An antibacterial and antiviral photocatalytic composite material and its preparation method and application

By applying carbon quantum dots and silicon-based sol-gel-combined photocatalytic composites on automotive interior parts, the problem of poor antibacterial effect of existing photocatalytic materials under visible light is solved, and efficient antibacterial under visible light is achieved and antiviral effects, and improve the wear resistance and adhesion of the coating.

CN115121292BActive Publication Date: 2024-11-01HONG KONG PRODUCTIVITY COUNCIL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110334889.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-29
Publication Date
2024-11-01
Estimated Expiration
2041-03-29

AI Technical Summary

Technical Problem

Due to the problem of ultraviolet light barrier in car cars, existing photocatalytic materials have limited antibacterial efficacy and poor antibacterial effect under visible light, making it difficult to effectively remove bacteria and viruses in car cars.

Method used

Using an antibacterial and antiviral photocatalytic composite material, carbon quantum dots and silicon are formed by mixing ethanol, sodium hydroxide, tetraethoxysilane, silane coupling agent, photoinitiator and photocatalytic material under specific conditions. Base sol-gel, combined with ultrasonic treatment, prepares antibacterial and antiviral coatings that can function in visible light, and are applied to different automotive interior parts by spraying.

Benefits of technology

This composite material significantly enhances antibacterial and antiviral properties through the electron transfer between photocatalytic materials and carbon quantum dots, has good binding force and wear resistance, and is suitable for use in a variety of automotive interior parts, which can maintain antibacterial and anti-viral for a long time. Viral function is not damaged even under mechanical friction and compressed air blowing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002997050140000091
    Figure BDA0002997050140000091
Patent Text Reader

Abstract

The present invention provides an antibacterial and antiviral photocatalytic composite material and its preparation method and application. The method includes: 990-995 parts by mass of ethanol, 5-10 parts by mass of pure water, and 2-10 parts by mass of sodium hydroxide are mixed evenly to obtain a solution; then the solution is electrolyzed for 10-60 minutes to obtain an ethanol transparent solution mixed with carbon quantum dots, and then the obtained solution is neutralized with acetic acid to a pH value of 5.5-7; 5-100 parts by mass of tetraethoxysilane, 2-50 parts by mass of silane coupling agent, 0.5-10 parts by mass of photoinitiator, 0.5-20 parts by mass of pure water and 100-1000 parts by mass of the ethanol solution mixed with carbon quantum dots obtained before are mixed evenly to obtain a mixed solution; the mixed solution is stirred at 50-60 ° C for 10-60 minutes for hydrolysis to obtain a silicon-based sol-gel; 0.5-20 parts by mass of photocatalytic material are added to the silicon-based sol-gel, and ultrasonic mixing is performed for 10-30 minutes to obtain a composite material. The composite material of the present invention can enhance its antibacterial and antiviral properties through good electron transfer between the photocatalytic material and the carbon quantum dots.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of antibacterial coatings, and in particular relates to an antibacterial and antiviral photocatalytic composite material and a preparation method and application thereof. Background Art

[0002] In daily life, urbanites take public transportation, and the cleanliness and sanitation of the interior of the vehicle naturally attract public attention. The closed-loop environment in the ventilation system of most cars now easily accumulates harmful pollutants, chemicals (such as volatile organic compounds), bacteria and viruses. This problem is particularly serious in modern metropolises with large transportation networks and high traffic volumes, such as Hong Kong, China.

[0003] There are several types of surface coatings on the market that are commonly used for air purification, antibacterial and antiviral purposes. One of them uses visible light catalytic materials as the main coating material. The photocatalytic function oxidizes pollutants and has antibacterial and antiviral capabilities, which can remove bacteria and viruses on the surface of the material. Titanium dioxide in the form of anatase is one of the commonly used photocatalytic materials. When exposed to ultraviolet light of a specific wavelength, it can exert photocatalytic antibacterial effects. However, since the glass used in automobiles can almost completely block all ultraviolet light, the intensity of ultraviolet light in the car is relatively low, which greatly reduces its antibacterial effect. Relatively speaking, titanium dioxide can only exert limited effectiveness. Photocatalytic materials such as bismuth oxybromide and tungsten oxide can exert antibacterial effects under visible light, but due to reasons such as the recombination of electron-hole pairs, the antibacterial effect is not good under visible light. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a highly efficient antibacterial and antiviral photocatalytic composite material and its preparation method and application. It can be applied to the materials of different automotive interior parts and can function when excited by visible light to solve the antibacterial problem of various substrates in the car.

[0005] In order to achieve the above-mentioned object, the present invention provides a method for preparing an antibacterial and antiviral photocatalytic composite material, comprising the following steps:

[0006] S1: 990-995 parts by mass of ethanol, 5-10 parts by mass of pure water, and 2-10 parts by mass of sodium hydroxide are mixed uniformly to obtain a solution; then the solution is electrolyzed for 10-60 minutes at a current density of 0.01-0.2 A / cm 2 , obtaining a transparent ethanol solution mixed with carbon quantum dots, and then neutralizing the obtained solution with acetic acid to a pH value of 5.5-7;

[0007] S2: 5-100 parts by mass of tetraethoxysilane, 2-50 parts by mass of a silane coupling agent, 0.5-10 parts by mass of a photoinitiator, 0.5-20 parts by mass of pure water and 100-1000 parts by mass of the solution obtained in step S1 are uniformly mixed to obtain a mixed solution;

[0008] S3: stirring the mixed solution obtained in step S2 at 50-60° C. for 10-60 minutes to hydrolyze to obtain a silica-based sol-gel;

[0009] S4: adding 0.5-20 parts by weight of photocatalytic material to the silicon-based sol-gel obtained in step S3, ultrasonicating for 10-30 minutes, and mixing evenly to obtain the antibacterial and antiviral composite material.

[0010] Furthermore, in step S1, the content of carbon quantum dots in the transparent ethanol solution is 30-500 mg / L.

[0011] Furthermore, in step S1, the electrode used for electrolysis is selected from at least one of a platinum electrode and a graphite electrode; the electrode includes an anode and a cathode, and the anode or cathode can be a platinum electrode or a graphite electrode or a combination of the two. The current density of the electrolysis is 0.01-0.2A / cm 2 .

[0012] Furthermore, in step S2, the silane coupling agent is selected from aminosilane coupling agent, vinyl silane coupling agent, epoxy silane coupling agent or long-chain alkyl silane coupling agent, and different types can be selected for different substrates. For different substrates in the car, aminosilane coupling agent is preferred because it is suitable for more surfaces, such as glass, plastic, stainless steel, etc.

[0013] Furthermore, in step S2, the photoinitiator is selected from acylphosphine oxide photoinitiators, benzil photoinitiators, and benzophenone photoinitiators. Since acylphosphine oxide photoinitiators have a short curing time and are not easy to turn yellow, acylphosphine oxide photoinitiators are preferred.

[0014] Furthermore, in step S4, the photocatalytic material is selected from BiOBr, CdS, Fe2O3, WO3, Bi2O3 or BiVO4.

[0015] Furthermore, in step S4, the frequency of the ultrasound is 30-60 KHz.

[0016] In order to achieve the above-mentioned purpose, the present invention also provides an antibacterial and antiviral photocatalytic composite material, which is prepared by the above-mentioned method.

[0017] In order to achieve the above-mentioned purpose, the present invention also provides a method for using an antibacterial and antiviral photocatalytic composite material, comprising the following steps: forming a film of the composite material on a substrate by spraying, spin coating or scraping to form a film with a thickness of 5-30 microns, and then drying it naturally. Since the spraying method is simple to operate and convenient for large-scale production, the spraying method is preferred. During spraying, the pressure-feed spray gun is kept perpendicular to the substrate surface, and the working distance is 20-30 cm.

[0018] Furthermore, the substrate is selected from one of glass, metal, leather, plastic and fabric.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The composite material of the present invention can enhance its antibacterial and antiviral properties through good electron transfer between the photocatalytic material and the carbon quantum dots. In addition, the coating has good bonding force with the surfaces of various types of workpieces to improve wear resistance, and can also solve the problem of poor adhesion between individual substrates and the coating in the car compartment, and can be applied to the materials of different automotive interior decoration parts. This coating has good wear resistance and is suitable for application to the surfaces of decorative parts and seats that are frequently touched in the car, so that the car compartment maintains long-term antibacterial and antiviral functions, and can even be applied to frequently touched parts indoors, such as: door handles, handrails, door locks, elevator buttons and handrails, etc. The coating can adhere well to stainless steel, PET plastic, glass, cotton canvas, flannel, polyurethane and artificial leather, and the coating can withstand the blowing of compressed air and mechanical friction, and the coating has no visible damage. DETAILED DESCRIPTION

[0021] The present invention provides an antibacterial and antiviral photocatalytic composite material and a preparation method and application thereof. The specific implementation method is described below with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0022] Example 1

[0023] This embodiment provides a method for preparing an antibacterial and antiviral composite material, comprising the following steps:

[0024] S1: 995 parts by mass of ethanol, 5 parts by mass of pure water, and 5 parts by mass of sodium hydroxide were mixed evenly, and then the solution was electrolyzed for 60 minutes at a current density of 0.01 A / cm 2 , a transparent ethanol solution mixed with about 100 mg / L carbon quantum dots was obtained, and then the obtained solution was neutralized with acetic acid to a pH value of 6.

[0025] S2: 50 parts by mass of tetraethoxysilane, 20 parts by mass of silane coupling agent, 5 parts by mass of photoinitiator, 5 parts by mass of pure water, and 1000 parts by mass of the solution obtained in step S1 are mixed uniformly to obtain a mixed solution.

[0026] S3: The mixed solution obtained in step S2 is stirred at 50° C. for 20 minutes to be hydrolyzed to obtain a silica-based sol-gel.

[0027] S4: adding 7 parts by mass of the photocatalytic material bismuth oxybromide BiOBr to the silicon-based sol-gel obtained in step S3, and mixing them evenly by ultrasonication (ultrasonic frequency: 40 KHz) for 15 minutes to obtain the composite material.

[0028] First, use ethanol and cloth to clean the surface of the workpiece. After the ethanol on the surface of the workpiece is completely evaporated, the composite material prepared above is directly applied to the surface of metal, leather, plastic or fabric by spraying. During spraying, the pressure-feed spray gun is kept perpendicular to the substrate surface, and the working distance is 30 cm to form a film with a thickness of about 20 microns. After that, the coating is naturally air-dried to obtain the antibacterial and antiviral coating.

[0029] Example 2

[0030] This embodiment provides a method for preparing an antibacterial and antiviral composite material, comprising the following steps:

[0031] S1: 995 parts by mass of ethanol, 5 parts by mass of pure water, and 7 parts by mass of sodium hydroxide were mixed evenly, and then the solution was electrolyzed for 30 minutes at a current density of 0.02 A / cm 2 , a transparent ethanol solution mixed with about 100 mg / L carbon quantum dots was obtained, and then the resulting solution was neutralized with acetic acid to a pH of 6.

[0032] S2: 100 parts by mass of tetraethoxysilane, 50 parts by mass of a silane coupling agent, 5 parts by mass of a photoinitiator, 10 parts by mass of pure water, and 1000 parts by mass of the solution obtained in step S1 are mixed uniformly to obtain a mixed solution.

[0033] S3: The mixed solution obtained in step S2 is stirred at 50° C. for 20 minutes to be hydrolyzed to obtain a silica-based sol-gel.

[0034] S4: adding 7.5 parts by mass of the photocatalytic material bismuth oxybromide BiOBr to the silicon-based sol-gel obtained in step S3, and mixing them evenly by ultrasonication (ultrasonic frequency: 40 KHz) for 15 minutes to obtain the composite material.

[0035] First, use ethanol and cloth to clean the surface of the workpiece. After the ethanol on the surface of the workpiece is completely evaporated, the composite material prepared above is directly applied to the surface of metal, leather, plastic or fabric by spraying. During spraying, the pressure-feed spray gun is kept perpendicular to the substrate surface, and the working distance is 30 cm to form a thin film with a thickness of about 15 microns. After that, the coating is naturally air-dried to obtain the antibacterial and antiviral coating.

[0036] Example 3

[0037] This embodiment provides a method for preparing an antibacterial and antiviral composite material, comprising the following steps:

[0038] S1: 995 parts by mass of ethanol, 5 parts by mass of pure water, and 4 parts by mass of sodium hydroxide were mixed evenly, and then the solution was electrolyzed for 60 minutes at a current density of 0.015 A / cm 2 , to obtain a transparent ethanol solution mixed with about 150 mg / L carbon quantum dots, and then the resulting solution was neutralized with acetic acid to a pH of 6.5.

[0039] S2: 100 parts by mass of tetraethoxysilane, 50 parts by mass of silane coupling agent, 10 parts by mass of photoinitiator, 10 parts by mass of pure water, and 1000 parts by mass of the solution obtained in step S1 are mixed uniformly to obtain a mixed solution.

[0040] S3: The mixed solution obtained in step S2 is stirred at 50° C. for 20 minutes to be hydrolyzed to obtain a silica-based sol-gel.

[0041] S4: adding 20 parts by mass of the photocatalytic material bismuth oxybromide BiOBr to the silicon-based sol-gel obtained in step S3, and mixing them uniformly by ultrasonication (ultrasonic frequency: 40 KHz) for 30 minutes to obtain the composite material.

[0042] First, use ethanol and cloth to clean the surface of the workpiece. After the ethanol on the surface of the workpiece is completely evaporated, the prepared composite material is directly applied to the surface of metal, leather, plastic or fabric by spraying. During spraying, the pressure-feed spray gun is kept perpendicular to the substrate surface, and the working distance is 30 cm to form a thin film with a thickness of about 30 microns. After that, the coating is naturally air-dried to obtain the antibacterial and antiviral coating.

[0043] Example 4

[0044] This embodiment provides a method for preparing an antibacterial and antiviral composite material, comprising the following steps:

[0045] S1: 990 parts by mass of ethanol, 10 parts by mass of pure water, and 4 parts by mass of sodium hydroxide were mixed evenly, and then the solution was electrolyzed for 50 minutes with a current density of 0.015 A / cm 2, a transparent ethanol solution mixed with about 125 mg / L carbon quantum dots was obtained, and then the resulting solution was neutralized with acetic acid to a pH of 7.

[0046] S2: 50 parts by mass of tetraethoxysilane, 100 parts by mass of a silane coupling agent, 5 parts by mass of a photoinitiator, 25 parts by mass of pure water, and 1000 parts by mass of the solution obtained in step S1 are mixed uniformly to obtain a mixed solution.

[0047] S3: The mixed solution obtained in step S2 is stirred at 50° C. for 20 minutes to be hydrolyzed to obtain a silica-based sol-gel.

[0048] S4: adding 15 parts by mass of the photocatalytic material bismuth oxybromide BiOBr to the silicon-based sol-gel obtained in step S3, and mixing them uniformly by ultrasonication (ultrasonic frequency: 40 KHz) for 20 minutes to obtain the composite material.

[0049] First, use ethanol and cloth to clean the surface of the workpiece. After the ethanol on the surface of the workpiece is completely evaporated, the prepared composite material is directly applied to the surface of metal, leather, plastic or fabric by spraying. During spraying, the pressure-feed spray gun is kept perpendicular to the substrate surface, and the working distance is 25 cm to form a thin film with a thickness of about 25 microns. The coating is then naturally air-dried to obtain the antibacterial and antiviral coating.

[0050] Example 5

[0051] This embodiment provides a method for preparing an antibacterial and antiviral composite material, comprising the following steps:

[0052] S1: 995 parts by mass of ethanol, 5 parts by mass of pure water, and 4 parts by mass of sodium hydroxide were mixed evenly, and then the solution was electrolyzed for 15 minutes with a current density of 0.05 A / cm 2 , a transparent ethanol solution mixed with about 125 mg / L carbon quantum dots was obtained, and then the resulting solution was neutralized with acetic acid to a pH of 6.

[0053] S2: 50 parts by mass of tetraethoxysilane, 50 parts by mass of a silane coupling agent, 10 parts by mass of a photoinitiator, 10 parts by mass of pure water, and 1000 parts by mass of the solution obtained in step S1 are mixed uniformly to obtain a mixed solution.

[0054] S3: The mixed solution obtained in step S2 is stirred at 50° C. for 30 minutes to be hydrolyzed to obtain a silica-based sol-gel.

[0055] S4: adding 10 parts by mass of the photocatalytic material bismuth oxybromide BiOBr to the silicon-based sol-gel obtained in step S3, and mixing them uniformly by ultrasonication (ultrasonic frequency: 40 KHz) for 20 minutes to obtain the composite material.

[0056] First, use ethanol and cloth to clean the surface of the workpiece. After the ethanol on the surface of the workpiece is completely evaporated, the composite material prepared above is directly applied to the surface of metal, leather, plastic or fabric by spraying. During spraying, the pressure-feed spray gun is kept perpendicular to the substrate surface, and the working distance is 20 cm to form a thin film with a thickness of about 20 microns. After that, the coating is naturally air-dried to obtain the antibacterial and antiviral coating.

[0057] Example 6

[0058] This embodiment provides a method for preparing an antibacterial and antiviral composite material, comprising the following steps:

[0059] S1: 993 parts by mass of ethanol, 7 parts by mass of pure water, and 5 parts by mass of sodium hydroxide were mixed evenly, and then the solution was electrolyzed for 15 minutes with a current density of 0.05 A / cm 2 , a transparent ethanol solution mixed with about 125 mg / L carbon quantum dots was obtained, and then the resulting solution was neutralized with acetic acid to a pH value of 5.5.

[0060] S2: 100 parts by mass of tetraethoxysilane, 40 parts by mass of a silane coupling agent, 10 parts by mass of a photoinitiator, 10 parts by mass of pure water, and 1000 parts by mass of the solution obtained in step S1 are mixed uniformly to obtain a mixed solution.

[0061] S3: The mixed solution obtained in step S2 is stirred at 50° C. for 15 minutes to be hydrolyzed to obtain a silica-based sol-gel.

[0062] S4: adding 15 parts by mass of the photocatalytic material bismuth oxybromide BiOBr to the silicon-based sol-gel obtained in step S3, and mixing them uniformly by ultrasonication (ultrasonic frequency: 40 KHz) for 30 minutes to obtain the composite material.

[0063] First, use ethanol and cloth to clean the surface of the workpiece. After the ethanol on the surface of the workpiece is completely evaporated, the composite material prepared above is directly applied to the surface of metal, leather, plastic or fabric by spraying. During spraying, the pressure-feed spray gun is kept perpendicular to the substrate surface, and the working distance is 30 cm to form a thin film with a thickness of about 25 microns. After that, the coating is naturally air-dried to obtain the antibacterial and antiviral coating.

[0064] Example 7

[0065] This embodiment provides a method for preparing an antibacterial and antiviral composite material, comprising the following steps:

[0066] S1: 992 parts by mass of ethanol, 8 parts by mass of pure water, and 5 parts by mass of sodium hydroxide were mixed evenly, and then the solution was electrolyzed for 60 minutes at a current density of 0.02 A / cm 2, a transparent ethanol solution mixed with about 200 mg / L carbon quantum dots was obtained, and then the resulting solution was neutralized with acetic acid to a pH value of 6.5.

[0067] S2: 70 parts by mass of tetraethoxysilane, 50 parts by mass of a silane coupling agent, 10 parts by mass of a photoinitiator, 10 parts by mass of pure water, and 1000 parts by mass of the solution obtained in step S1 are mixed uniformly to obtain a mixed solution.

[0068] S3: The mixed solution obtained in step S2 is stirred at 50° C. for 50 minutes to be hydrolyzed to obtain a silica-based sol-gel.

[0069] S4: adding 20 parts by mass of the photocatalytic material bismuth oxybromide BiOBr to the silicon-based sol-gel obtained in step S3, and mixing them uniformly by ultrasonication (ultrasonic frequency: 40 KHz) for 30 minutes to obtain the composite material.

[0070] First, use ethanol and cloth to clean the surface of the workpiece. After the ethanol on the surface of the workpiece is completely evaporated, the prepared composite material is directly applied to the surface of metal, leather, plastic or fabric by spraying. During spraying, the pressure-feed spray gun is kept perpendicular to the substrate surface, and the working distance is 30 cm to form a thin film with a thickness of about 30 microns. After that, the coating is naturally air-dried to obtain the antibacterial and antiviral coating.

[0071] Example 8

[0072] This embodiment provides a method for preparing an antibacterial and antiviral composite material, comprising the following steps:

[0073] S1: 995 parts by mass of ethanol, 5 parts by mass of pure water, and 5 parts by mass of sodium hydroxide were mixed evenly, and then the solution was electrolyzed for 30 minutes with a current density of 0.03A / cm 2 , a transparent ethanol solution mixed with about 150 mg / L carbon quantum dots was obtained, and then the resulting solution was neutralized with acetic acid to a pH of 6.

[0074] S2: 75 parts by mass of tetraethoxysilane, 40 parts by mass of a silane coupling agent, 7 parts by mass of a photoinitiator, 5 parts by mass of pure water, and 1000 parts by mass of the solution obtained in step S1 are mixed uniformly to obtain a mixed solution.

[0075] S3: The mixed solution obtained in step S2 is stirred at 50° C. for 60 minutes to be hydrolyzed to obtain a silica-based sol-gel.

[0076] S4: adding 10 parts by mass of the photocatalytic material bismuth oxybromide BiOBr to the silicon-based sol-gel obtained in step S3, and mixing them evenly by ultrasonication (ultrasonic frequency: 40 KHz) for 15 minutes to obtain the composite material.

[0077] First, use ethanol and cloth to clean the surface of the workpiece. After the ethanol on the surface of the workpiece is completely evaporated, the composite material prepared above is directly applied to the surface of metal, leather, plastic or fabric by spraying. During spraying, the pressure-feed spray gun is kept perpendicular to the substrate surface, and the working distance is 30 cm to form a thin film with a thickness of about 25 microns. After that, the coating is naturally air-dried to obtain the antibacterial and antiviral coating.

[0078] Example 9

[0079] This embodiment provides a method for preparing an antibacterial and antiviral composite material, comprising the following steps:

[0080] S1: 995 parts by mass of ethanol, 5 parts by mass of pure water, and 4 parts by mass of sodium hydroxide were mixed evenly, and then the solution was electrolyzed for 45 minutes with a current density of 0.02 A / cm 2 , a transparent ethanol solution mixed with about 150 mg / L carbon quantum dots was obtained, and then the resulting solution was neutralized with acetic acid to a pH of 7.

[0081] S2: 50 parts by mass of tetraethoxysilane, 60 parts by mass of a silane coupling agent, 5 parts by mass of a photoinitiator, 10 parts by mass of pure water, and 1000 parts by mass of the solution obtained in step S1 are mixed uniformly to obtain a mixed solution.

[0082] S3: The mixed solution obtained in step S2 is stirred at 50° C. for 60 minutes to be hydrolyzed to obtain a silica-based sol-gel.

[0083] S4: adding 15 parts by mass of the photocatalytic material bismuth oxybromide BiOBr to the silicon-based sol-gel obtained in step S3, and mixing them uniformly by ultrasonication (ultrasonic frequency: 40 KHz) for 30 minutes to obtain the composite material.

[0084] First, use ethanol and cloth to clean the surface of the workpiece. After the ethanol on the surface of the workpiece is completely evaporated, the composite material prepared above is directly applied to the surface of metal, leather, plastic or fabric by spraying. During spraying, the pressure-feed spray gun is kept perpendicular to the substrate surface, and the working distance is 30 cm to form a film with a thickness of about 20 microns. After that, the coating is naturally air-dried to obtain the antibacterial and antiviral coating.

[0085] Example 10

[0086] This embodiment provides a method for preparing an antibacterial and antiviral composite material, comprising the following steps:

[0087] S1: 990 parts by mass of ethanol, 10 parts by mass of pure water, and 5 parts by mass of sodium hydroxide were mixed evenly, and then the solution was electrolyzed for 50 minutes at a current density of 0.02 A / cm 2, a transparent ethanol solution mixed with about 165 mg / L carbon quantum dots was obtained, and then the resulting solution was neutralized with acetic acid to a pH value of 5.5.

[0088] S2: 80 parts by mass of tetraethoxysilane, 40 parts by mass of a silane coupling agent, 5 parts by mass of a photoinitiator, 15 parts by mass of pure water, and 1000 parts by mass of the solution obtained in step S1 are mixed uniformly to obtain a mixed solution.

[0089] S3: The mixed solution obtained in step S2 is stirred at 50° C. for 15 minutes to be hydrolyzed to obtain a silica-based sol-gel.

[0090] S4: adding 8 parts by weight of the photocatalytic material bismuth oxybromide BiOBr to the silicon-based sol-gel obtained in step S3, and mixing them evenly by ultrasonication (ultrasonic frequency: 40 KHz) for 15 minutes to obtain the composite material.

[0091] First, use ethanol and cloth to clean the surface of the workpiece. After the ethanol on the surface of the workpiece is completely evaporated, the composite material prepared above is directly applied to the surface of metal, leather, plastic or fabric by spraying. During spraying, the pressure-feed spray gun is kept perpendicular to the substrate surface, and the working distance is 25 cm to form a thin film with a thickness of about 15 microns. After that, the coating is naturally air-dried to obtain the antibacterial and antiviral coating.

[0092] Test Case

[0093] The antibacterial and antiviral coatings prepared in Examples 1-10 were subjected to a visible light catalytic antibacterial test (reference standard: GB / T30706-2014). The test results are shown in Table 1.

[0094] Table 1

[0095] Antibacterial rate Escherichia coli Staphylococcus aureus Example 1 More than 99% More than 99% Example 2 More than 99% More than 99% Example 3 More than 99% More than 99% Example 4 More than 99% More than 99% Example 5 More than 99% More than 99% Example 6 More than 99% More than 99% Example 7 More than 99% More than 99% Example 8 More than 99% More than 99% Example 9 More than 99% More than 99% Example 10 More than 99% More than 99%

[0096] It can be seen from the data in Table 1 that the composite materials prepared in Examples 1-10 of the present invention have obvious inhibitory effects on Escherichia coli and Staphylococcus aureus, and the antibacterial rate reaches more than 99%.

[0097] The antibacterial and antiviral coatings prepared in Examples 1-10 were subjected to visible light catalytic antibacterial tests on different substrates (reference standard: GB / T 30706-2014). The test results are shown in Table 2.

[0098] Table 2

[0099]

[0100] From the data in Table 2, it can be seen that the composite materials prepared in Examples 1-10 of the present invention have obvious inhibitory effects on Staphylococcus aureus on different substrates (PET plastic, glass, cotton canvas, flannel, polyurethane, and artificial leather), and the antibacterial rate is greater than 99%, indicating that the coating has obvious antibacterial effects on the above different substrates, and is suitable for use in places where a variety of materials are mixed, such as seats and armrests inside cars, and other places that are frequently touched, to provide long-term antibacterial and antiviral effects.

[0101] The antibacterial and antiviral coating prepared in Example 1 was subjected to a visible light catalytic antiviral test (reference standard: ISO21702:2019), and the test results are shown in Table 3.

[0102] Table 3

[0103] Virus Name Example 1 Antiviral Activity Rate Influenza A virus H1N1 99.76% Influenza A virus H3N2 99.88% Poliovirus-Type I vaccine strain 85.68% Enterovirus 71 82.57%

[0104] It can be seen from the data in Table 3 that the composite material prepared in Example 1 of the present invention has a significant inhibitory effect on influenza A virus H1N1, H3N2, polio virus-I vaccine strain, and enterovirus 71, especially for influenza A virus H1N1 and H3N2, the antiviral activity rate reaches more than 99%.

[0105] The antibacterial and antiviral coating prepared in Example 1 was compared with bismuth oxybromide BiOBr photocatalytic material in a visible light catalytic antibacterial test (reference standard: GB / T 30706-2014). The test results are shown in Table 4.

[0106] Table 4

[0107] Material BnB Examples 1-10 Antibacterial rate of Staphylococcus aureus 78% 99%

[0108] From the data in Table 4, it can be seen that the antibacterial effect of the BiOBr photocatalytic material of Examples 1-10 of the present invention on Staphylococcus aureus is significantly improved, and the antibacterial rate is increased by more than 20%.

[0109] The antibacterial and antiviral coatings prepared in Examples 1-10 were subjected to wear resistance tests, with a friction speed of 50 times / min, a load of 100g, and 5000 reciprocating times. The overall coating (the substrate is metal, glass, PET plastic) had no visible wear and the coating was uniform overall. This proves that the coating can reach the level of wear resistance and can provide long-term antibacterial and antiviral effects on frequently touched accessories and seats in the car.

[0110] Finally, it should be noted that the above-described embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing an antibacterial and antiviral photocatalytic composite material, characterized in that: The following steps are involved: S1: 990-995 parts by mass of ethanol, 5-10 parts by mass of pure water, and 2-10 parts by mass of sodium hydroxide are mixed uniformly to obtain a solution; then the solution is electrolyzed for 10-60 minutes to obtain an ethanol transparent solution mixed with carbon quantum dots, and then the obtained solution is neutralized with acetic acid to a pH value of 5.5-7; the content of carbon quantum dots in the ethanol transparent solution is 30-500 mg / L; S2: 5-100 parts by weight of tetraethoxysilane, 2-50 parts by weight of silane coupling agent, 0.5-10 parts by weight of photoinitiator, 0.5-20 parts by weight of pure water and 100-1000 parts by weight of the solution obtained in step S1 are uniformly mixed to obtain a transparent solution; the photoinitiator is selected from an acylphosphine oxide photoinitiator or a benzil photoinitiator; S3: stirring the transparent solution obtained in step S2 at 50-60° C. for 10-60 minutes to hydrolyze to obtain a silica-based sol-gel; S4: adding 0.5-20 parts by weight of photocatalytic material to the silicon-based sol-gel obtained in step S3, ultrasonicating for 10-30 minutes, and mixing evenly to obtain the antibacterial and antiviral photocatalytic composite material; the photocatalytic material is selected from BiOBr, CdS, Fe2O3, WO3, Bi2O3 or BiVO4.

2. The preparation method according to claim 1, characterized in that In step S1, the electrode used for electrolysis is selected from at least one of a platinum electrode and a graphite electrode; the current density of the electrolysis is 0.01-0.2 A / cm 2 .

3. The preparation method according to claim 1, characterized in that: In step S2, the silane coupling agent is selected from an aminosilane coupling agent, a vinylsilane coupling agent, an epoxysilane coupling agent or a long-chain alkylsilane coupling agent.

4. The preparation method according to claim 1, characterized in that: In step S4, the frequency of the ultrasound is 30-60 KHz.

5. An antibacterial and antiviral composite material, characterized in that: The composite material is prepared by the method according to any one of claims 1 to 4.

6. A method for using the antibacterial and antiviral photocatalytic composite material according to claim 5, characterized in that: The method comprises the following steps: forming a film of the composite material on a substrate by spraying, spin coating or scraping to form a film with a thickness of 5-30 microns, and then drying naturally to obtain a coating.

7. The method of use according to claim 6, characterized in that: The substrate is selected from one of glass, metal, leather, plastic or fabric.