A composite structure proton type solid oxide electrolytic cell and preparation method thereof

Through the casting-phase conversion method and impregnation method, the transition metal and alkali metal oxides were modified to prepare a composite structure proton solid oxide electrolytic cell, which solved the gas diffusion of proton electrolytic cells in the application of high-temperature electrolytic carbon dioxide in the prior art. and carbon deposits have achieved high activity and stability, and have promoted its development in the field of high-temperature electrolysis.

CN115161689BActive Publication Date: 2024-11-12SHANDONG UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211023732.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-23
Publication Date
2024-11-12
Estimated Expiration
2042-08-23

AI Technical Summary

Technical Problem

Proton-type solid oxide electrolytic cells have potential in high-temperature electrolytic carbon dioxide due to their excellent carbon deposit resistance and high activity. However, the existing preparation methods limit their performance and stability, especially the preparation of porous cathode support and proton conductor films. The method causes slow gas diffusion and severe carbon deposit reaction, which affects its application.

Method used

The multi-stage structural barium cerate support is prepared by casting-phase conversion method, spin-coated barium zirconate electrolyte stabilization layer, and modified the transition metal and alkaline metal oxide nanocomposites in a large-size open finger pore structure by impregnation method Particles, combined with acid-base-reduction treatment, prepare highly active, carbon-resistant composite structure proton-type solid oxide electrolytic cells.

Benefits of technology

Improves gas diffusion activity and electrocatalytic activity, enhances carbon deposit resistance and structural stability, reduces concentration polarization resistance, significantly improves the current density and stability of electrolytic carbon dioxide, and promotes SOEC in the field of high-temperature electrolytic carbon dioxide application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115161689B_ABST
    Figure CN115161689B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a composite structure proton type solid oxide electrolytic cell, comprising the following steps: preparing a barium cerate support based on a tape casting phase conversion method, including a dense layer, a sponge layer and a large-size open finger hole layer; preparing a barium zirconate electrolyte stabilization layer on the dense layer of the barium cerate support; preparing a proton-oxygen ion-electron three-conductor anode layer on a double-layer proton conductor electrolyte of the support; vacuum impregnating a transition metal ion solution and an alkaline metal ion solution in the large-size open finger hole layer of the barium cerate support respectively to obtain a transition metal-alkaline metal impregnation layer; acid-base-reduction treatment of the transition metal-alkaline metal impregnation layer to obtain a composite structure proton type solid oxide electrolytic cell. The composite structure proton type solid oxide electrolytic cell has high reactivity and carbon deposition resistance, has great application potential in the high-temperature electrocatalytic CO2 reaction process, and is conducive to promoting the development and application of SOEC in high-temperature electrolysis of carbon dioxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid oxide electrolytic cells, and in particular to a composite structure proton type solid oxide electrolytic cell and a preparation method thereof. Background Art

[0002] At present, various electrocatalytic CO2 conversion technologies and related new materials are being actively developed both at home and abroad. Electrolysis of CO2 is one of the important ways to achieve energy conservation, emission reduction and resource utilization. Solid oxide electrolysis cell (SOEC) is considered to have great industrial potential in direct electrolysis of CO2 because of its relatively high current density, Faraday efficiency and durability in the electrocatalytic CO2 reduction reaction (CO2RR), and the use of cheap oxides as catalysts, which results in low cost. However, the CO2RR rate-limiting process and carbon deposition reaction still limit performance. The development of cathode catalysts with high electrocatalytic activity and resistance to carbon deposition and the corresponding electrolysis cell system are key research directions for high-temperature CO2 electrolysis.

[0003] Ni-based fluorite oxide composites, such as commercial Ni-Zr 0.8 Y 0.2 O 1.9 , which is a commonly used oxygen ion conducting SOEC cathode. Due to the serious carbon deposition reaction of Ni and the weak auxiliary carbon removal effect of the oxygen ion conductor YSZ electrolyte, the application of this electrolytic cell system in high-temperature electrolysis of carbon dioxide is still limited. The cathode of the proton type solid oxide electrolytic cell mostly uses alkaline perovskite, which can effectively enhance the carbon removal activity of the Ni surface. At present, the dry pressing method and casting method are commonly used to prepare the cathode support. The internal pore structure obtained is uncontrollable. A large number of closed pores are distributed near the cathode and electrolyte three-phase interface, which easily causes the reaction gas CO2 to diffuse slowly and form a large concentration polarization resistance. At the same time, the product gas CO accumulates locally in the pores and is prone to disproportionation reaction and carbon deposition. In addition, the proton type SOEC also has problems with electrolyte sintering and stability. For example, cerium-based perovskite oxides have high sintering activity but poor stability in carbon dioxide, and zirconium-based perovskite oxides have high stability but are difficult to sinter densely. The currently commonly used drop coating and dry pressing methods still have limitations in the preparation of dense proton conductor electrolyte membranes and need to be further optimized.

[0004] In summary, proton-based solid oxide electrolyzers have great potential for high-temperature electrolysis of carbon dioxide due to their excellent resistance to carbon deposition and high activity. However, the current preparation methods of proton conductor electrolyte membranes and porous cathode supports limit the performance and stability of proton-based solid oxide electrolyzers, which in turn limits their further promotion and application in the field of high-temperature electrolysis of carbon dioxide. Summary of the invention

[0005] In order to solve the above technical problems, the present invention discloses a composite structure proton type solid oxide electrolytic cell and its preparation method. The present invention combines the phase transformation method and the tape casting method to prepare a multi-level structure support body, which has a dense layer, a sponge layer and a large-size open finger pore structure, and uses the spin coating method to modify the barium zirconate electrolyte protective layer on the surface of the dense layer, and uses the impregnation method to modify a sufficient amount of transition metal and alkaline metal oxide nanocomposite particles in the uniform pores to prepare a highly active, anti-carbon deposition composite structure proton type solid oxide electrolytic cell, which is applied to the field of high-temperature electrolysis of carbon dioxide, can effectively improve gas diffusion and electrocatalytic carbon dioxide activity, while enhancing anti-carbon deposition and structural stability.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] According to a first aspect of an embodiment of the present invention, a method for preparing a composite structure proton-type solid oxide electrolytic cell is provided.

[0008] In one embodiment, a method for preparing a composite structure proton type solid oxide electrolytic cell comprises the following steps:

[0009] S1. A barium ceria support is prepared based on a tape casting-phase conversion method, including a dense layer, a sponge layer and a large-size open finger hole layer;

[0010] S2, preparing a barium zirconate electrolyte stabilizing layer on the dense layer of the barium ceria support to obtain a double-layer proton conductor electrolyte;

[0011] S3, preparing a proton-oxygen ion-electron triple conductor anode layer on a double-layer proton conductor electrolyte;

[0012] S4, vacuum impregnating a transition metal ion solution and an alkaline metal ion solution into the large-size open finger hole layer of the barium ceria support to obtain a transition metal-alkaline metal impregnation layer;

[0013] S5. Performing acid-base reduction treatment on the transition metal-alkaline metal impregnation layer to obtain a composite structure proton-type solid oxide electrolytic cell.

[0014] Optionally, in step S1, the step of preparing the barium ceria support body based on the tape casting-phase conversion method includes:

[0015] S1-1, barium cerate, pore-forming agent, organic solvent, dispersant and binder are mixed and ground according to a certain proportion, the grinding speed is 350-420 r / min, and the grinding time is 24-60 h;

[0016] S1-2, preparing a green body with a thickness of 800 to 1500 μm by tape casting;

[0017] S1-3, placing the green body in deionized water for phase transformation for 20 to 50 hours, and calcining after phase transformation to obtain a barium ceria support body, the calcination temperature is 1000 to 1350° C., and the calcination time is 2 to 6 hours.

[0018] Optionally, in step S1-1, the pore-forming agent is graphite, the organic solvent is 1-methyl-2-pyrrolidone, the dispersant is polyvinylpyrrolidone, and the binder is polyethersulfone;

[0019] The mass fractions of barium cerate, pore-forming agent, organic solvent, dispersant and binder are as follows:

[0020]

[0021] Optionally, in step S2, the step of preparing a barium zirconate electrolyte stabilizing layer on the dense layer of the barium ceria support comprises:

[0022] The barium zirconate electrolyte is spin-coated on the dense layer of the barium ceria support body at a spin-coating rate of 500-1200 rpm and a spin-coating time of 3-15 seconds; after drying at room temperature for 4-10 hours, the electrolyte is calcined at 1380-1450° C. for 15-36 hours to obtain a double-layer proton conductor electrolyte.

[0023] Optionally, step S3, the step of preparing a proton-oxygen ion-electron three-conductor anode, comprises:

[0024] The proton-oxygen ion-electron three-conductor anode and a pine alcohol solution containing 6wt% ethyl cellulose are mixed and ground in a mass ratio of 3:1, the grinding speed is 50-150r / min, the grinding time is 0.5-1.5h, and the mixture is coated on the surface of the barium zirconate electrolyte stabilization layer obtained in step S2, and calcined at a calcination temperature of 900-1150°C for 2-5h.

[0025] Optionally, the proton-oxygen ion-electron triple conductor anode is BaCo 0.7 Fe 0.2 Zr 0.1 O 3-δ ,BaFe 0.7 Zr 0.2 Y 0.1 O 3-δ , BaCo 0.6 Zr 0.2 Y 0.2 O 3-δ One of them.

[0026] Optionally, in step S4, the step of vacuum impregnating a transition metal ion solution and an alkaline metal ion solution into the large-size open finger hole layer of the barium ceria support to obtain a transition metal-alkaline metal impregnation layer comprises:

[0027] Under a vacuum degree of 0.1-0.05 MPa, a large-size open finger hole layer of a barium ceria support is impregnated with a transition metal ion solution, and calcined at 400-500° C. for 0.5-1.0 h, and the impregnation and calcination are repeated until the impregnation amount is 30-55 wt %; and then calcined at 700-900° C. for 0.5-2 h to obtain a transition metal impregnation layer;

[0028] Under a vacuum degree of 0.09-0.03 MPa, the large-size open finger hole layer is continuously impregnated with an alkaline metal ion solution and treated at 400-500°C for 0.5-1.0 h. The impregnation and calcination are repeated until the impregnation amount is 5.0-8.0 wt%, and then treated at 900-1150°C for 2-5 h to obtain a transition metal-alkaline metal impregnation layer.

[0029] Optionally, the transition metal ion solution is one of nickel nitrate, copper nitrate and zinc nitrate solutions, and the concentration is 0.5-2.0 mol / L.

[0030] Optionally, the alkaline metal ion solution is one of sodium carbonate, potassium carbonate, strontium nitrate solution, calcium nitrate solution, and magnesium nitrate solution, and the concentration is 0.05-0.5 mol / L.

[0031] Optionally, in step S5, the step of performing acid-base reduction treatment on the transition metal-alkaline metal impregnation layer includes:

[0032] A mixture of carbon dioxide and nitrogen is used for acid-base treatment, wherein the volume fraction of carbon dioxide is 0.5-6.5 vol%, the treatment temperature is 500-700°C, and the treatment time is 0.1-1.0 h; a mixture of hydrogen and nitrogen is used for reduction treatment, wherein the volume fraction of hydrogen is 5-20 vol%, the treatment temperature is 500-700°C, and the treatment time is 0.1-1.0 h.

[0033] According to a second aspect of an embodiment of the present invention, a composite structure proton-type solid oxide electrolytic cell prepared by the above method is proposed.

[0034] The beneficial effects of the present invention are:

[0035] 1. Prepare the barium ceria support by the tape casting-phase conversion method, spin-coat barium zirconate on the surface of the dense layer of the barium ceria support to obtain a proton conductor electrolyte dense layer and a stable layer, solve the problem of sintering density and stability of the proton-type solid oxide electrolytic cell, and form a skeleton with high porosity and regular macroporous structure; in the large-size open finger pore structure of the barium ceria support, use the impregnation method to prepare nickel and anti-carbon deposition metal copper or zinc composite nanoparticles in the large-size pores, protect Ni, reduce carbon deposition reaction, expand the three-phase interface, and improve CO2 electrocatalytic activity; further coat the transition metal particles with alkaline metal oxides to obtain composite nanoparticles, which can effectively improve the carbon removal reaction on the cathode surface of SOEC and enhance the anti-carbon deposition property;

[0036] 2. The composite structure proton-type solid oxide electrolytic cell of the present invention has a large-size open finger pore structure, which helps to improve the diffusion activity of CO2 in the electrode pores, surface adsorption and electrocatalytic reduction activity of CO2, and can reduce concentration polarization resistance; at the same time, the desorption and diffusion activity of the product CO are greatly improved, reducing carbon deposits formed by the disproportionation reaction.

[0037] In summary, the composite structure proton-type solid oxide electrolyzer has high reactivity and resistance to carbon deposition, and has great application potential in the high-temperature electrocatalytic CO2 reaction process, which is conducive to promoting the development and application of SOEC in high-temperature electrolysis of carbon dioxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a schematic diagram of the process of the present invention;

[0039] Figure 2 Schematic diagram of the barium ceria support prepared by casting and phase conversion in Example 1 of the present invention;

[0040] Figure 3 This is a schematic diagram of impregnating transition metal and alkaline metal ions into the large-sized open finger pores of cerium in Example 1 of the present invention. DETAILED DESCRIPTION

[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] Example 1

[0043] A method for preparing a composite structure proton type solid oxide electrolytic cell, such as Figure 1 As shown, the following steps are included:

[0044] S1. 97.5 g of barium ceria, 6.0 g of graphite, 39.0 g of 1-methyl-2-pyrrolidone, 6.3 g of polyethersulfone, and 1.2 g of polyvinyl pyrrolidone were mixed, and the mixture was ball-milled at a speed of 380 r / min for 36 h; a green body with a thickness of 1000 μm was obtained by tape casting; the green body was immersed in deionized water for phase conversion for 24 h, and then taken out, and calcined at 1100° C. for 4 h to obtain a barium ceria support, including a dense layer, a sponge layer, and a large-size open finger hole layer, such as Figure 2 As shown;

[0045] S2, spin coating barium zirconate on the surface of the dense layer of the barium ceria support at a spin coating rate of 600 rpm for 4 seconds, drying for 5 hours and calcining at 1450° C. for 20 hours to obtain a double-layer proton conductor electrolyte;

[0046] S3, 1.5g BaCo 0.7 Fe 0.2 Zr 0.1 O 3-δ (BCFZ) was mixed with a pine alcohol solution containing 6 wt% ethyl cellulose in a mass ratio of 3:1, and ball-milled at a speed of 120 r / min for 0.5 h to obtain an anode slurry, and the obtained anode slurry was coated on one side of the barium zirconate electrolyte stabilizing layer prepared above, and calcined at 950 ° C for 2 h to obtain a BCFZ anode layer;

[0047] S4. Under a vacuum degree of 0.1 MPa, the large-sized open finger-hole layer containing the cerium oxide support was impregnated with nickel nitrate and copper nitrate solutions with a concentration of 1.0 mol / L each for 50 times, and each time was calcined at 400°C for 1 hour, and finally calcined at 900°C for 2 hours, with an impregnation amount of 45.2wt%, to obtain a transition metal impregnation layer; under a vacuum degree of 0.06 MPa, the large-sized open finger-hole layer was impregnated with a sodium carbonate solution with a concentration of 0.1 mol / L for 12 times, and each time was calcined at 400°C for 1 hour, and finally calcined at 900°C for 2 hours, with an impregnation amount of 2.6wt%, to obtain a transition metal-alkaline metal impregnation layer, such as Figure 3 As shown;

[0048] S5. Use a mixture of carbon dioxide (2.0 vol%) and nitrogen to treat the transition metal-alkaline metal impregnation layer at 700°C for 0.4 h, and then use a mixture of hydrogen (15 vol%) and nitrogen to continue treating at 650°C for 0.5 h to obtain an electrolytic cell.

[0049] A mixture of carbon dioxide (75 vol%) and carbon monoxide (25 vol%) was introduced into the fuel electrode side of the electrolytic cell at a flow rate of 100 mL / min, and nitrogen was introduced into the anode side at a flow rate of 80 mL / min. An electrolysis voltage of 1.5 V was applied at 800 °C, and the current density reached 0.32 A / cm 2 , and a 30h stability test was carried out, and the current density remained basically unchanged.

[0050] Example 2

[0051] A method for preparing a composite structure proton type solid oxide electrolytic cell comprises the following steps:

[0052] S1. 128 g of barium ceria, 7.0 g of graphite, 54.2 g of methyl-2-pyrrolidone, 9.0 g of polyethersulfone, and 1.8 g of polyvinyl pyrrolidone were mixed, and the mixture was ball-milled at a speed of 400 r / min for 30 h; a green body with a thickness of 1260 μm was obtained by tape casting; the green body was immersed in deionized water for phase conversion for 26 h, and then taken out, and calcined at 1200° C. for 4 h to obtain a barium ceria support body, including a dense layer, a sponge layer, and a large-size open finger hole layer;

[0053] S2, spin coating barium zirconate on the surface of the dense layer of the barium ceria support at a spin coating rate of 500 rpm for 5 seconds, drying for 5 hours and calcining at 1450° C. for 36 hours to obtain a barium zirconate electrolyte stabilization layer;

[0054] S3, add 1.0g BaFe 0.7 Zr 0.2 Y 0.1 O 3-δ (BFZY) was mixed with a pine alcohol solution containing 6 wt % ethyl cellulose in a mass ratio of 3:1, and ball-milled at a speed of 100 r / min for 1 h to obtain an anode slurry, and the obtained anode slurry was coated on one side of the barium zirconate electrolyte stabilizing layer prepared above, and calcined at 1000 ° C for 2 h to obtain a BFZY anode layer;

[0055] S4. Under a vacuum degree of 0.1 MPa, the large-sized open finger-hole layer containing the cerium oxide support was impregnated with nickel nitrate and copper nitrate solutions with a concentration of 1.5 mol / L each for 50 times, and calcined at 450°C for 1 hour each time, and finally calcined at 900°C for 2 hours, with an impregnation amount of 45.9wt%, to obtain a transition metal impregnation layer; under a vacuum degree of 0.06 MPa, the large-sized open finger-hole layer was impregnated with a magnesium nitrate solution with a concentration of 0.5 mol / L for 8 times, and calcined at 450°C for 1 hour each time, and finally calcined at 900°C for 2 hours, with an impregnation amount of 3.8wt%, to obtain a transition metal-alkaline metal impregnation layer;

[0056] S5. Use a mixture of carbon dioxide (5.0 vol%) and nitrogen to treat the transition metal-alkaline metal impregnation layer at 700° C. for 0.2 h, and then use a mixture of hydrogen (10 vol%) and nitrogen to continue treating at 700° C. for 0.6 h to obtain an electrolytic cell.

[0057] A mixture of carbon dioxide (60 vol%), carbon monoxide (25 vol%) and nitrogen (15 vol%) was introduced into the fuel electrode side of the electrolytic cell at a flow rate of 120 mL / min, and nitrogen was introduced into the anode side at a flow rate of 90 mL / min. An electrolysis voltage of 1.5 V was applied at 850 °C, and the current density reached 0.58 A / cm 2 , and carried out 24h stability test, the current density remained basically unchanged.

[0058] Example 3

[0059] A method for preparing a composite structure proton type solid oxide electrolytic cell comprises the following steps:

[0060] S1, 127.4g barium ceria, 7.8g graphite, 52.2g 1-methyl-2-pyrrolidone, 10.6g polyethersulfone, 2.0g polyvinyl pyrrolidone are mixed, and ball milled at a speed of 360r / min for 32h; a green body with a thickness of 1400μm is obtained by tape casting; the green body is immersed in deionized water for phase conversion for 36h, then taken out, and calcined at 1250℃ for 3h to obtain a barium ceria support body, including a dense layer, a sponge layer and a large-size open finger hole layer;

[0061] S2, spin coating barium zirconate on the surface of the barium ceria dense film, the spin coating rate is set to 700 rpm, the time is 3 s, and after drying for 5 hours, calcining at 1400° C. for 30 hours to obtain a barium zirconate electrolyte stabilization layer;

[0062] S3, 0.8g BaCo 0.6 Zr 0.2 Y 0.2 O 3-δ (BCZY) was mixed with a pine alcohol solution containing 6 wt% ethyl cellulose in a mass ratio of 3:1, and ball-milled at 80 r / min for 0.5 h to obtain an anode slurry. The obtained anode slurry was coated on one side of the barium zirconate electrolyte stabilizing layer prepared above, and calcined at 1050 ° C for 2 h to obtain a BCZY anode layer;

[0063] S4, under a vacuum degree of 0.1 MPa, impregnating nickel nitrate and zinc nitrate solutions with a concentration of 2.0 mol / L for 40 times, and calcining at 400°C for 1 hour each time, and finally calcining at 900°C for 2 hours, the impregnation amount is 41.6wt%, and a transition metal impregnation layer is obtained; under a vacuum degree of 0.06 MPa, impregnating calcium nitrate solution with a concentration of 0.5 mol / L for 9 times, and calcining at 400°C for 1 hour each time, and finally calcining at 900°C for 2 hours, the impregnation amount is 4.9wt%, and a transition metal-alkaline metal impregnation layer is obtained;

[0064] S5. Use a mixture of carbon dioxide (1.0 vol%) and nitrogen to treat the transition metal-alkaline metal impregnation layer at 700° C. for 0.5 h, and then use a mixture of hydrogen (5 vol%) and nitrogen to continue treating at 650° C. for 0.6 h to obtain an electrolytic cell.

[0065] A mixture of carbon dioxide (65 vol%) and carbon monoxide (35 vol%) was introduced into the fuel electrode side of the electrolytic cell at a flow rate of 100 mL / min, and nitrogen was introduced into the anode side at a flow rate of 80 mL / min. The electrolysis voltage was 1.48 V at 800 °C, and the current density reached 0.29 A / cm 2 , and a 15h stability test was carried out, and the current density remained basically unchanged.

[0066] The proton type solid oxide electrolytic cell uses alkaline perovskite cathode material, which has the advantage of anti-carbon deposition and has great potential in high-temperature electrolysis of carbon dioxide. In order to optimize the problems of large gas diffusion resistance, insufficient three-phase interface, severe disproportionate carbon deposition caused by irregular pores in the traditional cathode support, and to improve the problems of difficult sintering and poor stability of the proton membrane, the present invention adopts a combination of tape casting-phase conversion-impregnation, spin-coating the barium zirconate electrolyte stabilization layer on the dense layer of the barium cerate support obtained by tape casting-phase conversion, vacuum impregnating the transition metal and alkaline metal salt solution in the large-size open finger holes, and undergoing acid-base-reduction reaction regulation treatment to obtain a composite structure proton type solid oxide electrolytic cell. When the obtained composite structure proton type solid oxide electrolytic cell is applied to high-temperature electrolysis of carbon dioxide, it can effectively improve the gas diffusion and electrocatalytic carbon dioxide reduction reaction activity, while enhancing the anti-carbon deposition and structural stability.

[0067] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.

Claims

1. A method for preparing a composite structure proton type solid oxide electrolytic cell, It is characterized in that The following steps are involved: S1. A barium ceria support is prepared based on a tape casting-phase conversion method, including a dense layer, a sponge layer and a large-size open finger hole layer; S2, preparing a barium zirconate electrolyte stabilizing layer on the dense layer of the barium ceria support to obtain a double-layer proton conductor electrolyte; S3, preparing an anode layer on a double-layer proton conductor electrolyte; S4, vacuum impregnating a transition metal ion solution and an alkaline metal ion solution into the large-size open finger hole layer of the barium ceria support to obtain a transition metal-alkaline metal impregnation layer; S5, performing acid-base-reduction treatment on the transition metal-alkaline metal impregnation layer to obtain a composite structure proton-type solid oxide electrolytic cell; In step S1, the step of preparing the barium ceria support body based on the tape casting-phase conversion method includes: S1-1, barium cerate, pore-forming agent, organic solvent, dispersant and binder are mixed and ground according to a certain proportion, the grinding speed is 350-420 r / min, and the grinding time is 24-60 h; S1-2 tape casting method was used to prepare green bodies with a thickness of 800~1500 µm; S1-3: placing the green body in deionized water for phase transformation for 20-50 h, calcining after phase transformation to obtain a barium ceria support body, the calcination temperature is 1000-1350 °C, and the calcination time is 2-6 h; In step S1-1, the pore-forming agent is graphite, the organic solvent is 1-methyl-2-pyrrolidone, the dispersant is polyvinylpyrrolidone, and the binder is polyethersulfone; The mass fractions of barium cerate, pore-forming agent, organic solvent, dispersant and binder are as follows: 63.7-65.1 parts of barium cerate; Pore-forming agent 5.6~3.5 parts; 24.8-28.1 parts of organic solvent; Dispersant 1.1~0.5 parts; 6.5~3.2 parts of binder; In step S4, the steps of vacuum impregnating the large-size open finger hole layer of the barium ceria support with a transition metal ion solution and an alkaline metal ion solution to obtain a transition metal-alkaline metal impregnation layer include: Under a vacuum degree of 0.1-0.05 MPa, the large-size open finger-hole layer of the barium cerate support is impregnated with a transition metal ion solution, and calcined at 400-500 °C for 0.5-1.0 h, and the impregnation and calcination are repeated until the impregnation amount is 30-55 wt%; and then calcined at 700-900 °C for 0.5-2 h to obtain a transition metal impregnation layer; Under a vacuum degree of 0.09-0.03 MPa, the large-size open finger-hole layer is continuously impregnated with an alkaline metal ion solution, and treated at 400-500 °C for 0.5-1.0 h, and the impregnation and calcination are repeated until the impregnation amount is 5.0-8.0 wt%, and then treated at 900-1150 °C for 2-5 h to obtain a transition metal-alkaline metal impregnation layer; The transition metal ion solution is one of nickel nitrate, copper nitrate and zinc nitrate solutions, and the concentration is 0.5-2.0 mol / L; The alkaline metal ion solution is one of sodium carbonate, potassium carbonate, strontium nitrate solution, calcium nitrate solution, and magnesium nitrate solution, and the concentration is 0.05-0.5 mol / L; In step S5, the step of performing acid-base reduction treatment on the transition metal-alkaline metal impregnation layer includes: A mixture of carbon dioxide and nitrogen is used for acid-base treatment, wherein the volume fraction of carbon dioxide is 0.5~6.5vol%, the treatment temperature is 500~700℃, and the treatment time is 0.1~1.0h. A mixture of hydrogen and nitrogen is used for reduction treatment, wherein the volume fraction of hydrogen is 5~20vol%, the treatment temperature is 500~700℃, and the treatment time is 0.1~1.0h.

2. The method for preparing the composite structure proton type solid oxide electrolytic cell according to claim 1, It is characterized in that In step S2, the step of preparing a barium zirconate electrolyte stabilizing layer on the dense layer of the barium ceria support body comprises: The barium zirconate electrolyte is spin-coated on the dense layer of the barium ceria support at a spin-coating rate of 500-1200 rpm for a spin-coating time of 3-15 s. After drying at room temperature for 4-10 h, the electrolyte is calcined at 1380-1450 °C for 15-36 h to obtain a double-layer proton conductor electrolyte.

3. The method for preparing the composite structure proton type solid oxide electrolytic cell according to claim 1, It is characterized in that In step S3, the step of preparing an anode layer on a double-layer proton conductor electrolyte comprises: The proton-oxygen ion-electron three-conductor anode and a pine alcohol solution containing 6 wt% ethyl cellulose are mixed and ground in a mass ratio of 3:1, the grinding speed is 50-150 r / min, the grinding time is 0.5-1.5 h, and the mixture is coated on the surface of the barium zirconate electrolyte stabilization layer obtained in step S2, and calcined at a calcination temperature of 900-1150 ° C for 2-5 h.

4. The method for preparing the composite structure proton type solid oxide electrolytic cell according to claim 3, It is characterized in that The proton-oxygen ion-electron triple conductor anode is BaCo 0.7 Fe 0.2 Zr 0.1 O 3-δ ,BaFe 0.7 Zr 0.2 Y 0.1 O 3-δ 、BaCo 0.6 Zr 0.2 Y 0.2 O 3-δ One of them.

5. A composite structure proton type solid oxide electrolytic cell prepared by the method according to any one of claims 1 to 4.