A cooling liquid recovery and treatment process for silicon single crystal diamond wire slicing

Through the mixing of adsorbent materials and waste coolant, efficient recycling of coolant and ultra-fine silicon powder in the silicon single-crystal diamond wire slicing process is achieved, solving the problems of powder impact and waste liquid treatment cost during the cutting process, and reducing production cost.

CN115194964BActive Publication Date: 2024-11-15天津市环智新能源技术有限公司 +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202110383550.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-09
Publication Date
2024-11-15
Estimated Expiration
2041-04-09

AI Technical Summary

Technical Problem

During the cutting process of silicon single crystal diamond wire, the ultra-fine silicon powder mixed into the coolant leads to a disadvantage in the cutting process, and the high COD concentration of the waste coolant cannot be simply discharged, and the existing technology is difficult to effectively recycle and reuse, resulting in an increase in production costs. .

Method used

Adsorption is mixed with waste coolant for induction of adsorption. Through solid-liquid separation, ion exchange, desorption and screening filtration, regenerating coolant and ultra-fine silicon powder are recovered separately, and the adsorbed material is regenerated to realize the coolant and Reuse of adsorbent materials.

Benefits of technology

The recycling of high-purity ultra-fine silicon powder and the regeneration of high-quality coolant is achieved, which reduces operating costs, and the use of adsorbent materials is small, and the overall operating costs are 1/3-1/5 of the prior art.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115194964B_ABST
    Figure CN115194964B_ABST
Patent Text Reader

Abstract

The present invention provides a process for recovering and treating coolant for silicon single crystal diamond wire slicing, comprising the following steps: mixing waste coolant with adsorbent material to induce adsorption; performing solid-liquid separation on the mixed waste coolant and adsorbent material; performing ion exchange on the separated liquid to obtain regenerated coolant; mixing the separated solid with alkaline solution to desorb ultrafine silicon powder from the adsorbent material; screening and filtering the desorbed solid to separate ultrafine silicon powder and adsorbent material; filtering and dehydrating the separated ultrafine silicon powder to obtain high-purity ultrafine silicon powder; mixing the separated adsorbent material with an acid solution to obtain a regenerated adsorbent material. The beneficial effects of the present invention are that the recovery process is advanced, high-quality coolant can be recovered, and high-purity ultrafine silicon powder can be recovered; the operating cost is reduced, the amount of adsorbent material used is small and renewable, and the overall operating cost is 1 / 3 to 1 / 5 of the existing technical method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of single crystal cutting, and in particular relates to a cooling liquid recovery and treatment process for silicon single crystal diamond wire slicing. Background Art

[0002] The integrated circuit industry is the most important high-tech to promote the development of national economy and social informatization. As the most commonly used semiconductor material, single crystal silicon wafers are widely used in the production process of integrated circuits. At present, most silicon single crystal cutting adopts diamond wire cutting. In the process of diamond wire cutting, in order to timely remove the heat generated during the cutting process and flush away the solid powder generated during the cutting process, coolant must be used. In actual cutting, a large amount of ultrafine silicon powder (d 50 =0.8μm) will continue to mix into the wire cutting coolant, causing more dirty silicon wafers and adversely affecting the cutting process. Therefore, when the solid powder in the coolant reaches a certain concentration, it is necessary to replace the coolant for cutting, resulting in an increase in production costs. Since the waste coolant contains a certain concentration of organic matter, its COD concentration is high and cannot be simply discharged into the environment.

[0003] According to the differences in the composition and properties of the cooling waste liquid used for silicon single crystal diamond wire slicing, solid / liquid separation is generally performed first, and then the liquid phase is purified. The solid / liquid separation process mainly includes centrifugal separation, cyclone separation, flotation process, grading process and screening process, while the main processes for liquid phase purification are filter press, membrane filtration and distillation. Since the cooling waste liquid has a certain viscosity and the silicon powder contained in the waste liquid has a fine particle size, the commonly used solid / liquid separation method is difficult to meet the requirements. The chemical flocculation method can reduce the content of ultrafine silicon powder to a certain extent, but it also changes the composition of the coolant and cannot be reused, resulting in increased production costs. The filter press method also removes some silicon powder in the cooling waste liquid. Although it does not change the composition of the coolant, the processing capacity is low and it is difficult to meet the needs of increased production capacity. Summary of the invention

[0004] In view of the above problems, the present invention provides a process for recovering and treating coolant for silicon single crystal diamond wire slicing to solve the above or other former problems existing in the prior art.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a process for recovering and treating coolant for silicon single crystal diamond wire slicing, comprising the following steps:

[0006] Mixing the waste coolant with the adsorption material to induce adsorption;

[0007] performing solid-liquid separation on the mixed waste coolant and the adsorption material;

[0008] The separated liquid is subjected to ion exchange to obtain a regenerated coolant;

[0009] The separated solid is mixed with an alkaline solution to desorb the ultrafine silicon powder from the adsorption material;

[0010] The desorbed solid is screened and filtered to separate the ultrafine silicon powder and the adsorption material;

[0011] The separated ultrafine silicon powder is filtered and dehydrated to obtain high-purity ultrafine silicon powder;

[0012] The separated adsorbent material is mixed with an acid solution to obtain a regenerated adsorbent material.

[0013] Furthermore, in the step of mixing the waste coolant with the adsorption material for inducing adsorption, the weight ratio of the adsorption material to the waste coolant is 1:100-1:250.

[0014] Furthermore, the waste coolant and the adsorption material are stirred and mixed in an adsorption stirring tank, the stirring speed of the adsorption stirring tank is 80-120 r / min, and the stirring time is 1-3 min.

[0015] Further, in the step of mixing the separated solid with an alkaline solution to desorb the ultrafine silicon powder from the adsorbent material, the alkaline solution is an alkaline solution with a mass fraction of 4-6wt%;

[0016] Preferably, the alkali solution is sodium hydroxide solution or potassium hydroxide solution.

[0017] Furthermore, the separated solid and the alkali solution are stirred and mixed in a conditioning stirring tank, the stirring speed of the conditioning stirring tank is 150-200 r / min, and the stirring time is 3-5 min.

[0018] Furthermore, in the step of mixing the separated adsorbent material with the acid solution, the acid solution is a hydrochloric acid solution having a mass fraction greater than 3 wt %;

[0019] Preferably, the acid solution is a hydrochloric acid solution with a mass fraction of 4-6wt%.

[0020] Furthermore, the separated adsorption material and the acid solution are stirred and mixed in a regeneration stirring tank, the stirring speed of the regeneration stirring tank is 80-120 r / min, and the stirring time is 5-10 min.

[0021] Furthermore, the adsorption material is a mineral material or a polymer material.

[0022] Furthermore, the mineral material is manganese dioxide, and the polymer material is anion exchange resin.

[0023] Furthermore, the particle size of the adsorbent material is 100-2000 μm.

[0024] Furthermore, in the step of performing solid-liquid separation on the mixed waste coolant and the adsorbent material, the solid-liquid separation is performed in a centrifuge, the centrifugal speed of the centrifuge is 2500-3500 r / min, and the centrifugal time is 10-20 s.

[0025] Furthermore, in the step of subjecting the separated liquid to ion exchange, the separated liquid is subjected to ion exchange in a centrifugal exchange bed, which is an anion resin exchange bed.

[0026] Furthermore, in the step of screening and filtering the desorbed solid to separate the ultrafine silicon powder and the adsorption material, the desorbed solid is screened and filtered in a rotary vibrating screen, and the screening particle size of the rotary vibrating screen is 90-120 μm.

[0027] Furthermore, in the step of filtering and dehydrating the separated ultrafine silicon powder, the separated ultrafine silicon powder is filtered and dehydrated in a filter press.

[0028] Due to the adoption of the above technical scheme, the adsorption material and the waste coolant are stirred and mixed, and then centrifuged, the adsorption material adsorbs the ultrafine silicon powder in the waste coolant, so that the ultrafine silicon powder is separated from the coolant, and then the coolant and the ultrafine silicon powder are treated separately to obtain regenerated coolant and ultrafine silicon powder, and the adsorption material is treated at the same time to obtain regenerated adsorption material, so that the coolant and the adsorption material can be reused, and the high-purity ultrafine silicon powder can be recovered, which reduces the operating cost, and a large amount of waste coolant can be recycled with less adsorption material, so that high-quality coolant and high-purity ultrafine silicon powder can be obtained, the recovery process is advanced, the adsorption material used in the recovery process is small in amount and renewable, and the overall operating cost is 1 / 3-1 / 5 of that of the existing technical method. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic diagram of the process flow of a method for recovering coolant for silicon single crystal diamond wire slicing according to one embodiment of the present invention.

[0030] Figure 2 It is a schematic structural diagram of a cooling liquid recovery and processing system for silicon single crystal diamond wire slicing according to an embodiment of the present invention.

[0031] In the figure:

[0032] 1. Adsorption stirring section 2. Separation section 3. Conditioning stirring section

[0033] 4. Screening section 5. Filter press section 6. Ion exchange section

[0034] 7. Regeneration mixing unit DETAILED DESCRIPTION

[0035] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0036] Figure 1 A process flow chart of an embodiment of the present invention is shown. This embodiment relates to a coolant recovery and treatment process for silicon single crystal diamond wire slicing, which is used to recover the waste coolant after silicon single crystal slicing, so that the coolant can be recycled and reused, and at the same time, the silicon powder in the coolant is recovered to obtain high-purity ultrafine silicon powder; adsorption materials and waste coolant are used for recovery and treatment, and the amount of adsorption materials used is small and renewable, thereby reducing the overall operating cost.

[0037] A process for recovering coolant for silicon single crystal diamond wire slicing, such as Figure 1 As shown, the following steps are included:

[0038] Mixing the waste coolant with the adsorption material to induce adsorption;

[0039] The coolant used in diamond wire cutting of silicon single crystals contains coolant to be recycled and ultrafine silicon powder in the waste coolant formed after cutting. The waste coolant is recycled, that is, the coolant and ultrafine silicon powder are recycled and reused. Therefore, when recycling the coolant, the waste coolant is first mixed with the adsorption material, the ultrafine silicon powder in the waste coolant is adsorbed by the adsorption material, and the ultrafine silicon powder and the waste coolant are separated into solid and liquid.

[0040] When the waste coolant is mixed with the adsorption material, the waste coolant discharged from the diamond wire slicer is transported to the adsorption stirring tank, and the adsorption material is placed in the adsorption stirring tank to mix the waste coolant with the adsorption material. When adding the adsorption material, the weight ratio of the adsorption material to the waste coolant is 1:100-1:250, and a small amount of adsorption material can be used to treat a large amount of waste coolant; and the waste coolant and the adsorption material are stirred and mixed in the adsorption stirring tank, the stirring speed of the adsorption stirring tank is 80-120r / min, and the stirring time is 1-3min, so that the waste coolant and the adsorption material are fully mixed, so that the adsorption material can completely adsorb the ultrafine silicon powder in the waste coolant, so that the coolant and the ultrafine silicon powder in the waste coolant are completely separated, and they are recycled and reused respectively.

[0041] The weight ratio of the adsorption material to the waste coolant can be 1:100, 1:150, 1:200 or 1:250, which is selected according to actual needs and no specific requirements are made here.

[0042] The speed of the stirring tank can be 80r / min, 90r / min, 100r / min, 110r / min or 120r / min. It can be selected according to actual needs. No specific requirements are made here.

[0043] The stirring time when the adsorption material and the waste coolant are stirred and mixed can be 1 minute, 2 minutes or 3 minutes, which is selected according to actual needs. No specific requirements are made here.

[0044] The above-mentioned adsorption material is a mineral material or a polymer material, wherein the mineral material is manganese dioxide and the polymer material is an anion exchange resin. The particle size of the adsorption material is 100-2000 μm, which is selected according to actual needs.

[0045] The above-mentioned adsorption stirring tank is a stirring tank, which is a commercially available product. It is selected according to actual needs and no specific requirements are made here.

[0046] performing solid-liquid separation on the mixed waste coolant and the adsorption material;

[0047] In this step, the adsorption material containing ultrafine silicon powder is separated from the coolant, and solid-liquid separation is performed in a centrifuge. The waste coolant containing the adsorption material-ultrafine silicon powder composite is transported to the centrifuge. The centrifugal speed of the centrifuge is 2500-3500r / min, and the centrifugal time is 10-20s. Under the centrifugal action of the centrifuge, the adsorption material containing ultrafine silicon powder and the coolant are separated, so as to facilitate the subsequent treatment of the adsorption material containing ultrafine silicon powder and the coolant separately.

[0048] The centrifugal speed of the centrifuge can be 2500r / min, 2700r / min, 3000r / min, 3200r / min or 3500r / min. It can be selected according to actual needs. No specific requirements are made here.

[0049] The centrifugation time can be 10s, 12s, 14s, 16s, 18s or 20s, which can be selected according to actual needs. No specific requirements are made here.

[0050] The above-mentioned centrifuge is a commercially available product and is selected according to actual needs. No specific requirements are made here.

[0051] The separated liquid is subjected to ion exchange to obtain a regenerated coolant;

[0052] In this step, the separated liquid is a coolant, and the separated coolant is transported to a centrifugal exchange bed, where the separated coolant undergoes ion exchange to remove ions and reduce conductivity, thereby obtaining a regenerated coolant, which is a recyclable high-quality coolant, so that the coolant can be used again. In this embodiment, the centrifugal exchange bed is preferably an anion resin exchange bed, which is a commercially available product and is selected according to actual needs.

[0053] The separated solid is mixed with an alkaline solution to desorb the ultrafine silicon powder from the adsorption material;

[0054] In this step, the separated solids are stirred and mixed with the alkali solution in a tempering and stirring tank, the separated solids are transported to the tempering and stirring tank, and the alkali solution is added to the tempering and stirring tank for stirring and mixing. The solid impurities are adsorption materials containing ultrafine silicon powder. After stirring and mixing, the ultrafine silicon powder in the adsorption material is separated from the adsorption material under the action of the alkali solution, so that the ultrafine silicon powder is no longer adsorbed on the adsorption material, thereby achieving desorption of the ultrafine silicon powder and the adsorption material.

[0055] When the separated solid is stirred and mixed with the alkali solution, the stirring speed of the tempering stirring tank is 150-200r / min, and the stirring time is 3-5min. The stirring speed can be 150r / min, 160r / min, 170r / min, 180r / min, 190r / min or 200r / min, which is selected according to actual needs, and no specific requirements are made here.

[0056] The stirring time can be 3 minutes, 4 minutes or 5 minutes, which is selected according to actual needs. No specific requirements are made here.

[0057] The above-mentioned alkali solution is an alkali solution with a mass fraction of 4-6wt%, which is selected according to actual needs. In the present embodiment, preferably, the alkali solution is an alkali solution containing hydroxide ions, that is, the alkali solution is an alkaline solution with a mass fraction of 4-6wt% of hydroxide ions, for example, sodium hydroxide solution or potassium hydroxide solution, etc., which is selected according to actual needs and no specific requirements are made here.

[0058] In this embodiment, preferably, the alkali solution is a sodium hydroxide solution with a mass fraction of 4-6wt%, or the alkali solution is a strong potassium oxide solution with a mass fraction of 4-6wt%.

[0059] The above-mentioned tempering stirring tank is a stirring tank, which is a commercially available product and is selected according to actual needs. No specific requirements are made here.

[0060] The desorbed solid is screened and filtered to separate the ultrafine silicon powder and the adsorption material;

[0061] In this step, the desorbed solid is screened and filtered in a rotary vibrating screen, and the desorbed ultrafine silicon powder and the adsorption material are conveyed to the rotary vibrating screen together to separate the ultrafine silicon powder and the adsorption material, wherein the screening particle size of the rotary vibrating screen is 90-120μm, and the screening particle size can be 90μm, 100μm, 110μm or 120μm, which is selected according to actual needs, and no specific requirements are made here.

[0062] The separated ultrafine silicon powder is filtered and dehydrated to obtain high-purity ultrafine silicon powder;

[0063] In this step, the separated ultrafine silicon powder is transported to a filter press for filter pressing and dehydration to obtain recyclable high-purity ultrafine silicon powder.

[0064] mixing the separated adsorbent material with an acid solution to obtain a regenerated adsorbent material;

[0065] In this step, the separated adsorbent material is stirred and mixed with the acid solution in the regeneration stirring tank, and the separated adsorbent material is transported to the regeneration stirring tank. At the same time, the acid solution is added to the regeneration stirring tank and stirred and mixed sufficiently to regenerate the adsorbent material so that the adsorbent material can be used again.

[0066] In this embodiment, the acid solution is a hydrochloric acid solution, and the acid solution is a hydrochloric acid solution with a mass fraction greater than 3wt%. Preferably, the acid solution is a hydrochloric acid solution with a mass fraction of 4-6wt%.

[0067] The above-mentioned regeneration stirring tank is a stirring tank, which is a commercially available product. It is selected according to actual needs and no specific requirements are made here.

[0068] When the separated adsorption material is stirred and mixed with the acid solution, the stirring speed of the regeneration stirring tank is 80-120r / min. The stirring speed can be 80r / min, 90r / min, 100r / min, 110r / min or 120r / min, which is selected according to actual needs. No specific requirements are made here.

[0069] The stirring time is 5-10 minutes, which can be 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes or 10 minutes. It is selected according to actual needs. No specific requirements are made here.

[0070] When the above-mentioned silicon single crystal diamond wire slicing coolant recovery and treatment process is carried out, a silicon single crystal diamond wire slicing coolant recovery and treatment system is used, such as Figure 2 As shown, specifically, the coolant recovery and processing system includes:

[0071] The adsorption and stirring part 1 is used to mix the waste coolant with the adsorption material, and the adsorption material adsorbs the ultrafine silicon powder in the waste coolant to separate the coolant from the ultrafine silicon powder;

[0072] The separation part 2 is used for solid-liquid separation of the mixed waste coolant and the adsorption material, so as to facilitate the subsequent treatment of the separated coolant and the separated adsorption material respectively;

[0073] The ion exchange part 6 is used to perform ion exchange on the separated liquid to remove ions and reduce the conductivity to obtain a regenerated coolant, which is a recyclable high-quality coolant so that the coolant can be used again;

[0074] The conditioning and stirring part 3 is used to mix the separated solid with the alkaline solution to desorb the ultrafine silicon powder and the adsorption material, so that the ultrafine silicon powder and the adsorption material are separated, so that the separated ultrafine silicon powder and the separated adsorption material can be processed separately in the future;

[0075] The screening part 4 is used to screen and filter the desorbed solid to separate the ultrafine silicon powder and the adsorption material;

[0076] The filter press section 5 is used to filter and dehydrate the separated ultrafine silicon powder to obtain recyclable high-purity ultrafine silicon powder;

[0077] The regeneration stirring part 7 is used to mix the separated adsorbent material with the acid solution to regenerate the adsorbent material so that the adsorbent material can be used again;

[0078] The adsorption and stirring section 1, the separation section 2, the tempering and stirring section 3, the screening section 4 and the filter press section 5 are connected in sequence, and the separation section 2 is connected to the ion exchange section 6, and the screening section 4 is connected to the regeneration and stirring section 7. The waste coolant and the adsorption material are mixed and separated, and the separated coolant is ion exchanged to obtain recyclable high-quality regenerated coolant. At the same time, the separated solid is tempered and screened to obtain ultrafine silicon powder and adsorption material, the ultrafine silicon powder is filter-filtered to obtain high-purity ultrafine silicon powder, and the adsorption material is regenerated to obtain regenerated adsorption material, thereby completing the recovery of the waste coolant.

[0079] The above-mentioned adsorption stirring section 1, conditioning stirring section 3 and regeneration stirring section 7 are all stirring tanks, which are commercially available products and are selected according to actual needs. No specific requirements are made here.

[0080] Among them, the stirring speed of the adsorption stirring part 1 is 80-120r / min, and the speed of the stirring tank can be 80r / min, 90r / min, 100r / min, 110r / min or 120r / min, which is selected according to actual needs. No specific requirements are made here.

[0081] The stirring speed of the tempering and stirring part 3 is 150-200r / min. The stirring speed can be 150r / min, 160r / min, 170r / min, 180r / min, 190r / min or 200r / min. It is selected according to actual needs and no specific requirements are made here.

[0082] The stirring speed of the regeneration stirring part 7 is 80-120r / min. The stirring speed can be 80r / min, 90r / min, 100r / min, 110r / min or 120r / min. It is selected according to actual needs and no specific requirements are made here.

[0083] The separation part 2 is a centrifuge, the centrifugal speed of the centrifuge is 2500-3500 r / min, and the centrifugal time is 10-20 s. The centrifugal speed of the centrifuge can be 2500 r / min, 2700 r / min, 3000 r / min, 3200 r / min or 3500 r / min, which is selected according to actual needs, and no specific requirements are made here.

[0084] The centrifugation time can be 10s, 12s, 14s, 16s, 18s or 20s, which can be selected according to actual needs. No specific requirements are made here.

[0085] The above-mentioned centrifuge is a commercially available product and is selected according to actual needs. No specific requirements are made here.

[0086] In this embodiment, the ion exchange part 6 is preferably a centrifugal exchange bed, and the centrifugal exchange bed is an anion resin exchange bed.

[0087] The screening part 4 is a rotary vibrating screen, and the screening particle size of the rotary vibrating screen is 90-120 μm. The screening particle size of the rotary vibrating screen is 90-120 μm, and the screening particle size can be 90 μm, 100 μm, 110 μm or 120 μm, which is selected according to actual needs, and no specific requirements are made here.

[0088] The filter press section 5 is a filter press, which is selected according to actual needs and no specific requirements are made here.

[0089] The following describes in detail some specific embodiments.

[0090] Example 1

[0091] like Figure 1The process route shown is to take 1t of cooling waste liquid used for silicon single crystal diamond wire slicing and place it in an adsorption stirring tank, add 6.0kg of adsorbent material manganese dioxide (particle size 150μm), stir and mix at 80r / min for 2min, so that the adsorbent material can fully adsorb the ultrafine silicon powder; transfer the cooling waste liquid containing the adsorbent material-ultrafine silicon powder composite into a centrifuge, treat it at a speed of 3500r / min for 20s, and complete solid / liquid separation; the separated cooling liquid is transferred to a 50L anion resin exchange bed, and the conductivity of the cooling liquid is reduced by removing ions to obtain high-quality regenerated cooling liquid; the separated solid is transferred to a tempering stirring tank, 40L of 4wt.% sodium hydroxide solution is added, and stirred at 150r / min for 5min to desorb the ultrafine silicon powder and the adsorbent material; then the material is transferred together to a rotary vibrating screen (screening particle size is 100μm) to separate the ultrafine silicon powder and the adsorbent material; the separated adsorbent material is transferred to a regeneration stirring tank, and 20L 4wt.% hydrochloric acid solution, stirred at 120r / min for 10min, to obtain regenerated adsorption material; the separated ultrafine silicon powder was transferred to the filtration device, filtered and recovered. The solid content and conductivity of the regenerated coolant were 0.14% and 17.8μS / cm respectively, the recovery rate of ultrafine silicon powder containing only 0.001%~0.01% chloride ions was 95.2%, and the recovery rate of adsorption material was 99.9%.

[0092] Example 2

[0093] like Figure 1 The process route shown is to take 1t of cooling waste liquid used for silicon single crystal diamond wire slicing and place it in an adsorption stirring tank, add 8.0kg of adsorbent material manganese dioxide (particle size 150μm), stir and mix at 100r / min for 2min, so that the adsorbent material can fully adsorb the ultrafine silicon powder; transfer the cooling waste liquid containing the adsorbent material-ultrafine silicon powder composite into a centrifuge, treat it at a speed of 3000r / min for 20s, and complete solid / liquid separation; the separated cooling liquid is transferred to a 50L anion resin exchange bed, and the conductivity of the cooling liquid is reduced by removing ions to obtain high-quality regenerated cooling liquid; the separated solid is transferred to a tempering stirring tank, 40L of 4wt.% sodium hydroxide solution is added, and stirred at 150r / min for 5min to desorb the ultrafine silicon powder and the adsorbent material; then the material is transferred to a rotary vibrating screen (screening particle size is 100μm) to separate the ultrafine silicon powder and the adsorbent material; the separated adsorbent material is transferred to a regeneration stirring tank, and 20L 4wt.% hydrochloric acid solution, stirred at 100r / min for 10min, to obtain regenerated adsorbent material; the separated ultrafine silicon powder was transferred to the filtration device, filtered and recovered. The solid content and conductivity of the regenerated coolant were 0.005% and 18.1μS / cm respectively, the recovery rate of ultrafine silicon powder was 99.4%, and the recovery rate of adsorbent material was 99.9%.

[0094] Example 3

[0095] like Figure 1 The process route shown is to take 1t of cooling waste liquid used for silicon single crystal diamond wire slicing and place it in an adsorption stirring tank, add 8.0kg of adsorption material anion exchange resin (particle size 200μm), stir and mix at 120r / min for 2min, so that the adsorption material can fully adsorb the ultrafine silicon powder; transfer the cooling waste liquid containing the adsorption material-ultrafine silicon powder composite into a centrifuge, treat it at a speed of 2500r / min for 20s, and complete solid / liquid separation; the separated cooling liquid is transferred to a 50L anion resin exchange bed, and the conductivity of the cooling liquid is reduced by removing ions to obtain high-quality regenerated cooling liquid; the separated solid is transferred to a tempering stirring tank, 40L of 4wt.% sodium hydroxide solution is added, and stirred at 200r / min for 3min to desorb the ultrafine silicon powder and the adsorption material; then the material is transferred to a rotary vibrating screen (screening particle size is 100μm) to separate the ultrafine silicon powder and the adsorption material; the separated adsorption material is transferred to a regeneration stirring tank, and 20L 4wt.% hydrochloric acid solution, stirred at 100r / min for 10min, to obtain regenerated adsorbent material; the separated ultrafine silicon powder was transferred to the filtration device, filtered and recovered. The solid content and conductivity of the regenerated coolant were 0.005% and 18.0μS / cm respectively, the ultrafine silicon powder recovery rate was 92.9%, and the adsorbent material recovery rate was 99.9%.

[0096] Example 4

[0097] like Figure 1The process route shown is to take 1t of cooling waste liquid used for silicon single crystal diamond wire slicing and place it in an adsorption stirring tank, add 8.0kg of adsorption material anion exchange resin (particle size 1200μm), stir and mix at 120r / min for 2min, so that the adsorption material can fully adsorb the ultrafine silicon powder; transfer the cooling waste liquid containing the adsorption material-ultrafine silicon powder composite into a centrifuge, treat it at a speed of 3500r / min for 10s, and complete solid / liquid separation; the separated cooling liquid is transferred to a 50L anion resin exchange bed, and the conductivity of the cooling liquid is reduced by removing ions to obtain high-quality regenerated cooling liquid; the separated solid is transferred to a tempering stirring tank, 40L of 4wt.% sodium hydroxide solution is added, and stirred at 200r / min for 5min to desorb the ultrafine silicon powder and the adsorption material; then the material is transferred to a rotary vibrating screen (screening particle size is 100μm) to separate the ultrafine silicon powder and the adsorption material; the separated adsorption material is transferred to a regeneration stirring tank, and 20L 4wt.% hydrochloric acid solution, stirred at 120r / min for 10min, to obtain regenerated adsorbent material; the separated ultrafine silicon powder was transferred to the filtration device, filtered and recovered. The solid content and conductivity of the regenerated coolant were 0.003% and 17.9μS / cm respectively, the recovery rate of ultrafine silicon powder was 99.4%, and the recovery rate of adsorbent material was 99.9%.

[0098] The above-mentioned multiple embodiments are analyzed. In multiple embodiments, when the separated solid is transferred to the conditioning stirring tank, 40L of 4wt.% sodium hydroxide solution is added, and when the separated adsorbent material is transferred to the regeneration stirring tank, 20L of 4wt.% hydrochloric acid solution is added. The sieve particle size of the rotary vibrating screen is 100μm.

[0099]

[0100] It can be seen from the above table that with the increase of the particle size of the adsorption material, the adsorption stirring speed, the adsorption stirring time, the centrifugal speed, the centrifugal time, the tempering stirring speed, the tempering stirring time, the regeneration stirring speed and the regeneration stirring time, the solid content of the regenerated coolant decreases, the conductivity of the regenerated coolant remains basically unchanged, the recovery rate of the ultrafine silicon powder increases, and the recovery rate of the adsorption material remains basically unchanged; therefore, when recycling the coolant for silicon single crystal diamond wire slicing, the adsorption material and the particle size of the adsorption material, the adsorption stirring speed and stirring time, the tempering stirring speed and stirring time, the regeneration stirring speed and stirring time can be reasonably selected to obtain the regenerated coolant, ultrafine silicon powder and regenerated adsorption material that meet the use requirements, thereby realizing the recycling and reuse of the waste coolant, ultrafine silicon powder and adsorption material.

[0101] Due to the adoption of the above technical scheme, the adsorption material and the waste coolant are stirred and mixed, and then centrifuged, the adsorption material adsorbs the ultrafine silicon powder in the waste coolant, so that the ultrafine silicon powder is separated from the coolant, and then the coolant and the ultrafine silicon powder are treated separately to obtain regenerated coolant and ultrafine silicon powder, and the adsorption material is treated at the same time to obtain regenerated adsorption material, so that the coolant and the adsorption material can be reused, and the high-purity ultrafine silicon powder can be recovered, which reduces the operating cost, and a large amount of waste coolant can be recycled with less adsorption material, so that high-quality coolant and high-purity ultrafine silicon powder can be obtained, the recovery process is advanced, the adsorption material used in the recovery process is small in amount and renewable, and the overall operating cost is 1 / 3-1 / 5 of that of the existing technical method.

[0102] The embodiments of the present invention are described in detail above, but the contents described are only preferred embodiments of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A process for recovering coolant for silicon single crystal diamond wire slicing, Features: The following steps are involved: Mixing the waste coolant with the adsorption material for induced adsorption, and the ultrafine silicon powder in the waste coolant is adsorbed by the adsorption material; in the step of mixing the waste coolant with the adsorption material for induced adsorption, the weight ratio of the adsorption material to the waste coolant is 1:100-1:250; performing solid-liquid separation on the mixed waste coolant and the adsorption material; The separated liquid is subjected to ion exchange to obtain a regenerated coolant; The separated solid is mixed with an alkali solution to desorb the ultrafine silicon powder from the adsorbent material; in the step of mixing the separated solid with the alkali solution to desorb the ultrafine silicon powder from the adsorbent material, the alkali solution is a sodium hydroxide solution or a potassium hydroxide solution with a mass fraction of 4-6wt%; The desorbed solid is screened and filtered to separate the ultrafine silicon powder and the adsorption material; The separated ultrafine silicon powder is filtered and dehydrated to obtain high-purity ultrafine silicon powder; mixing the separated adsorbent material with an acid solution to obtain a regenerated adsorbent material, wherein in the step of mixing the separated adsorbent material with the acid solution, the acid solution is a hydrochloric acid solution having a mass fraction greater than 3 wt %; The adsorption material is a mineral material or a polymer material. The mineral material is manganese dioxide, and the polymer material is an anion exchange resin.

2. The process for recovering coolant for silicon single crystal diamond wire slicing according to claim 1, Features: The waste coolant and the adsorption material are stirred and mixed in an adsorption stirring tank, the stirring speed of the adsorption stirring tank is 80-120 r / min, and the stirring time is 1-3 min.

3. The process for recovering coolant for silicon single crystal diamond wire slicing according to claim 1, Features: The separated solid and the alkali solution are stirred and mixed in a tempering stirring tank, the stirring speed of the tempering stirring tank is 150-200r / min, and the stirring time is 3-5min.

4. The process for recovering coolant for silicon single crystal diamond wire slicing according to any one of claims 1 to 3, Features: The acid solution is a hydrochloric acid solution with a mass fraction of 4-6 wt%.

5. The process for recovering coolant for silicon single crystal diamond wire slicing according to claim 4, Features: The separated adsorption material and the acid solution are stirred and mixed in a regeneration stirring tank, the stirring speed of the regeneration stirring tank is 80-120 r / min, and the stirring time is 5-10 min.

6. The process for recovering coolant for silicon single crystal diamond wire slicing according to claim 1, Features: The particle size of the adsorption material is 100-2000 μm.

7. The process for recovering coolant for silicon single crystal diamond wire slicing according to any one of claims 1 to 3 and 5 to 6, Features: In the step of performing solid-liquid separation on the mixed waste coolant and the adsorption material, the solid-liquid separation is performed in a centrifuge, the centrifugal speed of the centrifuge is 2500-3500 r / min, and the centrifugal time is 10-20 s.

8. The process for recovering coolant for silicon single crystal diamond wire slicing according to any one of claims 1 to 3 and 5 to 6, Features: In the step of subjecting the separated liquid to ion exchange, the separated liquid is subjected to ion exchange in a centrifugal exchange bed, and the centrifugal exchange bed is an anion resin exchange bed.

9. The process for recovering coolant for silicon single crystal diamond wire slicing according to any one of claims 1 to 3 and 5 to 6, Features: In the step of screening and filtering the desorbed solid to separate the ultrafine silicon powder and the adsorption material, the desorbed solid is screened and filtered in a rotary vibrating screen, and the screening particle size of the rotary vibrating screen is 90-120 μm.

10. The process for recovering coolant for silicon single crystal diamond wire slicing according to any one of claims 1 to 3 and 5 to 6, Features: In the step of filtering and dehydrating the separated ultrafine silicon powder, the separated ultrafine silicon powder is filtered and dehydrated in a filter press.

Citation Information

Patent Citations

  • Method for recovering water-soluble cutting fluid from silicon wafer cutting fluid

    CN102746934A

  • Processing method for fluoride waste water in production of solar cells

    CN103011453A

  • Recovery method and system for waste cooling liquids produced during diamond wire cutting

    CN105174522A

  • Diamond wire slicing cooling liquid integrated treatment method for sapphire and silicon wafers

    CN106378876A

  • Diamond wire cutting silicon chip coolant liquid recovery system

    CN204792698U