Cationic dyeable polyester composition and preparation method thereof
By using the combination of sulfonate groups and polyether structural units in polyester fibers, the group position and content are controlled, and the viscosity and strength problems caused by cross-linking of sulfonate groups are solved, and dyeing is improved Performance and spinning properties are suitable for applications in high strength fields.
Patent Information
- Application Number
- CN202110311872.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-24
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-03-24
AI Technical Summary
During the dyeing process, existing polyester fibers have increased viscosity and decreased strength due to physical cross-linking of sulfonate groups, and the terminal blocking of cationic components affects the dyeing performance and reactivity, limiting their application in the field of high strength.
Using a cationic dyeable polyester composition containing sulfonate groups and polyether structural units, the sulfonate compound is bonded at the end of the polyester molecular chain to control the sulfonate group content between 1000 and 3500 ppm, and the polyether structure is added. Units are 0.1 to 10.0 wt%, and metal phosphate salt is added in limited amounts to optimize dyeing properties and spinning properties.
It improves the dyeing performance and strength of polyester fibers, reduces spinning filter pressure, extends the component exchange cycle, reduces production costs, and is suitable for applications in high-strength fields.
Smart Images

Figure 188543DEST_PATH_IMAGE006 
Figure 312990DEST_PATH_IMAGE005
Abstract
Description
Technical Field
[0001] The invention relates to a cationic dyeable polyester composition, in particular to a polyester composition containing terminal blocked sulfonate groups and polyether structural units. Background Art
[0002] Polyester resin, due to its excellent mechanical properties and chemical characteristics, is widely used in clothing, industrial fibers, magnetic tapes, surface coating films, as well as tire radials, network cables and other industrial fields.
[0003] When used as clothing fiber, in order to improve the dyeability of polyester, isophthalic acid components containing sulfonate groups, represented by sodium 5-sulfoisophthalic acid, are made into copolymer monomers to obtain copolymer modified cationic dyeable polyester. However, sulfonate groups are prone to physical cross-linking in polyester, resulting in a significant increase in the melt viscosity of polyester when the inherent viscosity (IV) is not high, resulting in low yarn strength; at the same time, the strength retention rate of the yarn before and after dyeing is poor, which limits its application in some fields with high strength requirements.
[0004] Japanese Patent Laid-Open No. 5-25708 discloses a modified polyester fiber, which is modified by using terminal blocking cationic components, polyether and diol components. The cationic groups in the modified polyester are mainly connected to the ends of the molecular chains, and there are no interacting physical cross-linking groups in the middle of the molecular chains, which greatly reduces the viscosity of the polyester. The strength of the obtained cationic polyester fiber is improved to a certain extent compared with the polyester modified by the isophthalic acid component of the existing sulfonate group, and there is no problem with the spinning performance. However, since the cationic groups are mainly connected to the ends of the molecular weight, the dyeing performance of the modified polyester is affected. In addition, the above-mentioned cationic polyester has the problem of increased filtration pressure during spinning, the production component exchange cycle is short, and the production cost is high. Summary of the invention
[0005] The object of the present invention is to provide a dyeable polyester composition which is easy to dye and has good spinning filter pressure and a preparation method thereof.
[0006] The technical solution of the present invention:
[0007] A cationic dyeable polyester composition is mainly composed of aromatic dicarboxylic acid structural units and polyether structural units. The polyester composition contains a sulfonate group as shown in Formula 1, and the content of the group as shown in Formula 1 accounts for 1000 to 5000 ppm of the total amount of the polyester composition in terms of sulfur element; the polyester composition contains a polyether structural unit; the content of the metal phosphate in the polyester composition is less than 20 ppm in terms of phosphorus atoms;
[0008] Formula 1,
[0009] In Formula 1, Y is an alkyl group having 2 to 20 carbon atoms, a phenyl group or an alkylbenzene group, and Z is a Li ion, a Na ion or a K ion.
[0010] Preferably, the polyether structural unit accounts for 0.1 to 10.0 wt % of the total amount of the polyester composition.
[0011] The phosphate is preferably one or more of potassium phosphate, sodium phosphate or lithium phosphate.
[0012] The content of the group described in Formula 1 is preferably 1000 to 3500 ppm based on the total amount of the polyester composition, calculated as sulfur element.
[0013] The present invention also discloses a method for preparing the cationic dyeable polyester composition, comprising: firstly, obtaining an oligomer by esterification or transesterification reaction of an aromatic dicarboxylic acid or its esterified derivative with an aliphatic diol, and then subjecting the oligomer to polymerization to obtain the polyester composition; before the polymerization reaction begins, adding a sulfonate compound as shown in formula 2, a polyether, and an alkali metal or alkaline earth metal compound in an amount of 1000 to 5000 ppm in terms of sulfur element relative to the total amount of the polyester composition to the oligomer; and before the polymerization reaction ends, adding a phosphorus compound;
[0014] Formula 2,
[0015] In Formula 2, Y is an alkyl group having 2 to 20 carbon atoms, a phenyl group or an alkylbenzene group, and Z is a Li ion, a Na ion or a K ion.
[0016] The amount of the polyether added is preferably equivalent to 0.1 to 10.0 wt % of the total amount of the polyester composition.
[0017] The amount of the sulfonate salt as shown in Formula 2 added is preferably 1000 to 3500 ppm in terms of sulfur element relative to the total amount of the polyester composition.
[0018] The alkali metal or alkaline earth metal compound is preferably one or more of lithium acetate, sodium acetate or potassium acetate, and the added amount thereof is preferably equivalent to 5 to 2000 ppm of the total amount of the polyester composition.
[0019] The phosphorus compound is preferably added 5 to 20 minutes before the end of the polymerization reaction.
[0020] The phosphorus compound is preferably one or more of phosphoric acid, trimethyl phosphate and triethyl phosphate.
[0021] The polyester composition of the present invention is easy to dye and has good filter pressure, and can be applied to fibers. DETAILED DESCRIPTION
[0022] In the prior art, cationic dyeability is generally imparted to polyester by copolymerizing a cationic dyeable component containing a sulfonate group, such as isophthalic acid-5-sulfonate, in the polyester. However, since the sulfonate group is distributed in the middle of the molecular weight of the polyester, the sulfonate group is easily physically cross-linked in the polyester, resulting in an increase in the viscosity of the polyester and a decrease in the strength of the polyester. At the same time, the hydrolysis resistance of the polyester is also deteriorated.
[0023] Adding terminal blocking cationic components to polyester, the cationic groups in the resulting modified polyester are mainly connected to the ends of the molecular chains, and there are no interacting physical cross-linking groups in the middle of the molecular chains, which can improve the melt viscosity of the polyester. However, since the cationic groups are mainly connected to the ends of the molecular weight, the dyeing properties of the modified polyester are affected. At the same time, the addition of terminal blocking cationic components generally leads to poor polyester reactivity, and the molecular weight of the resulting polyester is not large, which has the problem of low strength. By using polyether to modify polyester, the dyeing properties of polyester can be improved, and the molecular weight of the modified polyester can be increased, thereby increasing the strength of the polyester fiber and improving the strength retention rate of the polyester fiber before and after dyeing.
[0024] The cationic dyeable component used in the present invention is a sulfonate compound as shown in Formula 2,
[0025] Formula 2,
[0026] In Formula 2, Y is an alkyl group having 2 to 20 carbon atoms, a phenyl group or an alkylbenzene group, and Z is a Li ion, a Na ion or a K ion.
[0027] The sulfonate compound shown in Formula 2 contains only one hydroxyl reactive group. In the polyester, the sulfonate compound is mainly connected to the end of the molecular chain, and there is no interacting physical cross-linking group in the middle of the molecular chain, so it can ensure that the obtained polyester has a higher molecular weight and better strength.
[0028] As shown in Formula 2, the sulfonate compound specifically includes 2-sodium carboxybenzenesulfonate, 2-potassium carboxybenzenesulfonate, 3-sodium carboxybenzenesulfonate, 3-lithium carboxybenzenesulfonate, 4-sodium carboxybenzenesulfonate, 2-sodium methyl benzoate, 3-sodium methyl benzoate, 4-sodium methyl benzoate, 2-sodium ethyl benzoate, 2-potassium ethylene glycol benzoate, 3-sodium ethyl benzoate, 4-sodium ethylene glycol benzoate, 3-lithium ethylene glycol benzoate, etc., among which 3-sodium carboxybenzenesulfonate is preferred.
[0029] The polyester composition to which the cationic dyeable component such as the sulfonate compound shown in Formula 2 is added contains the sulfonate group shown in Formula 1,
[0030] Formula 1,
[0031] In Formula 1, Y is an alkyl group having 2 to 20 carbon atoms, a phenyl group or an alkylbenzene group, and Z is a Li ion, a Na ion or a K ion.
[0032] The content of the sulfonate groups as shown in Formula 1 in the polyester composition of the present invention is 1000-5000ppm of the total amount of the polyester composition in terms of sulfur element. When the content of the sulfonate groups as shown in Formula 1 in the polyester composition is less than 1000ppm, it is difficult for the obtained product to achieve a satisfactory color concentration in the subsequent dyeing process; when the content of the sulfonate groups as shown in Formula 1 in the polyester composition is higher than 5000ppm, the growth of the polyester molecular chain will be inhibited, and the polymerization system will terminate the polymerization before reaching the target viscosity, and a polyester composition with good physical properties cannot be obtained. Considering the dyeability and the physical properties of the polyester composition, the content of the sulfonate groups as shown in Formula 1 is preferably 1000-3500ppm of the polyester composition in terms of sulfur element.
[0033] In order to further improve the dyeing performance and strength of the polyester composition, the polyester composition of the present invention also contains a polyether structural unit, and the polyether structural unit is derived from polyethylene glycol, poly 1,3-propylene glycol, poly 2-methyl-1,3-propylene glycol or polybutylene glycol, etc., preferably from a polyethylene glycol structural unit.
[0034] When the content of the polyether structural unit in the polyester composition is too low, it does not improve the dyeing performance and strength of the polyester composition; when the content of the polyether structural unit in the polyester composition is too high, the polyester composition has poor heat resistance and is prone to thermal decomposition during subsequent processing, affecting the quality of the polyester composition product. The content of the polyether structural unit in the polyester composition of the present invention is preferably 0.1 to 10.0 wt%, more preferably 0.1 to 5.0 wt%.
[0035] In the prior art, phosphorus compounds are generally added to the polyester composition reaction to improve the heat resistance of the polyester composition. However, the phosphorus compounds usually added to the cationic dyeable polyester composition are prone to form foreign substances such as phosphate metal salts, thereby affecting the filter pressure during spinning of the polyester composition, resulting in a shortened component replacement cycle, an increased yarn breakage rate, and poor spinnability. Therefore, in order to ensure that the polyester composition has good spinnability, the content of the phosphate metal salt compound in the polyester composition of the present invention is less than 20 ppm, preferably less than 10 ppm, in terms of phosphorus atoms.
[0036] The metal phosphate includes but is not limited to potassium phosphate, sodium phosphate, lithium phosphate, cesium phosphate, magnesium phosphate, calcium phosphate, etc. In the present invention, the metal phosphate is preferably one or more of potassium phosphate, sodium phosphate or lithium phosphate.
[0037] The present invention also discloses a method for preparing the cationic dyeable polyester composition, wherein an aromatic dicarboxylic acid or its esterified derivative and an aliphatic diol are first subjected to an esterification or transesterification reaction to obtain an oligomer, and then the oligomer is subjected to a polymerization reaction to obtain the polyester composition. Before the polymerization reaction begins, a sulfonate compound, a polyether and a metal compound as shown in Formula 2 are added to the oligomer in an amount of 1000 to 5000 ppm in terms of sulfur element relative to the total amount of the polyester composition;
[0038] Formula 2,
[0039] In Formula 2, Y is an alkyl group, a phenyl group or an alkylbenzene having 2 to 20 carbon atoms, and Z is a Li ion, a Na ion or a K ion. Specific examples include 2-carboxybenzene sulfonate sodium, 2-carboxybenzene sulfonate potassium, 3-carboxybenzene sulfonate sodium, 3-carboxybenzene sulfonate lithium, 4-carboxybenzene sulfonate sodium, 2-sulfonate sodium methyl benzoate, 3-sulfonate sodium methyl benzoate, 4-sulfonate sodium methyl benzoate, 2-sulfonate sodium ethyl benzoate, 2-sulfonate potassium benzoate ethylene glycol, 3-sulfonate sodium ethyl benzoate, 4-sulfonate sodium benzoate ethylene glycol, 3-sulfonate lithium benzoate, etc., among which 3-carboxybenzene sulfonate sodium is preferred.
[0040] The amount of the sulfonate compound as shown in Formula 2 is 1000-5000ppm in terms of sulfur element relative to the total amount of the polyester composition. When the amount of the sulfonate compound as shown in Formula 2 is less than 1000ppm, it is difficult for the obtained product to achieve a satisfactory color concentration in the subsequent dyeing process; when the amount of the sulfonate compound as shown in Formula 2 is more than 5000ppm, it will inhibit the growth of the polyester molecular chain, causing polymerization head phenomenon, and it is impossible to obtain a polyester composition with good physical properties. Considering the dyeability and the physical properties of the polyester composition, the amount of the sulfonate compound as shown in Formula 2 is preferably 1000-3500ppm in terms of sulfur element relative to the total amount of the polyester composition.
[0041] As shown in Formula 2, the sulfonate compound is a powdery substance. Therefore, when adding, according to the conventional practice in the art, the sulfonate compound as shown in Formula 2 is first dissolved in an aliphatic diol to prepare an aliphatic diol solution, and then added. Specifically, the sulfonate compound as shown in Formula 2 and the aliphatic diol are dissolved at a mass ratio of 1:0.5 to 1:10.0 at 70 to 198°C to form a uniform solution. The weight ratio of the sulfonate as shown in Formula 2 and the aliphatic diol is preferably 1:1.0 to 1:2.0, and the dissolution temperature is preferably 80 to 130°C. The preparation of the aliphatic diol solution can be carried out according to the above method, but is not limited to the above method.
[0042] In addition, in order to improve the dyeing performance and strength of the polyester composition, the present invention adds polyether at any stage before the end of the polymerization reaction. The polyether can increase the flexible chain of the polyester composition, improve the mobility of the polyester composition, and make the dye molecules easily enter the interior of the polyester, thereby improving the dyeing property of the polyester composition. At the same time, the polyether can also promote the polymerization reactivity of the polyester composition and increase the molecular weight of the polyester composition, thereby facilitating the yarn orientation in the spinning process, improving the strength of the yarn, and improving the strength retention rate of the yarn before and after dyeing. The polyether can be polyethylene glycol, poly-1,3-propylene glycol, poly-2-methyl-1,3-propylene glycol or polybutylene glycol, etc., wherein polyethylene glycol is preferred.
[0043] The amount of the polyether added is preferably 0.1 to 10.0 wt% relative to the total amount of the polyester composition. When the amount of the polyether added is too little, it will not improve the dyeing performance and strength of the polyester composition; when the amount of the polyether added is too high, the polyester composition has poor heat resistance and is prone to thermal decomposition during subsequent processing, affecting the quality of the polyester composition product. The amount of the polyether added in the present invention is more preferably 0.1 to 5.0 wt%.
[0044] In addition to controlling the amount of polyether added to prevent the deterioration of the heat resistance of the polyester composition caused by the decomposition of the polyether, the present invention also adds an alkali metal or alkaline earth metal compound before the polymerization reaction begins. The alkali metal or alkaline earth metal compound can not only inhibit the thermal decomposition of the polyether, but also inhibit the formation of DEG, thereby improving the light resistance and UV resistance of the polyester composition. The alkali metal or alkaline earth metal compound can be one or more of sodium acetate, lithium acetate, potassium acetate, cesium acetate, sodium hydroxide, potassium hydroxide, lithium hydroxide, cesium hydroxide, sodium carbonate, potassium carbonate, cesium carbonate, magnesium acetate, and calcium acetate, among which one or more of lithium acetate, potassium acetate, or sodium acetate is preferred.
[0045] The amount of the alkali metal or alkaline earth metal compound added in the present invention is preferably equivalent to 5 to 2000 ppm of the total amount of the polyester composition. When the amount of the alkali metal or alkaline earth metal compound added is too small, it cannot inhibit DEG and improve the light resistance and UV resistance performance; when the amount of the alkali metal or alkaline earth metal compound added is too large, it is easy to cause thermal decomposition of the polymer, and the physical properties of the polymer and the fiber deteriorate.
[0046] During the preparation process of the polyester composition described in the present invention, a stabilizer phosphorus compound is also added. In general polyester reactions, the stabilizer phosphorus compound is added before the polymerization reaction. During the polymerization reaction, alkali metal or alkaline earth metal compounds react easily with heat stabilizer phosphorus compounds to generate foreign metal phosphates, which affect the spinning filter pressure, and have a high rate of broken fibers and poor spinnability. In order to inhibit the formation of metal phosphates, the present invention chooses to add a stabilizer phosphorus compound before the end of the polymerization reaction, thereby reducing the reaction probability of the stabilizer phosphorus compound and the alkali metal or alkaline earth metal compound. However, the addition of the alkali metal or alkaline earth metal compound cannot be too late, otherwise it will cause uneven mixing of the alkali metal or alkaline earth metal compound in the polyester composition, resulting in poor heat resistance of the polyester composition. The present invention preferably adds the stabilizer phosphorus compound 5 to 20 minutes before the end of the polymerization reaction.
[0047] The stabilizer phosphorus compound can be a trivalent phosphorus compound or a pentavalent phosphorus compound, and specific examples include phosphoric acid, phosphorous acid, trimethyl phosphate, triethyl phosphoacetate, triethyl phosphate, triphenyl phosphate, triphenyl phosphite, etc., among which one or more of phosphoric acid, trimethyl phosphate, and triethyl phosphate are preferred. The addition amount of the phosphorus compound stabilizer is preferably equivalent to 5 to 150 ppm of the weight of the polyester in terms of phosphorus element.
[0048] The aromatic dicarboxylic acid or its esterified derivatives of the present invention can be terephthalic acid, isophthalic acid, naphthalene dicarboxylic acid, dimethyl terephthalate, dimethyl isophthalate, dimethyl naphthalate, dimethyl phthalate, etc., among which terephthalic acid or dimethyl terephthalate is preferred. The aliphatic diol can be ethylene glycol, propylene glycol, butanediol, 1,2-propylene glycol, pentanediol, neopentyl glycol, 1,2-butanediol, etc., among which ethylene glycol, propylene glycol or butanediol is preferred.
[0049] The esterification reaction may be carried out in an esterification reaction tank where oligomers are pre-existing while continuously adding a slurry of aliphatic diol and aromatic dicarboxylic acid in a molar ratio of 1.05 to 1.50; or the esterification reaction may be carried out in an esterification reaction tank where oligomers are pre-existing after all aliphatic diol and aromatic dicarboxylic acid are added before the esterification reaction starts.
[0050] The transesterification reaction can be carried out by adjusting the molar ratio of the aliphatic diol to the aromatic dicarboxylic acid esterified derivative to be within the range of 1.50 to 2.50 to control the appropriate transesterification reaction rate. The catalyst used in the process can be various known catalysts, such as oxides or acetates of metals such as cobalt, magnesium, manganese, and titanium, which can be used in combination or alone.
[0051] The catalyst in the polymerization reaction can be any known polymerization catalyst, such as antimony compounds, germanium compounds, titanium compounds, etc. These catalysts can be used in combination or alone.
[0052] The esterification and polymerization reaction apparatus for producing the easily dyeable, hydrolysis-resistant, high-strength cationic dyeable polyester composition of the present invention can be any commonly used reaction apparatus.
[0053] The polyester composition of the invention is easy to dye, the filter pressure of the spinning assembly increases slowly, and the spinnability is good. The polyester composition can be used in fibers.
[0054] The determination methods and evaluation methods of various indicators of the present invention are as follows:
[0055] (1) Intrinsic viscosity (IV)
[0056] 0.8 g of the polyester composition chips were dissolved in 10 ml of o-chlorophenol solution, and the intrinsic viscosity was measured using an Ubbelohde viscometer at a water bath temperature of 25±0.2°C.
[0057] (2) Filter pressure difference ΔPa
[0058] The filter pressure test was conducted using a small filterability test machine. Under certain discharge conditions, cationic dyeable polyester was passed through the filter screen, the filter screen aperture was 5μm, the test temperature was the melting point of polyester + 25°C, the discharge volume was 10g / min, and the pressure before the filter screen 30 minutes after the start of feeding was recorded as the initial pressure Pa1, and the final pressure Pa2 was recorded 1 hour after the initial pressure, then the filter pressure rise value for 1 hour was ΔPa=Pa2-Pa1. The smaller the ΔPa, the less foreign matter there is in the polyester, and the more stable the spinning.
[0059] (3) Phosphate metal salt content
[0060] The filter after the filtration pressure test in method (2) is dissolved and filtered using the solvent hexafluoroisopropanol, and the foreign matter on the filter paper is subjected to ICP element analysis to analyze the composition and content of the foreign matter.
[0061] (4) Sulfur content in polyester composition
[0062] The sulfur content in the polymer was quantitatively analyzed by ICP element analyzer.
[0063] (5) Dyeability evaluation
[0064] The polyester composition was spun to obtain a drawn yarn, and then two drawn fibers were paralleled to obtain a sock under a 22-gauge condition. The sock was dyed in a hot water bath at 110°C for 60 minutes with a dye (Blue.TR) 3% owf, acetic acid 0.5 ml / l, sodium acetate 0.2 g / l, and a bath ratio of 1:100. The dyed samples were overlapped to be opaque and then measured with a spectrophotometer (Datacolor 650 manufactured by Datacolor Asia Pacific (HK) Ltd.) under CEI standard light sources D65, 10 o L* is obtained by measuring color under angular conditions.
[0065] (6) Polyether content in polyester composition
[0066] A certain amount of the polyester composition is taken, and the content of the polyether in the polyester composition is calculated by measuring the characteristic peak of hydrogen element (such as -CH3 or -CH2 in the polyether) by H-NMR.
[0067] The advantages of the present invention will be described in detail below by referring to the following examples and comparative examples. The present invention is not limited to the following examples.
[0068] Example 1
[0069] Terephthalic acid (PTA) and ethylene glycol (EG) were mixed evenly and put into a reactor to carry out esterification reaction at 240°C. After the esterification reaction was completed, the reaction product was transferred to a polycondensation reactor, and an ethylene glycol solution of a sulfonate as shown in Formula 2, polyethylene glycol, a catalyst antimony trioxide and sodium acetate were added before the polymerization reaction, and the polycondensation reaction was carried out at 290°C. Phosphoric acid, a heat stabilizer, was added 10 minutes before the end of the polymerization reaction, and then the desired polyester composition was obtained by discharging and pelletizing. The intrinsic viscosity IV of the polyester composition was 0.60 dl / g.
[0070] The polyester composition was spun to obtain drawn yarn, and then the drawn fiber was used to make a sock, which was dyed in a hot water bath at 110°C for 60 minutes with a dye (Blue.TR) 3% owf, acetic acid 0.5 ml / l, sodium acetate 0.2 g / l, and a bath ratio of 1:100. The L value after dyeing was 25.
[0071] Embodiment 2-3
[0072] The addition period of phosphoric acid was changed, and other conditions were the same as those in Example 1 to prepare a cationic dyeable polyester composition. Specific physical properties are shown in Table 1.
[0073] Embodiment 4-5
[0074] The cationic dyeable polyester composition was prepared by changing the type of metal compound and keeping the other conditions the same as in Example 1. The specific physical properties are shown in Table 1.
[0075] Embodiments 6 to 8
[0076] The amount of sulfonate added as shown in Formula 2 was changed, and other conditions were the same as in Example 1 to prepare a cationic dyeable polyester composition. Specific physical properties are shown in Table 1.
[0077] Embodiments 9-10
[0078] The cationic dyeable polyester composition was prepared by changing the type of polyether and keeping the other conditions the same as in Example 1. The specific physical properties are shown in Table 2.
[0079] Examples 11 to 15
[0080] The amount of polyether added was changed, and other conditions were the same as in Example 1 to prepare a cationic dyeable polyester composition. Specific physical properties are shown in Table 2.
[0081] Comparative Example 1
[0082] Terephthalic acid (PTA) and ethylene glycol (EG) are mixed evenly and put into a reactor for esterification reaction at 240°C. After the esterification reaction is completed, the reaction product is transferred to a polycondensation reactor, and an ethylene glycol solution of a sulfonate as shown in Formula 2, a catalyst antimony trioxide and a heat stabilizer trimethyl phosphate are added before the polymerization reaction, and a polycondensation reaction is carried out at 290°C. After the polymer reaches the required viscosity, it is discharged and pelletized to obtain the required polyester composition.
[0083] The polyester composition was spun to obtain drawn yarn to make a sock, which was then dyed in a hot water bath at 110°C for 60 minutes with a dye (Blue.TR) 3% owf, acetic acid 0.5 ml / l, sodium acetate 0.2 g / l, and a bath ratio of 1:100. The L value after dyeing was 40.
[0084] Since no polyether was added, the resulting polyester composition had a poor color tone after dyeing.
[0085] Comparative Example 2
[0086] Terephthalic acid (PTA) and ethylene glycol (EG) are mixed evenly and put into a reactor for esterification reaction at 240°C. After the esterification reaction is completed, the reaction product is transferred to a polycondensation reactor, and polyethylene glycol, an ethylene glycol solution of a sulfonate as shown in Formula 2, a catalyst antimony trioxide, and a heat stabilizer trimethyl phosphate and sodium acetate are added before the polymerization reaction, and the polycondensation reaction is carried out at 290°C. After the polymer reaches the required viscosity, it is discharged and pelletized to obtain the required polyester composition.
[0087] The polyester composition was spun to obtain drawn yarn to make a sock, which was then dyed in a hot water bath at 110°C for 60 minutes with a dye (Blue.TR) 3% owf, acetic acid 0.5 ml / l, sodium acetate 0.2 g / l, and a bath ratio of 1:100. The L value after dyeing was 25.
[0088] Since sodium acetate is added before the start of polymerization, the foreign matter content in the polyester composition is high and the polymer filter pressure increases greatly.
[0089]
[0090]
Claims
1. A method for preparing a cationic dyeable polyester composition, comprising: firstly subjecting an aromatic dicarboxylic acid or an esterified derivative thereof to an aliphatic diol through an esterification or transesterification reaction to obtain an oligomer, and then subjecting the oligomer to a polymerization reaction to obtain the polyester composition, wherein: Before the polymerization reaction begins, 1000 to 5000 ppm of a sulfonate compound as shown in formula 2, a polyether, and an alkali metal or alkaline earth metal compound are added to the oligomer in terms of sulfur element relative to the total amount of the polyester composition; a phosphorus compound is added 5 to 20 minutes before the polymerization reaction ends; the content of the metal phosphate in the obtained polyester composition is 3 to 20 ppm in terms of phosphorus atoms; Formula 2, In Formula 2, Y is an alkyl group having 2 to 20 carbon atoms, a phenyl group or an alkylbenzene group, and Z is a Li ion, a Na ion or a K ion.
2. The method for preparing a cationic dyeable polyester composition according to claim 1, wherein: The amount of the polyether added is equivalent to 0.1 to 10.0 wt % of the total amount of the polyester composition.
3. The method for preparing a cationic dyeable polyester composition according to claim 1, wherein: The amount of the sulfonate salt as shown in Formula 2 added is 1000 to 3500 ppm in terms of sulfur element relative to the total amount of the polyester composition.
4. The method for preparing a cationic dyeable polyester composition according to claim 1, wherein: The alkali metal or alkaline earth metal compound is one or more of lithium acetate, sodium acetate or potassium acetate, and the added amount thereof is equivalent to 5 to 2000 ppm of the total amount of the polyester composition.
5. The method for preparing a cationic dyeable polyester composition according to claim 1, wherein: The phosphorus compound is one or more of phosphoric acid, trimethyl phosphate and triethyl phosphate.
6. The cationic dyeable polyester composition prepared by the preparation method of the cationic dyeable polyester composition according to claim 1, mainly composed of aromatic dicarboxylic acid structural units and polyether structural units, characterized in that: The polyester composition contains a sulfonate group as shown in Formula 1, and the content of the group as shown in Formula 1 accounts for 1000-5000 ppm of the total amount of the polyester composition in terms of sulfur element; the polyester composition contains a polyether structural unit; the polyester composition contains an alkali metal or alkaline earth metal compound; the content of the phosphate metal salt in the polyester composition is 3-20 ppm in terms of phosphorus atoms; Formula 1, In Formula 1, Y is an alkyl group having 2 to 20 carbon atoms, a phenyl group or an alkylbenzene group, and Z is a Li ion, a Na ion or a K ion.
7. The cationic dyeable polyester composition according to claim 6, characterized in that: The polyether structural unit accounts for 0.1 to 10.0 wt % of the total amount of the polyester composition.
8. The cationic dyeable polyester composition according to claim 6 or 7, characterized in that: The metal phosphate is one or more of potassium phosphate, sodium phosphate or lithium phosphate.
9. The cationic dyeable polyester composition according to claim 6, characterized in that: The content of the group described in Formula 1 is 1000 to 3500 ppm based on the total amount of the polyester composition, calculated as sulfur element.