A coupling agent water glass polyurethane environmentally friendly adhesive composition and preparation method thereof
By adding a silane coupling agent, especially γ-aminopropyltriethoxysilane, to the water glass glue and optimizing the ratio, the problems of low bonding strength and poor water resistance between water glass glue between metals were solved, and the problem was achieved. It has low viscosity, high strength, and environmentally friendly glue, which is suitable for the production of bonding and composite materials in building materials and industrial and mining enterprises.
Patent Information
- Application Number
- CN202210664845.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2016-01-17
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2036-01-17
AI Technical Summary
The existing water glass adhesive has low bonding strength between metals and metals and metals and non-metals, and has poor water resistance and weather resistance. Traditional foam adhesives have environmental and safety hazards and are difficult to meet the high strength requirements of building materials and industrial and mining enterprises. and low viscosity requirements.
Use a two-component glue solution composed of sodium water glass or potassium water glass and polyisocyanate and its prepolymer, and add a silane coupling agent, especially γ-aminopropyltriethoxysilane, to the solution by optimizing the ratio. Combined with additives, it improves bonding strength and weather resistance while reducing viscosity.
It has achieved a low-viscosity, high-strength, environmentally friendly glue with good bonding performance, waterproofness and anti-corrosion properties. It is suitable for the bonding and composite material production of building materials and industrial and mining enterprises, and can be effectively cured under low temperature conditions.
Abstract
Description
Technical Field
[0001] This application is a divisional application of application number 2016100271055, a low-viscosity, high-strength, environmentally friendly two-component adhesive and its preparation method. The present invention relates to a composition that can be used for bonding between objects in building materials, industrial and mining enterprises and daily life, matrix reinforcement, composite material production and object surface protection, especially the use of a coupling agent in a cheap two-component composition containing water glass, isocyanate and its prepolymer. Background Art
[0002] Water glass is a cheap and environmentally friendly inorganic adhesive, but its bonding strength and water resistance are difficult to achieve satisfactory levels when used as an adhesive or as an adhesive for dipping and laminating composite materials. Although the curing time can be shortened and the strength can be increased by adding sodium fluorosilicate and / or metal oxides, it is difficult to be used in metal-to-metal, metal-to-nonmetal, and nonmetal-to-nonmetal applications due to its inherent brittleness. The coatings formulated with it often experience halogen blooming and peeling due to the migration of small molecules and the alkali aggregate effect on silicon-containing substrates. Adding silane coupling agents to water glass seems to improve its bonding properties. Due to the alkalinity and water-based characteristics of water glass, there are subtle relationships and complex reactions between the compositions. In addition, the content of nano-sized monosilicon and oligosilicon in the water glass component itself will gradually decrease during storage, especially after mixing at higher temperatures, it is easy to form complex polymers, and its bonding strength is often disappointing.
[0003] The adhesives currently used for bonding building materials, decorative materials, door cores and panels are mostly polyurethane foam glue, and the manufacturer requires that its positive tensile bonding strength is not less than 0.5MPa. It is mainly a polyurethane prepolymer containing residual terminal NCO groups formed by the reaction of polyester polyols or polyether polyols with polyisocyanates, and usually an appropriate amount of catalyst and about 50% of dichloromethane are added as a diluent. The NCO content of domestic foam glue is generally about 3%-6%, with good toughness, high bonding strength and easy use. However, the price of foam glue is relatively high, the colloid is flammable, and the combustion produces thick black smoke and releases toxic gases. The use of the rubber will release a large amount of dichloromethane with potential carcinogenicity, which is harmful to health. Dichloromethane will produce hydrogen chloride under hot and humid conditions, which has potential corrosion risks. Although many research institutions and enterprises have tried to replace foam glue with lower-cost inorganic glue or water-based glue, the technical problems of weak initial adhesion, low bonding strength, long surface drying time, brittle glue layer, poor water and weather resistance, and water and moisture absorption have not been solved in the bonding between metal and metal, metal and wood and other rigid non-metal. Water-based glue is also prone to metal corrosion due to its high water content and slow curing.
[0004] European patent EP03010871.9 and Chinese patent CN1788064A disclose the invention application of "polyisocyanate ingredients for sandwich panels" of Huntsman International Ltd., which prepares an adhesive suitable for A2-grade flame-retardant Euro-grade sandwich panels by reacting an alkali metal silicate solution with polyisocyanate, has a combustion heat of no more than 25MJ / kg, is flame-retardant and environmentally friendly, but has poor bonding strength and stability between wood and steel; Chinese patent CN103627330A discloses the invention application "a composite adhesive", which improves the bonding strength and weather resistance of the adhesive by adding an organic synergist and / or additives to water glass and then mixing it with polyisocyanate and its polyester and / or polyether polyol prepolymer, but has a high viscosity, especially in low-temperature areas and low-temperature seasons, and is not suitable for occasions requiring lower viscosity.
[0005] Theoretically, reducing the amount of inorganic filler added and adding coupling agents may also achieve greater bonding strength without too high a viscosity. Coupling agents can improve the interfacial properties between fillers and polymer materials. In their molecular structure, there is a functional group that can react chemically with the polymer matrix or at least have good compatibility and another functional group that can form a chemical bond with the inorganic filler. Since inorganic fillers and polymer molecules are very different in chemical structure and physical form and lack affinity, coupling agents can improve the interfacial properties between polymer materials and fillers and improve the adhesion of the interface. Among the many types of coupling agents, silane coupling agents are one of the earliest studied and widely used varieties. The general formula of silane coupling agents can be written as RSiX3, where R is an active functional group that has affinity and reactivity with polymer molecules, such as vinyl chloropropyl, epoxy, methacryl, amine and thiol; X is an alkoxy group that can be hydrolyzed, such as methoxy and ethoxy. The main methods of using silane coupling agents are surface pretreatment and direct addition. The former is to treat the filler surface with a diluted coupling agent, and the latter is to add the original solution of the coupling agent when the resin and filler are premixed. The silane coupling agent can be directly added to the adhesive component, and the general amount added is 1-5% of the base resin. After the glue is applied, the coupling agent molecules migrate to the bonding interface to produce a coupling effect by relying on the diffusion of molecules. For adhesives that need to be cured, they need to be placed for a period of time after the glue is applied before curing, so that the coupling agent can complete the migration process and obtain better results. The silane coupling agent is formulated into a solution, which is conducive to the dispersion of the silane coupling agent on the surface of the material. The solvent is a solution prepared from water and alcohol. The solution is generally 20% silane, 72% alcohol, and 8% water. The hydrolysis rate of silane is related to the pH value. The neutral is the slowest, and the acidic and alkaline are faster. Because silane cannot be stored for a long time after hydrolysis, it should be prepared and used immediately, and it is best to use it up within one hour. Since alkaline aqueous solution will accelerate the decomposition of coupling agent and promote the formation of polymers, thus causing the coupling agent to lose its effectiveness. However, the inventors have tried the most promising surfactants such as γ-(2,3-epoxypropoxy)propyltrimethoxysilane and γ-mercaptopropyltriethoxysilane, but failed to achieve the expected effect and were even very disappointed. As a two-component adhesive, water glass is a strong alkaline aqueous solution. Simple experiments can easily prove that adding a lot of silane coupling agent to water glass will result in very disappointing experimental results due to the particularity of water glass and the complexity of the two components. Although adding some silane coupling agent to component B has a certain enhancement effect, improper addition is prone to lose effectiveness.
[0006] To solve the above problems, the inventors conducted active exploration and a large number of experiments under difficult circumstances, and the results were encouraging and unexpected. Summary of the invention
[0007] The purpose of the present invention is to provide an environmentally friendly flame retardant, low-viscosity, low-cost, high-strength, stable, water-resistant and weather-resistant adhesive, which is achieved by the following technical solutions:
[0008] A coupling agent water glass polyurethane environmentally friendly adhesive composition and a preparation method thereof, comprising sodium water glass and / or potassium water glass components and polyisocyanate and prepolymer components thereof, characterized in that the water glass component at least further comprises a silane coupling agent suitable for matching with the water glass, or a silane coupling agent and liquid polyol ester and / or alcohol ether; the polyurethane component comprises polyisocyanate and a terminal NCO prepolymer of polyester polyol and / or polyether polyol thereof, the mixture contains 10-28% NCO, and the relative proportion thereof increases with the increase of the water glass modulus, wherein the mass proportion of the water glass component with a modulus of 1.5-2.9 and the polyurethane component with a polyisocyanate and its derivatives is 1:0.7-2.3, and the mass proportion of the water glass component with a modulus of 3.0-3.6 and the polyurethane component is 1:1.3-2.5.
[0009] The silane coupling agent is a silane coupling agent containing amino, epoxy, hydroxyl and / or mercapto groups.
[0010] The viscosity of the liquid polyol ester and / or alcohol ether at 20° C. is lower than 500 mPa.s.
[0011] The silane coupling agent contains at least γ-aminopropyltriethoxysilane.
[0012] The silane coupling agent is preferably γ-aminopropyltriethoxysilane.
[0013] The amount of the silane coupling agent added is 0.3-2.0% of the mass of the water glass.
[0014] The preferred addition amount of the silane coupling agent is 0.5-1.8% of the mass of water glass.
[0015] The preferred addition amount of the silane coupling agent is 0.6-1.2% of the mass of water glass.
[0016] The polyol ester and / or alcohol ether is one or a combination of dodecanol ester (2,2,4-trimethyl-1,3-pentanediol monoisobutyrate), hexadecanol ester (2,2,4-trimethyl-1,3-pentanediol diisobutyrate), ethylene glycol monobutyl ether, triethylene glycol monobutyl ether, triethylene glycol monoethyl ether, tripropylene glycol monobutyl ether, and glycerol triacetate.
[0017] The polyol ester may also be castor oil, epoxidized soybean oil, and the like.
[0018] The amount of polyol ester and / or alcohol ether added is 0.3-10% of the mass of water glass.
[0019] The polyol ester and / or alcohol ether is preferably added in an amount of 0.6-8% of the mass of the water glass.
[0020] The polyol ester and / or alcohol ether is further preferably added in an amount of 1 to 5% of the mass of the water glass.
[0021] The alcohol ester and / or alcohol ether is dodecyl alcohol ester, triethylene glycol monobutyl ether, or a combination thereof with propylene glycol or ethylene glycol butyl ether, and the added amount is 1-5% of the mass of the water glass.
[0022] The modulus of the sodium water glass or potassium water glass is 2.2-2.9. The mass ratio of the water glass component to the polyurethane component is 1:0.7-1.5, preferably 1:1-1.3.
[0023] The modulus of the sodium water glass or potassium water glass is 3.1-3.4. The mass ratio of the water glass component to the polyurethane component is 1: 1.2-2.5, preferably 1: 1.3-2.
[0024] The water glass component is further added with 0.5-5% of the mass of water glass emulsifier and / or 0.5-10% of pigment filler and / or other conventional additives. The additives may also be emulsifier, phosphate ester, styrene, polyol or viscosity reducer, catalyst.
[0025] The emulsifier may be OP-10 and / or silicone oil such as dimethyl silicone oil, preferably dihydroxy silicone oil, ethylene glycol, propylene glycol, etc., which can be soluble in water glass and polyol ester or alcohol ether at the same time.
[0026] The NCO content of the polyurethane component is preferably 12-18%.
[0027] The polyurethane component contains 5% to 50% of the total weight of the polyurethane component.
[0028] The solvent in the polyurethane component is dimethyl carbonate and / or acetone.
[0029] The polyisocyanate is diphenylmethane diisocyanate (MDI) and polymethylene polyphenyl polyisocyanate (PAPI) or a combination of diphenylmethane diisocyanate and one or more of hexamethylene diisocyanate and xylene diisocyanate and polymethylene polyphenyl polyisocyanate (PAPI), and the ratio of the two is 1:0.5-2. The polyester polyol is Sovermol 750 and ethylene terephthalate. The polyether polyol has an average functionality of 2-5, a molecular weight of 400-2000, a hydroxyl value of 35-500 mgkOH / g, and is one or more of polyether polyol 220N or 330N, trimethylolpropane-propylene oxide polyether triol, pentaerythritol polyether, and polypropylene oxide polyether triol.
[0030] The polyurethane prepolymer referred to in the present invention also includes a method of directly mixing the polyester polyol, polyether polyol, polyisocyanate and diluent, that is, the polyester and / or polyether polyol can be added with a diluent and then mixed with the polyisocyanate, or the polyisocyanate can be diluted and then mixed with the polyester and / or polyether polyol. Although this method has a slight effect on the bonding strength of the rubber, it is more convenient to operate and has a lower cost, and can also solve the technical problem of the present invention.
[0031] The method for preparing the water glass polyurethane environmentally friendly two-component glue is characterized in that, at room temperature or controlled at a temperature below 48°C, 0.3-2% of the silane coupling agent of the total mass of the water glass is first added to part of the water glass, and stirred rapidly, and the remaining part of the water glass is added during stirring, stirred for 10-30 minutes, and then 0.3-10% of polyol ester and / or alcohol ether or a mixture of polyol ester and / or alcohol ether and a co-solvent or emulsifier is added, and a small amount of other additives are added if necessary. The co-solvent refers to a solvent that is soluble in both polyol ester and / or alcohol ether and water glass.
[0032] The polyurethane component can also be prepared by the following method: first react PAPI with polyester polyol and / or polyether polyol to prepare a prepolymer and then add polymeric MDI, then adjust the viscosity with 0-1 / 3, especially 0-2 / 15, of the total mass of the component using a viscosity reducer and / or solvent, or finally add 0.3-2% of the total mass of the silane coupling agent or silane coupling agent and polyol ester and / or alcohol ether.
[0033] The above method of adding the silane coupling agent or the silane coupling agent and the polyol ester and / or alcohol ether to the water glass or polyurethane component is to prepare at 95~20°C, preferably 50~25°C, more preferably 35~25°C, or to add 0.3~8 times the weight of water, preferably 0.5~3 times the weight of water, more preferably 1~2 times the weight of water, of the silane coupling agent at 15°C above the freezing point for preparation. Stir while adding dropwise to prevent agglomeration. After stirring evenly, put into a barrel and cover in time to prevent evaporation and film formation. Mixing at an appropriate temperature can obtain a more stable glue solution.
[0034] Of course, other temperatures that do not cause decomposition of the active ingredients, such as temperatures greater than 95°C, 100°C or even higher, can also achieve better results.
[0035] The water glass polyurethane environmentally friendly two-component adhesive is used for door core or building material processing or geological defect treatment or glass fiber reinforced plastic production.
[0036] The alkali metal water glass can be liquid sodium water glass, potassium water glass, or it can be said to be fast-soluble solid water glass. The solid water glass is added with water lost during the drying process to turn the solid water glass back into liquid water glass. Considering the cost problem, sodium water glass is preferred, and sodium water glass can also be used as the main material with some potassium water glass mixed in. The modulus of water glass is too high, the activity is small, the cross-linking progress is slow, the reaction is insufficient, and the mechanical strength and bonding strength of the cement are not good, especially under low temperature conditions. It is preferably 2.0~2.9, especially 2.0~2.5. Of course, high modulus water glass can also be used alone or in combination with high modulus water glass after adding alkali solution, alkaline stabilizer or active modifier. Increasing the proportion of the polyurethane component is conducive to improving the comprehensive performance of the high modulus water glass-polyurethane system. For the 1.6~2.6 low modulus water glass-polyurethane system, the weight ratio of A to B is 1:0.8~1.2; for the 2.6~3.6 high modulus water glass-polyurethane system, the ratio of A to B is 1:1.5~2.5.
[0037] The experiment surprisingly found that coupling agents, especially silane coupling agents such as γ-aminopropyl triethoxysilane and its addition amount have a subtle relationship with the modulus of water glass and the components and relative amounts of polyurethane prepolymers. Low modulus water glass has relatively large adaptability to coupling agents and polyurethane components, while high modulus water glass only works when there are polyisocyanates and prepolymers of certain types and qualities and the relative amounts are large. The experiment also surprisingly found that polyol esters such as dodecyl alcohol esters and hexadecanol esters have significant synergistic effects with coupling agents such as γ-aminopropyl triethoxysilane, and the addition amount and addition method also significantly affect the bonding effect. Adding the coupling agent first is conducive to its uniform dispersion and action in the water glass, which is conducive to reducing the antagonistic effects caused by chemical consumption, destruction and physical aggregation, and isolation. Of course, adding an appropriate amount of dodecyl alcohol ester and hydroxy alcohol esters of similar structures first, and then adding the coupling agent after sufficient emulsification can also reduce the antagonistic effect, especially when processed at a lower temperature. The addition of a proper amount of dodecyl alcohol ester and hydroxy alcohol esters of similar structures can significantly improve the bonding strength, optimize the physical and chemical properties of the adhesive, reduce the viscosity of the rubber, and enhance the waterproof and weather-resistant effect of the adhesive. Adding too much not only increases the cost, but sometimes reduces the bonding strength. The experiment found that alcohol ethers such as ethylene glycol monobutyl ether, triethylene glycol monobutyl ether, triethylene glycol monoethyl ether, and tripropylene glycol monobutyl ether also have similar synergistic effects with the silane coupling agent.
[0038] The coupling agent can also be other silanes, titanates, aluminate compounds, organic chromium complexes containing functional groups that can be bonded to the composite water glass-polyurethane, such as other silane coupling agents containing amino, mercapto, epoxy groups or titanate monoalkoxy type, monoalkoxy pyrophosphate type, chelate type and other coupling agents. If added in a constant amount, its content is too low to improve the bonding performance, and the bonding strength is not significantly increased. In the test, one end of the steel is often a large piece or completely white with little adhesive. Adding too much is costly and the effect is not significantly increased. The hydroxy alcohol ester can also be triethylene glycol bis (2-hexyl acetate), 2,4-trimethyl- 1,3-pentanediol diisobutyrate, triethylene glycol dicaprylate, triethylene glycol diisooctanoate ethylene glycol monobutyl ether stearate, diethylene glycol diricinoleate, glycerol triacetate (triester), oleic acid diethanolamide and its boric acid, ethylene glycol butyl ether acetate (BGA), the dodecanol ester is 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, including various derivatives thereof, such as low-viscosity derivatives containing halogen, carboxyl, phenyl, vinyl, propenyl, and phosphate groups.
[0039] The polyisocyanate in the polyurethane component can be diphenylmethane diisocyanate (MDI), modified MDI, polymeric MDI (black material), polymethylene polyisocyanate (PAPI) and can also be isofluorinated dione diisocyanate (IPDI), toluene diisocyanate (TDI), hexamethylene diisocyanate trimer (HDT), cyclopentane diisocyanate, dicyclohexylmethane diisocyanate, diphenyl diisocyanate, phenyl diisocyanate, and one or more combinations of the derivatives of the isocyanate; the polyester / polyether polyol for preparing the polyurethane prepolymer or foaming glue can be ethylene terephthalate including ethylene terephthalate prepared by alcoholysis of recycled old bottle materials, Sovermol750, 220N, 330N and combinations thereof, and can also be added with polyoxypropylene glycol, polymer polyol (POP), polyurea polyol (PHD), polymer polyol (PIPA) , high molecular weight low saturation polymer polyols and other conventional polyester / polyether polyols; a small amount of surfactants can be added to the water glass component, such as sodium dodecylbenzene sulfonate, cocamidopropyl betaine, OP-10, Tween or TX-10, hydroxy silicone oil, etc., preferably an active emulsifier that can cross-link with the polyurethane component, such as polyhydroxy silicone oil, propylene glycol, etc., which can be one or more combinations, and a small amount of sodium tripolyphosphate and / or sodium pyrophosphate can be added if necessary. When the temperature is low, such as below 15°C, water can be added to a silane coupling agent such as γ-aminopropyl triethoxysilane and stirred evenly, and then added to the water glass under stirring, and then other components can be added after uniformity, which can promote the coupling agent such as γ-aminopropyl triethoxysilane to be evenly dispersed in the water glass component, and can prevent the surface conjunctiva from affecting the mixing and use. Unexpectedly, in water glass or water glass and aqueous solution in an alkaline environment, coupling agents such as γ-aminopropyl triethoxysilane have good stability due to interaction. However, adding coupling agents such as γ-aminopropyltriethoxysilane to the polyurethane component is not very stable and affects the shelf life due to the reaction.
[0040] The low-viscosity adhesive of the present invention can be used for bonding the core and door body of anti-theft doors and fireproof doors, producing furniture and panels, bonding ceramic tiles, stones, thermal insulation materials and other building decoration materials, filling seams, plugging leaks and reinforcing walls, stone sculptures, mines, construction sites, dangerous rocks, etc., bonding and fixing equipment and workpieces, bonding fire-fighting equipment and facilities, and can also be used for the production of glass fiber reinforced plastics, especially flame-retardant glass fiber reinforced plastics products or other composite materials and anti-corrosion flame-retardant coatings.
[0041] The positive effects of the present invention are:
[0042] Since the coupling agents such as γ-aminopropyltriethoxysilane and hydroxyl alcohol esters and / or dodecyl alcohol esters and / or alcohol ethers have relatively low viscosity and a small proportion, the proportion of water glass is large, the adhesive has low viscosity, good wettability and permeability, and is suitable for mechanical spraying and environmentally friendly fiberglass and other composite material production and grouting operations, and is flame retardant and rust-proof; since the adhesive can be produced and used at room temperature or at a relatively low temperature, and can be cured at room temperature, it is low-carbon and environmentally friendly; due to the interaction and wonderful effects of coupling agents such as γ-aminopropyltriethoxysilane and hydroxyl alcohol esters and / or alcohol ethers such as dodecyl alcohol esters, the bonding strength can be significantly improved, the adhesion, waterproof and weather resistance and / or stability of the adhesive can be improved, and the early strength is high, and the surface of the adhesive is smooth, so that the adhesive obtains higher bonding strength, mechanical strength, and acid, alkali and water resistance. A small amount of water-insoluble hydroxy alcohol esters and / or alcohol ethers distributed on the surface of component A can also prevent the reaction between carbon dioxide in the air and water glass, thereby extending the service life; there are few types of raw materials, low production costs, and simple processes, which are very suitable for production in low-temperature areas or low-temperature seasons. Implementation
[0043] Among the raw materials used in the embodiments of the present invention, 2.2~2.5 mold (density 1.526~1.599 g / cm3 at 20°C), 2.6~2.9 mold (density 1.436~1.465 g / cm3 at 20°C), and 3.1~3.4 mold (density 1.368~1.394 g / cm3 at 20°C) series water glass are provided by Chongqing Yongsheng Water Glass Factory; 3-aminopropyltrimethoxysilane (kh540), γ-aminopropyltriethoxysilane (kh550), 3-(2,3-epoxypropoxy)propyltrimethoxysilane (kh560), and N-2-(aminoethyl)-3-aminopropyltrimethoxysilane (kh792) are produced by Nanjing Liansi Chemical Co., Ltd.; 2,2,4-trimethyl- 1,3-pentanediol monoisobutyrate (dodecyl ester) is produced by Jiangsu Ruitai Chemical Co., Ltd.; polyurethane prepolymer and foaming glue are produced by Chongqing Banan Jucai Adhesive Factory, using polymethylene polyphenyl polyisocyanate (PAPI), polyether polyol (220N, 330N) and polyester polyol (ethylene terephthalate made by alcoholysis of recycled bottle materials in the conventional method, polyether / polyester polyol Sovermol 750) as raw materials, wherein the molecular weight of polyether polyol is 3000~6000, and the molecular weight of polyester polyol is 1000~3000, and the weight ratio of the two is 1~2:1, and the content of -NCO groups in the prepolymer is about 8%~13%. Foaming glue is the product of prepolymer diluted with dichloromethane, dichloromethane accounts for about 30~50%, and amine or tin catalyst is added 0~0.1%. Isocyanate is polymerized MDI (NCO28~32%) produced by Wanhua. Other chemical raw materials were purchased from Chongqing Shipingqiao Chemical Market. The screws used in the test were round-headed, 12mm in diameter, 87mm in length, and polished on the end faces of the nail heads. They were bonded to the smooth-surfaced fir strips coated with the present invention. After gluing, the surface was dried for 20 to 60 minutes at a natural temperature of 8 to 15°C. The test was conducted after 48 to 72 hours. During the test, a weight was hung vertically downward from the screw rod, increasing by 1kg each time until the screw fell off. The hanging weight was recorded. If the weight did not fall off within 30 seconds, the weight was increased again. Each treatment was repeated 3 to 5 times, and abnormal samples were eliminated to take the average value. The average weight of the upper and lower limits of the bonding strength is calculated for reference only.
[0044] Unless otherwise specified, the average weight fractions in the following comparative examples and embodiments are obtained by mixing 1 weight part of water glass component with 1 weight part of polyurethane component, wherein the polyurethane component is prepared by mixing 1 weight part of polymerized MDI (black material) with 2 weight parts of foaming glue, or 1 weight part of polyurethane prepolymer, and 0.6 weight part of 1,1-dichloroethane or ethyl acetate diluent.
[0045] Adhesive preparation:
[0046] Water glass components:
[0047] 100% sodium water glass or a mixture of sodium water glass and potassium water glass. If necessary, the required modulus can be adjusted by blending water glasses of different moduli or adding alkali solution or silica gel.
[0048] Inject a certain modulus of water glass into a stirrable container, add a certain amount of silane coupling agent, such as γ-aminopropyltriethoxysilane, during stirring, stir for a while, and seal the package directly after it is evenly mixed, or seal the package after adding additives, or proceed to the next step.
[0049] Add hydroxy alcohol ester and / or alcohol ether such as lauryl alcohol ester to the above mixture during stirring, add emulsifier and / or dispersant if necessary, or mix hydroxy alcohol ester and / or alcohol ether such as lauryl alcohol ester with emulsifier or active solvent that can be miscible in water glass and hydroxy alcohol ester and / or alcohol ether and then add, add certain color filler if necessary, stir evenly and then directly seal and package or seal and package after homogenization and filtration.
[0050] Polyurethane components:
[0051] After the excess polyisocyanate reacts with the polyester polyol and / or the polyether polyol to the end point, the temperature is lowered to below 40°C, and a diluent is added under stirring to make the NCO content account for 10-28% of the total mass of the polyurethane component, preferably 12-20%; or 1 part of a polyurethane prepolymer formed by the reaction of polyester / polyether polyol terephthalate, 330N and / or 750 with PAPI and / or MDI containing 8-12% NCO, and a diluent such as 1, 1-dichloroethane, dichloromethane, propylene carbonate, dimethyl carbonate and / or acetone are mixed with 0.6 parts, and then 1 part of polymerized MDI or black material is added, or the foaming glue containing 50-70% of the prepolymer is directly mixed with MDI or PAPI and other black materials at a ratio of 1:0.5-1; or a certain amount of the silane coupling agent is added to the above-mentioned various polyurethane components under stirring, and stirred until uniform, or the hydroxy alcohol ester and / or alcohol ether are added under stirring, and continued to stir until uniform. The polyurethane component with the silane coupling agent or the silane coupling agent and the hydroxy alcohol ester and / or alcohol ether can also be combined with 100% water glass.
[0052] The preparation method of the adhesive in the embodiment of the present invention is as follows:
[0053] Preparation of water glass components:
[0054] The 100% water glass component is used only in combination with the polyurethane component 004B to which the silane coupling agent or the silane coupling agent and alcohol ester / alcohol ether are added.
[0055] Add γ-aminopropyltriethoxysilane to a container containing a certain amount of water glass and stir until uniform. This can be used as a separate component.
[0056] 2. Add the dodecanol ester pre-mixed with ethylene glycol butyl ether to the water glass component with γ-aminopropyltriethoxysilane added thereto, and stir until uniform;
[0057] 3. The preparation temperature is preferably below 100°C, preferably below 50°C, more preferably 25-35°C or room temperature. At 5-15°C, add an appropriate amount of water to γ-aminopropyltriethoxysilane and stir evenly before adding it to water glass during stirring. After stirring evenly, add hydroxy alcohol esters and / or alcohol ethers such as dodecyl alcohol ester at the boiling point of the added components, stir evenly, grind until homogenized if necessary, and finally sieve or directly put the material into barrels and seal;
[0058] Preparation of polyisocyanate prepolymer components:
[0059] 001B Polyether polyol 330N 20 kg Polyethylene terephthalate made from recycled bottle materials 15 kg 7500.7kg Polymethylene polyphenyl polyisocyanate PAPI 18.5 kg Stir at room temperature for 20-60 minutes, finally add 55 kgMDI and stir evenly, adjust the viscosity with 1 / 5 of the total mass of 1,1 dichloroethane diluent, filter and package in barrels.
[0060] Simply mix the special foaming glue containing 62.5% prepolymer with the black material at a ratio of 1:0.625.
[0061] Add 58 kg of polymeric MDI into a container with a stirrer, dilute with 35 kg of acetone, and add 22 kg of polyether polyol 220N, 15 kg of polyethylene terephthalate made from recycled bottle materials, 0.5 kg of polyether / polyester polyol Sovermol 750, and 20.5 kg of polymethylene polyphenyl polyisocyanate PAPI during stirring. Stir at room temperature for 20 to 60 minutes and package in barrels.
[0062] 20 kg of polyether polyol 330N, 15 kg of polyethylene terephthalate made from recycled bottle materials, 0.7 kg of 750, 18.5 kg of polymethylene polyphenyl polyisocyanate PAPI. Stir at room temperature for 20 to 60 minutes, finally add 55 kg of MDI and stir evenly, dilute with 1 / 5 of the total mass of acetone and stir evenly, then add 1.8 kg of γ-aminopropyltriethoxysilane, stirring while adding, and pack in barrels after stirring evenly.
[0063] Comparative Example 1
[0064] 2.2~2.5 modulus sodium water glass 50 001B polyisocyanate prepolymer component 50
[0065] Bond strength (Mpa) 0.51 Steel adhesion condition Nail head
[0066] Comparative Example 2
[0067] 2.6~2.9 modulus sodium water glass 50 001B polyisocyanate prepolymer component 50
[0068] Bond strength (Mpa) 0.48 Steel adhesion condition Nail head
[0069] 2.6~2.9 modulus potassium water glass 50 001B polyisocyanate prepolymer component 80
[0070] Bond strength (Mpa) 0.72 Steel adhesion condition Nail head
[0071] Comparative Example 3
[0072] 3.1~3.4 modulus sodium water glass 50 001B polyisocyanate prepolymer component 50
[0073] Bond strength (Mpa) 0.36 Steel adhesion condition Nail head
[0074] 3.1~3.4 modulus sodium water glass 50 001B polyisocyanate prepolymer component 100
[0075] Bond strength (Mpa) 0.65 Steel adhesion condition Nail head
[0076] Comparative Example 4
[0077] 3.1~3.4 modulus sodium water glass 50 γ-aminopropyl trimethoxysilane 1; 001B polyisocyanate prepolymer component 50
[0078] Bond strength (Mpa) 0.51 Steel adhesion condition Nail head
[0079] Comparative Example 5
[0080] 2.6~2.9 modulus sodium water glass 50 γ-mercaptopropyltriethoxysilane 2; 001B polyisocyanate prepolymer component 50
[0081] Bond strength (Mpa) 0.49 Steel adhesion condition Nail head
[0082] Comparative Example 6
[0083] 2.2~2.5 modulus sodium water glass 50 N-2-(aminoethyl)-3-aminopropyltrimethoxysilane 1.5; 001B polyisocyanate prepolymer component 50
[0084] Bond strength (Mpa) 0.52 Steel adhesion condition Nail head Example
[0085] 1.5~1.9 sodium water glass 100 γ-aminopropyl triethoxysilane 0.8 organic tin catalyst 0.2 dodecanol ester 4.5 take 50g 001B polyisocyanate prepolymer component take 50g
[0086] Bond strength (Mpa) 1.48 There is 1 / 3~1 / 5 veneer on the nail head Example
[0087] 2.2~2.5 modulus sodium water glass 100 γ-aminopropyl triethoxysilane 0.5 organic tin catalyst 0.3 take 50g 001B polyisocyanate prepolymer component take 50g
[0088] Bond strength (Mpa) 1.25 There is 1 / 3~1 / 5 veneer on the nail head Example
[0089] 2.2~2.5 water glass 100 γ-aminopropyl triethoxysilane 1.0 organic tin catalyst 0.3 take 50 grams 003B polyisocyanate prepolymer component take 55 grams
[0090] Bond strength (Mpa) 1.61 1 / 2 veneer attached to nail head Example
[0091] 2.2~2.5 sodium water glass 100 γ-aminopropyl triethoxysilane 1.0 organic tin catalyst 0.3 dodecanol ester 5.5 OP-10 1.5 Take 50 grams 001B polyisocyanate prepolymer component Take 50 grams
[0092] Bond strength (Mpa) 2.48 Full nail head veneer Example
[0093] 2.2~2.5 modulus potassium water glass 100. γ-aminopropyl triethoxysilane 0.5 glycerol triacetate 3.0 take 50 grams 001B polyisocyanate prepolymer component take 48 grams
[0094] Bond strength (Mpa) 1.47 1 / 3~1 / 2 veneer attached to the nail head Example
[0095] 2.2~2.5 modulus sodium water glass 80, 2.2~2.5 modulus potassium water glass 20 γ-aminopropyl triethoxysilane 1.0 dodecanol ester 5.5 take 50 grams 001B polyisocyanate prepolymer component take 50 grams
[0096] Bond strength (Mpa) 2.66 Full nail head veneer Example
[0097] 3.1~3.4 modulus sodium water glass 100 γ-aminopropyl triethoxysilane 1.5 γ-aminopropyl trimethoxysilane 0.5 water 1.5 dodecanol ester 0.8 002B polyisocyanate prepolymer component 149 grams
[0098] Bond strength (Mpa) 1.30 Nail head full of veneer Example
[0099] 2.2~2.5 modulus sodium water glass 50, 2.2~2.5 modulus potassium water glass 50 γ-aminopropyl triethoxysilane 1.5 dodecanol ester 2.0 triethylene glycol monobutyl ether 1 take 50g 001B polyisocyanate prepolymer component take 60g
[0100] Bond strength (Mpa) 2.55 Almost full nail head veneer Example
[0101] 2.2~2.5 modulus sodium water glass 100 γ-aminopropyl triethoxysilane 1.5 dodecanol ester 8.0 take 50g 001B polyisocyanate prepolymer component take 45g
[0102] Bond strength (Mpa) 2.35 Full nail head veneer Example
[0103] 2.2~2.5 modulus sodium water glass 100 γ-aminopropyl triethoxysilane 0.3 dodecanol ester 0.5 take 50g 001B polyisocyanate prepolymer component take 50g
[0104] Bond strength (Mpa) 1.15 There is 1 / 3~1 / 5 veneer on the nail head Example
[0105] 2.2~2.5 modulus sodium water glass 100 γ-aminopropyl triethoxysilane 0.5 dodecanol ester 1.0 take 50g 004B polyisocyanate prepolymer component take 60g
[0106] Bond strength (Mpa) 1.85 There is veneer on the nail head Example
[0107] Take 50g of 2.6~2.9 model sodium water glass and 70g of 004B polyisocyanate prepolymer component
[0108] Bond strength (Mpa) 1.55 There is veneer on the nail head Example
[0109] 2.6~2.9 sodium silicate 100 γ-aminopropyl triethoxysilane 0.3 phthalate 0.3 dodecanol ester 3.5 tripropylene glycol monobutyl ether 2 take 50g 003B polyisocyanate prepolymer component take 75g
[0110] Bond strength (Mpa) 1.35 There is 1 / 3~1 / 5 veneer on the nail head Example
[0111] 2.6~2.9 sodium water glass 100 γ-aminopropyl triethoxysilane 1.0 dodecanol ester 5.5 take 50g 001B polyisocyanate prepolymer component take 90g
[0112] Bond strength (Mpa) 2.12 Almost full nail head veneer Example
[0113] 2.6~2.9 modulus potassium water glass 100 γ-aminopropyl triethoxysilane 1.5 γ-mercaptopropyl triethoxysilane 0.3 water 3.0 dodecanol ester 1.8 002B polyisocyanate prepolymer component 140 grams
[0114] Bond strength (Mpa) 1.45 Nail head full of veneer Example
[0115] 3.1~3.4 sodium water glass 100 γ-aminopropyl triethoxysilane 1.5 dodecanol ester 8.0 Take 50g 002B polyisocyanate prepolymer component Take 90g
[0116] Bond strength (Mpa) 2.85 Full nail head veneer Example
[0117] 3.1~3.4 sodium water glass 100 γ-aminopropyl triethoxysilane 0.3 dodecanol ester 0.5 take 50g 002B polyisocyanate prepolymer component take 120g
[0118] Bond strength (Mpa) 1.25 There is 1 / 4~1 / 5 veneer on the nail head Example
[0119] 2.2~2.5 modulus sodium water glass 100 γ-aminopropyl triethoxysilane 1.5 water 1.5 dodecanol ester 1.5 002B polyisocyanate prepolymer component 157g
[0120] Bond strength (Mpa) 1.82 Nail head full of veneer Example
[0121] 2.2~2.5 modulus sodium water glass 85.0 γ-aminopropyl triethoxysilane 0.55 dodecanol ester 4.0 acrylic resin 1.0 sodium tripolyphosphate 1.0 ethylene glycol monobutyl ether 1.0 propylene glycol 5.0 sodium sulfate 5.0 ethylene glycol 5.0
[0122] Take 20 grams of 002B polyisocyanate prepolymer component and take 18.4 grams
[0123] Bond strength (Mpa) 1.58 Most nail head glue and veneer account for 2 / 3 Example
[0124] 2.6~2.9 modulus sodium water glass 100 γ-aminopropyl triethoxysilane 1.65 γ-mercaptopropyl triethoxysilane 1 water 6.6 dodecanol ester 1.2 002B polyisocyanate prepolymer component 164g
[0125] Bond strength (Mpa) 1.59 Nail head full of veneer Example
[0126] 2.2~2.5 modulus sodium water glass 85.0 γ-aminopropyl triethoxysilane 0.55 dodecanol ester 4.00 acrylic resin 1.00 sodium tripolyphosphate 1.00 ethylene glycol monobutyl ether 1.00 glycerol 5 sodium sulfate 5.00 ethylene glycol 5.00
[0127] Take 20 grams of 002B polyisocyanate prepolymer component and take 18.4 grams
[0128] Bond strength (Mpa) 1.58 Most nail head glue and veneer account for 2 / 3 Example
[0129] 2.6~2.9 modulus sodium water glass 100 γ-aminopropyl triethoxysilane 1.65 water 0.8 dodecanol 0.8002B polyisocyanate prepolymer component 149g
[0130] Bond strength (Mpa) 1.22 Nail head full of veneer Example
[0131] 2.2~2.5 modulus sodium water glass 100 γ-aminopropyl triethoxysilane 1.35 water 6.75 dodecanol 0.8002B polyisocyanate prepolymer component 149 grams
[0132] Bond strength (Mpa) 1.21 Nail head full of veneer Example
[0133] 2.6~2.9 modulus potassium water glass 100 γ-aminopropyl triethoxysilane 1.5 water 1.5 dodecanol ester 1.2 002B polyisocyanate prepolymer component 150g
[0134] Bond strength (Mpa) 1.30 Nail head full of veneer Example
[0135] 2.6~2.9 modulus potassium water glass 50 2.6~2.9 modulus sodium water glass 50 γ-aminopropyl triethoxysilane 1.3 water 3.9 dodecanol ester 1.1 002B polyisocyanate prepolymer component 150g
[0136] Bond strength (Mpa) 1.38 Nail head full of veneer Example
[0137] 3.1~3.4 modulus sodium water glass 100 γ-aminopropyl triethoxysilane 1.65 dodecanol ester 2.8 002B polyisocyanate prepolymer component 149g
[0138] 2-hour bond strength (Mpa) 1.31 Nail head full of veneer
[0139] Embodiment 27
[0140] 2.6~2.9 sodium water glass 100 γ-aminopropyl triethoxysilane 1.5 dodecanol ester 0.8 002B polyisocyanate prepolymer component 149g
[0141] Bond strength (Mpa) 1.35 12 months test
[0142] Embodiment 28
[0143] 2.2~2.5 modulus sodium water glass 100 γ-aminopropyl triethoxysilane 1.5 dodecanol ester 0.8 002B polyisocyanate prepolymer component 149g
[0144] 48-hour steel plate-bamboo strip bonding strength (Mpa) 4.56 The nail head is almost full of glue with a small amount of bamboo chips (the end of the bamboo strip is bonded to the steel sheet)
[0145] 2 / 3 of the water glass component with γ-aminopropyltriethoxysilane added in the embodiment of the present invention is prepared at a natural temperature of 8~15°C, and has been sealed and stored for 2 months under the natural conditions, without obvious abnormal phenomena, and can still achieve good bonding strength after being matched with the polyurethane component. Another 1 / 3 is produced at 48°C and stored at 25°C for more than 1 month, and can also be used normally. The density of the adhesive component A of the present invention is about 1.25~2.25g / cm3, the viscosity is within 400~1500mpas (20°C), and the adaptation period is 5~90 minutes. The glass fiber reinforced plastic prepared by laminating the glass fiber cloth coated with the present invention is both rigid and flexible. After boiling in tap water for 4 days and 1% sodium hydroxide solution for 2 days, no abnormal conditions such as delamination and cracking were found, and the surface gloss did not change significantly. After 7 days of oil resistance immersion, 7 days of moisture and heat resistance immersion, 3 days of salt resistance immersion, and 15 times of cold and hot cycles, the coating did not wrinkle or fall off. And it is difficult to ignite.
[0146] The 2 / 3 water glass component with γ-aminopropyltriethoxysilane added in the embodiment of the present invention is prepared at a temperature of 8~85°C and has been sealed and stored under natural conditions for 12 months without obvious abnormal phenomena. After being combined with the polyurethane component, it can still achieve a good bonding effect, and the bonding strength is similar to that in the initial stage.
[0147] After preliminary testing, 3 samples of the embodiment of the present invention were randomly selected for testing after curing for 3 days. The results showed that the compressive strength was ≥40Mpa and the bonding strength was ≥3Mpa (iron-iron), and all samples were non-flammable.
[0148] In addition to being used as construction, decoration glue, door glue, metal, stone, wood and furniture glue, the present invention can also be used as glue for composite materials such as fiberglass, and can also be used as grouting glue for treating geological defects such as mines and dangerous rocks, engineering construction and road repair, and can be used for fire isolation.
Claims
1. A coupling agent water glass polyurethane environmentally friendly adhesive composition, which is composed of sodium water glass and / or potassium water glass components and polyurethane components, and is characterized by: The composition is added with a coupling agent suitable for cooperating with the water glass component, wherein the coupling agent is γ-aminopropyl triethoxysilane, and the addition amount thereof is at least 0.3-2.0% of the mass of the water glass. The γ-aminopropyl triethoxysilane or its modified derivative is firstly dripped into the water glass under stirring at 25° C. to 85° C., and then 0.3-10% of the mass of the water glass is added after stirring, or 0.5-3 times the weight of water of the γ-aminopropyl triethoxysilane is firstly added into the γ-aminopropyl triethoxysilane at 15° C., and then the mixture is dripped into the water glass under stirring, and then 0.3-10% of the mass of the water glass is added with polyol ester and / or alcohol ether; the polyol ester and / or alcohol ether is dodecanol ester (2,2,4-trimethyl- 1,3-pentanediol monoisobutyrate), hexadecanol ester, ethylene glycol monobutyl ether, triethylene glycol monobutyl ether, triethylene glycol monoethyl ether, tripropylene glycol monobutyl ether, glycerol triacetate, or a combination of one or more of triethylene glycol bis (2-hexyl acetate), 2,4-trimethyl-1,3-pentanediol diisobutyrate, triethylene glycol dioctanoate, triethylene glycol diisooctanoate ethylene glycol monobutyl ether stearate, diethylene glycol diricinoleate, glycerol triacetate, oleic acid diethanolamide and its boric acid, ethylene glycol butyl ether acetate (BGA) and its derivatives; the polyurethane component is composed of a polyisocyanate and a terminal NCO prepolymer of a polyester polyol and / or a polyether polyol, and the polyisocyanate is diphenylmethane diisocyanate (MDI) and polymethylene polyphenyl polyisocyanate (PAPI) in a ratio of 1:
0. 5~2, or a ratio of one or more of diphenylmethane diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate and polymethylene polyphenyl polyisocyanate (PAPI) is 1:0.5~2; the mixture contains NCO10~28%, the average functionality of the polyether polyol is 2~5, the molecular weight is 500~6000, and the hydroxyl value is 35~500mgkOH / g; the polyurethane component contains 5%~50% of the total weight of the polyurethane component The solvent, the relative proportion of the polyurethane component increases with the increase of the water glass modulus.
2. The coupling agent water glass polyurethane environmentally friendly glue composition as claimed in claim 1, characterized in that The added amount of the γ-aminopropyltriethoxysilane is 0.5-1.8% of the mass of the water glass.
3. The coupling agent water glass polyurethane environmentally friendly glue composition as claimed in claim 1, characterized in that Mix at 25-50℃, or add 1-2 times the weight of water at 15℃ above freezing point and below freezing point. Stir while adding dropwise to prevent caking. After stirring evenly, put into barrels and seal the lid in time to prevent evaporation and film formation.
4. The coupling agent water glass polyurethane environmentally friendly adhesive composition according to any one of claims 1 to 3, characterized in that The water glass component also contains 0.5-5% of the mass of water glass as emulsifier and / or 0.5-10% of color filler and / or other conventional additives, wherein the additives may be emulsifier, phosphate, styrene, polyol 、 Viscosity reducer or catalyst.
5. The coupling agent water glass polyurethane environmentally friendly adhesive composition according to any one of claims 1 to 3, characterized in that The amount of polyol ester and / or alcohol ether added is 1-5% of the mass of water glass.
6. The coupling agent water glass polyurethane environmentally friendly adhesive composition as claimed in claim 1, characterized in that The modulus of the sodium water glass or potassium water glass is 2.2-2.9, and the mass ratio of the water glass component to the polyurethane component is 1:1-1.
3.
7. The coupling agent water glass polyurethane environmentally friendly adhesive composition as claimed in claim 1, characterized in that The modulus of the sodium water glass or potassium water glass is 3.1-3.4, and the mass ratio of the water glass component to the polyurethane component is 1:1.3-2.
8. The coupling agent water glass polyurethane environmentally friendly adhesive composition as claimed in claim 1, characterized in that For the low modulus water glass-polyurethane system of 1.6~2.6, the weight ratio is 1:0.8~1.2; for the high modulus water glass-polyurethane system of 2.6~3.6, the ratio is 1:1.5~2.
5.
9. The coupling agent water glass polyurethane environmentally friendly adhesive composition as claimed in claim 1, characterized in that The mass ratio of the water glass component to the polyurethane component is 1:0.7-1.
3.
10. The coupling agent water glass polyurethane environmentally friendly adhesive composition according to any one of claims 1 to 3 and 6 to 9, characterized in that The polyester polyol is Sovermol 750 and ethylene terephthalate; the polyether polyol has an average functionality of 2-5, a molecular weight of 400-2000, a hydroxyl value of 35-500 mgkOH / g, and is one or a combination of more than one of polyether polyol 220N or 330N, trimethylolpropane-propylene oxide polyether triol, pentaerythritol polyether, and polypropylene oxide polyether triol.
11. The coupling agent water glass polyurethane environmentally friendly adhesive composition according to any one of claims 1 to 3 and 6 to 9, characterized in that The NCO content of the polyurethane component is 12-18%.
12. The coupling agent water glass polyurethane environmentally friendly adhesive composition according to any one of claims 1 to 3 and 6 to 9, characterized in that The solvent in the polyurethane component is dimethyl carbonate and / or acetone.
13. The coupling agent water glass polyurethane environmentally friendly adhesive composition as described in any one of claims 1 to 3 and 6 to 9 is prepared by the following method: the temperature is controlled below 48° C., 0.3 to 2% of the silane coupling agent of the total mass of the water glass is first added to part of the water glass, and the mixture is stirred rapidly. The remaining part of the water glass is added during stirring, and the mixture is stirred for 10 to 30 minutes. Then, 0.3 to 10% of a mixed solution of one or more of polyol esters, alcohol ethers, co-solvents, and emulsifiers is added, wherein the co-solvent refers to a solvent that is soluble in both polyol esters and / or alcohol ethers and water glass; PAPI is first reacted with polyester polyols and / or polyether polyols to prepare a prepolymer, and then polymerized MDI is added, and then the viscosity is adjusted with a viscosity reducer and / or solvent of 0 to 1 / 3 of the total mass of the component, or finally 0.3 to 2% of the total mass of the silane coupling agent, polyol esters, and alcohol ethers. One or more combinations of the above are added.
14. The coupling agent water glass polyurethane environmentally friendly adhesive composition according to any one of claims 1 to 3 and 6 to 9 is characterized in that Used for door core or building material processing or geological defect treatment or fiberglass production.
Citation Information
Patent Citations
Composite rubber material
CN103627330A
Polyisocyanate-based adhesive formulation for use in sandwich panels
CN1788064A
Polyolefin composition
EP1477525B1
Adhesive composition for concrete and filler composition
JP2002020698A