Multilayer packaging materials and photovoltaic modules
Through the multi-layer packaging material structure, including micro crosslinking layer, reflective glue layer and support glue layer, the use of pre-crosslinking and filler distribution, the high cost and whitening problems of white packaging materials of photovoltaic components are solved, and cost reduction and performance improvement are achieved. .
Patent Information
- Application Number
- CN202210763226.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-06-30
- Filing Date
- 2022-06-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-06-30
AI Technical Summary
The white packaging materials of existing photovoltaic modules are costly, making it difficult to drop to the same level as transparent EVA, and fillers or pigments are prone to overflow during high-temperature lamination, contaminating the battery cells.
The multi-layer packaging material structure is adopted, including a micro-crosslinking layer, a reflective glue layer and a support glue layer. Through pre-crosslinking and reasonable distribution of fillers, the amount of titanium dioxide is reduced and the cost is reduced. The reflective glue layer is covered by a micro-crosslinking layer. Avoid whitening problems.
It realizes the reduction of the cost of photovoltaic module packaging materials, while avoiding the whitening of the reflective glue layer during lamination, alleviating the compressive stress of the battery cell, and improving the stability and performance of the module.
Smart Images

Figure CN115124947B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photovoltaic packaging materials, and in particular to a multi-layer packaging material and a photovoltaic module. Background Art
[0002] With the continuous advancement of the goal of grid parity for photovoltaic modules, the pursuit of shorter lamination time and higher module power for photovoltaic modules is pursued. At the same time, with the increasing promotion of photovoltaic modules, there is also a demand for personalized appearance, such as photovoltaic modules encapsulated with white packaging materials, black packaging materials, and colored packaging materials. This often requires adding fillers or pigments to the packaging materials to increase reflectivity or achieve the purpose of color adjustment. However, when photovoltaic modules are laminated at high temperatures, fillers or pigments will overflow irregularly with the extrusion of the lamination process, and even pollute the power generation area on the surface of the cell. In order to solve the above problems, the defects of filler or pigment overflow in the packaging material can be improved by partially pre-crosslinking the packaging material in advance and taking advantage of the fact that the filler in the pre-crosslinked packaging material cannot flow freely.
[0003] Among colored packaging materials, white packaging materials are currently the most widely used. White EVA has significant cost advantages over white POE, and the front layer transparent EVA also has significant cost advantages over transparent POE, so it has been the first to be widely used. However, with the continuous advancement of the goal of grid parity for photovoltaic modules, photovoltaic module manufacturers hope that the price of white EVA can be reduced to the same level as transparent EVA. On the market, various white EVA suppliers currently basically adopt a single-layer formula of titanium dioxide + EVA. The price of titanium dioxide is about 1.5 times the price of EVA resin, which makes the cost of white EVA significantly higher than that of transparent EVA, and it is difficult to reduce it to the same price as transparent EVA. Summary of the invention
[0004] The main purpose of the present invention is to provide a multi-layer packaging material and a photovoltaic module to solve the problem of high packaging material cost in the prior art.
[0005] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a multilayer packaging material is provided, the multilayer packaging material comprises a micro-crosslinked layer, a reflective adhesive layer and a supporting adhesive layer stacked in sequence, or the multilayer packaging material comprises a reflective adhesive layer, a micro-crosslinked layer and a supporting adhesive layer stacked in sequence, the pre-crosslinking degree of the micro-crosslinked layer is ≤10%, the reflective adhesive layer has a titanium dioxide content of 2 to 30% by mass, the mass content of the filler in the supporting adhesive layer is 10 to 40%, the mass content of titanium dioxide in the supporting adhesive layer is less than 12%, the mass content of titanium dioxide in the micro-crosslinked layer is less than 12%, and the thickness of the micro-crosslinked layer is 5 to 38% of the total thickness of the multilayer packaging material.
[0006] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, there is provided a photovoltaic module, comprising a front panel, a transparent adhesive film, a battery cell unit, a back layer adhesive film and a back panel which are laminated in sequence, wherein the back layer adhesive film is any one of the above-mentioned multi-layer packaging materials, and the supporting adhesive layer of the multi-layer reflective packaging adhesive film is arranged away from the battery cell unit.
[0007] By applying the technical solution of the present invention, the present application sets the packaging material into multiple layers, and even if the thickness of the reflective adhesive layer is reduced, the set packaging effect can still be achieved, and only a large amount of titanium dioxide is set in the reflective adhesive layer to achieve the effect of high reflection, and the mass content of titanium dioxide is controlled to be lower than 12% in the micro-crosslinked layer and the supporting adhesive layer, that is, it includes two situations: no titanium dioxide is set and titanium dioxide is set and the mass content of titanium dioxide is lower than the above value, thereby reducing the amount of titanium dioxide used in the entire multi-layer packaging material, and at the same time, fillers are used in the supporting adhesive layer to further reduce the cost of the supporting adhesive layer, thereby reducing the cost of the multi-layer packaging film. However, the content of the filler should not be too much, otherwise it will cause the hardness of the supporting adhesive layer to be too large. Furthermore, in the multi-layer packaging material of the present application, a micro-crosslinked layer is used to cover the reflective adhesive layer, thereby effectively avoiding the problem of white overflow of the reflective adhesive layer 20 during the lamination process. At the same time, the content of titanium dioxide in the micro-crosslinked layer is low, so the compressive stress on the battery cell is small, thereby effectively alleviating the problem of battery cell splitting or hidden cracking. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0009] Figure 1 A schematic structural diagram of a multi-layer packaging material provided according to an embodiment of the present invention is shown;
[0010] Figure 2 A schematic diagram showing the structure of a multi-layer packaging material provided in another embodiment of the present invention is shown; and
[0011] Figure 3 A schematic diagram of the disassembled structure of a photovoltaic assembly provided according to an embodiment of the present invention is shown.
[0012] The above drawings include the following reference numerals:
[0013] 10. micro-cross-linking layer; 20. reflective adhesive layer; 30. supporting adhesive layer;
[0014] 1. Front panel; 2. Transparent film; 3. Battery cell unit; 4. Back layer film; 5. Back panel. DETAILED DESCRIPTION
[0015] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0016] As analyzed in the background of this application, the white adhesive film in the prior art uses titanium dioxide as a pigment, which results in high cost. In order to solve this problem, this application provides a multi-layer packaging material and a photovoltaic module.
[0017] In a typical embodiment of the present application, a multi-layer packaging material is provided, such as Figure 1 and 2 As shown, the multilayer packaging material includes a micro-crosslinked layer 10, a reflective adhesive layer 20 and a supporting adhesive layer 30 stacked in sequence, the pre-crosslinking degree of the micro-crosslinked layer 10 is ≤10%, the reflective adhesive layer 20 contains titanium dioxide with a mass content of 2-30%, the mass content of the filler in the supporting adhesive layer 30 is 10-40%, the mass content of titanium dioxide in the supporting adhesive layer 30 is less than 12%, the mass content of titanium dioxide in the micro-crosslinked layer 10 is less than 12%, and the thickness of the micro-crosslinked layer 10 is 5-38% of the total thickness of the multilayer packaging material.
[0018] The present application sets the packaging material to be multi-layered, and even if the thickness of the reflective adhesive layer 20 is reduced, the set packaging effect can still be achieved, and only a large amount of titanium dioxide is set in the reflective adhesive layer 20 to achieve a high reflection effect, and the mass content of titanium dioxide is controlled to be lower than 12% in the micro-crosslinked layer 10 and the supporting adhesive layer 30, that is, it includes two situations: no titanium dioxide is set and titanium dioxide is set and the mass content of titanium dioxide is lower than the above value, thereby reducing the amount of titanium dioxide used in the entire multi-layer packaging material, and at the same time, fillers are used in the supporting adhesive layer 30 to further reduce the cost of the supporting adhesive layer 30, thereby reducing the cost of the multi-layer packaging film. However, the content of fillers should not be too much, otherwise it will cause the hardness of the supporting adhesive layer 30 to be too large. Further, in the multi-layer packaging material of the present application, the micro-crosslinked layer 10 is used to cover the reflective adhesive layer 20, thereby effectively avoiding the problem of white overflow of the reflective adhesive layer 20 during the lamination process. At the same time, the titanium dioxide content in the micro-crosslinked layer 10 is low, so the compressive stress on the battery cell is small, thereby effectively alleviating the problem of battery cell splitting or hidden cracking.
[0019] The micro-crosslinked layer 10 can be achieved by conventional radiation crosslinking methods. In one embodiment, electron radiation is preferred, wherein the electron beam energy of the electron radiation is preferably 200keV to 5000keV, and the radiation dose of the electron radiation is 5 to 250kGy.
[0020] Since the flexibility of the micro-crosslinked layer 10 is reduced after pre-crosslinking, it is easy to cause hidden cracks or splits in the battery cell. In order to improve the flexibility of the micro-crosslinked layer 10 and effectively solve the problem of whitening, the pre-crosslinking degree of the micro-crosslinked layer 10 is preferably 0.5-5%, and the thickness of the micro-crosslinked layer 10 is 0.06-0.35 mm. As mentioned above, due to the composite effect of the multi-layer structure of the multi-layer packaging material of the present application, the thickness of the reflective adhesive layer 20 is reduced and the amount of titanium dioxide is reduced, so the risk of whitening is reduced, and then the micro-crosslinked layer 10 with the above-mentioned lower pre-crosslinking degree can still achieve the effect of preventing the reflective adhesive layer 20 from overflowing into the battery cell area on the basis of having the above-mentioned thickness.
[0021] Pre-crosslinking is only the crosslinking of the micro-crosslinked layer 10 before subsequent crosslinking, so the pre-crosslinking degree is also the crosslinking degree.
[0022] In one embodiment of the present application, in order to further improve the flexibility of the multilayer packaging material and optimize the buffering effect of the lamination pressure during the lamination process, it is preferred that the above-mentioned reflective adhesive layer 20 and the supporting adhesive layer 30 each independently have a cellular structure. Since the reflective adhesive layer 20 and the supporting adhesive layer 30 each contain a relatively high proportion of titanium dioxide and filler, after the cellular structure is set, the titanium dioxide and filler may fall out of the pores due to deformation during lamination. In order to avoid the occurrence of this problem, the cellular density of the reflective adhesive layer 20 and the supporting adhesive layer 30 is preferably 80 to 10 10 Unit cells / cm 3 , the cell diameter of the unit cell is 0.1μm~0.1mm. The above cell density can be controlled by controlling the proportion of the added foaming agent and the foaming process, such as controlling the temperature of the foaming chamber to 90~170℃ and the foaming time to 5s~5min. For the same adhesive layer, when the foaming time is the same, within the above temperature range, the higher the foaming temperature, the greater the cell density and the better the flexibility; on the contrary, the lower the temperature, the smaller the cell density and the lower the flexibility. For the same adhesive layer, when the foaming temperature is the same, the longer the foaming time, the greater the cell density and the better the flexibility; the shorter the foaming time, the smaller the cell density and the worse the flexibility.
[0023] When having a cellular structure, the compressibility of the adhesive layer is optimized, but the thickness of the adhesive layer before lamination will also increase accordingly. In order to minimize the thickness of the photovoltaic module, the thickness ratio of the micro-cross-linked layer 10 to the reflective adhesive layer 20 is preferably 3.5:1 to 1:10, and the thickness ratio of the micro-cross-linked layer 10 to the supporting adhesive layer 30 is preferably 3.5:1 to 1:14.
[0024] Since the reflective adhesive layer 20 contains titanium dioxide and fillers, it is easy to flow and deform due to high temperature melting during lamination, thereby affecting the appearance of the photovoltaic module. To optimize the appearance of the photovoltaic module, such as Figure 2As shown, when the multi-layer packaging material includes a reflective adhesive layer 20, a micro-crosslinked layer 10 and a supporting adhesive layer 30 stacked in sequence, the reflective adhesive layer 20 is preferably a pre-crosslinked film, and the pre-crosslinking degree of the pre-crosslinked film is 0.5-70%, preferably 0.5-60%, and more preferably 0.5-50%. In particular, when the reflective adhesive layer 20 has a cellular structure, after pre-crosslinking, although the flexibility of the adhesive layer is reduced to a certain extent, due to its high dimensional stability, the problem of titanium dioxide overflowing to the edge of the photovoltaic module is well controlled, and the problem of titanium dioxide falling into the pores is also effectively solved. Of course, in order to improve the dimensional stability of the multi-layer packaging material, the supporting adhesive layer 30 can also be a pre-crosslinked film, and the pre-crosslinking degree can be 0.5-50%, preferably 0.5-40%, and more preferably 0.5-30%.
[0025] When the reflective adhesive layer 20 and / or the supporting adhesive layer 30 has a cellular structure, it is only necessary to add a foaming agent to the raw materials for preparing the reflective adhesive layer 20 and / or the supporting adhesive layer 30 and perform foaming during the process of preparing the adhesive layer.
[0026] As described above, the purpose of setting the supporting adhesive layer 30 is mainly to further reduce the cost of using a large amount of titanium dioxide. In the current prior art, for example, fillers commonly used in cable adhesive films can be considered for application in this application. On the one hand, it meets the requirement of reducing costs, and on the other hand, it meets the requirement of high dielectric properties. In order to facilitate technicians in the field to select appropriate fillers, the volume resistivity of the supporting adhesive layer 30 is preferably greater than 1.0×10 14 Ω·cm, and the filler is preferably selected from any one or more combinations of CaCO3, lithopone, wollastonite, mica powder, magnesium hydroxide, aluminum hydroxide, calcium hydroxide, talc, barium sulfate, glass microspheres, zinc sulfide, kaolin, and montmorillonite.
[0027] The multilayer packaging material of the present application can be a combined mold, which meets the above-mentioned bonding requirements after lamination or is bonded by an adhesive, or it can be a co-extruded film. Preferably, the multilayer packaging material is a co-extruded adhesive film to make the stability of the entire adhesive film better.
[0028] The micro-crosslinked layer 10 may have the same composition as the conventional transparent adhesive layer or white film in the prior art except for the content of titanium dioxide, but its thickness is greatly reduced relative to the thickness of the conventional transparent adhesive layer and white film in the prior art. Preferably, the raw materials for forming the micro-crosslinked layer 10 include: 100 parts by weight of the first photovoltaic matrix resin, 0.01 to 10 parts by weight of a tackifier, 0.01 to 5 parts by weight of a crosslinking agent, 0 to 2 parts by weight of a first auxiliary crosslinking agent, 0 to 15 parts by weight of titanium dioxide, 0 to 3 parts by weight of an auxiliary agent, and 0 to 10 parts by weight of a first polyolefin synthetic oil. The micro-crosslinked layer 10 may or may not use a filler, and the use of a filler further reduces its cost; and the filler may be the same as or different from the filler in the supporting adhesive layer 30, and those skilled in the art may freely choose from the fillers listed above, which will not be described in detail here.
[0029] In some embodiments, the first photovoltaic matrix resin is selected from any one or more of the following polymers: ethylene-vinyl acetate copolymer, metallocene-catalyzed polyethylene, metallocene-catalyzed ethylene-butene copolymer, metallocene-catalyzed ethylene-octene copolymer, metallocene-catalyzed ethylene-pentene copolymer, ethylene-propylene copolymer, ethylene-methyl acrylate copolymer, ethylene-methyl methacrylate copolymer, ethylene-glycidyl methacrylate copolymer, ethylene-glycidyl methacrylate-vinyl acetate copolymer, ethylene-glycidyl methacrylate-methyl acrylate copolymer;
[0030] The use of the first auxiliary cross-linking agent is mainly to delay the cross-linking progress of the micro-cross-linked layer 10 during the radiation process, so as to accurately control the degree of cross-linking. In some embodiments, the first auxiliary cross-linking agent is preferably a first sensitizer, and the first sensitizer is preferably an allyl sensitizer. The first sensitizer is preferably any one or more of the following compounds: trimethylallyl isocyanate, triallyl isocyanurate, triallyl cyanurate, divinylbenzene, di-isopropenylbenzene, diallyl phthalate, allyl acrylate, allyl methacrylate, diallyl maleate, diallyl phthalate. The self-inhibition effect of allyl is used to delay the cross-linking progress of the reflective adhesive layer 20 during the radiation process, and during the lamination process, the allyl sensitizer can promote cross-linking and improve the cross-linking efficiency during lamination.
[0031] In some embodiments, the first polyolefin synthetic silicone oil is selected from any one or more of poly-α-olefin synthetic oil, polybutene synthetic oil, and alkylbenzene synthetic oil. More preferably, the first polyolefin synthetic silicone oil is a liquid ethylene polymer oil; preferably, the liquid ethylene polymer oil is derived from a combination of ethylene A and an α-olefin B having 3 to 20 carbon atoms or a combination of ethylene A, an α-olefin B having 3 to 20 carbon atoms, and a non-conjugated polyene C, and the liquid ethylene polymer oil satisfies the following conditions 1) to 4); the non-conjugated polyene C contains a total of two or more partial structures selected from the group consisting of the following general formulas (I) and (II) in the molecule,
[0032]
[0033] Wherein, 1) the molar ratio of ethylene A / α-olefin B is 40:60 to 95:5; 2) the weight fraction of the structural unit derived from the non-conjugated polyene C in the liquid ethylene polymer oil is 0 to 10%; 3) the weight average molecular weight Mw of the ethylene-α-olefin-non-conjugated polyene copolymer, the weight fraction of the structural unit derived from the non-conjugated polyene C and the weight average molecular weight Mw of the non-conjugated polyene C satisfy: Mw×weight fraction of C / molecular weight of C≤40; 4) the number average molecular weight Mn of the liquid ethylene polymer oil measured by gel permeation chromatography is less than 30,000; preferably, the first polyolefin synthetic silicone oil is an ethylene-propylene copolymer or an ethylene-propylene-non-conjugated diene terpolymer; preferably, ethylene The proportion of ethylene and propylene units in the olefin-propylene-non-conjugated diene terpolymer is greater than 90%; preferably, the ethylene-α-olefin-non-conjugated polyene copolymer includes units derived from ethylene or units derived from propylene, preferably, the ethylene-α-olefin-non-conjugated polyene copolymer includes units derived from diene monomers, and preferably the diene monomers are any one or more of non-conjugated straight-chain hydrocarbon dienes, non-conjugated branched hydrocarbon dienes, and non-conjugated cyclic hydrocarbon dienes having 6 to 15 carbon atoms. Further, the weight average molecular weight of the first polyolefin synthetic silicone oil is 200 to 50,000, preferably 200 to 10,000, and preferably, the viscosity index of the first polyolefin synthetic silicone oil is 60 to 250, preferably 80 to 180.
[0034] Polyolefin synthetic oil has a low glass transition temperature, does not contain a crystalline structure, and has good compatibility with polyolefin resin substrates. After addition, it can reduce the crystallinity of the polyolefin resin substrate; increase the distance between molecules of the polyolefin resin substrate, reduce the intermolecular force, enhance the activity of the chain segments, and improve the flexibility of the molecular chain; or reduce the glass transition temperature of the polyolefin resin substrate, thereby increasing the softness of the encapsulation film, and ultimately reducing the fragmentation rate of the battery cell.
[0035] The above-mentioned reflective adhesive layer 20 can have the same composition as the single-layer reflective adhesive layer commonly used in the prior art, except that its thickness is greatly reduced compared with the thickness of the conventional single-layer reflective adhesive layer in the prior art. Preferably, the raw materials for forming the reflective adhesive layer 20 include: 100 parts by weight of the second photovoltaic matrix resin, 0.01-15 parts by weight of a tackifier, 0.01-5 parts by weight of a cross-linking agent, 0.05-5 parts by weight of a second auxiliary cross-linking agent, 2-40 parts by weight of titanium dioxide, 0-3 parts by weight of an auxiliary agent, 0-30 parts by weight of a foaming agent, 0-30 parts by weight of a foaming auxiliary agent and 0-10 parts by weight of a second polyolefin synthetic oil, wherein the titanium dioxide provides a reflectivity of more than 90%, and the tackifier further improves the bonding force between the reflective adhesive layer 20 and the other two layers; when the foaming agent is used, a reflective adhesive layer 20 with a cellular structure is formed.
[0036] Preferably, the second photovoltaic matrix resin is selected from any one or more of the following polymers: ethylene-vinyl acetate copolymer, metallocene-catalyzed polyethylene, metallocene-catalyzed ethylene-butene copolymer, metallocene-catalyzed ethylene-octene copolymer, metallocene-catalyzed ethylene-pentene copolymer, ethylene-propylene copolymer, ethylene-methyl acrylate copolymer, ethylene-methyl methacrylate copolymer, ethylene-glycidyl methacrylate copolymer, ethylene-glycidyl methacrylate-vinyl acetate copolymer, ethylene-glycidyl methacrylate-methyl acrylate copolymer, saponified ethylene-vinyl acetate copolymer and saponified ethylene-vinyl acetate-acrylate copolymer.
[0037] The second auxiliary cross-linking agent is beneficial to improve the cross-linking speed of the multi-layer packaging material of the present application during lamination. In order to further improve the above-mentioned effect of the second auxiliary cross-linking agent, the present application preferably uses the second auxiliary cross-linking agent as the second sensitizer and / or the third sensitizer, preferably the second sensitizer is an allyl sensitizer, and preferably the second sensitizer is any one or more of the following compounds: trimethylallyl isocyanate, triallyl isocyanurate, triallyl cyanurate, divinylbenzene, di-isopropenylbenzene, diallyl phthalate, allyl acrylate, allyl methacrylate, diallyl maleate and diallyl phthalate; preferably the third sensitizer is an acrylate-based sensitizer, and preferably the third sensitizer is any one or more of the following compounds: allyl acrylate, allyl methacrylate, diallyl maleate , diallyl phthalate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol triacrylate, ethoxylated glycerol triacrylate, tetramethylolmethane triacrylate, ethoxylated pentaerythritol tetraacrylate, dimethylolpropane tetraacrylate, trimethylolethane trimethacrylate, pentaerythritol tetraacrylate, tetramethylolmethane tetraacrylate, ditrimethylolpropane tetraacrylate, pentaerythritol tetramethacrylate, tetramethylolmethane tetramethacrylate, ditrimethylolpropane tetramethacrylate, dipentaerythritol polyacrylate, dipentaerythritol hexaacrylate, dipentaerythritol polymethacrylate, dipentaerythritol hexamethacrylate.
[0038] The above-mentioned foaming agent used in the present application includes a physical foaming agent and / or a chemical foaming agent, and the above-mentioned foaming agent includes but is not limited to a physical foaming agent and / or a chemical foaming agent. Preferably, the above-mentioned physical foaming agent includes but is not limited to any one or more combinations of nitrogen, carbon dioxide, organic hydrocarbon liquids with a boiling point <110°C, and core-shell microsphere foaming agents. Further, preferably, the organic hydrocarbon liquid includes but is not limited to any one or more of propane, butane, pentane, and methyl chloride; preferably, the chemical foaming agent is an inorganic foaming agent and / or an organic foaming agent, and preferably, the inorganic foaming agent includes but is not limited to any one or more combinations of sodium bicarbonate, ammonium carbonate, and sodium nitrite; preferably, the organic foaming agent includes but is not limited to any one or more combinations of sulfonylhydrazide compounds, azo compounds, and nitroso compounds, and preferably, the sulfonylhydrazide compounds are 4,4'-oxybisbenzenesulfonylhydrazide and / or p-toluenesulfonylhydrazide; preferably, the azo compound is azodicarbonamide; preferably, the nitroso compound is dinitroso-pentamethylene-tetramine. In some embodiments, the foaming aid is selected from any one or more combinations of metal oxides, metal salts, and metal organic complexes, such as ZnO, CaCO3, zinc stearate, MgO, etc., to achieve physical foaming or chemical foaming.
[0039] Further, the polyolefin synthetic silicone oil is selected from any one or more of polyα-olefin synthetic oil, polybutene synthetic oil, and alkylbenzene synthetic oil. More preferably, the polyolefin synthetic silicone oil is a liquid ethylene polymer oil; preferably, the liquid ethylene polymer oil is derived from a combination of ethylene A and an α-olefin B having 3 to 20 carbon atoms or a combination of ethylene A, an α-olefin B having 3 to 20 carbon atoms, and a non-conjugated polyene C, and the liquid ethylene polymer oil satisfies the following conditions 1) to 4); the non-conjugated polyene C contains a total of two or more partial structures selected from the group consisting of the following general formulas (I) and (II) in the molecule,
[0040]
[0041] Wherein, 1) the molar ratio of ethylene A / α-olefin B is 40:60 to 95:5; 2) the weight fraction of the structural unit derived from the non-conjugated polyene C in the liquid ethylene polymer oil is 0 to 10%; 3) the weight average molecular weight Mw of the ethylene-α-olefin-non-conjugated polyene copolymer, the weight fraction of the structural unit derived from the non-conjugated polyene C and the weight average molecular weight Mw of the non-conjugated polyene C satisfy: Mw×weight fraction of C / molecular weight of C≤40; 4) the number average molecular weight Mn of the liquid ethylene polymer oil measured by gel permeation chromatography is less than 30,000; preferably, the polyolefin synthetic silicone oil is an ethylene-propylene copolymer or an ethylene-propylene-non-conjugated diene terpolymer; preferably, The proportion of ethylene and propylene units in the ethylene-propylene-non-conjugated diene terpolymer is greater than 90%; preferably, the ethylene-α-olefin-non-conjugated polyene copolymer includes units derived from ethylene or units derived from propylene, preferably, the ethylene-α-olefin-non-conjugated polyene copolymer includes units derived from diene monomers, preferably, the diene monomer is any one or more of non-conjugated straight-chain hydrocarbon dienes, non-conjugated branched hydrocarbon dienes, and non-conjugated cyclic hydrocarbon dienes having 6 to 15 carbon atoms, further preferably, the weight average molecular weight of the polyolefin synthetic silicone oil is 200 to 50,000, preferably 200 to 10,000, preferably, the viscosity index of the polyolefin synthetic silicone oil is 60 to 250, preferably 80 to 180. Polyolefin synthetic oil has a low glass transition temperature, does not contain a crystalline structure, and has good compatibility with polyolefin resin substrates. After addition, it can reduce the crystallinity of the polyolefin resin substrate; increase the distance between molecules of the polyolefin resin substrate, reduce the intermolecular force, enhance the activity of the chain segments, and improve the flexibility of the molecular chain; or reduce the glass transition temperature of the polyolefin resin substrate, thereby increasing the softness of the encapsulation film, and ultimately reducing the fragmentation rate of the battery cell.
[0042] The main resin, cross-linking agent, tackifier, and auxiliary agent forming the above-mentioned support adhesive layer 30 can all refer to the corresponding materials used in the transparent adhesive film or reflective adhesive film in the prior art. In one embodiment, the raw materials forming the above-mentioned support adhesive layer 30 include: 100 parts by weight of the third photovoltaic matrix resin, 0.01 to 10 parts by weight of tackifier, 0.01 to 5 parts by weight of cross-linking agent, 0.05 to 2 parts by weight of the third auxiliary cross-linking agent, 0 to 10 parts by weight of foaming agent, 0 to 10 parts by weight of foaming auxiliary agent, 0 to 15 parts by weight of titanium dioxide, 15 to 60 parts by weight of filler, and 0 to 3 parts by weight of auxiliary agent. The tackifier can increase the bonding force between the support adhesive layer 30 and the reflective adhesive layer 20, the third auxiliary cross-linking agent delays the cross-linking progress of the support adhesive layer 30 during the radiation process, and 15 to 60 parts by weight of filler greatly reduces the cost of the support adhesive layer 30. Titanium dioxide is an optional component. The purpose of using titanium dioxide is to reduce the color difference between the supporting adhesive layer 30 and the reflecting adhesive layer 20 caused by the filler, so the content of titanium dioxide does not need to be too much.
[0043] Preferably, the third photovoltaic matrix resin is selected from any one or more of the following polymers: ethylene-vinyl acetate copolymer, metallocene-catalyzed polyethylene, metallocene-catalyzed ethylene-butene copolymer, metallocene-catalyzed ethylene-octene copolymer, metallocene-catalyzed ethylene-pentene copolymer, ethylene-propylene copolymer, ethylene-methyl acrylate copolymer, ethylene-methyl methacrylate copolymer, ethylene-glycidyl methacrylate-vinyl acetate copolymer, ethylene-glycidyl methacrylate-methyl acrylate copolymer, saponified ethylene-vinyl acetate copolymer, saponified ethylene-vinyl acetate-acrylate copolymer, low-density polyethylene, linear low-density polyethylene, linear ultra-low-density polyethylene, and modified polyolefin transparent resin polymers.
[0044] In order to ensure that the three-layer packaging material has sufficient pre-crosslinking degree in the lamination to form a photovoltaic module, the third auxiliary crosslinking agent is preferably a fourth sensitizer and / or a fifth sensitizer, and the fourth sensitizer is preferably an allyl sensitizer, and the fourth sensitizer is preferably any one or more of the following compounds: trimethylallyl isocyanate, triallyl isocyanurate, triallyl cyanurate, divinylbenzene, di-isopropenylbenzene, diallyl phthalate, allyl acrylate, allyl methacrylate, diallyl maleate and diallyl phthalate; the fifth sensitizer is preferably an acrylate-based sensitizer, and the fifth sensitizer is preferably any one or more of the following compounds: allyl acrylate, allyl methacrylate, maleate, and diallyl phthalate. Diallyl phthalate, diallyl phthalate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol triacrylate, ethoxylated glycerol triacrylate, tetramethylolmethane triacrylate, ethoxylated pentaerythritol tetraacrylate, dimethylolpropane tetraacrylate, trimethylolethane trimethacrylate, pentaerythritol tetraacrylate, tetramethylolmethane tetraacrylate, ditrimethylolpropane tetraacrylate, pentaerythritol tetramethacrylate, tetramethylolmethane tetramethacrylate, ditrimethylolpropane tetramethacrylate, dipentaerythritol polyacrylate, dipentaerythritol hexaacrylate, dipentaerythritol polymethacrylate, dipentaerythritol hexamethacrylate.
[0045] In addition, the cross-linking agent can be selected from peroxides commonly used in the art, such as di(4-methylbenzoyl) peroxide, tert-butyl peroxy isopropyl carbonate, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, tert-butyl peroxycarbonate-2-ethylhexyl ester, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane One or more of cyclohexane, 1,1-bis(tert-amyl peroxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amyl peroxy)cyclohexane, 1,1-bis(tert-butyl peroxy)cyclohexane, 2,2-bis(tert-butyl peroxy)butane, tert-amyl peroxy 2-ethylhexyl carbonate, 2,5-dimethyl 2,5-bis(benzoyl peroxy)-hexane, tert-amyl peroxycarbonate, tert-butyl peroxy 3,3,5-trimethylhexanoate, diisopropylbenzene peroxide, and dibenzoyl peroxide.
[0046] The above-mentioned adhesion promoter can be selected from silane coupling agents or trialkoxysilane oligomers commonly used in the art, such as γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane, diethylaminomethyltriethoxysilane, dichloromethyltriethoxysilane, and vinyltrimethoxysilane.
[0047] The foaming agent and foaming aid used in the supporting adhesive layer 30 can be selected from the foaming agent and foaming aid in the aforementioned reflective adhesive layer 20, and will not be described in detail here.
[0048] The above-mentioned additives are also some commonly used additives in the field, such as light stabilizers, ultraviolet light absorbers, plasticizers and acid absorbers. Among them, the acid absorber is hydrotalcite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, magnesium oxide, aluminum oxide, calcium oxide, zinc oxide, calcium carbonate, talcum powder, etc. Light stabilizers, ultraviolet light absorbers and plasticizers can all use corresponding substances commonly used in adhesive films, and this application will not list them one by one.
[0049] In another typical embodiment of the present application, a photovoltaic module is provided, such as Figure 3 As shown, the photovoltaic module includes a front panel 1, a transparent adhesive film 2, a battery cell unit 3, a back layer adhesive film 4 and a back panel 5 which are laminated in sequence. The back layer adhesive film 4 is any of the above-mentioned multi-layer packaging materials, and the supporting adhesive layer 30 of the multi-layer packaging material is arranged away from the battery cell unit 3.
[0050] The multi-layer reflective packaging film of the present application solves the problem of high cost caused by the large amount of titanium dioxide used. At the same time, the titanium dioxide in the reflective adhesive layer 20 provides a higher reflective ability for interstitial light, thereby achieving the purpose of improving the photoelectric conversion efficiency of photovoltaic modules.
[0051] The beneficial effects of the present application will be further illustrated below in combination with embodiments and comparative examples.
[0052] Example 1
[0053] The raw materials for the micro-cross-linked layer are provided according to the following weight portions: 100 weight portions of a first photovoltaic matrix resin, 5 weight portions of a thickener, 3 weight portions of a cross-linking agent, and 1 weight portion of a first auxiliary cross-linking agent. The first photovoltaic matrix resin is an EVA resin with a VA content of 40% (melt index of 60 g / 10 min); the thickener is γ-mercaptopropyltriethoxysilane, the cross-linking agent is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, and the first auxiliary cross-linking agent is di-isopropenylbenzene.
[0054] The raw materials of the reflective adhesive layer are provided according to the following weight parts: 100 weight parts of the second photovoltaic matrix resin, 10 weight parts of tackifier, 3 weight parts of crosslinking agent, 3 weight parts of the second crosslinking auxiliary agent, 30 weight parts of titanium dioxide, 3 weight parts of foaming agent, 3.5 weight parts of foaming auxiliary agent, and 5 parts of polyolefin synthetic silicone oil. The second photovoltaic matrix resin is an EVA resin with a VA content of 28% (melt index of 20g / 10min); the tackifier is γ-mercaptopropyl triethoxysilane, the crosslinking agent is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, the second crosslinking auxiliary agent is trimethylolpropane triacrylate, the foaming agent is azodicarbonamide, the foaming auxiliary agent is a mixture of zinc stearate: ZnO: stearic acid = 2:2:1 (mass ratio), the titanium dioxide is D50≤1μm and uses Screen The 3# filter (pore size of about 10μm) was tested, and the test results showed that the filtration pressure value was <0.5bar / g of titanium dioxide, the mass content of titanium dioxide was 19%, and the polyolefin synthetic silicone oil was Mitsui Chemicals' luctant ethylene-α-olefin copolymer.
[0055] The raw materials for the supporting adhesive layer are provided according to the following weight portions: 100 weight portions of a third photovoltaic matrix resin, 5 weight portions of a thickener, 3 weight portions of a cross-linking agent, 1 weight portion of a third auxiliary cross-linking agent, 20 weight portions of talc, 20 weight portions of montmorillonite, and the mass content of the filler is 26.8%, wherein the third photovoltaic matrix resin is an EVA resin with a VA content of 40% (melt index of 60 g / 10 min); the thickener is γ-mercaptopropyltriethoxysilane, the cross-linking agent is tert-butylperoxycarbonate-2-ethylhexyl ester, and the third auxiliary cross-linking agent is allyl acrylate.
[0056] After the raw materials are mixed separately, melt co-extrusion is carried out. The extruded materials of the micro-cross-linked layer, the reflective adhesive layer and the supporting adhesive layer are combined in a boundary manner in a distributor in a T-die head to form a melt flow and extruded in a film form to obtain a multi-layer reflective packaging adhesive film base film with a reflective adhesive layer 20 in the middle and micro-cross-linked layers 10 and supporting adhesive layers 30 on both sides. The base film is cooled and conveyed to the bottom of an electron radiation device with an energy of 500keV and a radiation intensity of 10kGy. After radiation, the base film is conveyed to a drying oven at 110℃ for foaming for 3 minutes, and cooled and rolled to obtain a three-layer packaging material E1. The apparent thickness of E1 is 0.67mm. According to SEM observation, the thickness of the micro-cross-linked layer is 60μm, the thickness of the reflective adhesive layer 20 is 0.2mm, and the thickness of the supporting adhesive layer 30 is 0.42mm.
[0057] A single micro-crosslinked layer raw material is used, melt extruded, and the gram weight is the gram weight parameter of the reflective adhesive layer in E1. After cooling, it is transferred to the bottom of an electron irradiation device with an energy of 500keV, and the radiation intensity is 10kGy. After irradiation, it is cooled to obtain a micro-crosslinked layer E1-1, and the pre-crosslinking degree of E1-1 is 1%; a single reflective adhesive layer raw material is used, extruded through a reflective adhesive layer screw, and the gram weight is the gram weight parameter of the reflective adhesive layer in E1. After cooling, it is transferred to the bottom of an electron irradiation device with an energy of 500keV, and the radiation intensity is 10kGy. After irradiation, the base film is transferred to a 110°C drying tunnel for foaming for 3 minutes, and then cooled and rolled to obtain a single-layer packaging adhesive film E1-2. A single supporting adhesive layer raw material is used, extruded through a supporting adhesive layer screw, and the gram weight is the gram weight parameter of the supporting adhesive layer in E1. After cooling, it is transferred to the bottom of an electron irradiation device with an energy of 500keV, and the radiation intensity is 10kGy. After irradiation, it is cooled and rolled to obtain a single-layer packaging adhesive film E1-3.
[0058] Example 2
[0059] The compositions of the micro-crosslinking layer and the reflective adhesive layer are the same as those in Example 1.
[0060] The raw materials for the supporting adhesive layer are provided according to the following weight portions: 100 weight portions of a third photovoltaic matrix resin, 5 weight portions of a thickener, 3 weight portions of a cross-linking agent, 1 weight portion of a third auxiliary cross-linking agent, 15 weight portions of glass beads, 1 weight portion of a foaming agent, and 1.5 weight portions of a foaming aid. The mass content of the filler is 11.86%, wherein the third photovoltaic matrix resin is an EVA resin with a VA content of 28% (melt index of 28 g / 10 min), the thickener is 3-aminopropyltrimethoxysilane, the cross-linking agent is diisopropyl peroxide, the third auxiliary cross-linking agent is allyl acrylate, the foaming agent is a mixture of azodicarbonamide and a foaming aid of zinc stearate: ZnO: stearic acid = 2:2:1 (mass ratio), and finally a three-layer packaging material E2 is obtained. The apparent thickness of E2 is 0.86 mm. According to SEM observation, the thickness of the micro-crosslinked layer is about 60 μm, the thickness of the reflective adhesive layer 20 is about 0.2 mm, and the thickness of the supporting adhesive layer 30 is about 0.42 mm.
[0061] A single micro-cross-linked layer raw material is used, and the material is melt-extruded to have a gram weight that is the gram weight parameter of the reflective adhesive layer in E2. After cooling, it is conveyed under an electron radiation device with an energy of 500keV and a radiation intensity of 10kGy. After radiation, the base film is conveyed to a 140°C drying oven for heat treatment for 2 minutes. After cooling, the micro-cross-linked layer E2-1 is obtained, wherein the pre-cross-linking degree of E2-1 is 3%. A single reflective adhesive layer raw material is used, and the reflective adhesive layer is screw-extruded to have a gram weight that is the gram weight parameter of the reflective adhesive layer in E2. After cooling, it is conveyed to a 1000keV electron radiation device for energy. The radiation intensity is 10kGy. After radiation, the base film is conveyed to a 140°C drying oven for foaming for 2 minutes. After cooling and winding, a single-layer packaging adhesive film E2-2 is obtained. A separate supporting adhesive layer raw material is used, which is extruded through a supporting adhesive layer screw, and has a gram weight parameter of the supporting adhesive layer in E2. After cooling, it is transmitted to the bottom of an electron radiation device with an energy of 1000keV, and the radiation intensity is 10kGy. After radiation, the base film is then transmitted to a 140°C drying oven for foaming for 2 minutes. After cooling and winding, a single-layer encapsulation adhesive film E2-3 is obtained.
[0062] Example 3
[0063] The compositions of the micro-crosslinking layer and the reflective adhesive layer are the same as those in Example 1.
[0064] The raw materials of the supporting adhesive layer are provided according to the following weight parts: 100 weight parts of the third photovoltaic matrix resin, 5 weight parts of tackifier, 3 weight parts of crosslinking agent, 1 weight part of the third auxiliary crosslinking agent, 20 weight parts of talcum powder, 20 weight parts of magnesium hydroxide, 20 weight parts of zinc barium white, the mass content of the filler is 35.5%, wherein the third photovoltaic matrix resin is an EVA resin with a VA content of 40% (melt index is 60g / 10min); the tackifier is γ-mercaptopropyl triethoxysilane, the crosslinking agent is tert-butyl peroxycarbonic acid-2-ethylhexyl ester, and the third auxiliary crosslinking agent is allyl acrylate, and finally a three-layer packaging material E3 is obtained. The apparent thickness of E3 is 1.88mm. According to SEM observation, the thickness of the micro-crosslinking layer is about 60μm, the thickness of the reflective adhesive layer 20 is about 0.2mm, and the thickness of the supporting adhesive layer 30 is about 0.42mm.
[0065] A single micro-cross-linked layer raw material is used, and after cooling, it is conveyed to the bottom of an electron radiation device with an energy of 1000keV, and the radiation intensity is 10kGy. After radiation, the base film is conveyed to a 170℃ drying oven for foaming for 4 minutes, and the micro-cross-linked layer E3-1 is obtained by melt extrusion, and the pre-cross-linking of E3-1 is 0.5%. A single reflective adhesive layer raw material is used, and the reflective adhesive layer is screw extruded, and the gram weight is the gram weight parameter of the reflective adhesive layer in E3. After cooling, it is conveyed to the bottom of an electron radiation device with an energy of 1000keV, and the radiation intensity is 10kGy. After radiation, the base film is conveyed to a 170℃ drying oven for foaming for 4 minutes, and after cooling and winding, a single-layer packaging adhesive film E3-2 is obtained. A separate supporting adhesive layer raw material is used, which is extruded through a supporting adhesive layer screw, and has a gram weight that is the supporting adhesive layer gram weight parameter in E3. After cooling, it is transmitted to the bottom of an electron radiation device with an energy of 1000keV, and the radiation intensity is 10kGy. After radiation, the base film is then transmitted to a 170°C drying oven for heat treatment for 4 minutes. After cooling and winding, a single-layer encapsulation adhesive film E3-3 is obtained.
[0066] Example 4
[0067] The difference from Example 1 is that the raw materials of the micro-cross-linked layer are provided according to the following weight parts: 100 weight parts of a first photovoltaic matrix resin, 0.5 weight parts of a tackifier, 0.01 weight parts of a cross-linking agent, 1 weight parts of a first auxiliary cross-linking agent, and 5 parts of polyolefin synthetic silicone oil. The first photovoltaic matrix resin is an EVA resin with a VA content of 28% (melt index of 28 g / 10 min), the tackifier is γ-methacryloxypropyltrimethoxysilane, the first auxiliary cross-linking agent is ethoxylated glycerol triacrylate, and the polyolefin synthetic silicone oil is Lion Chemical Trilene CP1100 ethylene-α-olefin-non-conjugated polyene copolymer synthetic oil.
[0068] After the raw materials are mixed separately, melt co-extrusion is carried out. The extruded materials of the micro-cross-linked layer, the reflective adhesive layer and the supporting adhesive layer are combined in a boundary manner in a distributor in a T-die head to form a melt flow and extruded in a film form to obtain a multi-layer reflective packaging adhesive film base film with a reflective adhesive layer 20 in the middle and micro-cross-linked layers 10 and supporting adhesive layers 30 on both sides. The base film is cooled and conveyed to the bottom of an electron radiation device with an energy of 500keV and a radiation intensity of 10kGy. After radiation, the base film is conveyed to a drying oven at 110℃ for foaming for 3min, cooled and rolled to obtain a three-layer packaging material E4. The apparent thickness of E4 is 0.68mm. According to SEM observation, the thickness of the micro-cross-linked layer is about 60μm, the thickness of the reflective adhesive layer 20 is about 0.2mm, and the thickness of the supporting adhesive layer 30 is about 0.42mm.
[0069] A single micro-cross-linked layer raw material is used, and the material is melt-extruded, with a gram weight being the gram weight parameter of the reflective adhesive layer in E4. After cooling, it is conveyed under an electron irradiation device with an energy of 500keV, and the radiation intensity is 10kGy. After irradiation, the base film is conveyed to a 110℃ drying oven for heat treatment for 3 minutes, and cooled to obtain a micro-cross-linked layer E4-1. The pre-cross-linking degree of E4-1 is 3%; a single reflective adhesive layer raw material is used, and the reflective adhesive layer is screw-extruded, with a gram weight being the gram weight parameter of the reflective adhesive layer in E4. After cooling, it is conveyed to a 500keV electron irradiation device, and the radiation intensity is 10kGy. After irradiation, the base film is conveyed to a 110℃ drying oven for foaming for 3 minutes, and cooled and rolled up to obtain a single-layer packaging adhesive film E4-2. A separate supporting adhesive layer raw material is used, which is extruded through a supporting adhesive layer screw, and has a gram weight of the supporting adhesive layer in E4. After cooling, it is transmitted to the bottom of an electron radiation device with an energy of 500keV and a radiation intensity of 10kGy. After radiation, the base film is then transmitted to a 110°C drying oven for foaming for 3 minutes. After cooling and winding, a single-layer encapsulation adhesive film E4-3 is obtained.
[0070] Example 5
[0071] The difference from Example 1 is that the raw materials of the micro-cross-linked layer are provided according to the following weight parts: 100 weight parts of a first photovoltaic matrix resin, 0.5 weight parts of a tackifier, and 2 weight parts of a first sensitizer, the first photovoltaic matrix resin is a metallocene-catalyzed ethylene-octene copolymer (MFR: 5 g / 10 min; octene content is 38 weight %), the tackifier is γ-methacryloxypropyltrimethoxysilane, and the first sensitizer is trimethylolpropane triacrylate. A single micro-cross-linked layer raw material is melt-extruded, and its gram weight is the gram weight parameter of the reflective adhesive layer in E5. After cooling, it is transmitted to the bottom of an electron radiation device with an energy of 500keV and an radiation intensity of 10kGy. After radiation, the base film is transmitted to a 110℃ drying oven for heat treatment for 3 minutes, and then cooled and rolled up to obtain a three-layer packaging material E5. The apparent thickness of E5 is 0.67mm. According to SEM observation, the thickness of the micro-cross-linked layer is about 60μm, the thickness of the reflective adhesive layer 20 is about 0.2mm, and the thickness of the supporting adhesive layer 30 is about 0.42mm.
[0072] After mixing the raw materials separately, melt co-extrusion is carried out. The extruded materials of the micro-cross-linked layer, the reflective adhesive layer and the supporting adhesive layer are combined in a T-die head with a boundary through a distributor to form a melt flow and extruded in a film form to obtain a multi-layer reflective packaging adhesive film base film with a reflective adhesive layer 20 in the middle and a micro-cross-linked layer 10 and a supporting adhesive layer 30 on both sides. The base film is cooled and conveyed to the bottom of an electron irradiation device with an energy of 500keV and a radiation intensity of 10kGy. After irradiation, the base film is further conveyed to a 110℃ drying oven for heat treatment for 3min. The micro-cross-linked layer E5-1 is obtained by cooling. The pre-cross-linking degree of E5-1 is 5%. A single reflective adhesive layer raw material is used, and the reflective adhesive layer is screw extruded. The gram weight is the reflective adhesive layer gram weight parameter in E5. The base film is cooled and conveyed to the bottom of an electron irradiation device with an energy of 500keV and a radiation intensity of 10kGy. After irradiation, the base film is further conveyed to a 110℃ drying oven for foaming for 3min. The single-layer packaging adhesive film E5-2 is obtained after cooling and winding. A separate supporting adhesive layer raw material is used, which is extruded through a supporting adhesive layer screw, and has a gram weight parameter of the supporting adhesive layer in E5. After cooling, it is transmitted to the bottom of an electron radiation device with an energy of 500keV and a radiation intensity of 10kGy. After radiation, the base film is then transmitted to a 110℃ drying oven for foaming for 3 minutes. After cooling and winding, a single-layer encapsulation adhesive film E5-3 is obtained.
[0073] Example 6
[0074] The composition of the micro-crosslinked layer, the reflective adhesive layer and the supporting adhesive layer is the same as that of Example 2, and the difference from Example 2 is that: the raw materials of the supporting adhesive layer are first mixed, and the extruded materials are extruded through a T-die in a film shape to obtain a packaging material base film of the supporting adhesive layer 30, which is then cooled and transferred to the bottom of an electron irradiation device with an energy of 500keV, and the radiation intensity is 30kGy. After irradiation, the base film is then transferred to a 170°C drying tunnel for foaming for 10 minutes, cooled and rolled up, and then transferred to the reflective adhesive layer extrusion die area, wherein the raw materials of the reflective adhesive layer 20 are mixed, melt-extruded, and extruded through a T-die in a film shape, and the above-mentioned supporting adhesive layer 20 is The adhesive layer is compounded, cooled and transferred to the bottom of an electron radiation device with an energy of 500keV and a radiation intensity of 10kGy. The base film is then transferred to a 90℃ drying oven for foaming for 30s. After cooling and rolling, it is transferred to the micro-cross-linked layer area, wherein the raw materials of the micro-cross-linked layer 10 are mixed, melt-extruded, and then cooled and rolled together with the reflective adhesive layer of the above-mentioned packaging material base film to obtain a three-layer packaging material E6. The apparent thickness of E6 is 1.25mm. SEM observation shows that the thickness of the micro-cross-linked layer is 350μm, the thickness of the reflective adhesive layer 20 is 0.15mm, and the thickness of the supporting adhesive layer 30 is 0.8mm.
[0075] A single micro-crosslinked layer raw material was used, and the micro-crosslinked layer E6-1 was obtained by melt extrusion; a single reflective adhesive layer raw material was used, and the reflective adhesive layer screw was extruded, and the gram weight was the reflective adhesive layer gram weight parameter in E6, and after cooling, it was conveyed to the bottom of an electron irradiation device with an energy of 500keV, and the radiation intensity was 10kGy. After irradiation, the base film was conveyed to a 90°C oven for foaming for 30s, and after cooling and rolling, a single-layer packaging adhesive film E6-2 was obtained. A single supporting adhesive layer raw material was used, and the supporting adhesive layer screw was extruded, and the gram weight was the supporting adhesive layer gram weight parameter in E6, and after cooling, it was conveyed to the bottom of an electron irradiation device with an energy of 500keV, and the radiation intensity was 30kGy. After irradiation, the base film was conveyed to a 170°C oven for foaming for 10min, and after cooling, it was conveyed to the bottom of an electron irradiation device with an energy of 500keV, and the radiation intensity was 10kGy. After irradiation, the base film was conveyed to a 90°C oven for foaming for 30s, and after rolling, a single-layer packaging adhesive film E6-3 was obtained. The density of the cells in the reflective adhesive layer 20 is 80 cell / cm 3 The diameter of the cell unit of the reflective adhesive layer is 0.1 μm; the density of the cells of the supporting adhesive layer 30 is 10 15 cell / cm 3 , pore diameter 100μm.
[0076] Example 7
[0077] The composition of the micro-crosslinked layer, the reflective adhesive layer and the supporting adhesive layer is the same as that of Example 2. The difference from Example 2 is that the raw materials of the reflective adhesive layer are first mixed, and the extruded material is extruded through a T-die head in a film form to obtain a packaging material base film of the reflective adhesive layer 20, which is then cooled and transferred to the bottom of an electron irradiation device with an energy of 500keV, and the radiation intensity is 30kGy. After irradiation, the base film is then transferred to a 170°C drying tunnel for foaming for 10 minutes, cooled and rolled up, and then transferred to the supporting adhesive layer extrusion die head area, wherein the raw materials of the supporting adhesive layer 30 are mixed, melt extruded, and then the base film is transferred to the supporting adhesive layer extrusion die head area, wherein the raw materials of the supporting adhesive layer 30 are mixed, melt extruded, and then the supporting adhesive layer 30 is formed. After coming out, it is extruded through a T-die in a film form and compounded with the above-mentioned reflective adhesive layer. The base film is then conveyed to a 170°C drying oven for foaming for 3 minutes. After cooling and winding, it is conveyed to the micro-cross-linking layer area, wherein the raw materials of the micro-cross-linking layer 10 are mixed, melt-extruded, and compounded with the reflective adhesive layer of the above-mentioned foaming base film. The three-layer packaging material E8 is obtained by cooling and winding. The apparent thickness of E8 is 1.6 mm. According to SEM observation, the thickness of the micro-cross-linking layer is 350 μm, the thickness of the reflective adhesive layer 20 is 0.6 mm, and the thickness of the supporting adhesive layer 30 is 0.7 mm.
[0078] A single micro-cross-linked layer raw material is used, and the micro-cross-linked layer E7-1 is obtained by melt extrusion; a single reflective adhesive layer raw material is used, and the reflective adhesive layer is screw extruded, and the gram weight is the reflective adhesive layer gram weight parameter in E7, and the base film is conveyed to the bottom of an electron irradiation device with an energy of 500keV, and the radiation intensity is 30kGy. After irradiation, the base film is conveyed to a 170℃ drying oven for foaming for 10 minutes, and is conveyed to the bottom of an electron irradiation device with an energy of 500keV, and the radiation intensity is 10kGy. After irradiation, the base film is conveyed to a 170℃ drying oven for foaming for 3 minutes, and is rolled up to obtain a single-layer packaging film E7-2. A single supporting adhesive layer raw material is used, and the supporting adhesive layer is screw extruded, and the gram weight is the supporting layer gram weight parameter in E7. The base film is conveyed to a 110℃ drying oven for foaming for 3 minutes, and is cooled and rolled up to obtain a single-layer packaging film E7-3. The density of the bubbles in the reflective adhesive layer is 10 15 cell / cm 3 The cell diameter is 160 μm, and the cell density of the supporting glue layer is 80 cell / cm 3 The diameter of the cell unit of the supporting glue layer cell is 0.3 mm.
[0079] Example 8
[0080] The composition of the micro-cross-linked layer, the reflective adhesive layer and the supporting adhesive layer is the same as that in Example 1. The difference from Example 1 is that the raw materials of the reflective adhesive layer are first mixed and melt-extruded, and then conveyed to the bottom of an electron irradiation device with an energy of 500keV after cooling, and the radiation intensity is 30kGy. After irradiation, the base film is conveyed to a 110°C drying oven for heat treatment for 3 minutes, and then conveyed to be compounded with the supporting adhesive layer and the micro-cross-linked layer respectively, and then conveyed to the bottom of an electron irradiation device with an energy of 500keV after cooling, and the radiation intensity is 10kGy. After irradiation, the three-layer packaging material E8 is rolled up to obtain a surface thickness of 0.68mm. According to SEM observation, the thickness of the micro-cross-linked layer is 60μm, the thickness of the reflective adhesive layer 20 is 0.2mm, and the thickness of the supporting adhesive layer 30 is 0.42mm.
[0081] A single micro-cross-linked layer raw material is used, which is melt-extruded, cooled and conveyed under an electron irradiation device with an energy of 500keV, with a radiation intensity of 10kGy. After irradiation, it is rolled up to obtain the micro-cross-linked layer E8-1; a single reflective adhesive layer raw material is used, which is screw-extruded through a reflective adhesive layer, with a gram weight being the gram weight parameter of the reflective adhesive layer in E8, cooled and conveyed under an electron irradiation device with an energy of 500keV, with a radiation intensity of 30kGy. After irradiation, the base film is further conveyed to a 110°C drying oven for heat treatment for 3 minutes, cooled and conveyed under an electron irradiation device with an energy of 500keV, with a radiation intensity of 10kGy. After irradiation, it is rolled up to obtain a single-layer packaging adhesive film E8-2. A separate supporting adhesive layer raw material is used, which is extruded through a supporting adhesive layer screw with a gram weight being the supporting adhesive layer gram weight parameter in E8. The product is cooled and transmitted to the bottom of an electron radiation device with an energy of 500keV and a radiation intensity of 10kGy. After radiation, the product is rolled up to obtain a single-layer packaging adhesive film E8-3, and the pre-crosslinking degree of the reflective adhesive layer is 70%.
[0082] Example 9
[0083] The difference from Example 1 is that the second photovoltaic resin of the reflective adhesive layer is EVA resin with a VA content of 28% (melt index of 4g / 10min), the second auxiliary cross-linking agent is ethoxylated glycerol triacrylate, and the pre-cross-linking degree of the reflective adhesive layer is 0.5%, and finally a three-layer packaging material E9 is obtained.
[0084] Example 10
[0085] The composition of the micro-cross-linked layer, the reflective adhesive layer and the supporting adhesive layer is the same as that in Example 1, the raw materials of the reflective adhesive layer are first mixed and melt-extruded, and then conveyed to the bottom of an electron irradiation device with an energy of 500keV after cooling, and the radiation intensity is 10kGy. After irradiation, the base film is conveyed to a 110°C drying oven for heat treatment for 3 minutes, and then conveyed to be compounded with the supporting adhesive layer and the micro-cross-linked layer respectively, and then conveyed to the bottom of an electron irradiation device with an energy of 500keV after cooling, and the radiation intensity is 10kGy. After irradiation, the three-layer packaging material E10 is rolled up to obtain a surface thickness of 0.68mm. According to SEM observation, the thickness of the micro-cross-linked layer is 60μm, the thickness of the reflective adhesive layer 20 is 0.2mm, and the thickness of the supporting adhesive layer 30 is 0.42mm.
[0086] A single micro-cross-linked layer raw material is used, which is melt-extruded, cooled and conveyed under an electron irradiation device with an energy of 500keV, the radiation intensity of which is 10kGy, and then rolled up to obtain the micro-cross-linked layer E10-1; a single reflective adhesive layer raw material is used, which is screw-extruded through a reflective adhesive layer, the gram weight is the gram weight parameter of the reflective adhesive layer in E10, cooled and conveyed under an electron irradiation device with an energy of 500keV, the radiation intensity of which is 10kGy, and after irradiation, the base film is further conveyed to a 110°C drying oven for heat treatment for 3 minutes, cooled and conveyed under an electron irradiation device with an energy of 500keV, the radiation intensity of which is 10kGy, and then rolled up to obtain a single-layer packaging adhesive film E10-2. A separate supporting adhesive layer raw material is used, which is extruded through a supporting adhesive layer screw, with a gram weight being the supporting adhesive layer gram weight parameter in E10, and then cooled and transmitted to the bottom of an electron radiation device with an energy of 500keV and a radiation intensity of 10kGy. After radiation, the device is rolled up to obtain a single-layer packaging adhesive film E10-3, and the pre-crosslinking degree of the reflective adhesive layer is 60%.
[0087] Embodiment 11
[0088] The difference from Example 1 is that the second photovoltaic resin of the reflective adhesive layer is an EVA resin with a VA content of 28% (melt index of 15 g / 10 min), and the pre-crosslinking degree of the reflective adhesive layer is 30%, and finally a three-layer packaging material E11 is obtained.
[0089] Example 12
[0090] The difference from Example 1 is that
[0091] The raw materials for the micro-cross-linked layer are provided according to the following weight parts: 100 weight parts of a first photovoltaic matrix resin, 5 weight parts of a thickener, 3 weight parts of a cross-linking agent, 1 weight part of a first auxiliary cross-linking agent, and 14 weight parts of titanium dioxide. The mass content of titanium dioxide is 11.7%. The first photovoltaic matrix resin is an EVA resin with a VA content of 40% (melt index is 60g / 10min); the thickener is γ-mercaptopropyltriethoxysilane, and the first auxiliary cross-linking agent is di-isopropenylbenzene.
[0092] The raw materials for the reflective adhesive layer are provided according to the following weight portions: 100 weight portions of a second photovoltaic matrix resin, 1 weight portion of a thickener, 1 weight portion of a cross-linking agent, 1 weight portion of a second auxiliary cross-linking agent, and 3 weight portions of titanium dioxide. The second photovoltaic matrix resin is an EVA resin with a VA content of 28% (melt index of 20g / 10min), the thickener is 3-aminopropyltrimethoxysilane, the second auxiliary cross-linking agent is allyl acrylate, the titanium dioxide has a D50≤1μm and is tested using a Screen 3# filter (pore size of approximately 10μm). The test results show that the filtration pressure value of the titanium dioxide is <0.5bar / g, and the mass content of the titanium dioxide is 2.8%. Finally, the three-layer packaging material E12 is obtained.
[0093] The thickness of the micro-crosslinked layer is 60 μm, the thickness of the reflective adhesive layer 20 is 0.2 mm, and the thickness of the supporting adhesive layer 30 is 0.42 mm.
[0094] Embodiment 13
[0095] The difference from Example 1 is that the raw materials of the reflective adhesive layer are provided according to the following weight parts: 100 weight parts of the second photovoltaic matrix resin, 1 weight part of tackifier, 1 weight part of crosslinking agent, 1 weight part of the second auxiliary crosslinking agent, 20 parts of polyolefin synthetic silicone oil, 80 weight parts of titanium dioxide, the second photovoltaic matrix resin is EVA resin with a VA content of 28% (melt index of 28g / 10min), the tackifier is 3-aminopropyltrimethoxysilane, the second auxiliary crosslinking agent is allyl acrylate, and the polyolefin synthetic silicone oil is Lion Chemical Trilene CP1100 ethylene-α-olefin-non-conjugated polyene copolymer synthetic oil. The titanium dioxide is D50≤1μm and is tested using Screen 3# filter (aperture of about 10μm). The test results show that the filtration pressure value is <0.5bar / g of titanium dioxide, and the mass content of titanium dioxide is 28%, and finally the three-layer packaging material E12 is obtained. Finally, the three-layer packaging material E13 is obtained.
[0096] The thickness of the micro-crosslinked layer is 60 μm, the thickness of the reflective adhesive layer 20 is 0.4 mm, and the thickness of the supporting adhesive layer 30 is 0.42 mm.
[0097] Embodiment 14
[0098] The difference from Example 1 is that
[0099] The raw materials for the supporting adhesive layer are provided according to the following weight portions: 100 weight portions of a third photovoltaic matrix resin, 1 weight portion of a tackifier, 1 weight portion of a cross-linking agent, 1 weight portion of a third auxiliary cross-linking agent, 20 weight portions of titanium dioxide, and 20 weight portions of montmorillonite, wherein the third photovoltaic matrix resin is an EVA resin with a VA content of 40% (melt index of 28 g / 10 min); the tackifier is γ-mercaptopropyltriethoxysilane, the cross-linking agent is tert-butyl peroxycarbonate-2-ethylhexyl ester, and the third auxiliary cross-linking agent is allyl acrylate.
[0100] The raw materials for the reflective adhesive layer are provided according to the following weight portions: 100 weight portions of a second photovoltaic matrix resin, 1 weight portion of a tackifier, 1 weight portion of a cross-linking agent, 1 weight portion of a second auxiliary cross-linking agent, and 2.5 weight portions of titanium dioxide. The second photovoltaic matrix resin is an EVA resin with a VA content of 28% (melt index of 28g / 10min), the tackifier is 3-aminopropyltrimethoxysilane, the second auxiliary cross-linking agent is allyl acrylate, the titanium dioxide has a D50≤1μm and is tested using a Screen 3# filter (pore size of approximately 10μm). The test results show that the filtration pressure value of the titanium dioxide is <0.5bar / g, and the mass content of the titanium dioxide is 2.8%. Finally, the three-layer packaging material E14 is obtained.
[0101] The thickness of the micro-crosslinked layer is 60 μm, the thickness of the reflective adhesive layer 20 is 0.2 mm, and the thickness of the supporting adhesive layer 30 is 0.42 mm.
[0102] Embodiment 15
[0103] The difference from Example 1 is that the first auxiliary cross-linking agent of the micro-cross-linked layer is divinylbenzene, the pre-cross-linking degree of the micro-cross-linked layer is 0.5%, and finally the three-layer packaging material E15 is obtained.
[0104] Example 16
[0105] The difference from Example 1 is that the first photovoltaic matrix resin of the micro-crosslinked layer is EVA resin with a VA content of 28% (melt index of 5 g / 10 min), and the pre-crosslinking degree of the micro-crosslinked layer is 5%, and finally a three-layer packaging material E16 is obtained.
[0106] Embodiment 17
[0107] The difference from Example 1 is that the weight of the micro-cross-linked layer is adjusted, and the thickness of the micro-cross-linked layer is 0.2 mm, and finally a three-layer packaging material E17 is obtained.
[0108] Embodiment 18
[0109] The difference from Example 1 is that the weight of the micro-cross-linked layer is adjusted, and the thickness of the micro-cross-linked layer is 0.35 mm, and finally the three-layer packaging material E18 is obtained.
[0110] Embodiment 19
[0111] The difference from Example 1 is that the weight of each layer is adjusted, the thickness of the micro-crosslinked layer is 0.35 mm, the thickness of the reflective adhesive layer 20 is 0.1 mm, and the thickness of the supporting adhesive layer 30 is 0.5 mm, and finally a three-layer packaging material E19 is obtained.
[0112] Comparative Example 1
[0113] The difference from Example 1 is that
[0114] The raw materials for the supporting adhesive layer are provided according to the following weight portions: 100 weight portions of a third photovoltaic matrix resin, 5 weight portions of a tackifier, 3 weight portions of a cross-linking agent, 1 weight portion of a third auxiliary cross-linking agent, 30 weight portions of talcum powder, 30 weight portions of magnesium hydroxide, 20 weight portions of zinc barium oxide, and the mass content of the filler is 42.3%, wherein the third photovoltaic matrix resin is an EVA resin with a VA content of 28%, the tackifier is 3-aminopropyltrimethoxysilane, the cross-linking agent is diisopropyl peroxide, and the third auxiliary cross-linking agent is allyl acrylate, and finally a three-layer packaging material S1 is obtained.
[0115] Comparative Example 2
[0116] The difference from Example 12 is that the packaging adhesive film is composed of a single reflective adhesive layer 20, and finally the adhesive film S2 is obtained.
[0117] Comparative Example 3
[0118] The difference from Comparative Example 2 is that the film S3 is directly rolled up without electron beam pre-crosslinking treatment.
[0119] Comparative Example 4
[0120] The difference from Example 2 is that the base film after electron beam irradiation is then sent to a 140° C. drying tunnel for foaming for 11 minutes, and then cooled and rolled up to obtain the packaging film S4.
[0121] Comparative Example 5
[0122] The difference from Example 13 is that the weight of each layer is adjusted, the thickness of the micro-cross-linked layer is 0.01 mm, the thickness of the reflective adhesive layer 20 is 0.35 mm, and the thickness of the supporting adhesive layer 30 is 0.35 mm, and finally a three-layer packaging material S5 is obtained.
[0123] The following tests were performed on the three-layer packaging materials E1 to E19, S1 to S5, single-layer slightly cross-linked layers E1-1 to E19-1, single-layer packaging films E1-2 to E19-2, single-layer packaging films E1-3 to E19-3, single-layer slightly cross-linked layers S1-1, S4-1, S5-1, single-layer packaging films S1-2 to S4-2, S5-2, single-layer packaging films S1-3, S4-3, S5-3, respectively, obtained in Examples 1 to 19 and Comparative Examples 1 to 5:
[0124] 1. Peel strength of packaging materials
[0125] The test method refers to the national standard GB / T2790 "Adhesive 180° Peel Strength Test Method Flexible Materials to Rigid Materials".
[0126] Preparation of the peel strength sample of the encapsulation film and the backplane: Take 3mm thick glass, encapsulation material, and backplane, and put them into a vacuum laminator in the order of glass / F406PS / encapsulation film (reflective layer facing F406PS) / isolation strip / backplane, and laminate and cure at 145℃ for 18 minutes. F406PS is a transparent EVA product commercially available from Hangzhou Foster Applied Materials Co., Ltd.
[0127] Preparation of the peel strength sample of packaging film and battery: Take 3mm thick glass, single-chip crystalline silicon battery, packaging material, and backplane, and put them into a vacuum laminator in the order of glass / F406PS / battery / isolation strip / packaging film / backplane, and laminate and cure at 145℃ for 18 minutes.
[0128] The test was carried out on a tensile testing machine with a peeling speed of 100 mm / min, and the tensile strength value was recorded.
[0129] The peel strength between the encapsulation film and the back sheet is recorded as “ / B”; the peel strength between the encapsulation film and the battery is recorded as “ / C”.
[0130] 2. Pre-crosslinking degree
[0131] The pre-crosslinking degree is tested by the method of xylene heating extraction. The ratio of the mass not dissolved by xylene to the initial mass is the pre-crosslinking degree. The arithmetic mean of the three samples is taken as the pre-crosslinking degree of the film, in %. The crosslinking degree before lamination (pre-crosslinking degree) is the pre-crosslinking degree of the packaging film directly extracted by xylene heating.
[0132] 3. Volume resistivity
[0133] The encapsulation film was laminated at 145°C for 18 minutes, and the thickness after lamination was 0.5mm. The laminated samples were cut into 8cm*8cm size and placed in an environment of 25°C and 50% relative humidity for 24 hours. According to the IEC62788-1-2 standard, the volume resistivity of the sample was tested using a KEITHLEY 6517B high resistance meter at 1000V and 60 minutes of polarization time. The arithmetic mean of the three samples was taken as the volume resistivity of the film.
[0134] 4. Density
[0135] Refer to the national standard GBT6343-1995 to test the apparent density of the packaging film.
[0136] 5. Cell diameter and cell density
[0137] The cell structure of the encapsulation film is characterized using a scanning electron microscope. In two or three scanning electron microscope images, the average size of at least 200 cell diameters in the encapsulation film is used as the cell diameter of the encapsulation film.
[0138] Cell density N0 (cells / cm 3 ) is calculated by the following formula:
[0139]
[0140] n is the number of cells; A is the SEM image area, cm 2 ρ s is the density of the unfoamed material, ρ f is the density of the foam material.
[0141] 6. Appearance evaluation of single glass modules with encapsulation film
[0142] Use the encapsulation film to carry out the single-glass module encapsulation test. Put the glass / F406P (as the front layer encapsulation material) / cell / encapsulation film of the present invention / backplane into the vacuum laminator in the order of glass / F406P (as the front layer encapsulation material) / cell / encapsulation film of the present invention / backplane. At 145°C, vacuumize first and then pressurize, and cure for a total of 18 minutes. Observe the appearance of the single-glass module, such as white overflow, wrinkles, and cracks. Hidden cracks can be confirmed by EL testing.
[0143] 7. Shore hardness A
[0144] Refer to GBT2411-2008 standard for testing.
[0145] 8. Reflectivity
[0146] Sample preparation: Take the packaging film and put it into the vacuum laminator in the order of release film / packaging film / release film, and laminate and cure at 145°C for 18 minutes. Take out the laminated film for testing.
[0147] The reflectivity of the film at 400-1100 nm was measured using a UV-visible spectrophotometer.
[0148] The test results are shown in Tables 1 to 3.
[0149] Table 1
[0150]
[0151]
[0152] Table 2
[0153]
[0154] Table 3
[0155]
[0156] Among them, Table 3 is the test data of each single layer of the three-layer packaging materials E1~E19, S1~S5 obtained in Examples 1 to 19 and Comparative Examples 1 to 5. Specifically, the micro-cross-linked layer refers to the test of the single-layer micro-cross-linked layers E1-1~E19-1, S1-1, S4-1, and S5-1 of the three-layer packaging materials E1~E19, S1, S4, and S5; the reflective adhesive layer refers to the test of the single-layer packaging adhesive films E1-2~E19-2 and S1-2~S5-2 of the three-layer packaging materials E1~E19, S1~S5; the supporting adhesive layer refers to the test of the single-layer packaging adhesive films E1-3~E19-3, S1-3, S4-3, and S5-3 of the three-layer packaging materials E1~E19, S1, S4, and S5.
[0157] From the comprehensive analysis of the data in Tables 1 to 3 above, it can be concluded that the overall performance of the three-layer packaging materials of Examples 1 to 19 is significantly better than that of the three-layer packaging materials of Comparative Examples 1 to 5.
[0158] Specifically, compared with Example 1, the filler content in the supporting adhesive layer in Example 2 is 11.86%, and the supporting adhesive layer is foamed, so the hardness of the packaging material is lower, but the foaming causes the peeling strength between the packaging material and the backplane to decrease.
[0159] In Example 3, the mass content of the filler in the supporting adhesive layer is 35.5%. By adjusting the foaming temperature, the foaming degree of the reflective adhesive layer is greatly improved, the pore diameter becomes larger, the Shore hardness is reduced, and the reflectivity is improved to a certain extent.
[0160] Compared with Example 1, polyolefin synthetic silicone oil is added to the micro-crosslinked layer in Example 4, so that the Shore hardness of the three-layer packaging material is lower and softer.
[0161] In Example 5, POE, i.e., metallocene-catalyzed ethylene-octene copolymer, is used as the main resin of the micro-crosslinked layer. Compared with EVA, its hardness is greater, resulting in a certain degree of increase in its hardness, but it is still within a good range.
[0162] In Examples 6 and 7, different foaming degrees are obtained by changing the foaming process, and the obtained three-layer packaging material has good Shore hardness and will not have hidden cracks.
[0163] In Examples 9 to 11, by adjusting the formula and irradiation process in the reflective adhesive layer, reflective adhesive layers with different pre-crosslinking degrees are obtained, and the performances all meet the composite requirements. It can be observed from the Shore hardness that as the pre-crosslinking degree of the reflective layer increases, its Shore hardness also increases. Especially compared with Example 8, it can be clearly seen that when the pre-crosslinking degree of the reflective adhesive layer exceeds 60%, the hardness has reached 82.5, which has a certain adverse effect on the hidden cracking of the battery cell. Therefore, it is preferred to control the pre-crosslinking degree of the reflective adhesive layer within the range of 0.5 to 60%.
[0164] In Examples 12 to 14, by adjusting the titanium dioxide content of the micro-cross-linked layer, the reflective adhesive layer and the supporting adhesive layer, it can be seen that in Example 13, the titanium dioxide content is added to 28%, and the reflectivity of the three-layer packaging material is greatly improved, but at the same time, even if 20 parts of polyolefin synthetic silicone oil are added to reduce its Shore hardness, its hardness is still relatively large; in Examples 12 and 14, titanium dioxide is added to the supporting adhesive layer and the micro-cross-linked layer, but the improvement in the reflectivity of the packaging material is not as obvious as in Example 13, and the cost of titanium dioxide is relatively high. Therefore, from a cost perspective, it is preferred that the total titanium dioxide content of the micro-cross-linked layer and the supporting adhesive layer is less than 12%.
[0165] In Examples 15 and 16, micro-cross-linked layers with different pre-cross-linking degrees are obtained by adjusting the content of the auxiliary cross-linking agent in the micro-cross-linked layer. Compared with Example 1, it can be intuitively concluded that as the pre-cross-linking degree of the micro-cross-linked layer increases, the hardness of the three-layer packaging material also increases. It can be seen from Example 15 that when the pre-cross-linking degree of the micro-cross-linked layer reaches 5%, the hardness of the three-layer packaging material has reached 82, which has a certain impact on the hidden cracking of the battery cell. Therefore, considering the hidden cracking of the battery cell, the preferred pre-cross-linking degree of the micro-cross-linked layer is 0.5-5%.
[0166] In Examples 17 and 18, packaging materials with micro-cross-linked layers of different thicknesses are obtained by adjusting the gram weight distribution of the micro-cross-linked layer in the extrusion process. It can be concluded from Examples 1, 17, and 18 that as the thickness of the micro-cross-linked layer increases, the improvement in the Shore hardness of the packaging material becomes more obvious, that is, the Shore hardness decreases, but at the same time, as the thickness of the micro-cross-linked layer increases, the reflectivity of the packaging material also decreases slightly. In order to take into account both the Shore hardness and the reflectivity, it is preferred to control the thickness of the micro-cross-linked layer to 0.06-0.35 mm.
[0167] In Example 19, by adjusting the gram weight distribution of each layer in the extrusion process, a packaging material with a micro-cross-linked layer thickness of 0.35 mm, a reflective adhesive layer 20 thickness of 0.1 mm, and a supporting adhesive layer 30 thickness of 0.5 mm is obtained. At this time, although the packaging material described in Example 19 has good Shore hardness and is relatively soft, at this time, the thickness of the micro-cross-linked layer accounts for 36.8%, and the thickness ratio of the micro-cross-linked layer to the reflective adhesive layer reaches the upper limit of 3.5:1. Compared with Example 1, the thickness of the reflective adhesive layer is reduced. Although it has good Shore hardness, its reflectivity is greatly lost.
[0168] Compared with Example 1, the filler content in the supporting adhesive layer of Comparative Example 1 reaches 42.3%, which exceeds the upper limit of the filler content in the supporting adhesive layer. Its Shore hardness is relatively large, which has a certain impact on the hidden cracks of the battery cell, and there is no obvious improvement in reflectivity.
[0169] Compared with Example 12, Comparative Example 2 has only one reflective adhesive layer, which shows that the micro-cross-linking layer is missing, and its Shore hardness cannot meet the standard, resulting in hidden cracks in the battery cell.
[0170] Comparative Example 3 was not cross-linked, and its reflective adhesive layer was not pre-cross-linked, resulting in a whitening problem on the appearance of the component.
[0171] Comparative Example 4 was foamed for a longer time based on Example 2, and the pore diameter of the reflective adhesive layer reached 0.32 mm. Although the Shore hardness and reflectivity were good, excessive foaming caused the reflective adhesive layer to have too low a tearing force, and the proportional strength of the packaging material and the battery cell was extremely poor, and the tearing began from the inside of the reflective adhesive layer and the supporting adhesive layer, which had an adverse effect on the strength of the component.
[0172] In Comparative Example 5, by adjusting the gram weight distribution of each layer in the extrusion process, the thickness of the micro-cross-linked layer is 0.01 mm, the thickness of the reflective adhesive layer is 0.35 mm, and the thickness of the supporting adhesive layer is 0.35 mm. It can be seen that the thickness of the micro-cross-linked layer is only 0.01 mm, and the micro-cross-linked layer accounts for 1.4% of the overall thickness, and the thickness ratio of the micro-cross-linked layer to the reflective adhesive layer is less than the lower limit of 0.1, which is only 0.028 (the thickness ratio of the micro-cross-linked layer to the supporting adhesive layer is less than the lower limit of 0.07). Although the thickness of the reflective adhesive layer accounts for a relatively high proportion, which ensures that the reflectivity of the packaging material is at an extremely high level, the thickness of the micro-cross-linked layer is too low, resulting in an excessively high Shore hardness, which causes hidden cracks in the battery cell.
[0173] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:
[0174] The packaging material of the present application is set to be multi-layer, and even if the thickness of the reflective adhesive layer is reduced, the set packaging effect can still be achieved, and more titanium dioxide is only set in the reflective adhesive layer to achieve a high reflection effect, and the mass content of titanium dioxide in the pre-crosslinked layer and the supporting adhesive layer is controlled to be lower than 12% (that is, including two situations: no titanium dioxide is set and titanium dioxide is set and the mass content of titanium dioxide is lower than 12%), thereby reducing the amount of titanium dioxide in the entire multi-layer packaging material, and at the same time, fillers are used in the supporting adhesive layer to further reduce the cost of the supporting adhesive layer, thereby reducing the cost of the multi-layer packaging film. However, the content of the filler should not be too much, otherwise it will cause the hardness of the supporting adhesive layer to be too large. Furthermore, in the multi-layer packaging material of the present application, a pre-crosslinked layer is used to cover the reflective adhesive layer, thereby effectively avoiding the problem of white overflow of the reflective adhesive layer during the lamination process.
[0175] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A multi-layer packaging material, characterized in that: The multi-layer packaging material comprises a micro-crosslinked layer (10), a reflective adhesive layer (20) and a supporting adhesive layer (30) stacked in sequence, or the multi-layer packaging material comprises a reflective adhesive layer (20), a micro-crosslinked layer (10) and a supporting adhesive layer (30) stacked in sequence, the pre-crosslinking degree of the micro-crosslinked layer (10) is 0.5-5%, the reflective adhesive layer (20) contains titanium dioxide with a mass content of 2-30%, the support adhesive layer (30) contains a filler with a mass content of 10-40%, the support adhesive layer (30) contains titanium dioxide with a mass content of less than 12%, the micro-crosslinked layer (10) contains titanium dioxide with a mass content of less than 12%, and the thickness of the micro-crosslinked layer (10) is 5-38% of the total thickness of the multi-layer packaging material.
2. The multi-layer packaging material according to claim 1, characterized in that: The thickness of the micro-crosslinked layer (10) is 0.06-0.35 mm.
3. The multi-layer packaging material according to claim 1, characterized in that: The reflective adhesive layer (20) and the supporting adhesive layer (30) each independently have a cellular structure.
4. The multi-layer packaging material according to claim 3, characterized in that: The cell density of the reflective adhesive layer (20) and the supporting adhesive layer (30) is 80 to 10 10 Unit cells / cm 3 The cell diameter of the unit cell is 0.1 μm to 0.1 mm.
5. The multi-layer packaging material according to claim 3 or 4, characterized in that: The thickness ratio of the micro-crosslinked layer (10) to the reflective adhesive layer (20) is 3.5:1 to 1:
10.
6. The multi-layer packaging material according to claim 3 or 4, characterized in that: The thickness ratio of the micro-crosslinking layer (10) to the supporting adhesive layer (30) is 3.5:1 to 1:
14.
7. The multi-layer packaging material according to any one of claims 1 to 4, characterized in that: The multi-layer packaging material comprises a reflective adhesive layer (20), a micro-crosslinked layer (10) and a supporting adhesive layer (30) stacked in sequence, the reflective adhesive layer (20) being a pre-crosslinked film, and the pre-crosslinking degree of the pre-crosslinked film being 0.5-70%.
8. The multi-layer packaging material according to claim 7, characterized in that: The pre-crosslinking degree of the pre-crosslinked film is 0.5-60%.
9. The multi-layer packaging material according to claim 1, characterized in that: The volume resistivity of the supporting adhesive layer (30) is greater than 1.0×10 14 Ω·cm.
10. The multi-layer packaging material according to claim 1, characterized in that: The filler is selected from any one or more combinations of CaCO3, lithopone, wollastonite, mica powder, magnesium hydroxide, aluminum hydroxide, calcium hydroxide, talcum powder, barium sulfate, glass microspheres, zinc sulfide, kaolin, and montmorillonite.
11. The multi-layer packaging material according to claim 1, characterized in that: The raw materials for forming the micro-crosslinked layer (10) include: 100 parts by weight of a first photovoltaic matrix resin, 0.01 to 10 parts by weight of a tackifier, 0.01 to 5 parts by weight of a crosslinking agent, 0 to 2 parts by weight of a first auxiliary crosslinking agent, 0 to 15 parts by weight of titanium dioxide, 0 to 3 parts by weight of an auxiliary agent, and 0 to 10 parts by weight of a first polyolefin synthetic oil; The first auxiliary cross-linking agent is a first sensitizer.
12. The multi-layer packaging material according to claim 11, characterized in that: The first photovoltaic matrix resin is selected from any one or more of the following polymers: ethylene-vinyl acetate copolymer, metallocene-catalyzed polyethylene, metallocene-catalyzed ethylene-butene copolymer, metallocene-catalyzed ethylene-octene copolymer, metallocene-catalyzed ethylene-pentene copolymer, ethylene-propylene copolymer, ethylene-methyl acrylate copolymer, ethylene-methyl methacrylate copolymer, ethylene-glycidyl methacrylate copolymer, ethylene-glycidyl methacrylate-vinyl acetate copolymer, ethylene-glycidyl methacrylate-methyl acrylate copolymer.
13. The multi-layer packaging material according to claim 11, characterized in that: The first sensitizer is an allyl sensitizer.
14. The multi-layer packaging material according to claim 11, characterized in that: The first sensitizer is any one or more of the following compounds: trimethallyl isocyanate, triallyl isocyanurate, triallyl cyanurate, divinylbenzene, di-isopropenylbenzene, diallyl phthalate, allyl acrylate, allyl methacrylate, diallyl maleate, and diallyl phthalate.
15. The multi-layer packaging material according to claim 11, characterized in that: The first polyolefin synthetic oil is selected from any one or more of poly-α-olefin synthetic oil, polybutene synthetic oil, and alkylbenzene synthetic oil.
16. The multi-layer packaging material according to claim 15, characterized in that: The first polyolefin synthetic oil is a liquid ethylene polymer oil.
17. The multi-layer packaging material according to claim 16, characterized in that: The liquid ethylene polymer oil is derived from a combination of ethylene A and an α-olefin B having 3 to 20 carbon atoms or a combination of ethylene A, an α-olefin B having 3 to 20 carbon atoms and a non-conjugated polyene C, and the liquid ethylene polymer oil satisfies the following conditions 1) to 4); the non-conjugated polyene C contains in the molecule a total of two or more partial structures selected from the group consisting of the following general formulas (I) and (II), Wherein, 1) the molar ratio of ethylene A / α-olefin B is 40:60 to 95:5; 2) the weight fraction of the structural units derived from the non-conjugated polyene C in the liquid ethylene polymer oil is 0 to 10%; 3) the weight average molecular weight Mw of the ethylene-α-olefin-non-conjugated polyene copolymer, the weight fraction of the structural units derived from the non-conjugated polyene C and the weight average molecular weight Mw of the non-conjugated polyene C satisfy: Mw×weight fraction of C / molecular weight of C ≤40; 4) the number average molecular weight Mn of the liquid ethylene polymer oil measured by gel permeation chromatography is less than 30,000.
18. The multi-layer packaging material according to claim 11, characterized in that: The first polyolefin synthetic oil is an ethylene-propylene copolymer or an ethylene-propylene-non-conjugated diene terpolymer.
19. The multi-layer packaging material according to claim 18, characterized in that: The proportion of ethylene and propylene units in the ethylene-propylene-non-conjugated diene terpolymer is greater than 90%.
20. The multi-layer packaging material according to claim 17, characterized in that: The ethylene-α-olefin-non-conjugated polyene copolymer includes a unit derived from ethylene or includes a unit derived from propylene.
21. The multi-layer packaging material according to claim 17, characterized in that: The ethylene-α-olefin-non-conjugated polyene copolymer includes units derived from a diene monomer.
22. The multi-layer packaging material according to claim 21, characterized in that The diene monomer is any one or more of a non-conjugated straight-chain hydrocarbon diene, a non-conjugated branched-chain hydrocarbon diene, and a non-conjugated cyclic hydrocarbon diene having 6 to 15 carbon atoms.
23. The multi-layer packaging material according to claim 11, characterized in that The weight average molecular weight of the first polyolefin synthetic oil is 200-50,000.
24. The multi-layer packaging material according to claim 23, characterized in that: The weight average molecular weight of the first polyolefin synthetic oil is 200-10000.
25. The multi-layer packaging material according to claim 11, characterized in that The viscosity index of the first polyolefin synthetic oil is 60-250.
26. The multi-layer packaging material according to claim 25, characterized in that The viscosity index of the first polyolefin synthetic oil is 80-180.
27. The multi-layer packaging material according to claim 1, characterized in that The raw materials for forming the reflective adhesive layer (20) include: 100 parts by weight of a second photovoltaic matrix resin, 0.01 to 15 parts by weight of a tackifier, 0.01 to 5 parts by weight of a cross-linking agent, 0.05 to 5 parts by weight of a second auxiliary cross-linking agent, 2 to 40 parts by weight of titanium dioxide, 0 to 3 parts by weight of an auxiliary agent, 0 to 30 parts by weight of a foaming agent, 0 to 30 parts by weight of a foaming auxiliary agent, and 0 to 10 parts by weight of a second polyolefin synthetic oil; The second auxiliary cross-linking agent is a second sensitizer and / or a third sensitizer.
28. The multi-layer packaging material according to claim 27, characterized in that The second photovoltaic matrix resin is selected from any one or more of the following polymers: ethylene-vinyl acetate copolymer, metallocene-catalyzed polyethylene, metallocene-catalyzed ethylene-butene copolymer, metallocene-catalyzed ethylene-octene copolymer, metallocene-catalyzed ethylene-pentene copolymer, ethylene-propylene copolymer, ethylene-methyl acrylate copolymer, ethylene-methyl methacrylate copolymer, ethylene-glycidyl methacrylate copolymer, ethylene-glycidyl methacrylate-vinyl acetate copolymer, ethylene-glycidyl methacrylate-methyl acrylate copolymer, saponified ethylene-vinyl acetate copolymer and saponified ethylene-vinyl acetate-acrylate copolymer.
29. The multi-layer packaging material according to claim 27, characterized in that The second sensitizer is an allyl sensitizer.
30. The multi-layer packaging material according to claim 27, characterized in that The second sensitizer is any one or more of the following compounds: trimethallyl isocyanate, triallyl isocyanurate, triallyl cyanurate, divinylbenzene, di-isopropenylbenzene, diallyl phthalate, allyl acrylate, allyl methacrylate, diallyl maleate and diallyl phthalate.
31. The multi-layer packaging material according to claim 27, characterized in that The third sensitizer is an acrylate-based sensitizer.
32. The multi-layer packaging material according to claim 31, characterized in that The third sensitizer is any one or more of the following compounds: allyl acrylate, allyl methacrylate, diallyl maleate, diallyl phthalate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol triacrylate, ethoxylated glycerol triacrylate, tetramethylolmethane triacrylate, ethoxylated pentaerythritol tetraacrylate, dimethylolpropane tetraacrylate, trimethylolethane trimethacrylate, pentaerythritol tetraacrylate, tetramethylolmethane tetraacrylate, ditrimethylolpropane tetraacrylate, pentaerythritol tetramethacrylate, tetramethylolmethane tetramethacrylate, ditrimethylolpropane tetramethacrylate, dipentaerythritol polyacrylate, dipentaerythritol hexaacrylate, dipentaerythritol polymethacrylate, and dipentaerythritol hexamethacrylate.
33. The multi-layer packaging material according to claim 27, characterized in that The second auxiliary cross-linking agent is a third sensitizer.
34. The multi-layer packaging material according to claim 27, characterized in that The second polyolefin synthetic oil is selected from any one or more of poly-α-olefin synthetic oil, polybutene synthetic oil, and alkylbenzene synthetic oil.
35. The multi-layer packaging material according to claim 34, characterized in that The second polyolefin synthetic oil is a liquid ethylene polymer oil.
36. The multi-layer packaging material according to claim 35, characterized in that The liquid ethylene polymer oil is derived from a combination of ethylene A and an α-olefin B having 3 to 20 carbon atoms or a combination of ethylene A, an α-olefin B having 3 to 20 carbon atoms and a non-conjugated polyene C, and the liquid ethylene polymer oil satisfies the following conditions 1) to 4); the non-conjugated polyene C contains in the molecule a total of two or more partial structures selected from the group consisting of the following general formulas (I) and (II), Wherein, 1) the molar ratio of ethylene A / α-olefin B is 40:60 to 95:5; 2) the weight fraction of the structural units derived from the non-conjugated polyene C in the liquid ethylene polymer oil is 0 to 10%; 3) the weight average molecular weight Mw of the ethylene-α-olefin-non-conjugated polyene copolymer, the weight fraction of the structural units derived from the non-conjugated polyene C and the weight average molecular weight Mw of the non-conjugated polyene C satisfy: Mw×weight fraction of C / molecular weight of C ≤40; 4) the number average molecular weight Mn of the liquid ethylene polymer oil measured by gel permeation chromatography is less than 30,000.
37. The multi-layer packaging material according to claim 27, characterized in that The second polyolefin synthetic oil is an ethylene-propylene copolymer or an ethylene-propylene-non-conjugated diene terpolymer.
38. The multi-layer packaging material according to claim 37, characterized in that The proportion of ethylene and propylene units in the ethylene-propylene-non-conjugated diene terpolymer is greater than 90%.
39. The multi-layer packaging material according to claim 36, characterized in that The ethylene-α-olefin-non-conjugated polyene copolymer includes a unit derived from ethylene or includes a unit derived from propylene.
40. The multi-layer packaging material according to claim 36, characterized in that The ethylene-α-olefin-non-conjugated polyene copolymer includes units derived from a diene monomer.
41. The multi-layer packaging material according to claim 40, characterized in that The diene monomer is any one or more of a non-conjugated straight-chain hydrocarbon diene, a non-conjugated branched-chain hydrocarbon diene, and a non-conjugated cyclic hydrocarbon diene having 6 to 15 carbon atoms.
42. The multi-layer packaging material according to claim 27, characterized in that The weight average molecular weight of the second polyolefin synthetic oil is 200-50,000.
43. The multi-layer packaging material according to claim 42, characterized in that The weight average molecular weight of the second polyolefin synthetic oil is 200-10,000.
44. The multi-layer packaging material according to claim 27, characterized in that The viscosity index of the second polyolefin synthetic oil is 60-250.
45. The multi-layer packaging material according to claim 44, characterized in that The viscosity index of the second polyolefin synthetic oil is 80-180.
46. The multi-layer packaging material according to claim 27, characterized in that The foaming agent is a physical foaming agent and / or a chemical foaming agent.
47. The multi-layer packaging material according to claim 46, characterized in that The physical foaming agent is selected from any one or more combinations of nitrogen, carbon dioxide, organic hydrocarbon liquid with a boiling point <110° C., and core-shell microsphere foaming agent.
48. The multi-layer packaging material according to claim 47, characterized in that The organic hydrocarbon liquid is selected from any one or more of propane, butane, pentane and methyl chloride.
49. The multi-layer packaging material according to claim 46, characterized in that The chemical foaming agent is an inorganic foaming agent and / or an organic foaming agent.
50. The multi-layer packaging material according to claim 49, characterized in that The inorganic foaming agent is selected from any one or more combinations of sodium bicarbonate, ammonium carbonate and sodium nitrite.
51. The multi-layer packaging material according to claim 49, characterized in that The organic foaming agent is selected from any one or more combinations of sulfonylhydrazide compounds, azo compounds and nitroso compounds.
52. The multi-layer packaging material according to claim 51, characterized in that The sulfonyl hydrazide compound is 4,4'-oxybisbenzenesulfonyl hydrazide and / or p-toluenesulfonyl hydrazide.
53. The multi-layer packaging material according to claim 51, characterized in that The azo compound is azodicarbonamide.
54. The multi-layer packaging material according to claim 51, characterized in that The nitroso compound is dinitroso-pentamethylene-tetramine.
55. The multi-layer packaging material according to claim 27, characterized in that The foaming aid is selected from any one or more combinations of metal oxides, metal salts, and metal organic complexes.
56. The multi-layer packaging material according to claim 1, characterized in that The raw materials for forming the supporting adhesive layer (30) include: 100 parts by weight of a third photovoltaic matrix resin, 0.01 to 10 parts by weight of a tackifier, 0.05 to 2 parts by weight of a third auxiliary cross-linking agent, 0 to 10 parts by weight of a foaming agent, 0 to 10 parts by weight of a foaming aid, 0 to 15 parts by weight of the titanium dioxide, 15 to 60 parts by weight of the filler and 0 to 3 parts by weight of an auxiliary agent.
57. The multi-layer packaging material according to claim 56, characterized in that The third photovoltaic matrix resin is selected from any one or more of the following polymers: ethylene-vinyl acetate copolymer, metallocene-catalyzed polyethylene, metallocene-catalyzed ethylene-butene copolymer, metallocene-catalyzed ethylene-octene copolymer, metallocene-catalyzed ethylene-pentene copolymer, ethylene-propylene copolymer, ethylene methyl acrylate copolymer, ethylene methyl methacrylate copolymer, ethylene-glycidyl methacrylate-vinyl acetate copolymer, ethylene-glycidyl methacrylate-methyl acrylate copolymer, saponified ethylene-vinyl acetate copolymer, saponified ethylene-vinyl acetate-acrylate copolymer, low-density polyethylene, linear low-density polyethylene, linear ultra-low-density polyethylene, and modified polyolefin transparent resin polymers.
58. The multi-layer packaging material according to claim 56, characterized in that The third auxiliary cross-linking agent is the fourth sensitizer and / or the fifth sensitizer.
59. The multi-layer packaging material according to claim 58, characterized in that The fourth sensitizer is an allyl sensitizer.
60. The multi-layer packaging material according to claim 59, characterized in that The fourth sensitizer is any one or more of the following compounds: trimethallyl isocyanate, triallyl isocyanurate, triallyl cyanurate, divinylbenzene, di-isopropenylbenzene, diallyl phthalate, allyl acrylate, allyl methacrylate, diallyl maleate and diallyl phthalate.
61. The multi-layer packaging material according to claim 58, characterized in that The fifth sensitizer is an acrylate-based sensitizer.
62. The multi-layer packaging material according to claim 61, characterized in that The fifth sensitizer is any one or more of the following compounds: allyl acrylate, allyl methacrylate, diallyl maleate, diallyl phthalate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol triacrylate, ethoxylated glycerol triacrylate, tetramethylolmethane triacrylate, ethoxylated pentaerythritol tetraacrylate, dimethylolpropane tetraacrylate, trimethylolethane trimethacrylate, pentaerythritol tetraacrylate, tetramethylolmethane tetraacrylate, ditrimethylolpropane tetraacrylate, pentaerythritol tetramethacrylate, tetramethylolmethane tetramethacrylate, ditrimethylolpropane tetramethacrylate, dipentaerythritol polyacrylate, dipentaerythritol hexaacrylate, dipentaerythritol polymethacrylate, and dipentaerythritol hexamethacrylate.
63. A photovoltaic module, comprising a front plate (1), a transparent adhesive film (2), a battery cell unit (3), a back layer adhesive film (4) and a back plate (5) which are laminated in sequence, characterized in that: The back layer adhesive film (4) is a multi-layer packaging material according to any one of claims 1 to 62, and the supporting adhesive layer (30) of the multi-layer packaging material is arranged away from the battery cell unit (3).