Optimization Method for Effective Nonlinear Optical Coefficients of Lanthanum Gallium Silicate Solid Solution Crystals
By adjusting the component ratio and group ion mixing of the gallium lanthanum silicate crystal, its polyhedral lattice structure and refractive index dispersion are optimized, solving the problem of insufficient nonlinear optical coefficients of the gallium lanthanum silicate crystal, and significantly improving the its frequency conversion efficiency.
Patent Information
- Application Number
- CN202210986346.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-17
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-08-17
AI Technical Summary
The existing lanthanum gallium silicate crystal has a small effective nonlinear coefficient during the nonlinear frequency conversion process, which limits its frequency conversion efficiency.
Solid solution crystals are formed by adjusting the proportion of gallium lanthanum silicate crystal components with the same structure, and using different ions in the B-site and D-site groups to mix and control the polyhedral lattice structure, degree of distortion, refractive index and refractive index dispersion. , reduce the phase matching angle and increase the nonlinear optical coefficient.
It effectively improves the nonlinear optical coefficient of the gallium lanthanum silicate crystal and improves its frequency conversion efficiency.
Smart Images

Figure CN115185137B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of nonlinear optical crystal and laser technology, and more particularly to a method for optimizing effective nonlinear optical coefficients of lanthanum gallium silicate solid solution crystals. Background Art
[0002] Lanthanum gallium silicate crystal (structural formula A 3 BC 3 D 2 O 14 , including AO 8 , BO 6 , CO 4 and DO 4 Four polyhedral groups) mainly include lanthanum gallium niobate (LGN) crystals, lanthanum gallium tantalate (LGT) crystals and lanthanum gallium silicate (LGS) crystals. Previous studies have shown that lanthanum gallium niobate (LGN) crystals in this family of crystals have the characteristics of wide transmission range and high laser damage threshold. They are mid-infrared nonlinear optical materials with excellent comprehensive performance, and have achieved effective output of femtosecond and nanosecond difference frequency mid-infrared lasers. In the process of nonlinear frequency conversion, the effective nonlinear coefficient of the nonlinear crystal material determines its conversion efficiency. The size of the effective nonlinear coefficient depends on the nonlinear coefficient of the material and the refractive index dispersion equation. The phase matching conditions of the existing lanthanum gallium silicate crystals determine that the effective nonlinear coefficient of infrared frequency conversion in this type of crystal is small, which limits its frequency conversion efficiency.
[0003] Therefore, based on the lanthanum gallium silicate family of solid solution crystals, improving the effective nonlinear optical coefficient while maintaining the excellent performance of this family of crystals is an issue that needs to be urgently addressed by those skilled in the art. Summary of the invention
[0004] In view of this, the present invention provides a method for optimizing the effective nonlinear optical coefficient of a lanthanum gallium silicate solid solution crystal; a solid solution crystal is formed by adjusting the proportion of lanthanum gallium silicate crystal components with the same structure, and different ions are mixed in the B-position group and the D-position group to control the polyhedral lattice structure and distortion degree of the crystal, and adjust the refractive index and refractive index dispersion of the solid solution crystal, so as to achieve a reduction in the phase matching angle and an increase in the nonlinear optical coefficient, and finally optimize the effective nonlinear optical coefficient.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A method for optimizing the effective nonlinear optical coefficient of a lanthanum gallium silicate solid solution crystal, characterized in that the lanthanum gallium silicate crystal A 3 BC 3 D 2 O 14It mainly includes lanthanum gallium niobate (LGN) crystals, lanthanum gallium tantalate (LGT) crystals, lanthanum gallium silicate (LGS) crystals, etc. The solid solution crystals are formed by adjusting the proportion of lanthanum gallium silicate crystal components with the same structure, so that different ions are mixed in the polyhedral groups, thereby changing the polyhedral lattice structure, distortion degree, refractive index and refractive index dispersion of the solid solution crystals.
[0007] Preferably, lanthanum gallium niobate crystals, lanthanum gallium tantalate crystals or lanthanum gallium silicate crystals with the same crystal structure and similar components are dissolved in different proportions to form solid solution crystals, so that the B-site and / or D-site structure of the lanthanum gallium silicate crystals are changed.
[0008] Preferably, the B group is Ga 3+ , Nb 5+ 、 5+ 、Ti 4+ 、Zr 4+ , Hf 4+ Sn 4+ , Sb 5+ Plasma mixing, regulating the refractive index, different ions have different electron cloud structures, regulating the refractive index and refractive index dispersion, thereby reducing the phase matching angle, increasing the effective nonlinear optical coefficient, and dissolving lanthanum gallium niobate (LGN) crystals and lanthanum gallium tantalate (LGT) crystals with the same crystal structure and similar components in different proportions to form lanthanum gallium niobate (LGNT) solid solution crystals; the B-position group adopts gallium ions (Ga 3+ ), niobium ions (Nb 5+ ) and tantalum ions (Ta 5+ ) three ions are co-occupied to adjust the distortion size of the B-site polyhedral group. Specifically, the crystal is a lanthanum gallium tantalate niobate (LGNT) solid solution crystal, and the proportion of the lanthanum gallium silicate crystal components is 0.9:0.1 or 0.7:0.3. The specific La 2 O 3 , Ga 2 O 3 , Nb 2 O 5 , 2 O 5 The molar ratio of the four raw materials is 0.3:0.55:0.045:0.005 or 0.3:0.55:0.035:0.015; this series of solid solution crystals maintains the crystal structure of lanthanum gallium niobate (LGN) and lanthanum gallium tantalate (LGT), and can continuously adjust the refractive index of this family of crystals, thereby changing the phase matching angle and increasing the effective nonlinear optical coefficient.
[0009] Preferably, the D group is Ga 3+ ,Ge 4+ 、Si 4+Plasma mixing can regulate the size of the D-position polyhedron distortion. At the same time, the different electron cloud structures of different ions can regulate the refractive index and refractive index dispersion, thereby reducing the phase matching angle and increasing the effective nonlinear optical coefficient.
[0010] Preferably, different ions are mixed in the two types of polyhedral groups at the B position and the D position, and Ga is used at the B position. 3+ 、Zr 4+ Ion mixed occupation, D position takes Ga 3+ 、Si 4+ The ions are mixed to form a solid solution crystal of lanthanum gallium zirconate silicate, and the polyhedral distortion at the B and D positions is regulated to increase the nonlinear optical coefficient. The refractive index and refractive index dispersion of the crystal are regulated to reduce the phase matching angle and increase the effective nonlinear optical coefficient.
[0011] It can be seen from the above technical scheme that, compared with the prior art, the present invention discloses a method for optimizing the effective nonlinear optical coefficient of a lanthanum gallium silicate solid solution crystal; by adjusting the proportion of lanthanum gallium silicate crystal components with the same structure to form a solid solution crystal, and using different ions to mix the B-position group and the D-position group, the polyhedral lattice structure and the degree of distortion of the crystal are regulated, and the refractive index and refractive index dispersion of the solid solution crystal are adjusted, so as to achieve a reduction in the phase matching angle and an increase in the nonlinear optical coefficient, and finally optimize the effective nonlinear optical coefficient. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0013] Figure 1 The accompanying figure shows Nb provided in Example 2 of the present invention. 5+ / Ta 5+ Refractive index comparison of lanthanum gallium tantalate niobate (LGNT) solid solution crystal with a ratio of 0.9:0.1 and 0.7:0.3, lanthanum gallium niobate (LGN) crystal and lanthanum gallium tantalate (LGT) crystal.
[0014] Figure 2 The accompanying figure shows Nb provided in Example 2 of the present invention. 5+ / Ta 5+ Comparison of nonlinear optical coefficients of lanthanum gallium niobate tantalate (LGNT) solid solution crystals with ratios of 0.9:0.1 and 0.7:0.3.
[0015] Figure 3 The accompanying figure shows Nb provided in Example 2 of the present invention.5+ / Ta 5+ Comparison of type I phase matching tuning curves of lanthanum gallium tantalate niobate (LGNT) solid solution crystals with ratios of 0.9:0.1 and 0.7:0.3 with lanthanum gallium niobate (LGN) crystals and lanthanum gallium tantalate (LGT) crystals.
[0016] Figure 4 The accompanying figure shows Nb provided in Example 2 of the present invention. 5+ / Ta 5+ Comparison of type II phase matching tuning curves of lanthanum gallium tantalate niobate (LGNT) solid solution crystals with ratios of 0.9:0.1 and 0.7:0.3 with lanthanum gallium niobate (LGN) crystals and lanthanum gallium tantalate (LGT) crystals.
[0017] Figure 5 The attached figure shows a lanthanum gallium silicate crystal A provided by the present invention. 3 BC 3 D 2 O 14 Schematic diagram of the structure. DETAILED DESCRIPTION
[0018] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] The embodiment of the present invention discloses a method for optimizing the effective nonlinear optical coefficient of a lanthanum gallium silicate solid solution crystal, characterized in that the lanthanum gallium silicate crystal A 3 BC 3 D 2 O 14 It mainly includes lanthanum gallium niobate (LGN) crystals, lanthanum gallium tantalate (LGT) crystals, lanthanum gallium silicate (LGS) crystals, etc. The solid solution crystals are formed by adjusting the proportion of lanthanum gallium silicate crystal components with the same structure, so that different ions are mixed in the polyhedral groups, thereby changing the polyhedral lattice structure, distortion degree, refractive index and refractive dispersion of the solid solution crystals.
[0020] In order to further optimize the above technical solution, lanthanum gallium niobate crystals, lanthanum gallium tantalate crystals or lanthanum gallium silicate crystals with the same crystal structure and similar components are dissolved in different proportions to form solid solution crystals, so that the B-site and / or D-site structure of the lanthanum gallium silicate crystals are changed.
[0021] To further optimize the above technical solution, the B-position group adopts Ga 3+ , Nb 5+ 、5+ 、Ti 4+ 、Zr 4+ , Hf 4+ Sn 4+ , Sb 5 + Plasma mixed.
[0022] To further optimize the above technical solution, the D group adopts Ga 3+ ,Ge 4+ 、Si 4+ Plasma mixed.
[0023] In order to further optimize the above technical solution, different ions are mixed in the two types of polyhedral groups at the B position and the D position. 3+ 、Zr 4+ Ion mixed occupation, D position takes Ga 3+ 、Si 4+ The ions mix and form lanthanum gallium zirconate solid solution crystals.
[0024] The nonlinear optical crystal provided is a solid solution crystal of lanthanum gallium niobate of the lanthanum gallium silicate family, and its chemical formula is La 3 Ga 5.5 (Nb 1-x Ta x ) 0.5 O 14 , belongs to the trigonal crystal system, 32 point groups, there are one type (the two incident beams have the same polarization mode, both are e-light) and two types of phase matching (the two incident beams have different polarization directions, one is o-light and the other is e-light), the corresponding effective second-order nonlinear coefficient is (a type of bit matching) and (Type II phase matching), θ is the phase matching angle, is the azimuth angle. The B-position group accommodates Ga 3+ , Nb 5+ 、 5+ 、Ti 4+ 、Zr 4+ , Hf 4+ Sn 4+ , Sb 5+ The use of different ion mixing methods can increase the distortion of the B-position group and increase the nonlinear optical coefficient. At the same time, the electron cloud structures of different ions are different, which can adjust the refractive index and refractive index dispersion of the crystal, reduce the phase matching angle, and thus increase the effective nonlinear optical coefficient. 3+ , Nb 5+ 、 5+ 、Ti 4+ 、Zr 4+ , Hf4+ Sn 4+ , Sb 5+ The ionic radius of various ions such as Ga is similar, with good lattice matching, which can form infinite solid solution crystals and easily obtain large-sized single crystals with high optical quality. At the same time, the D-position group can also accommodate a variety of ions, such as Ga 3+ ,Ge 4+ 、Si 4+ .
[0025] Example 1: Taking the solid solution crystal of lanthanum gallium niobate (LGN) and lanthanum gallium tantalate (LGT) as an example, we designed Nb 5+ / Ta 5+ The ratio of 0.5:0.5 is lanthanum gallium niobate (LGNT) solid solution crystal, and its specific La 2 O 3 , Ga 2 O 3 , Nb 2 O 5 , 2 O 5 The molar ratio of the four raw materials is 0.3:0.55:0.025:0.025. The crystal belongs to the trigonal system and 32 point group. 5+ / Ta 5+ With the change of the component ratio, the distortion degree of the B-position group increases, which is beneficial to increase the nonlinear optical coefficient; at the same time, the refractive index and refractive index dispersion of the crystal change accordingly, which can reduce the phase matching angle and is beneficial to increase the effective nonlinear optical coefficient of the crystal.
[0026] Example 2: We designed the following different Nb 5+ / Ta 5+ The proportion of lanthanum gallium niobate tantalate (LGNT) solid solution crystals, such as Nb 5 + / Ta 5+ The ratios are 0.9:0.1, 0.7:0.3, 0.3:0.7, 0.1:0.9 and other different Nb 5+ / Ta 5+ The proportion of lanthanum gallium niobate tantalate (LGNT) solid solution crystal, its specific La 2 O 3 , Ga 2 O 3 , Nb 2 O 5 , 2 O 5The molar ratio of the four raw materials can be 0.3:0.55:0.045:0.005, 0.3:0.55:0.035:0.015, 0.3:0.55:0.015:0.035, 0.3:0.55:0.005:0.045. This series of solid solution crystals also maintains the crystal structure of lanthanum gallium niobate (LGN) and lanthanum gallium tantalate (LGT), and can continuously adjust the refractive index of the crystal family, thereby changing the phase matching angle and increasing the effective nonlinear optical coefficient.
[0027] Example 3: Taking the solid solution crystal of lanthanum gallium zirconate (LGZr) and lanthanum gallium silicate (LGS) as an example, we can design Zr 4+ / Si 4+ The ratio of La is 0.5:0.5 3 Zr 0.5 Ga 5 Si 0.5 O 14 Crystal, its specific four raw materials La 2 O 3 , Ga 2 O 3 , ZrO 2 , SiO 2 The molar ratio is 0.3:0.5:0.1:0.1. The crystal belongs to the trigonal system, 32 point group, and the B and D positions are Ga 3+ / Zr 4+ and Ga 3+ / Si 4+ When the two ions co-occupy, the distortion degree of the B-position group and the D-position group increases, which is beneficial to increasing the nonlinear optical coefficient; at the same time, the refractive index and refractive index dispersion of the crystal change accordingly, which can reduce the phase matching angle and is beneficial to increasing the effective nonlinear optical coefficient of the crystal.
[0028] Example 4: Taking the solid solution crystal of lanthanum gallium zirconate (LGZr) and lanthanum gallium silicate (LGS) as an example, we can design different Zr 4+ / Si 4+ The proportion of lanthanum gallium zirconate silicate (LZGS) solid solution crystals, such as Zr 4+ / Si 4+ Solid solution crystals with different ratios of 0.9:0.1, 0.7:0.3, 0.3:0.7, 0.1:0.9, etc., among which La 2 O 3 , Ga 2 O 3 , ZrO 2 , SiO 2The molar ratio of the four raw materials can be 0.3:0.5:0.18:0.02, 0.3:0.5:0.14:0.06, 0.3:0.5:0.06:0.14, 0.3:0.5:0.02:0.18. This series of crystals also belongs to the trigonal system and 32 point group, and the B and D positions are Ga 3+ / Zr 4+ and Ga 3+ / Si 4+ The co-occupancy of the two ions increases the distortion of the B-position group and the D-position group, which is beneficial to increasing the nonlinear optical coefficient; at the same time, adjusting the refractive index and refractive index dispersion of the crystal can reduce the phase matching angle, which is beneficial to increasing the effective nonlinear optical coefficient of the crystal.
[0029] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.
[0030] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for optimizing the effective nonlinear optical coefficients of a lanthanum gallium silicate solid solution crystal, characterized in that: Lanthanum Gallium Silicate Crystal A3BC3D2O 14 Mainly including lanthanum gallium niobate LGN crystal, lanthanum gallium tantalate LGT crystal, lanthanum gallium silicate LGS crystal, by the same crystal structure, similar components of lanthanum gallium niobate crystal, lanthanum gallium tantalate crystal or lanthanum gallium silicate crystal in different proportions to form a solid solution crystal, so that different ions are mixed in the polyhedral group, the B-site and D-site structure of the lanthanum gallium silicate crystals are changed, and the polyhedral lattice structure, distortion, refractive index and refractive dispersion of the solid solution crystal are changed; At the same time, different ions are mixed in the two types of polyhedral groups at the B and D positions. Ga 3+ 、Zr 4+ Ion mixed occupation, D position takes Ga 3+ 、Si 4+ The ions mix and form lanthanum gallium zirconate solid solution crystals.
Citation Information
Patent Citations
Ceria-zirconia solid solution crystal fine grain and process for producing the same
CN101896429A
Fluorinated ferric sulfate salt compound as well as preparation method and application thereof
CN102332580A
Solid solution crystal and growing method
JP2001080988A