on a gold-silver cluster complex, wherein the guest material of the light-emitting layer of the device is one or more of a gold cluster complex and a gold-silver cluster complex, preferably [O(AuPPh2py)3]BF4 and / or [O(AuPPh2py)3Ag](BF4)2, and more preferably [O(AuPPh2py)3]BF4 or [O(AuPPh2py)3Ag](BF4)2.
[0006] In the light-emitting layer material, the mass fraction of the guest material is 0.2%-1.2%, preferably 0.3%-0.9%, and more preferably 0.4%-0.6%.
[0007] The present invention also aims to provide a method for preparing the deep blue light electroluminescent device based on the gold-silver cluster complex, which specifically comprises the following steps:
[0008] 1. preparing a conductive anode layer;
[0009] 2. preparing a hole injection layer by evaporating the hole injection layer on the anode conductive layer;
[0010] 3. preparing a hole transport layer, and evaporating the hole transport layer on the hole injection layer;
[0011] 4. preparing an electron blocking layer, wherein the electron blocking layer is evaporated on the hole transport layer;
[0012] 5. preparing a light-emitting layer, wherein the light-emitting layer is evaporated on the electron blocking layer;
[0013] 6. preparing a hole blocking layer, wherein the hole blocking layer is evaporated on the light-emitting layer;
[0014] 7. preparing an electron transport layer, wherein the electron transport layer is evaporated on the hole blocking layer;
[0015] 8. preparing an electron injection layer, wherein the electron injection layer is evaporated on the electron transport layer;
[0016] 9. Prepare a cathode conductive layer, encapsulate, and obtain a thermally excited delayed fluorescence electroluminescent device, wherein the cathode conductive layer is evaporated on the electron injection layer.
[0017] The deep blue light electroluminescent device based on the gold-silver cluster complex provided by the present invention has the following beneficial effects:
[0018] (1) In the present invention, a deep blue luminescent electroluminescent device is prepared by using a thermally stable gold cluster complex or a gold-silver cluster complex as the guest material of the light-emitting layer.
[0019] (2) Since the gold cluster complex or the gold-silver cluster complex has good thermal stability, the present invention successfully achieved the successful preparation of the device by vacuum evaporation. Unlike the spin coating device, the vacuum evaporation device has better film forming properties and is more stable.
[0020] (3) The electroluminescent device prepared in the present invention has an emission wavelength of 440 nm, exhibiting deep blue light emission.
[0021] (4) The electroluminescent device prepared by vacuum evaporation method of the present invention can reach a brightness of 80-88 cd / m 2 , the current efficiency can reach 0.42-0.45mA / cm 2 The power efficiency can reach 0.23-0.25lm / W, the external quantum efficiency is 0.34%-0.35%, it has good luminescence performance, good comprehensive performance, and is conducive to practical application. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The thermogravimetric analysis spectrum of [O(AuPPh2py)3]BF4 prepared in Example 1 of the present invention is shown;
[0023] Figure 2 The thermogravimetric analysis spectrum of [O(AuPPh2py)3Ag](BF4)2 prepared in Example 2 of the present invention is shown;
[0024] Figure 3 The voltage-current density relationship curve of the electroluminescent device prepared based on [O(AuPPh2py)3]BF4 in Example 3 of the present invention is shown;
[0025] Figure 4 The voltage-current density relationship curve of the electroluminescent device prepared based on [O(AuPPh2py)3Ag](BF4)2 in Example 4 of the present invention is shown;
[0026] Figure 5 The voltage-brightness relationship curve of the electroluminescent device prepared based on [O(AuPPh2py)3]BF4 in Example 3 of the present invention is shown;
[0027] Figure 6 The voltage-brightness relationship curve of the electroluminescent device prepared based on [O(AuPPh2py)3Ag](BF4)2 in Example 4 of the present invention is shown;
[0028] Figure 7 The brightness-current efficiency curve of the electroluminescent device prepared based on [O(AuPPh2py)3]BF4 in Example 3 of the present invention is shown;
[0029] Figure 8The brightness-current efficiency curve of the electroluminescent device prepared based on [O(AuPPh2py)3Ag](BF4)2 in Example 4 of the present invention is shown;
[0030] Fig. 9 The brightness-power efficiency curve of the electroluminescent device prepared based on [O(AuPPh2py)3]BF4 in Example 3 of the present invention is shown;
[0031] Fig.10 The brightness-power efficiency curve of the electroluminescent device prepared based on [O(AuPPh2py)3Ag](BF4)2 in Example 4 of the present invention is shown;
[0032] Fig.11 The brightness-maximum external quantum efficiency curve of the electroluminescent device prepared based on [O(AuPPh2py)3]BF4 in Example 3 of the present invention is shown;
[0033] Fig.12 The brightness-maximum external quantum efficiency curve of the electroluminescent device prepared based on [O(AuPPh2py)3Ag](BF4)2 in Example 4 of the present invention is shown;
[0034] Fig.13 The emission spectrum curve of the electroluminescent device prepared based on [O(AuPPh2py)3]BF4 in Example 3 of the present invention is shown;
[0035] Fig.14 The emission spectrum curve of the electroluminescent device prepared based on [O(AuPPh2py)3Ag](BF4)2 in Example 4 of the present invention is shown. DETAILED DESCRIPTION
[0036] The present invention is described in detail below through specific implementation modes, and the characteristics and advantages of the present invention will become clearer and more specific with these descriptions.
[0037] The present invention uses a gold cluster complex or a gold-silver cluster complex constructed with diphenyl-2-pyridylphosphine as a ligand as a guest material of a light-emitting layer to prepare an electroluminescent device. The metal cluster complex has good thermal stability, and is used as a guest light-emitting material for vacuum evaporation preparation. The peak of the electroluminescent spectrum is 430-450nm, and the deep blue light emission of the electroluminescent device is achieved. The comprehensive light-emitting performance is good, and it is expected to be promoted in practical applications.
[0038] The invention provides a deep blue photoelectroluminescent device based on a gold-silver cluster complex. The guest material of the light-emitting layer of the device is one or more of a gold cluster complex and a gold-silver cluster complex.
[0039] The gold cluster complex is a gold cluster complex using diphenyl-2-pyridylphosphine as a ligand.
[0040] The gold-silver cluster complex is a gold-silver cluster complex with diphenyl-2-pyridylphosphine as a ligand.
[0041] The guest material of the light-emitting layer of the device is preferably [O(AuPPh2py)3]BF4 and / or [O(AuPPh2py)3Ag](BF4)2, more preferably [O(AuPPh2py)3]BF4 or [O(AuPPh2py)3Ag](BF4)2, wherein O is oxygen, Au is gold, P is phosphorus, Ph is a benzene ring, py is pyridine, B is boron, F is fluorine, and Ag is silver.
[0042] The [O(AuPPh2py)3]BF4 is:
[0043]
[0044] The [O(AuPPh2py)3Ag](BF4)2 is:
[0045]
[0046] The [O(AuPPh2py)3]BF4 or [O(AuPPh2py)3Ag](BF4)2 is specifically described in the document Highly Luminescent Gold(I)-Silver(I)and Gold(I)-Copper(I)Chalcogenide Clusters, Chemistry-A European Journal, 2007, 13, 235, and is prepared by the preparation method in the above document.
[0047] In the light-emitting layer material, the mass fraction of the guest material is 0.2%-1.2%, preferably 0.3%-0.9%, and more preferably 0.4%-0.6%.
[0048] The deep blue light electroluminescent device based on the gold-silver cluster complex also includes a substrate layer, a conductive anode layer, a hole injection layer, a hole transport layer, an electron blocking layer, a light-emitting layer, a hole blocking layer, an electron transport layer, an electron injection layer and a cathode conductive layer.
[0049] The conductive anode layer material is selected from tin oxide conductive glass (ITO), transparent conductive polymers such as polyaniline, semi-transparent metals such as Au, preferably ITO or semi-transparent metals, more preferably ITO. The conductive anode layer thickness is 1-100nm, preferably 8-20nm, more preferably 10-15nm, such as 10nm.
[0050] The hole injection layer material is selected from molybdenum oxide or a mixture of poly 3,4-ethylenedioxythiophene and polystyrene sulfonate (PEDOT / PSS), preferably molybdenum oxide, more preferably MoO3. The hole injection layer thickness is 2-20nm, preferably 3-15nm, more preferably 5-10nm, such as 6nm.
[0051] The hole transport layer material is selected from aromatic amine derivatives, such as N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine (NPB). The hole transport layer thickness is 20-80nm, preferably 30-70nm, more preferably 40-60nm, such as 50nm.
[0052] The electron blocking layer material is selected from 9,9'-(1,3-phenyl)di-9H-carbazole (mCP) or bis[2-((oxy)diphenylphosphino)phenyl]ether (DPEPO), preferably 9,9'-(1,3-phenyl)di-9H-carbazole (mCP). The electron blocking layer has a thickness of 1-20 nm, preferably 3-12 nm, more preferably 4-8 nm, such as 5 nm.
[0053] The main material of the light-emitting layer is bis[2-((oxy)diphenylphosphino)phenyl]ether (DPEPO).
[0054] The evaporated thickness of the light-emitting layer is 10-50 nm, preferably 15-40 nm, more preferably 20-30 nm, such as 20 nm.
[0055] The hole blocking layer material is di[2-((oxy)diphenylphosphino)phenyl]ether (DPEPO). The hole blocking layer thickness is 1-16 nm, preferably 3-12 nm, more preferably 5-8 nm, such as 5 nm.
[0056] The electron transport layer material is selected from tris(8-hydroxyquinoline)aluminum (Alq3), 1,3,5-tris(1-phenyl-1H-benzimidazol-2-yl)benzene (TPBi), 4,7-diphenyl-1,10-phenanthroline (Bphen), 3-(biphenyl-4-yl)-5-(4-tert-butylphenyl)-4-phenyl-4H-1,2,4-triazole (TAZ), preferably Bphen. The thickness of the electron transport layer is 20-75nm, preferably 30-65nm, more preferably 40-55nm, such as 45nm.
[0057] The electron injection layer material is selected from lithium tetrakis (8-hydroxyquinoline) boron (LiBq4) or LiF, preferably LiF. The electron injection layer thickness is 0.1-8nm, preferably 0.5-5nm, more preferably 1-2nm, such as 1nm.
[0058] The cathode conductive layer material is selected from a single metal cathode or an alloy cathode, preferably calcium, magnesium, silver, aluminum, calcium alloy, magnesium alloy, silver alloy or aluminum alloy, such as aluminum. The cathode conductive layer thickness is 60-150nm, preferably 80-130nm, more preferably 100-110nm, such as 100nm.
[0059] The peak value of the electroluminescence spectrum of the deep blue electroluminescent device based on the gold-silver cluster complex is 430-450nm, such as 440nm.
[0060] The present invention also provides a method for preparing the deep blue light electroluminescent device based on the gold-silver cluster complex, which specifically comprises the following steps:
[0061] 1. preparing a conductive anode layer;
[0062] A glass or plastic substrate cleaned with deionized water is placed in a vacuum evaporator to prepare a conductive anode layer on the substrate layer.
[0063] Preferably, the vacuum degree of vacuum evaporation is 2×10 -4 ~7×10 -4 pa, preferably 3×10 -4 ~5×10 -4 pa, and the evaporation rate is set to 0.1-0.5 nm / s, preferably 0.1 nm / s-0.2 nm / s.
[0064] Preferably, the hole injection layer, the hole transport layer, the electron blocking layer, the light emitting layer, the hole blocking layer, the electron transport layer, the electron injection layer and the cathode conductive layer are prepared by vacuum evaporation.
[0065] 2. preparing a hole injection layer;
[0066] The hole injection layer was deposited on the anode conductive layer. The vacuum degree of vacuum deposition was 2×10 -4 ~7×10 -4 pa, preferably 3×10 -4 ~5×10 -4 pa, and the evaporation rate is set to 0.1-0.5 nm / s, preferably 0.1 nm / s-0.2 nm / s.
[0067] 3. Preparation of hole transport layer;
[0068] The hole transport layer was deposited on the hole injection layer. The vacuum degree of vacuum deposition was 2×10 -4 ~7×10 -4 pa, preferably 3×10 -4 ~5×10 -4 pa, and the evaporation rate is set to 0.1-0.5 nm / s, preferably 0.2 nm / s-0.3 nm / s.
[0069] 4. preparing an electron blocking layer;
[0070] The electron blocking layer is evaporated on the hole transport layer. The vacuum evaporation degree is 2×10 -4 ~7×10 - 4 pa, preferably 3×10 -4 ~5×10 -4 pa, and the evaporation rate is set to 0.1-0.5 nm / s, preferably 0.1 nm / s-0.2 nm / s.
[0071] 5. preparing a light-emitting layer;
[0072] The light-emitting layer is evaporated on the electron blocking layer. The vacuum evaporation degree is 2×10 -4 ~7×10 -4 pa, preferably 3×10 -4 ~5×10 -4 pa, and the evaporation rate is set to 0.1-0.5 nm / s, preferably 0.1 nm / s-0.2 nm / s.
[0073] 6. preparing a hole blocking layer;
[0074] The hole blocking layer is evaporated on the light-emitting layer. The vacuum evaporation degree is 2×10 -4 ~7×10 -4 pa, preferably 3×10 -4 ~5×10 -4 pa, and the evaporation rate is set to 0.1-0.5 nm / s, preferably 0.1 nm / s-0.2 nm / s.
[0075] 7. Preparing an electron transport layer;
[0076] The electron transport layer is evaporated on the hole blocking layer. The vacuum evaporation degree is 2×10 -4 ~7×10 - 4 pa, preferably 3×10 -4 ~5×10 -4 pa, and the evaporation rate is set to 0.1-0.5 nm / s, preferably 0.2 nm / s-0.3 nm / s.
[0077] 8. preparing an electron injection layer;
[0078] The electron injection layer is deposited on the electron transport layer. The vacuum degree of vacuum deposition is 2×10 -4 ~7×10 - 4 pa, preferably 3×10 -4 ~5×10-4 pa, and the evaporation rate is set to 0.1-0.7 nm / s, preferably 0.4 nm / s-0.5 nm / s.
[0079] 9. Prepare a cathode conductive layer, encapsulate, and obtain a thermally excited delayed fluorescence electroluminescent device. The cathode conductive layer is evaporated on the electron injection layer. The vacuum evaporation degree is 2×10 -4 ~7×10 -4 pa, preferably 3×10 -4 ~5×10 -4 pa, the evaporation rate is set to 1-7 nm / s, preferably 3 nm / s-4 nm / s.
[0080] In the present invention, a deep blue luminescent electroluminescent device is prepared by using a gold cluster complex or a gold-silver cluster complex with good thermal stability as a guest material of a light-emitting layer. The gold cluster complex or the gold-silver cluster complex has good thermal stability, and the device is successfully prepared by a vacuum evaporation method. The device by vacuum evaporation has better film-forming property, is more stable, has good luminescent performance, and has excellent comprehensive performance.
[0081] Example
[0082] Example 1
[0083] 0.45 g (about 11.2 mmol) of NaOH was added to 10 mL of deionized water; 1.88 g (about 11.0 mmol) of AgNO3 was added to 10 mL of deionized water; the two solutions were mixed to generate a precipitate, which was filtered and washed with deionized water and ethanol for several times before drying to obtain Ag2O.
[0084] 1.487 g (about 3 mmol) of Au(Dppy)Cl (Au(Dppy)Cl was prepared by the method described in Alcock, NW; Moore, P.; Lampe, PA; Mok, KF, Crystal and Molecular Structures of Two Complexes of Diphenyl(2-pyridy1)phosphine(L):[AuCIL]and[Ag2C12L3], J.Chem.Soc.Dalton.Trans.,1982,207.DOI:10.1002 / chin.198213065)) was dissolved in 100 mL of acetone, the prepared Ag2O was added, and then 1.866 g of NaBF4 (about 17.1 mmol) was added, and the mixture was stirred for 3 h at room temperature in the dark. After the reaction, the solid product was filtered and washed three times with 15 mL of dichloromethane (DCM), and the DCM washings were collected and concentrated to 5 mL by evaporation. Then, ether was added to precipitate the product, and [O(AuPPh2py)3]BF4 was prepared with a yield of 65%. (For details, see the document Highly Luminescent Gold(I)-Silver(I)and Gold(I)-Copper(I)ChalcogenideClusters.Chemistry-A European Journal, 2007, 13, 235)
[0085] Figure 1 Thermogravimetric analysis spectrum of [O(AuPPh2py)3]BF4 prepared, taking 5% weight loss as the pyrolysis temperature, from Figure 1 It can be seen that the cracking temperature of the prepared [O(AuPPh2py)3]BF4 is 283℃.
[0086] Example 2
[0087] Take 0.148g (about 0.1mmol) of [O(AuPPh2py)3]BF4 prepared in Example 1 and add it to 20mL DCM, then add 0.019g (about 0.1mmol) AgBF4, and stir for 30min at room temperature in the dark. After the reaction is completed, evaporate and concentrate the solvent to 5mL, add ether, precipitate solid, and obtain [O(AuPPh2py)3Ag](BF4)2. (For details, see the document Highly Luminescent Gold(I)-Silver(I)and Gold(I)-Copper(I)Chalcogenide Clusters.Chemistry-AEuropean Journal,2007,13,235)
[0088] Figure 2 Thermogravimetric analysis spectrum of [O(AuPPh2py)3Ag](BF4)2 prepared, taking 5% weight loss as the pyrolysis temperature, from Figure 2 It can be seen that the cracking temperature of the prepared [O(AuPPh2py)3]BF4 is 289℃.
[0089] Example 3
[0090] 1. Use acetone, anhydrous ethanol and deionized water to clean the ITO substrate 3 to 5 times respectively, and then clean it in a vacuum of 4×10 -4 pa and evaporation rate is 0.1nms -1 ~0.2nms -1 MoO3 material was evaporated under conditions to obtain a 6nm hole injection layer.
[0091] 2. When the vacuum degree is 4×10 -4 pa and evaporation rate is 0.2nms -1 ~0.3nms -1 NPB material was evaporated on the hole injection layer under conditions to obtain a 50nm hole transport layer.
[0092] 3. When the vacuum degree is 4×10 -4 pa and evaporation rate is 0.1nms -1 Under the conditions of , mCP material was evaporated on the hole transport layer to obtain a 5nm electron blocking layer.
[0093] 4. When the vacuum degree is 4×10 -4 pa and evaporation rate is 0.2nms -1 Under the conditions of , a light-emitting layer was evaporated on the electron blocking layer, the light-emitting layer was DPEPO as the main material, and the guest material [O(AuPPh2py)3]BF4 prepared in Example 1 was doped with a mass fraction of 0.5% to obtain a 20nm light-emitting layer.
[0094] 5. When the vacuum degree is 4×10 -4 pa and evaporation rate is 0.1nms -1 DPEPO material was evaporated on the light-emitting layer under conditions to obtain a 5 nm hole blocking layer.
[0095] 6. When the vacuum degree is 4×10 -4 pa and evaporation rate is 0.2nms -1 ~0.3nms -1 Under the conditions of , Bphen material was evaporated on the hole blocking layer to obtain a 45nm electron transport layer.
[0096] 7. When the vacuum degree is 4×10 -4 pa and evaporation rate is 0.5nms-1 LiF material was evaporated on the electron transport layer under the conditions of to obtain a 1nm electron injection layer.
[0097] 8. When the vacuum degree is 4×10 -4 pa and evaporation rate is 3nms -1 ~4nms -1 Under the conditions of , metal Al is evaporated on the electron injection layer to obtain a 100nm cathode conductive layer, which is then packaged to obtain an electroluminescent device.
[0098] Figure 3 The voltage-current density relationship curve of the electroluminescent device prepared based on [O(AuPPh2py)3]BF4 is shown in Figure 2. Figure 3 It can be seen that the maximum current density of the electroluminescent device is: 0.12mA / cm 2 .
[0099] Figure 5 The voltage-brightness relationship curve of the electroluminescent device based on [O(AuPPh2py)3]BF4 is shown in Figure 2. Figure 5 It can be seen that the maximum brightness of the electroluminescent device is 88.37cd / m 2 .
[0100] Figure 7 The brightness-current efficiency curve of the electroluminescent device based on [O(AuPPh2py)3]BF4 is shown in Figure 2. Figure 7 It can be seen that the maximum current efficiency of the electroluminescent device is 0.45 mA / cm 2 .
[0101] Fig. 9 The brightness-power efficiency curve of the electroluminescent device based on [O(AuPPh2py)3]BF4 is shown in Figure 2. Fig. 9 It can be seen that the maximum power efficiency of the electroluminescent device is 0.25lm / W.
[0102] Fig.11 The brightness-maximum external quantum efficiency curve of the electroluminescent device prepared based on [O(AuPPh2py)3]BF4 is shown in Figure 2. Fig.11 It can be seen that the maximum external quantum efficiency of the electroluminescent device is 0.35%.
[0103] Fig.13 The emission spectrum curve of the electroluminescent device based on [O(AuPPh2py)3]BF4 is shown in Figure 2. Fig.13 It can be seen that the peak of the electroluminescence spectrum of the electroluminescent device is 440nm.
[0104] Example 4
[0105] An electroluminescent device was prepared according to the method in Example 3, except that in step 4, the guest material with a doping mass fraction of 0.5% was [O(AuPPh2py)3Ag](BF4)2.
[0106] Figure 4 The voltage-current density relationship curve of the electroluminescent device based on [O(AuPPh2py)3Ag](BF4)2 is shown in Figure 2. Figure 4 It can be seen that the maximum current density of the electroluminescent device is: 0.30mA / cm 2 .
[0107] Figure 6 The voltage-brightness relationship curve of the electroluminescent device based on [O(AuPPh2py)3Ag](BF4)2 is shown in Figure 2. Figure 6 It can be seen that the maximum brightness of the electroluminescent device is 79.96cd / m 2 .
[0108] Figure 8 The brightness-current efficiency curve of the electroluminescent device based on [O(AuPPh2py)3Ag](BF4)2 is shown in Figure 2. Figure 8 It can be seen that the maximum current efficiency of the electroluminescent device is 0.42 mA / cm 2 .
[0109] Fig.10 The brightness-power efficiency curve of the electroluminescent device based on [O(AuPPh2py)3Ag](BF4)2 is shown in Figure 2. Fig.10 It can be seen that the maximum power efficiency of the electroluminescent device is 0.23lm / W.
[0110] Fig.12 The brightness-maximum external quantum efficiency curve of the electroluminescent device based on [O(AuPPh2py)3Ag](BF4)2 is shown in Figure 2. Fig.12 It can be seen that the maximum external quantum efficiency of the electroluminescent device is 0.34%.
[0111] Fig.14 The emission spectrum curve of the electroluminescent device based on [O(AuPPh2py)3Ag](BF4)2 is shown in Figure 2. Fig.14 It can be seen that the peak of the electroluminescence spectrum of the electroluminescent device is 440nm.
[0112] The present invention is described in detail above in conjunction with specific embodiments and / or exemplary examples and drawings, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, various equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a deep blue light electroluminescent device based on a gold-silver cluster complex, characterized in that: The guest material of the light-emitting layer of the device is [O(AuPPh2py)3]BF4 or [O(AuPPh2py)3]BF4 and [O(AuPPh2py)3Ag](BF4)2. In the light-emitting layer material, the mass fraction of the guest material is 0.3%-0.9%. The deep blue light electroluminescent device based on the gold-silver cluster complex also includes a substrate layer, a conductive anode layer, a hole injection layer, a hole transport layer, an electron blocking layer, a light-emitting layer, a hole blocking layer, an electron transport layer, an electron injection layer and a cathode conductive layer. The hole injection layer material is molybdenum oxide, and the hole injection layer thickness is 2-20 nm. The main material of the light-emitting layer is di[2-((oxy)diphenylphosphino)phenyl]ether, and the thickness of the light-emitting layer by evaporation is 10-50nm. The hole transport layer material is N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, and the hole transport layer thickness is 20-80nm. The electron blocking layer material is 9,9'-(1,3-phenyl)di-9H-carbazole, and the thickness of the electron blocking layer is 1-20 nm. The hole blocking layer material is di[2-((oxy)diphenylphosphino)phenyl]ether, and the hole blocking layer thickness is 3-12nm. The electron transport layer material is 4,7-diphenyl-1,10-phenanthroline, and the thickness of the electron transport layer is 20-75 nm. The electron injection layer material is LiF, and the thickness of the electron injection layer is 1-2nm. The method comprises the following steps:
1. preparing a conductive anode layer; 2. preparing a hole injection layer by evaporating the hole injection layer on the anode conductive layer; 3. preparing a hole transport layer, and evaporating the hole transport layer on the hole injection layer; 4. preparing an electron blocking layer, wherein the electron blocking layer is evaporated on the hole transport layer; 5. preparing a light-emitting layer, wherein the light-emitting layer is evaporated on the electron blocking layer; 6. preparing a hole blocking layer, wherein the hole blocking layer is evaporated on the light-emitting layer; 7. preparing an electron transport layer, wherein the electron transport layer is evaporated on the hole blocking layer; 8. preparing an electron injection layer, wherein the electron injection layer is evaporated on the electron transport layer; 9. Prepare a cathode conductive layer, encapsulate, and obtain a thermally excited delayed fluorescence electroluminescent device, wherein the cathode conductive layer is evaporated on the electron injection layer, The peak value of the electroluminescence spectrum of the deep blue electroluminescent device based on the gold-silver cluster complex is 430-450nm.
2. The preparation method according to claim 1, characterized in that: In the light-emitting layer material, the mass fraction of the guest material is 0.4%-0.6%.
3. The preparation method according to claim 1, characterized in that: The thickness of the hole injection layer is 3~15nm.
4. The preparation method according to claim 1, characterized in that: The evaporated thickness of the light-emitting layer is 15-40 nm.
5. The preparation method according to claim 1, characterized in that: In step one, Putting a glass or plastic substrate cleaned with deionized water into a vacuum evaporator to prepare a conductive anode layer on the substrate layer; The vacuum degree of vacuum evaporation is 2×10 -4 ~7×10 -4 pa, and the evaporation rate was set to 0.1~0.5nm / s.
6. The preparation method according to claim 1, characterized in that: The hole injection layer, the hole transport layer, the electron blocking layer, the light emitting layer, the hole blocking layer, the electron transport layer, the electron injection layer and the cathode conductive layer are prepared by vacuum evaporation.
7. The preparation method according to claim 1, characterized in that: In step 4, the vacuum degree of vacuum evaporation is 2×10 -4 ~7×10 -4 pa; the evaporation rate is set to 0.1~0.5nm / s.