Working electrode for electrochemical research of pipe scale, preparation method thereof and electrochemical device

By designing an electrochemical device for inert platinum sheet electrode and tubular scale layer, the problem of difficulty in studying the cathode electrochemical process of iron pipes in the prior art is solved, and the accurate test and analysis of tubular electrochemical reactions are achieved, and the prevention of tubular pipes is provided Research methods for iron release.

CN115201291BActive Publication Date: 2024-11-15RES INST FOR ENVIRONMENTAL INNOVATION SUZHOU TSINGHUA +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202210554106.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-20
Publication Date
2024-11-15
Estimated Expiration
2042-05-20

AI Technical Summary

Technical Problem

The prior art is difficult to directly study the electrochemical process of pipe scale in iron pipes, especially the iron oxide reduction reaction on the cathode side, which makes it difficult to understand and prevent the risk of iron release in pipelines.

Method used

A working electrode for electrochemical research on tube scale was designed, including an inert platinum sheet electrode, whose surface was coated with actual iron tube scale or its components, and graphite and perfluorosulfonic acid-based polymer were added as binder. , the formed electrochemical device can be electrochemically tested through a three-electrode system to study the cathode reaction characteristics.

Benefits of technology

This working electrode can reflect the pipe scale reduction process in actual iron pipes, has good conductivity and reaction performance, provides sensitive electrical signals and accurate test results, independently studying the characteristics of cathode pipe scale or iron oxides to avoid It is dependent on the anode reaction and is suitable for a variety of electrochemical studies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115201291B_ABST
    Figure CN115201291B_ABST
Patent Text Reader

Abstract

The present invention discloses a working electrode for electrochemical research of pipe scale, a preparation method thereof and an electrochemical device, wherein the working electrode comprises an inert platinum sheet electrode, at least one side surface of the inert platinum sheet electrode is provided with a pipe scale layer, the pipe scale layer contains actual iron pipe scale or at least one iron pipe scale component, and the corresponding preparation method is: taking a certain mass of iron pipe scale powder or iron pipe scale simulation powder containing at least one iron pipe scale component as a base powder, coating a suspension containing the base powder, graphite powder and a binder on the inert platinum sheet electrode, and the working electrode is applied to an electrochemical device of a three-electrode system, and the electrochemical device also comprises an inert platinum sheet auxiliary electrode and an Ag / AgCl reference electrode. The working electrode prepared by the present invention has good electrical conductivity and reaction performance, can obtain sensitive electrical signals in electrochemical tests, and is helpful for studying the cathode characteristics of the reduction reaction of complex iron pipe scale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electrochemical research on water supply pipelines, and in particular relates to a working electrode for electrochemical research on pipe scale, a preparation method thereof and an electrochemical device. Background Art

[0002] Iron pipes are the most widely used pipe material in municipal water supply pipelines. They have the advantages of high strength, long service life and relatively low cost. However, corrosion and scaling of pipes are inevitable during the water delivery process. Corrosion and a series of physical and chemical reactions gradually form stable pipe scale. Although it inhibits the occurrence of corrosion to a certain extent, it is still an important source of risk of iron release in the pipeline network.

[0003] Existing material characterization research methods have proved that fully developed iron pipe scale presents a distinct layered structure, which is divided from the inside to the outside into the iron pipe substrate, a relatively thick porous loose inner core layer, a relatively thin dense hard shell layer, and an attached surface layer. The pipeline substrate is common iron pipes such as cast iron, ductile iron or stainless steel. The composition of the porous inner core layer is relatively complex, which is a solid-liquid phase mixture, including trivalent iron compounds β-FeOOH, γ-FeOOH, Fe(OH)3, γ-Fe2O3, etc., divalent iron compounds Fe(OH)2, FeCO3, etc., and mixed valence compounds such as green rust (a class of highly active basic carbonate complexes), etc. The main components of the hard shell layer are Fe3O4, α-FeOOH and α-Fe2O3, etc., which are more dense and more stable in nature. The outermost surface layer is composed of CaCO3, Mg(OH)2 and some amorphous aluminosilicates. The rigid structure of the hard shell layer ensures the stability of the shape of the pipe scale. However, since the pipe scale cannot completely prevent the corrosion reaction, as the iron element in the pipeline substrate loses electrons and oxidizes, ferrous substances continue to enter the porous inner core layer, causing the accumulation of substances, resulting in greater pressure on the inside of the pipe scale than on the outside, creating a risk of pipe scale rupture to a certain extent.

[0004] Under normal circumstances, the hydraulic conditions (flow rate, flow direction, etc.) and water quality conditions (water temperature, pH, dissolved oxygen, residual chlorine, ion concentration, etc.) in the water supply pipeline remain stable, and the structure and properties of iron scale can also remain stable, which plays a role in blocking the surface of the pipeline and the water in the pipe network, inhibiting the occurrence of corrosion reactions, and also preventing the iron-containing substances in the porous inner core layer of the scale from entering the water in the pipe network, maintaining the stability of the water quality in the pipe network. However, when the operating state of the water supply pipeline changes, it may aggravate corrosion or cause the scale to become unstable, causing the iron in the pipe network to be released, causing the water color to turn yellow and the turbidity to increase, and in severe cases, it may also cause health risks.

[0005] The causes of iron release in pipe networks are complex and there are many influencing factors. One of the most important aspects is that when an oxygen-deficient environment appears in the pipeline, that is, the concentration of dissolved oxygen and residual chlorine is very low, and the redox potential of the water is very low, the iron oxides in the pipe scale will be reduced, which will cause the pipe scale to become thinner and the stability to decrease. When it reaches a certain level, it will cause the pipe scale to rupture, and a large amount of iron-containing substances inside the scale layer will dissolve, leading to iron release. In addition, the change of pipe scale also reduces its protective effect on the pipe wall, causing the corrosion rate to accelerate, which will also cause iron release. The above process was proposed by A. Kuch and is usually called the Kuch mechanism of iron release in pipe networks.

[0006] The process of iron oxide reduction in pipe scale expressed by the Kuch mechanism is essentially an electrochemical reaction process. For general corrosion reactions, the electrochemical nature is that iron loses electrons as the anode and is oxidized to ferrous ions, while the cathode is the dissolved oxygen or residual chlorine in the water that gains electrons and is reduced to hydroxide ions or chloride ions. Ferrous ions undergo a series of processes such as oxidation and precipitation to form pipe scale mainly containing trivalent iron. For the iron oxide reduction process expressed by the Kuch mechanism, the anode reaction is also iron losing electrons, but because the concentrations of dissolved oxygen and residual chlorine are very low, the trivalent iron oxide in the pipe scale becomes a new electron acceptor at this time, so the cathode reaction is the electron-gaining reduction of the trivalent iron oxide to produce ferrous ions. This process leads to changes in the composition of pipe scale, which in turn affects the stability of its structure and properties.

[0007] Since the structure of pipe scale itself is relatively complex and its composition is not uniform, it is a mixture of various crystalline and amorphous compounds. In addition, pipe scale grows on the wall of iron pipes and is difficult to study independently by separation. Therefore, the iron oxide reduction reaction occurring therein is difficult to directly examine. At present, the research methods related to the electrochemical process of corrosion and scaling of iron pipes are mainly focused on the anode metal side, and most of them regard the metal and the corrosion scale layer as a whole. There are almost no reports specifically studying the electrochemical process of pipe scale (cathode side). Therefore, it is urgent to take iron pipe scale as the research object and develop a working electrode, its preparation method and electrochemical device for electrochemical research of pipe scale. Summary of the invention

[0008] In view of the above-mentioned technical problems, the present invention provides a working electrode for electrochemical research on pipe scale, a preparation method and an electrochemical device thereof. The present invention takes iron pipe scale as the research object and provides research methods and means for the iron release caused by pipe scale destruction.

[0009] The technical solution of the present invention is:

[0010] The present invention provides a working electrode for electrochemical research of pipe scale, comprising an inert platinum sheet electrode, at least one side surface of the inert platinum sheet electrode is provided with a pipe scale layer, the pipe scale layer contains actual iron pipe scale or at least one iron pipe scale component, and the pipe scale layer also contains graphite and a binder.

[0011] Preferably, the iron pipe scale components include Fe3O4, α-FeOOH, γ-FeOOH, α-Fe2O3, and γ-Fe2O3, and the pipe scale layer contains at least one of Fe3O4, α-FeOOH, γ-FeOOH, α-Fe2O3, and γ-Fe2O3; and the binder is a perfluorosulfonic acid-based polymer.

[0012] Preferably, the thickness of the inert platinum sheet electrode is 0.20 mm, and the thickness of the pipe scale layer is 0.05 mm.

[0013] The present invention also provides a method for preparing the working electrode for the above-mentioned pipe scale electrochemical research, comprising the following steps:

[0014] S1. Take a certain mass of iron pipe scale powder or iron pipe scale simulation powder containing at least one iron pipe scale component as a base powder, mix the base powder with graphite powder in anhydrous ethanol, stir until the mixture is uniform, then add a binder solution, continue to stir evenly, and obtain a coating suspension;

[0015] S2, evenly coating the coating suspension on the inert platinum sheet electrode, so that it completely covers at least one side of the surface of the inert platinum sheet electrode, and the electrode surface after coating also remains flat;

[0016] S3. Place the coated electrode in a cool place to air dry naturally to obtain a working electrode for an electrochemical device.

[0017] Preferably, the preparation process of the iron pipe scale powder is as follows: the iron pipe scale on the iron pipe is peeled off from the pipe wall, carefully rinsed to remove the loosely attached sediments on the surface, and then dried and ground. The iron pipe scale powder needs to be ground into a fine powder that can pass through a 300-mesh sieve.

[0018] Preferably, the iron pipe scale simulation powder is one or a mixture of Fe3O4, α-FeOOH, γ-FeOOH, α-Fe2O3, γ-Fe2O3, and the iron pipe scale simulation powder needs to be ground into a fine powder that can pass through a 300-mesh sieve.

[0019] Preferably, the binder solution is a perfluorosulfonic acid-based polymer solution, and the mass fraction of the perfluorosulfonic acid-based polymer solution is 5%, 10% or 20%.

[0020] Preferably, the mass ratio of the base powder to the graphite powder is 1:0.5-2, the volume ratio of the perfluorosulfonic acid polymer solution to anhydrous ethanol is 1:100, and the amount of the base powder per milliliter of anhydrous ethanol is 0.02 g / mL.

[0021] The present invention also provides an electrochemical device, which is a three-electrode system electrochemical device, including the above-mentioned working electrode, and also including an inert platinum sheet auxiliary electrode, an Ag / AgCl reference electrode, a reaction container and an electrochemical workstation, wherein the reaction container is filled with an electrolyte solution, and the working electrode, the inert platinum sheet auxiliary electrode and the Ag / AgCl reference electrode are all connected to the electrochemical workstation through a wire, and the electrochemical workstation is also connected to a signal receiving and processing system. In the electrochemical device of the three-electrode system, including a working electrode provided with a pipe scale layer, the characteristics of its cathode reduction reaction, including reduction ability, reduction rate, cathode polarization, etc., can be studied by electrochemical testing methods such as constant potential polarization, constant current polarization, chronopotentiometry, chronoamperometry, cyclic voltammetry, etc.

[0022] Preferably, the electrolyte solution is one of tap water, chloride solution, sulfate solution and nitrate solution, and the concentration of the chloride solution, sulfate solution and nitrate solution is 0.1-50 mmol / L.

[0023] The beneficial effects of the present invention are:

[0024] (1) The present invention uses a working electrode provided with a pipe scale layer, the pipe scale layer contains actual iron pipe scale or iron pipe scale components, the electrochemical characteristics of the working electrode can reflect the reduction process of pipe scale in the actual iron pipeline, the working electrode has good electrical conductivity and reaction performance, can obtain sensitive electrical signals in electrochemical tests, and the test results are accurate;

[0025] (2) The present invention also provides an electrochemical device, which is a three-electrode system. The working electrodes used in general three-electrode systems are mostly metal single-electrode materials, such as iron sheets, zinc sheets, lead sheets, etc., and most of the research is on the characteristics of their anodic oxidation reactions. The working electrode of the electrochemical device of the invention uses a working electrode provided with a pipe scale layer, which can independently carry out research on cathode pipe scale or iron oxides without relying on anode reactions; the electrochemical device can be applied to a variety of different types of electrochemical research and has good test stability. The present invention can study the cathode characteristics of iron oxides in pipe scale through a variety of electrochemical tests to obtain more comprehensive and accurate test results. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:

[0027] Figure 1 is a working system diagram of the electrochemical device of the present invention;

[0028] Figure 2 Schematic diagram of the structure of the working electrode of the present invention;

[0029] Figure 3 The potential-current relationship curve of the constant potential polarization test of the working electrode prepared in Example 2;

[0030] Figure 4 The potential-time curve of the constant current chronopotentiometry performed on the working electrode prepared in Example 2.

[0031] The markings in the figure are: 1. working electrode; 11. inert platinum electrode; 12. pipe scale layer; 2. Ag / AgCl reference electrode; 3. inert platinum auxiliary electrode; 4. reaction vessel; 5. electrochemical workstation; 6. signal receiving and processing system. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0033] Example 1

[0034] (1) Take a 20-year-old grey cast iron water supply pipe, peel off a small piece of pipe scale at the corrosion and scaling of the inner wall of the pipe with a ceramic cutter, carefully rinse with tap water to remove the loose sediment attached to the surface, dry in a 40°C oven, and then grind in a mortar until it can pass through a 300-mesh sieve to obtain iron pipe scale powder;

[0035] (2) Take 0.10 g of finely ground iron pipe scale powder and mix it with 0.20 g of analytical pure graphite powder in 5 mL of anhydrous ethanol, stir until the two powders are evenly mixed, then add 50 μL of 5% perfluorosulfonic acid polymer solution (the solution is a standard product - DuPont Nafion solution) as a binder, continue to stir evenly, and obtain a coating suspension;

[0036] (3) Use a glass rod to dip the coating suspension and quickly and evenly apply it on a surface area of ​​1.0 cm 2 The inert platinum sheet electrode is coated with the coating to completely cover both sides of the inert platinum sheet substrate, and the coating thickness is uniform, and the electrode surface remains flat after coating;

[0037] (4) Place the coated electrode in a cool place to air dry for more than 10 minutes to obtain a working electrode for an electrochemical device. The thickness of the corresponding inert platinum sheet electrode is 0.20 mm, and the thickness of the pipe scale layer is 0.05 mm.

[0038] Example 2

[0039] (1) Grind analytically pure Fe3O4 powder until it can pass through a 300-mesh sieve;

[0040] (2) Take 0.10 g of finely ground Fe3O4 powder and mix it with 0.10 g of analytical pure graphite powder in 5 mL of anhydrous ethanol, stir until the two powders are evenly mixed, then add 50 μL of 5% perfluorosulfonic acid polymer solution (the solution is a standard product - DuPont Nafion solution) as a binder, continue to stir evenly, and obtain a coating suspension;

[0041] (3) Use a glass rod to dip the coating suspension and evenly apply it on a surface area of ​​1.0 cm 2 The inert platinum sheet electrode is coated with the coating so that it completely covers both sides of the inert platinum sheet electrode, and the coating thickness is uniform, and the electrode surface after coating also remains flat;

[0042] (4) The coated electrode was placed in a cool place to dry naturally for more than 10 minutes to obtain a working electrode for an electrochemical device. The thickness of the corresponding inert platinum sheet electrode was 0.20 mm, and the thickness of the pipe scale layer was 0.05 mm.

[0043] Comparative Example 1

[0044] (1) Take a 20-year-old grey cast iron water supply pipe, peel off a small piece of pipe scale at the corrosion and scaling location on the inner wall of the pipe with a ceramic cutter, carefully rinse with tap water to remove loose sediments attached to the surface, dry in a 40°C oven, and then grind in a mortar until it can pass through a 300-mesh sieve to obtain iron pipe scale powder;

[0045] (2) Using a powder tablet press, the above iron pipe scale powder was pressed into a circular tablet with a diameter of 1.0 cm and a thickness of 0.2 cm at a pressure of 10 MPa;

[0046] (3) The powder tablets are connected to copper wires using conductive glue to obtain working electrodes.

[0047] The working electrode structures prepared in Examples 1 and 2 are as follows: Figure 2 As shown, the working electrode prepared in Example 2 is selected as the working electrode for the electrochemical device, and the electrochemical device is an electrochemical device of a three-electrode system, such as Figure 1As shown, it includes the above-mentioned working electrode, an inert platinum sheet auxiliary electrode, an Ag / AgCl reference electrode, a reaction container and an electrochemical workstation. In order to better simulate the reduction reaction of pipe scale under actual conditions, tap water is filled in the reaction container as an electrolyte solution. The working electrode, the inert platinum sheet auxiliary electrode and the Ag / AgCl reference electrode are all connected to the electrochemical workstation through wires, and the electrochemical workstation is also connected to a signal receiving and processing system.

[0048] The characteristics of the working electrode prepared in Example 2 were studied by electrochemical testing methods of constant potential polarization and constant current chronopotentiometry. The corresponding potential-current relationship curve is shown in FIG. Figure 3 and Figure 4 As shown, Figure 3 This is the result of the constant potential polarization test. The range of the applied potential is -0.3 to 0.3 V (relative to the open circuit potential). It can be found that when the potential changes within a certain range, the current density remains almost unchanged, which is the "limiting current density", indicating that the electrochemical reaction occurring at this time is diffusion controlled and the applied potential does not affect the rate of the electrochemical reaction. By comparing the "limiting current density" of cathodes of different materials, the rate of the electrochemical reduction reaction at the cathode can be obtained. Figure 4 This is the result of the constant current chronopotentiometry test, with an applied current of 0.2 mA. By comparing the potentials of cathodes of different materials at the same current, we can get the reduction capacity of different iron oxides.

[0049] In addition, the working electrode prepared in Comparative Example 1 was also applied to Figure 1 In the electrochemical device shown, it was found that the conductivity of the working electrode was poor and a stable electrochemical signal could not be measured. In the preparation process of the working electrode of the present invention, an inert platinum sheet electrode is used as a basis, and a pipe scale layer is set on the surface of the inert platinum sheet electrode. In addition to iron pipe scale powder or iron pipe scale simulation powder, graphite powder and a conductive binder are added to the pipe scale layer. The pipe scale layer prepared by the uniform coating method of the present invention is also very small in thickness. The working electrode of the present invention has good conductivity and reaction performance at the same time, and the electrode area is small. A sensitive electrical signal can be obtained in the electrochemical test, and the test result is accurate.

[0050] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.

Claims

1. A working electrode for electrochemical research of pipe scale, characterized in that: The invention comprises an inert platinum sheet electrode, at least one side surface of which is provided with a pipe scale layer, the pipe scale layer contains actual iron pipe scale or at least one iron pipe scale component, and the pipe scale layer also contains graphite and a binder.

2. The working electrode for pipe scale electrochemical research according to claim 1, characterized in that: The iron pipe scale components include Fe3O4, α-FeOOH, γ-FeOOH, α-Fe2O3, and γ-Fe2O3; the pipe scale layer contains at least one of Fe3O4, α-FeOOH, γ-FeOOH, α-Fe2O3, and γ-Fe2O3; the binder is a perfluorosulfonic acid-based polymer.

3. The working electrode for scale electrochemical research according to claim 1, characterized in that: The thickness of the inert platinum sheet electrode is 0.20 mm, and the thickness of the pipe scale layer is 0.05 mm.

4. A method for preparing a working electrode for electrochemical research of pipe scale as claimed in claim 1, characterized in that: The steps include: S1. Take a certain mass of iron pipe scale powder or iron pipe scale simulation powder containing at least one iron pipe scale component as a base powder, mix the base powder with graphite powder in anhydrous ethanol, stir until the mixture is uniform, then add a binder solution, continue to stir evenly, and obtain a coating suspension; S2, evenly coating the coating suspension on the inert platinum sheet electrode, so that it completely covers at least one side of the surface of the inert platinum sheet electrode, and the electrode surface after coating also remains flat; S3. Place the coated electrode in a cool place to air dry naturally to obtain a working electrode for an electrochemical device.

5. The method for preparing a working electrode for electrochemical research of pipe scale according to claim 4, characterized in that: The preparation process of the iron pipe scale powder is as follows: the iron pipe scale on the iron pipe is peeled off from the pipe wall, carefully rinsed to remove the sediment loosely attached to the surface, and then dried and ground. The iron pipe scale powder needs to be ground into a fine powder that can pass through a 300-mesh sieve.

6. The method for preparing a working electrode for electrochemical research of pipe scale according to claim 4, characterized in that: The iron pipe scale simulation powder is one or a mixture of Fe3O4, α-FeOOH, γ-FeOOH, α-Fe2O3, γ-Fe2O3, and the iron pipe scale simulation powder needs to be ground into a fine powder that can pass through a 300-mesh sieve.

7. The method for preparing a working electrode for electrochemical research of pipe scale according to claim 4, characterized in that: The binder solution is a perfluorosulfonic acid-based polymer solution, and the mass fraction of the perfluorosulfonic acid-based polymer solution is 5%, 10% or 20%.

8. The method for preparing a working electrode for electrochemical research of pipe scale according to claim 7, characterized in that: The mass ratio of the base powder to the graphite powder is 1:0.5-2, the volume ratio of the perfluorosulfonic acid polymer solution to anhydrous ethanol is 1:100, and the amount of the base powder per milliliter of anhydrous ethanol is 0.02 g / mL.

9. An electrochemical device, characterized in that: The electrochemical device is a three-electrode system electrochemical device, including the working electrode as described in claim 1, and also including an inert platinum sheet auxiliary electrode, an Ag / AgCl reference electrode, a reaction container and an electrochemical workstation, the reaction container is filled with an electrolyte solution, the working electrode, the inert platinum sheet auxiliary electrode and the Ag / AgCl reference electrode are all connected to the electrochemical workstation through wires, and the electrochemical workstation is also connected to a signal receiving and processing system.

10. The electrochemical device according to claim 9, characterized in that The electrolyte solution is one of tap water, chloride solution, sulfate solution and nitrate solution, and the concentration of the chloride solution, sulfate solution and nitrate solution is 0.1-50 mmol / L.

Citation Information

Patent Citations

  • Oxygen evolution electrode material containing FeOOH and preparation method thereof

    CN102220601A

  • Method and device for evaluating scale inhibition performance of water treatment agent

    CN106770531A

  • Experimental simulation platform for studying electrochemical corrosion and pipe network water quality change of iron pipeline

    CN107941686A

  • Electrochemical device for simulating rapid formation of pipe scale and test method thereof

    CN110274940A

  • Electrochemical electrode for determining redox potential, has planar substrate containing ceramic oxide, glass ceramic or glass, potential serving board element made of platinum, contact pad and glass membrane having preset thickness

    DE102011118409A1