Modified sulfur and its production method

Through the melt polymerization of unsaturated fatty acids and sulfur, highly functional modified sulfur is produced, which solves the brittleness, environmental hazards and odor problems of traditional sulfur modifiers, and realizes the stable application and high performance of modified sulfur in road construction. .

CN115210178BActive Publication Date: 2024-12-03安必浩
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202080097705.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-01-20
Publication Date
2024-12-03
Estimated Expiration
2040-01-20

AI Technical Summary

Technical Problem

Traditional sulfur modifiers have the risk of explosive exothermic reactions, difficulty in controlling polymerization reactions, environmental hazards and odor problems, which limit their application in road construction.

Method used

The melt polymerization of unsaturated fatty acid-based modifiers and sulfur is used to terminate the reaction by controlling the temperature and viscosity to produce highly functional and environmentally friendly modified sulfur.

Benefits of technology

The high viscosity, chemical resistance, water resistance, fluid resistance and high functionality of modified sulfur are achieved, and the brittleness, environmental hazards and odor problems of traditional sulfur modifiers are solved. It is suitable for road construction and concrete compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115210178B_ABST
    Figure CN115210178B_ABST
Patent Text Reader

Abstract

The present specification relates to a modified sulfur and a preparation method thereof, wherein the modified sulfur comprises sulfur and a modifier, wherein the modifier is a modifier based on unsaturated fatty acid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to environmentally friendly modified sulfur and a method for producing the same. Background Art

[0002] Sulfur is a substance with a flash point of 207°C and an autoignition temperature of 245°C. It is flammable and easily burns when its surface is exposed to and in contact with air. Sulfur is not only natural sulfur derived from nature, but is also usually generated during the desulfurization process of crude oil or natural gas.

[0003] If sulfur itself has no defects, stable solid-phase sulfur has high strength, while solid-phase sulfur formed by cooling and solidifying liquid-phase sulfur generally exists as a mixture of the following three types of forms, namely, orthorhombic, monoclinic, and amorphous forms. In the case of solidified solid-phase sulfur, the mixing ratio of the three types of forms varies with cooling conditions, and the solidified sulfur itself may become defective and brittle (with brittleness) over time. Therefore, the application range of pure sulfur is very limited.

[0004] Although pure sulfur can be applied to a variety of construction and civil engineering materials, its application alone has limitations due to the above characteristics. Specifically, sulfur materials with brittle fracture characteristics are unstable materials, similar to typical Portland cement, in which almost no plastic deformation occurs, so all the forces applied to the material are used for destruction, resulting in instantaneous failure when the applied force is higher than the yield strength.

[0005] In order to solve these disadvantages, various types of sulfur modifiers are being considered. In particular, dicyclopentadiene (DCPD) is known to have high economic feasibility due to its low cost and is also effective in improving the brittleness of sulfur.

[0006] However, it is well known that the polymerization reaction of dicyclopentadiene and sulfur itself is difficult to control and there is a risk of explosive exothermic reaction, and the temperature and viscosity increase rapidly during the reaction.

[0007] In particular, when the polymerization reaction is carried out beyond an appropriate degree, it is known that a rubberization phenomenon may occur, thereby damaging the reactor used for the polymerization reaction, which makes the commercial use of the sulfur modifier made of a dicyclopentadiene-based modifier and sulfur very difficult. In addition, due to the supercooling phenomenon after the polymerization reaction, the production and application efficiency of dicyclopentadiene and sulfur is low, and there are difficulties in practical application in road construction due to the presence of environmental hazard problems and disgusting odors. In addition, due to the influence of external temperature, dicyclopentadiene and sulfur are difficult to maintain constant quality, so there are difficulties in unstable work after construction, such as cracking, sinking, etc.

[0008] [Prior art literature]

[0009] [Patent Document]

[0010] Korean Patent Publication No. 10-2014-0000160 Summary of the invention

[0011] Technical issues

[0012] The present invention aims to develop modified sulfur produced using environmentally friendly materials, which has high functionality to solve the problems of traditional modified sulfur, such as factors harmful to the environment, odor, etc.

[0013] Technical Solution

[0014] One aspect of the present specification provides modified sulfur including sulfur and a modifier, wherein the modifier is an unsaturated fatty acid-based modifier.

[0015] Another aspect of the present specification provides a method for producing modified sulfur, which includes: a first step of mixing sulfur and an unsaturated fatty acid-based modifier; a second step of introducing the mixture into a reactor and melting it by heating at a temperature of 100°C or higher and 130°C or lower; a third step of raising the temperature of the molten mixture to 130°C or higher and 200°C or lower; and a fourth step of terminating the reaction when the viscosity of the molten mixture reaches 6000 cP or higher and 25000 cP or lower at 160°C.

[0016] Another aspect of the present specification provides a concrete composition including the modified sulfur and aggregate.

[0017] Beneficial Effects

[0018] The modified sulfur according to an embodiment of the present specification is environmentally friendly because a petroleum-derived modifier is excluded or minimized and replaced with a natural-derived modifier when producing the modified sulfur.

[0019] Furthermore, the modified sulfur according to one embodiment of the present specification exhibits high functionality, that is, excellent properties in terms of adhesive strength, chemical resistance, flame retardancy, waterproofness, corrosion resistance, water tightness, anti-flowability, balance resistance, and the like. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 is a flow chart illustrating a method of producing modified sulfur according to one embodiment of the present specification.

[0021] Figure 2 is a graph showing the results of a wheel tracking test of Example 1, Comparative Example 1-2, and Comparative Example 1-3.

[0022] Figure 3It is a graph which measured the moisture absorption rate of Example 4-1 and Comparative Example 4-1.

[0023] Figure 4 An image comparing the chemical resistance of Examples 5-1 to 5-3 and Comparative Example 5-1 is shown.

[0024] Figure 5 is a photographic image (x750) of a modified sulfur microstructure according to one embodiment of the present specification. DETAILED DESCRIPTION

[0025] The advantages and features of the present invention and the methods for achieving the advantages and features will be apparent through the exemplary embodiments described in detail below with reference to the accompanying drawings. However, the present invention is not limited to the exemplary embodiments described below and can be implemented in various different forms. On the contrary, exemplary embodiments are provided to thoroughly and completely disclose the present invention and to fully inform the scope of the present invention to those of ordinary skill in the art to which the present invention belongs, and the present invention is defined only by the scope of the claims. Throughout the specification, the same reference numerals indicate the same elements.

[0026] Meanwhile, unless otherwise defined, all terms used herein, including technical or scientific terms, should be interpreted as having the same meaning as commonly understood by those of ordinary skill in the art to which the present invention belongs. Therefore, unless explicitly defined herein, terms such as those defined in commonly used dictionaries should not be interpreted in an unrealistic or excessive sense.

[0027] Throughout the specification, unless otherwise stated, when a part “includes” an element, it may further include another element, rather than excluding the presence of the other element.

[0028] Hereinafter, the present invention will be described in more detail.

[0029] Modified sulfur

[0030] One aspect of the present invention provides modified sulfur including sulfur and a modifier, wherein the modifier is an unsaturated fatty acid-based modifier.

[0031] According to one embodiment of the present invention, the viscosity of the modified sulfur at room temperature is 4000 cP or more and 25000 cP or less. Specifically, according to one embodiment of the present specification, the viscosity of the modified sulfur at room temperature may be 6000 cP or more and 10000 cP or less.

[0032] In this specification, sulfur includes common sulfur, examples of which include natural sulfur, sulfur obtained by desulfurization of petroleum or natural gas, etc. As the sulfur of the present invention, solid sulfur heated to a temperature above its melting point to promote the reaction may be used, or liquid sulfur discharged in related industries such as petrochemical products, etc. may be used. In addition, sulfur obtained by simply filtering waste sulfur containing impurities discharged from a steel plant may be used.

[0033] In the present specification, the unsaturated fatty acid-based modifier may refer to a compound including at least one carboxylic acid group and at least one carbon-carbon double bond therein.

[0034] According to one embodiment of the present specification, the unsaturated fatty acid-based modifier can be a material obtained by using fatty acids or unsaturated fatty acids, and then recycling the used fatty acids or unsaturated fatty acids, or a material derived from nature. Therefore, as described in one aspect of the present specification, the case of including the unsaturated fatty acid-based modifier is environmentally friendly compared to the conventional case of including a petroleum-derived modifier.

[0035] According to one embodiment, the modifier is one or two or more selected from the group consisting of erucic acid, palmitoleic acid, elaidic acid, myristic acid, linoleic acid, arachidonic acid, gondoic acid, oleic acid, eicosapentaenoic acid, docosahexaenoic acid (DHA), α-linolenic acid, γ-linolenic acid (GLA) and vegetable oil.

[0036] According to one embodiment, the vegetable oil can be selected from the group consisting of oils extracted from natural plant oils, such as Chamaecyparis obtusa oil, lemon oil, rose oil, lavender oil, sunflower seed oil, corn oil, mustard oil, castor oil, olive oil, cottonseed oil, Macadamia integrifolia oil, linseed oil, pine oil, Hippophae rhamnoides oil, Lunaria biennis oil, rapeseed oil, and the like.

[0037] According to the embodiment of this specification, based on 100 parts by weight of sulfur, the amount of the modifier included is 10 parts by weight or more and 450 parts by weight or less. Specifically, based on 100 parts by weight of sulfur, the amount of the modifier included can be 30 parts by weight or more and 300 parts by weight or less. When the content of the modifier is less than 10 parts by weight based on 100 parts by weight of sulfur, it may be difficult to keep the liquid phase after synthesis and expect the functionality of modified sulfur, and the brittleness of sulfur also still exists, which causes difficulty in use. On the other hand, when the content of the modifier is more than 450 parts by weight based on 100 parts by weight of sulfur, although the brittleness of sulfur is not retained, the functionality of modified sulfur, such as water resistance, corrosion resistance, adhesion, chemical resistance, etc., may be significantly reduced.

[0038] According to one embodiment, the modified sulfur exhibits spinnability. In the present invention, spinnability may be expressed as the ability to be spun, etc., and the presence or absence of spinnability is determined by an experiment in which, in the process of producing modified sulfur, a glass rod is immersed in and taken out of a mixture or a reaction product in a solution state, and when a phenomenon is observed that a part of the mixture or the reaction product in a solution state is continuously spun like a thread when connected to a glass rod (1 cm or more), the mixture or the reaction product can be defined as having spinnability.

[0039] According to one embodiment, the modified sulfur has a mesh structure or a honeycomb structure. Since the modified sulfur according to one embodiment of the present specification includes an unsaturated fatty acid-based modifier, the double bonds in the unsaturated fatty acid-based modifier can be cross-linked by polymerization to have a honeycomb structure or a mesh structure. In this case, the functionality of the modified sulfur can be enhanced, such as bonding strength, chemical resistance, flame retardancy, corrosion resistance, water tightness, anti-flowability, high strength, etc.

[0040] Figure 5 is a photographic image (x750) of a modified sulfur microstructure according to one embodiment of the present specification. Figure 5 It can be seen that the modified sulfur according to one embodiment of the present specification has a microstructure, specifically, the modified sulfur according to one embodiment of the present specification has a fiber structure.

[0041] According to one embodiment, the modified sulfur has amphiphilicity.Since the modified sulfur according to one embodiment of the present specification includes an unsaturated fatty acid-based modifier, amphiphilic modified sulfur may be provided.

[0042] Rusty and corroded metal surfaces require anti-corrosion treatment, and structures such as buildings require waterproofing to prevent leakage and cracking and enhance durability. Since conventional waterproofing and anti-corrosion materials have limitations in repeated coating formation, workability, environmental risks, etc., and exhibit low durability due to low chemical resistance and low bonding strength, there is a need to improve the life of the product.

[0043] Although high-viscosity rubberized solid-phase modified sulfur has sufficiently high chemical resistance and bonding strength to serve as a substitute for epoxy fiber reinforced plastic (FRP), a separate device for high-temperature pretreatment (e.g., a heated sprayer) is required to melt the modified sulfur in order to use the modified sulfur in the construction and repair / reinforcement of structures such as concrete structures or tunnel structures.

[0044] The modified sulfur according to one embodiment of the present specification may be an amphiphilic modified sulfur having both hydrophilicity and hydrophobicity. Due to the hydrophobicity, the modified sulfur can be used in a polymer concrete composition for paving and repairing / reinforcing roads by simply mixing the liquid phase modified sulfur and aggregate at room temperature without preheating and heating processes. In addition, due to the hydrophilicity, the modified sulfur can be used in an ordinary Portland cement working solution by adding water, aggregate, modified sulfur binder and hydraulic material (e.g., trace water reducer, defoamer, release agent, etc.) and mixing them at room temperature without preheating and heating processes.

[0045] According to one embodiment of the present specification, the modified sulfur may be in a liquid phase. In this case, high miscibility and high dispersibility with the material are exhibited, a separate heating process is not required when blended with the hydraulic material, and a high modification effect can be achieved even with a small amount. However, as required, the modified sulfur may be variously modified and may be applied in various forms, such as in a solid phase, a granular form, a powder form, etc.

[0046] According to one embodiment, the modified sulfur further comprises a second modifying agent different from the unsaturated fatty acid based modifying agent.

[0047] According to one embodiment, the second modifier may be one or two or more selected from the group consisting of a saturated fatty acid-based modifier, an unsaturated fatty acid-based modifier, an alcohol-based modifier, an ester-based modifier, and a dicyclopentadiene-based modifier.

[0048] Depending on the field of application, a second modifier may optionally be added in the synthesis of the modified sulphur.

[0049] According to an embodiment of the present specification, the saturated fatty acid-based modifier may be stearic acid, palmitic acid, etc., but the present invention is not limited thereto.

[0050] According to an embodiment of the present specification, the unsaturated fatty acid-based modifier may be oleic acid or the like, but the present invention is not limited thereto.

[0051] According to an embodiment of the present specification, the alcohol-based modifier may be glycerin or the like, but the present invention is not limited thereto.

[0052] According to an embodiment of the present specification, the ester-based modifier may be wax ester, dihydrocholesterol oleate, and the like, but the present invention is not limited thereto.

[0053] In this specification, the dicyclopentadiene-based modifier refers to a dicyclopentadiene-based modifier containing cyclopentadiene oligomers. Dicyclopentadiene (DCPD) is a dimer of cyclopentadiene (CPD) and can be produced during the pyrolysis of naphtha. Any commercially available product, as long as it includes dicyclopentadiene, can be used.

[0054] Specifically, the dicyclopentadiene-based modifier can be: 1) dicyclopentadiene (DCPD); 2) a mixture of dicyclopentadiene and at least one selected from the group consisting of cyclopentadiene (CPD), DCPD derivatives and CPD derivatives (methylcyclopentadiene (MCP), methyldicyclopentadiene (MDCP)); and 3) a mixture of 1) or 2) and at least one selected from the group consisting of olefin compounds (e.g., dipentene, vinyltoluene, styrene monomer, dicyclopentene, etc.).

[0055] According to an embodiment of the present specification, the amount of the second modifier included can be 0.01 parts by weight or more and 300 parts by weight or less based on 100 parts by weight of sulfur. The content range of the second modifier can be widely adjusted according to the application area of ​​the modified sulfur, specifically according to properties such as adhesion, hydrophobicity, water resistance, corrosion resistance, etc.

[0056] Specifically, when a dicyclopentadiene-based modifier is used as the second modifier, based on 100 parts by weight of sulfur, the amount of the dicyclopentadiene-based modifier included is 0.01 parts by weight or more and 5 parts by weight or less. In addition, when a saturated fatty acid-based modifier, an unsaturated fatty acid-based modifier, an alcohol-based modifier, or an ester-based modifier is used as the second modifier, based on 100 parts by weight of sulfur, the amount of the second modifier included is 10 parts by weight or more and 300 parts by weight or less.

[0057] In the case of using a dicyclopentadiene-based modifier as the second modifier, when the content of the dicyclopentadiene-based modifier is less than 0.01 parts by weight based on 100 parts by weight of sulfur, it is difficult to provide modified sulfur with desired functionality, and when the content of the dicyclopentadiene-based modifier is more than 5 parts by weight based on 100 parts by weight of sulfur, modified sulfur with desired functionality can be provided, but due to environmental risks and disgusting odors, it is difficult to use modified sulfur on site. More specifically, in the case of using dicyclopentadiene (DCPD) as the second modifier, when the content of DCPD is more than 100 parts by weight based on 100 parts by weight of sulfur, it is not easy to synthesize modified sulfur due to the peeling and cracking of DCPD during the synthesis reaction, and although the viscosity after synthesis is 10000 cP or more, the modified sulfur is in a solid phase after cooling, so it is difficult to use without heating, and due to the disgusting odor, it is almost impossible to apply it on site.

[0058] According to an embodiment of the present specification, the modified sulfur may further include one or two or more selected from the group consisting of an initiator, a surfactant, a coupling agent, a catalyst, an additive, a cross-linking agent, and a dispersant.

[0059] Specifically, the initiator, surfactant, coupling agent, catalyst, additive, crosslinking agent and dispersant are not particularly limited as long as they do not interfere with the polymerization reaction of the modified sulfur of the present invention and are materials generally classified under the above names. The initiator, surfactant, coupling agent, catalyst, additive, crosslinking agent and dispersant can be used to enhance the dispersion of the modified sulfur, form hydrophilic or hydrophobic reactive groups in the modified sulfur, and inhibit or promote crosslinking in the modified sulfur produced by the polymerization reaction.

[0060] According to an embodiment of the present specification, the initiator can be one or two or more selected from the group consisting of sulfur, modified sulfur, asphalt, sulfide, polysulfide and hydrocarbon compounds. The initiator can be added simultaneously with the modifier or added separately during the reaction. When the initiator is sulfur, sulfur can be added during the reaction and applied as an initiator.

[0061] As an initiator, sulfur can be elemental sulfur, crystalline sulfur, amorphous sulfur, colloidal sulfur, or a mixture thereof. In addition, sulfur can be any one selected from the group consisting of α-sulfur (orthorhombic sulfur), β-sulfur (monoclinic sulfur), γ-sulfur and a combination thereof. Asphalt refers to straight-run asphalt or modified asphalt, and sulfide can be a sulfur-containing compound, such as carbon disulfide, etc., but the present invention is not limited thereto. Polysulfide can be a polysulfide-modified epoxy resin, etc., but the present invention is not limited thereto. Hydrocarbon compounds refer to compounds composed of carbon and hydrogen, and include straight-chain, branched, cyclic and aromatic hydrocarbon compounds. The initiator can be prepolymerized modified sulfur, and is not limited to modified sulfur produced by a specific method.

[0062] According to an embodiment of the present specification, the initiator may be one or two or more selected from the group consisting of trans-cinnamaldehyde, benzyl acetate, diethylaniline, nitroethane, formaldehyde hydrate, benzyl acetate, dodecylbenzenesulfonic acid, hexadecyltrimethylammonium bromide (CTMAB), methylmorpholine and morpholine, and dimethylaniline.

[0063] The above-exemplified initiators may be used alone, in combination of two or more thereof, or together with an initiator not exemplified above.

[0064] Initiators may be used to promote or regulate the polymerization of the unsaturated fatty acid based modifier and sulfur.

[0065] According to an embodiment of the present specification, the initiator may be included in an amount of 0.01 parts by weight or more and 2 parts by weight or less based on 100 parts by weight of sulfur.

[0066] According to the embodiments of the present specification, the initiator can adjust the properties of the generated modified sulfur by changing the specific type of the applied initiator, the amount and point of addition, the reaction conditions, and the like.

[0067] In the present specification, the surfactant may be one or two or more selected from the group consisting of anionic surfactants, cationic surfactants, nonionic surfactants and amphoteric surfactants.

[0068] Anionic surfactants are sulfate-based anionic surfactants, sulfonate-based anionic surfactants or other anionic surfactants. Examples of sulfate-based anionic surfactants include: alkyl sulfates, alkyl ester sulfates, alkyl ether sulfates, alkyl ethoxy ether sulfates, sulfated alkanolamides, sulfated glycerides, etc., but the present invention is not limited thereto. Examples of sulfonate-based anionic surfactants include: dodecylbenzene sulfonates, including alkylbenzene sulfonates (ABS) and linear alkylbenzene sulfonates (LAS), hydrotropes and short-tail alkylbenzene sulfonates, α-olefin sulfonates, lignin sulfonates, sulfocarboxylic acid compounds, including sodium dodecyl sulfoacetate, etc., but the present invention is not limited thereto. Examples of other anionic surfactants include organophosphorus surfactants, alkyl amino acids including lauryl sarcosinates, sarcosine, etc., but the present invention is not limited thereto.

[0069] The cationic surfactant is a linear alkylamine, including fatty amines, linear alkylammonium, including quaternary alkylammonium, linear diamine, n-dodecylpyridinium chloride, imidazole, morpholine compound, etc., but the present invention is not limited thereto.

[0070] The nonionic surfactant is an ethoxylated alcohol, an alkylphenol, a fatty acid ester or a nitrogenated nonionic surfactant. Examples of ethoxylated alcohol and alkylphenol nonionic surfactants include linear ethoxylated alcohols, ethoxylated alkylphenols, ethoxylated mercaptans, nonylphenol, octylphenol, etc., but the present invention is not limited thereto. Examples of fatty acid ester nonionic surfactants include polyethoxylated esters, glycerides, hexitol, cyclodehydrated hexitol esters, etc., but the present invention is not limited thereto. Examples of nitrogenated nonionic surfactants include ethoxylated amines, imidazoles (cycloalkyl diamines), ethoxylated alkyl amides, tertiary amine oxides, etc., but the present invention is not limited thereto.

[0071] The amphoteric surfactant is aminopropionic acid, iminopropionic acid, a quaternary compound, etc. Examples of the quaternary compound include a sulfobetaine-based surfactant, etc., but the present invention is not limited thereto.

[0072] In the present specification, when the surfactant is selected and applied according to the application field of the modified sulfur, specific functionality required according to the application field in the production of the modified sulfur can be enhanced.

[0073] In the present specification, the coupling agent may be one or two or more selected from the group consisting of a silane-based coupling agent, a titanate-based coupling agent, and a chromium-based coupling agent, and a surfactant used in the art may be used.

[0074] The silane-based coupling agent may be any one selected from the group consisting of sulfide-based silane compounds, mercapto-based silane compounds, vinyl-based silane compounds, amino-based silane compounds, glycidoxy-based silane compounds, nitro-based silane compounds, chlorine-based silane compounds, methacrylic acid-based silane compounds and combinations thereof, but the present invention is not limited thereto.

[0075] The titanate-based coupling agent may be any one selected from the group consisting of triisostearoyl isopropyl titanate, tri(dodecylbenzenesulfonyl) isopropyl titanate, tri(dioctyl pyrophosphate) isopropyl titanate, di(tridecyl phosphite) tetraisopropyl titanate, di(dioctyl phosphite) tetraisopropyl titanate, tetraoctyloxytitanium (tricosyl phosphite) and combinations thereof, but the present invention is not limited thereto.

[0076] In the present specification, when a coupling agent is used, the interfacial bonding strength of the modified sulfur can be enhanced, and when the modified sulfur is used in combination with a heterogeneous material, the bonding with the heterogeneous material can be enhanced, which is beneficial to form a composite material.

[0077] In the present specification, the additive may be an inorganic or resin additive, and specifically may be one or two or more selected from the group consisting of silica sand, diatomaceous earth, wollastonite, clay, chopped glass fiber, dye, pigment, aluminum sulfate, water glass, Ca(OH)2, zinc oxide, naphthalene, Mg(OH)2, CaCl2, Al(OH)3, borax, CaSO4·2H2O, Fe2O3, zeolite, carbon black, talc, carbon fiber, clay, whisker, Na2SO3, MgSO4·7H2O, fly ash, acrylic emulsion, epoxy resin, latex, carbon fiber or flakes, steel fiber, liquid mineral, titanium dioxide, fiber filler, fiber particles, flaky particles, crushed recycled waste and combinations thereof.

[0078] According to an embodiment of the present specification, the additive may be included in an amount of 0.1 parts by weight or more and 30 parts by weight or less based on 100 parts by weight of sulfur.

[0079] The crosslinking agent may be a sulfur-based crosslinking agent, an organic peroxide, a resin crosslinking agent or a metal oxide, such as magnesium oxide, etc. The sulfur-based crosslinking agent may be an inorganic crosslinking agent, such as powdered sulfur (S), insoluble sulfur (S), precipitated sulfur (S), colloidal sulfur, etc., or an organic crosslinking agent, such as tetramethylthiuram disulfide (TMTD), tetraethylthiuram disulfide (TETD), dimorpholine disulfide, etc., but the present invention is not limited thereto. Specifically, the sulfur-based crosslinking agent may be a vulcanizing agent that is elemental sulfur or forms sulfur (such as amine disulfide), polymer sulfur, etc., but the present invention is not limited thereto. The organic peroxide may be any one selected from the group consisting of benzoyl peroxide, diisopropylbenzene peroxide, di-tert-butyl peroxide, tert-butyl peroxide isopropylbenzene, methyl ethyl ketone peroxide, isopropylbenzene hydroperoxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 1,3-bis(tert-butylperoxypropyl)benzene, di-tert-butylperoxydiisopropylbenzene, tert-butylperoxybenzene, 2,4-dichlorobenzoyl peroxide, 1,1-dibutylperoxy-3,3,5-trimethylsiloxane, n-butyl-4,4-di-tert-butylperoxyvalerate, and combinations thereof, but the present invention is not limited thereto.

[0080] Dispersants can be used to enhance the miscibility between modified sulfur and surfactants, between modified sulfur and coupling agents, or between modified sulfur and reinforcing materials. As dispersants, any dispersant can be used as long as it can improve the dispersibility when modified sulfur is mixed with surfactants, coupling agents, reinforcing materials, etc. In addition, surfactants can also be used as dispersants, which are used to improve the dispersibility during the mixing process to a certain extent.

[0081] As the dispersant, any one polymer dispersant selected from the group consisting of polyvinyl pyrrolidone, polyethylene imine, polyacrylic acid, carboxymethyl cellulose, polyacrylamide, polyvinyl alcohol, polyethylene oxide, starch, gelatin, and a combination thereof may be used, but the present invention is not limited thereto.

[0082] One or two or more selected from the group consisting of an initiator, a surfactant, a coupling agent, a catalyst, an additive, a cross-linking agent, and a dispersant may be mixed with the modified sulfur in a solvent.

[0083] As the solvent, any conventional solvent may be used without limitation as long as it facilitates mixing of the modified sulfur with the initiator, surfactant, coupling agent, catalyst, additive, crosslinking agent and / or dispersant and does not interfere with the polymerization of the modified sulfur.

[0084] The solvent may be one or two or more selected from the group consisting of water, aromatic hydrocarbon-based solvents, aliphatic hydrocarbon-based solvents, ether-based solvents, alcohol-based solvents, polyol solvents, amide-based solvents, acetate-based solvents, non-aqueous inorganic solvents, amine-based solvents, ester-based solvents, ketone-based solvents and sulfone-based solvents.

[0085] The aliphatic or aromatic hydrocarbon-based solvent may be any one selected from the group consisting of toluene, xylene, aromasol, chlorobenzene, hexane, heptane, octane, dodecane, cyclohexane, decane, tetradecane, hexadecane, octadecane, octadecene, nitrobenzene, o-nitrotoluene, anisole, mesitylene, and combinations thereof, but the present invention is not limited thereto.

[0086] The ether-based solvent may be any one selected from the group consisting of diethyl ether, dipropyl ether, dibutyl ether, dioxane, tetrahydrofuran, diisobutyl ether, isopropyl ether, octyl ether, tri(ethylene glycol) dimethyl ether, and combinations thereof, but the present invention is not limited thereto.

[0087] The alcohol-based solvent may be any one selected from the group consisting of methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutanol, hexanol, isopropanol, ethoxyethanol, ethyl lactate, octanol, isopropanol, ethylene glycol monomethyl ether, benzyl alcohol, 4-hydroxy-3-methoxybenzaldehyde, isodecanol, butyl carbitol, terpineol, α-terpineol, β-terpineol, eucalyptol and combinations thereof, but the present invention is not limited thereto.

[0088] The polyol solvent can be any one selected from the group consisting of glycerol, glycol, ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, butylene glycol, hexylene glycol, 1,2-pentanediol, 1,2-hexanediol, glycerol, polyethylene glycol, polypropylene glycol, ethylene glycol monomethyl ether (methyl cellosolve), ethylene glycol monoethyl ether (ethyl cellosolve), ethylene glycol monobutyl ether (butyl cellosolve), diethylene glycol monoethyl ether, diethylene glycol monobutyl ether and combinations thereof, but the present invention is not limited thereto.

[0089] The amide-based solvent may be any one selected from the group consisting of N-methyl-2-pyrrolidone (NMP), 2-pyrrolidone, N,N-dimethylacetamide, and a combination thereof, but the present invention is not limited thereto.

[0090] The amine-based solvent can be any one selected from the group consisting of primary amines such as propylamine, n-butylamine, hexylamine, octylamine, etc., secondary amines such as diisopropylamine, di(n-butyl)amine, etc., tertiary amines such as trioctylamine, tri-n-butylamine, etc., alkylamines such as ethylamine, propylamine, butylamine, hexylamine, octylamine, trioctylamine, etc., cyclic amines, aromatic amines and combinations thereof, but the present invention is not limited thereto.

[0091] The ester-based solvent may be any one selected from the group consisting of PEGMEA, ethyl acetate, n-butyl acetate, γ-butyrolactone, 2,2,4-trimethylpentanediol-1,3-monoisobutyrate, butyl carbitol acetate, butyl oxalate, dibutyl phthalate, dibutyl benzoate, butyl cellosolve acetate, ethylene glycol diacetate, ethylene glycol diacetate, and combinations thereof, but the present invention is not limited thereto.

[0092] The ketone-based solvent may be any one selected from the group consisting of acetone, methyl ethyl ketone, methyl isobutyl ketone, 1-methyl-2-pyrrolidone, cyclohexanone, and combinations thereof, but the present invention is not limited thereto.

[0093] The amide-based solvent may be any one selected from the group consisting of N-methyl-2-pyrrolidone (NMP), 2-pyrrolidone, N,N-dimethylacetamide, and a combination thereof, but the present invention is not limited thereto.

[0094] The sulfone-based solvent may be any one selected from the group consisting of diethyl sulfone, sulfolane, and a combination thereof, but the present invention is not limited thereto.

[0095] The acetate-based solvent may be any one selected from the group consisting of ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, and combinations thereof.

[0096] The non-aqueous inorganic solvent may be carbon disulfide, liquid ammonia, etc., but the present invention is not limited thereto.

[0097] According to one embodiment of the present specification, modifier is an adhesive produced by the melt polymerization of sulfur and environmentally friendly modifier, and is generally in liquid phase or gel phase at room temperature. In addition, according to the intended purpose, the modifier in solid phase (powder or particle form) obtained by maximizing the polymerization in melt polymerization may include any one of the groups consisting of ethanol, methanol, methyl ethyl ketone (MEK), toluene, meta-xylene, para-xylene, etc., when used as a material for waterproofing agent and preservative, as a diluent to be mixed. The intended purpose may refer to increasing hydrophobicity, waterproofness, corrosion resistance, chemical resistance, adhesiveness, high strength, etc. as required.

[0098] Production method of modified sulfur

[0099] Another aspect of the present invention provides a method for producing modified sulfur, which comprises: a first step of mixing sulfur and an unsaturated fatty acid-based modifier; a second step of introducing the resulting mixture into a reactor and melting it by heating at 100° C. or higher and 130° C. or lower; a third step of raising the temperature of the molten mixture to 130° C. or higher and 200° C. or lower; and a fourth step of terminating the reaction when the viscosity of the molten mixture reaches 6000 cP or higher and 25000 cP or lower at 160° C.

[0100] According to the embodiment of the present specification, the modified sulfur produced by the method may be applied in the same manner as in the description of the above modified sulfur unless it contradicts the following description.

[0101] According to one embodiment of the present specification, the first step of mixing sulfur and the unsaturated fatty acid-based modifier is performed such that the unsaturated fatty acid-based modifier is included in an amount of 10 parts by weight or more and 450 parts by weight or less based on 100 parts by weight of sulfur.

[0102] According to one embodiment, in the first step, a second modifier may be further included within the above content range.

[0103] According to one embodiment, one or two or more selected from the group consisting of initiators, surfactants, coupling agents, catalysts, additives, crosslinking agents and dispersants may be further included within the above content range. According to one embodiment, the first step may be performed at room temperature (about 15° C. to 25° C.) or higher.

[0104] According to one embodiment of the present specification, the mixture of sulfur and the unsaturated fatty acid-based modifier prepared in the first step has a viscosity of 0 cP at room temperature before heating.

[0105] According to one embodiment of the present specification, in the second step, the mixture may be melted by heating at 100° C. or higher and 130° C. or lower. Specifically, in the second step, the mixture may be melted by heating at an internal temperature of about 120° C. and polymerization may be initiated.

[0106] Specifically, in the second step, the mixture is introduced into the polymerization reactor, the temperature of the polymerization reactor is set to about 120° C. using a temperature controller, the introduction of the mixture into the polymerization reactor is terminated, and melt polymerization can be started. In addition, when the polymerization reactor temperature is about 120° C., melt polymerization can be performed while the reactor blades are stopped until sulfur and other mixed materials completely become liquid, and then rotated when the mixture is converted into liquid.

[0107] According to one embodiment of the present specification, after the mixture becomes liquid in the second step, a third step of increasing the temperature of the liquid phase mixture may be performed.

[0108] According to one embodiment of the present specification, the third step of increasing the temperature of the molten mixture may be performed by continuously increasing the temperature of the molten mixture to 130° C. or higher and 200° C. or lower. Specifically, the third step of increasing the temperature of the molten mixture may be performed by continuously increasing the temperature of the molten mixture to 130° C. or higher and 180° C. or lower. More specifically, in the third step, the temperature may be increased by adjusting the temperature controller of the polymerization reactor so that when the molten mixture produced in the second step is converted into a liquid, the temperature is set to about 135° C.

[0109] According to one embodiment, the third step of increasing the temperature of the molten mixture may be performed so that the temperature outside the reactor differs from the temperature of the molten mixture by 20°C or less. Specifically, the temperature of the polymerization reactor may be gradually increased by 2°C-3°C to about 135°C so that the temperature variation inside and outside the reactor is as small as possible (about 5°C or less). When the temperature increase rate is high, an exothermic reaction of sulfur and the modifier occurs, so the temperature inside the reactor increases rapidly, resulting in difficulty in temperature control and carbonization.

[0110] According to one embodiment of the present specification, when the temperature of the molten mixture is 160°C or higher, the state and viscosity of the molten mixture are measured three or more times per hour, and the fourth step of terminating the reaction can be performed according to the application field. Specifically, the reaction is terminated when the viscosity reaches 6000cP or higher and 15000cP or lower at 160°C, and the modified sulfur produced can be used for room temperature asphalt or modified sulfur polymer concrete, and the reaction is terminated when the viscosity reaches 6000cP or higher and 25000cP or lower at 160°C, and the modified sulfur produced can be used for waterproof paint or anti-corrosion paint.

[0111] According to one embodiment of the present specification, the viscosity of the melted mixture at 135° C. is 4000 cP or more and 25000 cP or less.

[0112] When the reaction time of the third step is prolonged, rubberized modified sulfur with high viscosity can be provided. In this case, the modified sulfur can be used for waterproof materials and anticorrosive materials by using a diluent. In addition, when added in the construction of roads and concrete structures, the high-viscosity modified sulfur produced in a solid phase or powder form can provide properties such as waterproofness, corrosion resistance, high adhesion, chemical resistance, etc., and can be applied to various applications due to its high viscosity, such as quick-setting repair agents, quick-setting water-stopping agents, waterproofing sheets, antimicrobial silicones, paints, waterproofing agents, and tile adhesives, etc.

[0113] According to one embodiment of the present specification, when the viscosity of the molten mixture whose temperature has been raised in the third step reaches 6000 cP or more and 25000 cP or less at 160° C., the fourth step of terminating the reaction may be performed. That is, according to one embodiment of the present invention, the time point at which the viscosity of the molten mixture whose temperature has been raised in the third step reaches 6000 cP or more and 25000 cP or less at 160° C. may be referred to as the reaction endpoint.

[0114] According to one embodiment of the present specification, when the reaction is terminated when the viscosity of the molten mixture reaches 6000 cP or more and 25000 cP or less at 160° C., the modified sulfur produced therefrom may exhibit spinnability or have a network structure or a honeycomb structure.

[0115] Specifically, the endpoint of the reaction can be determined as the time point at which a microstructure such as a fibrous or flaky structure due to an increase in the adhesive force of the molten mixture is observed (determined by a phenomenon in which, when a small rod is dipped into the collected sample and taken out therefrom, the sample is continuously spun like a thread (3 cm or more), and by a phenomenon in which, when the fingers of a disposable silicone glove to which the sample is applied are separated from each other, the sample is finely stretched into several strands (1 cm or more) like a thread).

[0116] Furthermore, the end point of the reaction may be between the time point at which spinnability is exhibited and the time point at which rubberization proceeds before carbonization occurs, and the reaction may also be terminated when the modified sulfur thus produced has a microstructure (e.g., a fiber structure, a honeycomb structure, or a network structure) or exhibits spinnability.

[0117] According to one embodiment of the present specification, when the reaction is terminated when the viscosity of the molten mixture reaches 6000 cP or more and 25000 cP or less at 160°C in the fourth step of terminating the reaction, the temperature in the reactor may be increased up to about 160°C to about 200°C.

[0118] The reaction product of the fourth step of the termination reaction has a viscosity of 5,000 cP to 2,000,000 cP at about 160° C. to about 200° C.

[0119] According to an embodiment of the present specification, an aging step is further included after the third step and before the fourth step. The aging step is performed by aging the molten mixture at a temperature of 40° C. or higher. When the aging step is further included, the reaction of the molten mixture whose temperature has been raised in the third step can be terminated before the reaction product shows spinnability, and the viscosity of the modified sulfur can be adjusted according to the application field.

[0120] Specifically, the aging step may be performed at 40° C. or higher and 120° C. or lower. More specifically, the aging step may be performed at about 40° C. to about 120° C. or lower. In the aging step, the viscosity of the modified sulfur may be adjusted according to the application field.

[0121] According to one embodiment of the present specification, the method of producing modified sulfur, ie, the first to fourth steps, may be performed for about 6 hours to about 18 hours, but the processing time may vary depending on the amount of the mixture and the structure or material of the polymerization reactor.

[0122] In the method for producing modified sulfur, the mixture of sulfur and the modifier is gradually polymerized while undergoing the second step (polymerization start step), and in the third step of increasing the temperature, the molten mixture may undergo color changes in the order of yellow, light brown, dark brown, and opaque black. An initiator may be added between the time points where the mixture changes color, and another initiator may be added before the end of the reaction.

[0123] According to one embodiment of the present specification, the mixture produced in the first step, the polymerization temperature and time, and the reaction endpoint may be adjusted according to the application field of the modified sulfur to adjust the spinning shape and / or viscosity.

[0124] Furthermore, according to one embodiment of the present specification, the addition point, type, and addition amount of the initiator can be adjusted according to the application field of the modified sulfur to adjust the properties of the modified sulfur.

[0125] Concrete composition

[0126] Another aspect of the present specification provides a concrete composition including the modified sulfur and aggregate.

[0127] According to the embodiment of the present specification, the modified sulfur included in the concrete composition may be applied in the same manner as in the description of the above-mentioned modified sulfur unless it contradicts the following description.

[0128] Since the concrete composition according to the embodiment of the present specification includes modified sulfur, fluidity is enhanced, which is conducive to mixing with aggregate in a short time. In addition, since the modified sulfur has a honeycomb structure or a mesh structure, bonding strength, waterproofness, elasticity and / or strength can be enhanced. In addition, the modified sulfur according to the embodiment of the present specification solves problems such as brittleness and odor of sulfur and is environmentally friendly.

[0129] In the present specification, the aggregate may be any one selected from the group consisting of recycled industrial waste, steel sand, crushed stone, fly ash, sea sand, quartz sand, gravel, silica, quartz powder, lightweight aggregate, clay mineral, glass powder, and combinations thereof.

[0130] For example, the recycled industrial waste refers to waste lime powder sludge in which lime powder generated when aggregate is crushed is precipitated with a sodium acrylate copolymer flocculant, and since it is treated as waste, it is a waste that is difficult to landfill. However, any industrial waste can be used as recycled industrial waste as long as it can be used as aggregate, and the present invention is not limited to waste lime powder sludge.

[0131] When fine aggregate having a particle size of 1 to 10 mm is used as aggregate, the aggregate can be used for mortar, and when the fine aggregate and coarse aggregate having a particle size of 10 to 18 mm are used together as aggregate, the aggregate can be used for concrete.

[0132] According to one embodiment of the present specification, the modified sulfur may be included in an amount of 1 part by weight or more and 80 parts by weight or less, and the aggregate may be included in an amount of 70 parts by weight or more and 95 parts by weight or less, based on 100 parts by weight of the concrete composition.

[0133] According to one embodiment of the present specification, the concrete composition may be a polymer concrete composition, that is, a resin concrete composition.

[0134] According to one embodiment of the present specification, the concrete composition can be applied to the field of latex modified concrete (LMC) or ultra-fast hardening cement alone or in combination.

[0135] According to one embodiment of the present specification, the concrete composition may be a hydraulic polymer concrete composition.

[0136] According to one embodiment of the present specification, the hydraulic polymer concrete composition can be dissolved in water at room temperature, i.e., has hydrophilicity. Therefore, the concrete composition can be used after being dissolved in water and then melt-mixed with a water reducer, a mold release agent, a defoamer, and other modifiers, or can be used after first being melted and melt-mixed with a water reducer, a mold release agent, a defoamer, and other modifiers.

[0137] According to one embodiment of the present specification, the concrete composition may further include a binder. As the binder, resins such as latex, varnish, epoxy resin, and methyl methacrylate (MMA) may be used.

[0138] Since the concrete composition according to the embodiment of the present specification is thermoplastic like conventional asphalt, it can be uniformly mixed during the melt mixing process.

[0139] According to one embodiment of the present specification, the concrete composition may further include a filler.

[0140] According to an embodiment of the present specification, the filler may be included in an amount of 1 part by weight or more and 60 parts by weight or less based on 100 parts by weight of the concrete composition.

[0141] In the present specification, the filler may be one or two or more selected from the group consisting of lime powder, Portland cement, slaked lime, fly ash, recycled dust, steelmaking dust, reinforcing material, and crushed waste aggregate and waste powder.

[0142] Crushed waste aggregate and waste powder may refer to waste asphalt concrete (ASCON), waste concrete, waste tires, steel slag, waste plastics, waste glass, waste sand and mud, waste lime powder, waste glass powder, etc.

[0143] According to one embodiment of the present specification, the concrete composition may further include a hardener.

[0144] According to one embodiment of the present specification, the hardener may be a commonly used hardener, for example, one or a mixture of two or more selected from MgO, cement, etc., but the present invention is not limited thereto. In addition, light MgO and heavy MgO may be used as the hardener according to the application field. In addition, the amount of the hardener may be adjusted to adjust the hardening time and increase and decrease the strength.

[0145] Furthermore, in the present specification, a composition including modified sulfur and a hardener may be provided, and the composition including modified sulfur and a hardener may be used as a quick-setting repair agent and a quick-setting adhesive, and for achieving waterproofness, corrosion resistance, and the like.

[0146] According to one embodiment of the present specification, when the hardener is cement, the hardener is included in an amount of 10 parts by weight or more and 70 parts by weight or less based on 100 parts by weight of the aggregate.

[0147] According to one embodiment of the present specification, when the hardener is MgO, the hardener is included in an amount of 1 part by weight or more and 40 parts by weight or less based on 100 parts by weight of the aggregate.

[0148] When the hardener is cement, a ribbon mixer or a common ready-mixed concrete mixer can be used to lay roads on site at room temperature using cement without adding water. Specifically, since the modified sulfur according to one embodiment of the present specification has a honeycomb structure or a mesh structure, the modified sulfur can use a thixotropic phenomenon and contain moisture itself. Therefore, when using the aqueous modified sulfur according to the embodiment of the present specification, roads can be constructed by ordinary concrete construction methods without additional water supply, and the hardener can be adjusted to reduce the curing time (1 day to 7 days) of the modified sulfur polymer concrete.

[0149] The concrete composition according to the embodiment of the present specification can be applied to various civil engineering and construction materials, road pavement, repair and reinforcement, emergency repair, and the like.

[0150] According to one embodiment of the present specification, the method of paving a road at room temperature using a concrete composition (bitumen, asphalt concrete) can be applied to environmentally friendly road pavement construction using only a mixer and a roller without using a heating device, anytime and anywhere, excluding hot ASCON pavement construction and pavement construction with a heating scheme. In addition, since the concrete composition including modified sulfur has high adhesiveness, an initial oil coating operation is not required in asphalt pavement construction, so a primer (tack coat) operation can be omitted.

[0151] According to one embodiment of the present specification, an instant construction method using a concrete composition on site at room temperature compensates for the shortcomings of conventional asphalt or concrete, so that high adhesion, chemical resistance, waterproofness, corrosion resistance, high elasticity, high wear resistance, etc. can be enhanced, and environmentally friendly and economical effects such as environmental friendliness, low cost, high quality and shortened construction period, which are the characteristics of semi-rigid asphalt, can be obtained.

[0152] In addition, the production of modified sulfur, the development of road pavement materials and repair and reinforcement materials, and the construction of various modified sulfur polymer concrete structures by reprocessing waste obtained from industrial and domestic waste recovered from landfills and incineration plants have huge environmental benefits, such as reducing air pollution and landfill, as well as huge economic benefits, such as fast construction speed and low cost.

[0153] The concrete composition including liquid-phase modified sulfur according to the embodiment of the present specification replaces the conventional hot asphalt to allow the construction of modified sulfur polymer concrete (semi-rigid asphalt) at room temperature, i.e., using only a ready-mixed concrete mixer and a roller without using heating equipment, by mixing the modified sulfur binder on site, to carry out simple road construction and repair / reinforcement work.

[0154] Furthermore, since the concrete composition according to the embodiment of the present specification is not easily deformed even in hot weather and exhibits excellent durability, and allows concrete construction without water supply, the concrete composition may be suitable for paving roads in desert areas, mountainous areas, Africa, the Middle East, Southeast Asia, etc.

[0155] In addition, traditional asphalt construction is not easy to carry out in cold winters because the properties of the asphalt are likely to change due to differences in ambient temperature, however, the modified sulfur according to the implementation scheme of the present specification allows the construction and repair / reinforcement of roads even in sub-zero weather (about -5°C) due to the properties of sulfur, such as heat generation and strong resistance to low-temperature cracking.

[0156] In particular, road construction may be carried out using only ordinary aggregates and modified sulfur, making it most suitable for island regions such as the Philippines, Indonesia, Cuba and the Caribbean, where there are many islands and no asphalt batching plant is required. In addition, in island regions, there are huge environmental and economic benefits by reprocessing waste obtained by recycling industrial and domestic waste.

[0157] Furthermore, in the case of tunnel construction, when heating construction is performed, there are economic benefits such as low shedding rate (rebound rate) due to strong adhesive strength and waterproofness, and shortened construction period due to omission of moisture-proofing work.

[0158] In addition, since the modified sulfur according to the embodiment of the present specification continues to harden in water, the modified sulfur is very effective for sewage pit repair work, facilitating emergency repairs and the establishment of emergency roads by adjusting the hardening time during construction and allowing the roads to be opened in a short time, thus producing a wide range of economic impacts.

[0159] In addition, due to the strong salt resistance, sand or aggregate with salinity (including marine debris) can be used, and due to the strong bonding strength and high strength, temporary roads can be built using only ordinary soil or sand to pave temporary roads.

[0160] The modified sulfur according to the embodiment of the present specification can be applied to emergency road repair by adjusting the hardening time, and can be applied to the repair and reinforcement of old asphalt roads, wherein the existing old asphalt can be recycled by scrapping only the upper part (5 cm) thereof using a road crusher, crushing the discarded waste ASCON or waste aggregate (to a 13 mm aggregate level) on site, mixing the crushed waste ASCON or waste aggregate with the modified sulfur of the present invention at room temperature, depositing the resulting mixture on a road whose upper part has been scrapped to a thickness of 5 cm, and compacting it.

[0161] The edge joints (usually 30 cm to 1 m wide) of conventional asphalt roads are usually made of cement or concrete, and due to the fatigue resistance and moisture sensitivity of the road and the adhesion between the heterogeneous materials, the edge joints will crack over time. On the other hand, in the case of using the modified sulfur of the present invention, construction can be carried out without considering the joint part, and even if the joint part is independently constructed with ordinary aggregate or waste aggregate, the above problems can be solved due to the cohesion between the homogeneous materials.

[0162] In addition, according to the embodiment of the present specification, the concrete composition can be used as a material for a waterproofing agent, an antiseptic, etc. The modified sulfur according to the embodiment of the present specification has high functionality, that is, high chemical resistance, corrosion resistance, waterproofness, high strength, high bonding strength, rapid solidification performance, etc. Therefore, by enhancing specific functions according to the application field, the concrete composition can be used as a material for a waterproofing agent, an antiseptic, a water stopper, various types of adhesives, paints, etc.

[0163] According to an embodiment of the present specification, when the concrete composition is used as a material for a waterproofing agent and an antiseptic, a diluent may be further included. According to one embodiment, the diluent may include any one selected from the group consisting of ethanol, methanol, methyl ethyl ketone (MEK), toluene, m-xylene, p-xylene, etc.

[0164] Furthermore, in the case of using the concrete composition for anticorrosion and waterproofing, when the anticorrosion coating is formed, an additive that can enhance the strength of the anticorrosion coating may be further included.

[0165] The concrete composition according to an embodiment of the present specification can be used to replace epoxy resin or polyurethane, and is environmentally friendly and economical in terms of time and cost because it is not necessary to apply multiple coatings such as a top coating, a middle coating, and a primer as in the case of conventional epoxy resin or polyurethane.

[0166] Hereinafter, the present invention will be described in detail with reference to the embodiments. However, the embodiments of the present invention may be modified in several different forms, and the scope of the present invention is not limited to the embodiments described below. The embodiments of the present invention are provided so that this disclosure will be thorough and complete, and the concept of the embodiments will be fully conveyed to those skilled in the art.

[0167] Example 1

[0168] Production of modified sulfur

[0169] 100 g of sulfur and 150 g of oleic acid are introduced into a polymerization reactor at room temperature. The temperature of the polymerization reactor is set to about 120°C using a temperature controller, and melt polymerization is carried out while stopping the reactor blades until the sulfur and other mixed materials are completely liquid, and then rotated when the mixture is converted into a liquid. After the molten mixture is converted into a liquid, the temperature of the polymerization reactor is gradually increased to about 135°C by an amplitude of 2°C-3°C, so that the temperature difference inside and outside the synthetic product is as small as possible (about 5°C or less). When the temperature of the molten mixture is 160°C or higher, the state and viscosity of the molten mixture are measured three or more times per hour, and the reaction is terminated when its viscosity reaches 10000 cP, thereby obtaining modified sulfur.

[0170] Comparative Example 1-1

[0171] 150g of sulfur and 150g of dicyclopentadiene (DCPD) are introduced into a polymerization reactor at room temperature. The temperature of the polymerization reactor is set to about 120°C using a temperature controller, and then melt polymerization is performed until sulfur and other mixed materials become liquid completely. After the molten mixture is converted into a fully mixed liquid, the temperature of the polymerization reactor is set to about 160°C and gradually increased to 200°C, and then reacted. When the molten mixture becomes a dark brown liquid phase synthetic product and its viscosity reaches 10000cP, the reaction is terminated, and the synthetic product is cooled to obtain solid phase modified sulfur.

[0172] In the case of the modified sulfur produced in Comparative Example 1-1, water resistance and corrosion resistance can be confirmed. However, when sulfur and DCPD are mixed (in the early stage), due to its disgusting odor, a gas mask must be worn when mixing sulfur and DCPD, and a gas mask must be worn even after the reaction is terminated. Therefore, it is difficult to actually apply this modified sulfur to the industrial field.

[0173] Wheel tracking test

[0174] In order to confirm the dynamic stability of the modified sulfur produced in Example 1, 210 g of the modified sulfur produced in Example 1, 2 kg of sand, 1000 g of aggregate (13 mm) and 210 g of MgO were mixed at room temperature for 7 minutes, and then the mixture was compacted 65 times using an asphalt sample compactor. After 10 minutes of compaction, the mold was removed and the compacted mixture was allowed to stand for 12 hours to manufacture a specimen.

[0175] The samples prepared by Twining, Inc., standard straight run asphalt (Comparative Examples 1-2) and styrene-butadiene-styrene (SBS) asphalt (Comparative Examples 1-3) were subjected to rutting tests in a testing agency (Twining, Inc., California, USA). The results are shown in FIG. Figure 2 shown.

[0176] from Figure 2 It can be seen from the results that, compared with straight-run asphalt and SBS modified asphalt, the modified sulfur according to the embodiment of the present specification exhibits excellent dynamic stability.

[0177] Example 2

[0178] In order to confirm that a concrete composition including modified sulfur according to an embodiment of the present specification can be used to construct an asphalt road at room temperature, the following experiment was conducted.

[0179] Example 2-1

[0180] At room temperature, 150 g of sulfur, 150 g of oleic acid, 2 g of pine oil (phytoncide), 2 g of methyl dicyclopentadiene (MDCP) and 2 g of carbon black are introduced into a reactor, and melt polymerization is carried out while the temperature is increased to 160° C., thereby producing liquid-phase modified sulfur with a viscosity of 6000 cP or more.

[0181] 1000 g of aggregate (13 mm), 2 kg of sand and 150 g of MgO as a hardener were mixed at room temperature, and then the mixture was introduced into a fine aggregate mixer. Subsequently, 180 g of the resulting modified sulfur was introduced into the mixer and mixed for 7 minutes, and then the resulting mixture was compacted 65 times using an asphalt sample compactor. Ten minutes after compaction, the mold was removed. One day later, the resulting sample was placed in a hot water tank and soaked in 60°C water for 1 hour. Then, the stability and flow value of the sample were measured.

[0182] When measured at a weight ratio of 1 kg / sample, the stability and flow value of the sample were 12353 and 23, respectively. During the manufacturing process of the sample, the smell of sulfur or other additives was hardly felt.

[0183] Example 2-2

[0184] 150 g of sulfur, 187.5 g of oleic acid, 2 g of pine oil (phytoncide) and 2 g of carbon black were introduced into a reactor at room temperature and polymerized for 4 hours while raising the temperature to 160° C. Subsequently, 2 g of phytoncide was added thereto, and after one hour, the polymerization was terminated when the viscosity reached 15000 cP or more, thereby producing dark brown liquid-phase modified sulfur.

[0185] 1,000 g of aggregate (13 mm), 2 kg of sand and 270 g of MgO as a hardener were mixed at room temperature, and then the mixture was introduced into a fine aggregate mixer. Subsequently, 210 g of the resulting modified sulfur was introduced into the mixer and mixed for 5 minutes, and then the resulting mixture was compacted 65 times using an asphalt sample compactor. Then, the mold was removed, and 12 hours after the mold was removed, the resulting sample was placed in a hot water tank and soaked in 60°C water for 1 hour. Then, the stability and flow value of the sample were measured, and the results were 15652 and 18, respectively.

[0186] It can be seen that although the mixing time during the sample preparation process is shortened compared to Example 2-1, the mixing effect is good. This is because the mixing is carried out using a larger amount of modified sulfur.

[0187] Example 2-3

[0188] 150 g of sulfur, 150 g of oleic acid, 2 g of methyldicyclopentadiene (MDCP) and 2 g of carbon black were introduced into a reactor, and polymerization was performed while increasing the temperature to about 160° C. to 200° C. Subsequently, 2 g of phytoncide was added thereto, and the polymerization was terminated when the viscosity reached 10,000 cP or more, thereby producing almost black liquid-phase modified sulfur.

[0189] Cool the modified sulfur to obtain rubberized solid-phase modified sulfur, and 200g of the rubberized solid-phase modified sulfur is crushed into small pieces and diluted with 10g of ethanol as a diluent to impart fluidity. In addition, 1000g of aggregate (13mm), 2kg of sand and 150g of MgO as a hardener are mixed at room temperature, and the mixture is then introduced into a fine aggregate mixer. Subsequently, the diluted modified sulfur is introduced into the mixer and mixed for 5 minutes, and then the resulting mixture is compacted 65 times using an asphalt sample compactor. Then, the mold is removed, and after removing the mold for 1 day, the resulting sample is placed in a hot water tank and soaked in 60°C water for 1 hour. Then, the stability and flow value of the sample are measured, and the results are 12286 and 21, respectively.

[0190] In the case of Examples 2-3, it can be seen that satisfactory stability and satisfactory flow values ​​were obtained despite the use of a smaller amount of hardener for mixing when preparing the test specimens.

[0191] Examples 2-1 to 2-3 relate to concrete compositions for asphalt construction at room temperature. It can be seen from the results of Examples 2-1 to 2-3 that not only the inherent disadvantages of sulfur (brittleness) are overcome, but also the odor is eliminated. The concrete compositions are environmentally friendly when constructed at room temperature and exhibit enhanced durability, which is beneficial to the maintenance and repair of roads.

[0192] Particularly, in the case of Example 2-2, it can be seen that the concrete composition is also suitable for emergency repairs because the hardening is completed within 30 minutes and the generated modified sulfur also has a phytoncide aroma.

[0193] Example 3

[0194] In order to confirm that a concrete composition including modified sulfur according to an embodiment of the present specification and a waste source can be used to construct an asphalt road, the following experiment was conducted.

[0195] Example 3-1

[0196] 750 g of waste glass and 315 g of modified sulfur produced in Example 1 were mixed with 2000 g of sand, 750 g of gravel (13 mm) and 225 g of hardener (MgO), and the mixture was compacted 65 times using an asphalt sample compactor. After compaction for 24 hours, the stability and flow values ​​of the obtained sample were measured, and the results were 39496 and 26, respectively. The stability value is much higher than 2500, which is the standard stability value of conventional room temperature asphalt, and the concrete composition can be used for the lower layer of the road.

[0197] Example 3-2

[0198] 240 g of waste vinyl resin (vinyl) and 315 g of modified sulfur produced in Example 1 were mixed with 3000 g of sand, 1260 g of gravel (13 mm) and 315 g of hardener (MgO) to prepare two samples (A and B), and the samples were compacted 65 times using an asphalt sample compactor. After compaction for 24 hours, the stability and flow values ​​of the obtained samples were measured, and as a result, the stability values ​​of A and B were 14641 and 16515, respectively, and their flow values ​​were 31 and 34, respectively. Since the final composition of the crushed waste plastics was different, two types of test scores (A and B) were obtained. The stability values ​​of the two samples were also significantly higher than 2500, which is the standard stability value of conventional room temperature asphalt, and these concrete compositions can be used for the lower part of the road.

[0199] Example 3-3

[0200] 900 g of steelmaking slag and 315 g of modified sulfur produced in Example 1 were mixed with 3000 g of sand, 600 g of gravel (13 mm) and 225 g of hardener (MgO), and the mixture was compacted 65 times using an asphalt sample compactor. After compaction for 24 hours, the stability and flow values ​​of the obtained sample were measured, and the results were 13292 and 16, respectively. The stability value is much higher than 2500, which is the standard stability value of conventional room temperature asphalt, and the concrete composition can be used for the lower layer of the road.

[0201] The stability and flow values ​​of the specimens of Examples 3-1 to 3-3 are the results of measurements in a qualified laboratory in Korea according to the KS F 2337:2017 test method.

[0202] It can be seen from the results of Examples 3-1 to 3-3 that the modified sulfur according to the embodiment of the present invention excels in cohesion, cross-linking, fluidity, compactability, and storage stability, and thus the pulverized waste source can be reused instead of aggregates.

[0203] Example 4

[0204] The moisture absorption rates of hydraulic concrete samples including the modified sulfur produced in Example 1 and ordinary concrete samples were compared. The composition of the concrete samples was designed with a blending ratio so that the compressive strength of the concrete was 25 MPa and the slump was 20 cm, and was mixed based on the blending ratio according to the Korea Expressway Corporation's road pavement repair, bridge pavement and resurfacing guide.

[0205] Example 4-1

[0206] 660g of Portland cement (Shuanglong Cement), 345g of water, 55g of modified sulfur produced in Example 1 and 75g of water reducer were mixed, and the mixture, 1000g of aggregate (13mm) and 2kg of crushed stone were introduced into an aggregate mixer and mixed for 10 minutes. Then, the resulting mixture was introduced into a sample mold. After three days, the mold was removed and the resulting sample was cured for a total of 28 days.

[0207] Comparative Example 4-1

[0208] Concrete specimens were manufactured in the same manner as in Example 4-1, except that the modified sulfur and the water reducing agent produced in Example 1 were not included.

[0209] 15L of water was introduced into a 20L plastic bucket, and then each concrete specimen manufactured in Example 4-1 and Comparative Example 4-1 was immersed in the bucket. After immersion for 1 month, the moisture absorption rate was measured, and the results were as follows: Figure 3 In addition, the moisture absorption rate measured after immersion for 3 months is shown in Table 1 below.

[0210] [Table 1]

[0211]

[0212]

[0213] From Table 1 and Figure 3 It can be seen from the results shown in that the hydraulic polymer concrete composition including the modified sulfur according to the embodiment of the present specification exhibits low moisture absorption rate, excellent chemical resistance, and high bonding strength.

[0214] Example 5

[0215] The chemical resistance of concrete compositions including modified sulfur according to embodiments of the present specification was compared.

[0216] Examples 5-1 to 5-3

[0217] Concrete specimens were prepared in the same manner as in Example 4-1, except that the weight of modified sulfur added was 2%, 5%, and 7.5% of cement, respectively.

[0218] Comparative Example 5-1

[0219] Concrete specimens were manufactured in the same manner as in Example 5-1, except that modified sulfur was not included.

[0220] Each concrete specimen manufactured in Examples 5-1 to 5-3 and Comparative Example 5-1 was immersed in each of 30% calcium chloride, 30% sodium chloride and 30% sulfuric acid diluted with water for 9 months. Then, the obtained concrete specimens were compared. The results are as follows: Figure 4 shown.

[0221] from Figure 4 As can be seen from the results shown, the concrete composition including the modified sulfur according to the embodiment of the present specification exhibits chemical resistance superior to that of the concrete composition not including the modified sulfur. Specifically, it can be seen that even though a relatively small amount of modified sulfur is included compared to Embodiments 5-2 and 5-3, Example 5-1 exhibits chemical resistance superior to that of Comparative Example 5-1 not including the modified sulfur.

Claims

1. A method for providing modified sulfur that can be used in concrete, coatings or waterproofing agents, include: mixing sulfur and an unsaturated fatty acid-based modifier, wherein the amount of the unsaturated fatty acid-based modifier is 10 to 450 parts by weight based on 100 parts by weight of the sulfur; introducing the resulting mixture into a reactor and melting the mixture by heating to at least 120° C. so that the sulfur in the mixture melts into a liquid state; While stirring the mixture, gradually raising the temperature of the mixture to a temperature in excess of 160° C. over a period of time such that an exothermic reaction does not occur but rather a rapid temperature increase and carbonization occurs, thereby polymerizing the resulting liquid sulfur / modifier mixture; and When the obtained modified sulfur exhibits spinnability or has a network or honeycomb structure at room temperature, the reaction is terminated. The duration of the method is from 6 to 18 hours.

2. The method of claim 1, wherein the unsaturated fatty acid-based modifier comprises oleic acid. 3 . The method according to claim 1 , wherein the modified sulfur prepared by the method has a viscosity of 4000 cP to 25,000 cP at room temperature.

4. The process according to claim 1, wherein the temperature is raised to 180°C before terminating the reaction.

5. The method of claim 1, wherein the concrete is asphalt concrete.

6. An asphalt concrete composition comprising modified sulfur prepared according to the method of claim 1, a hardener and aggregate.

7. A concrete composition comprising modified sulfur prepared according to the method of claim 1, aggregate and a hardener.

8. The concrete composition according to claim 7, wherein the hardener is magnesium oxide or cement.

9. The concrete composition according to claim 7, wherein the aggregate is sand.

10. A method for preparing a concrete composition, comprising preparing modified sulfur by the method of claim 1, and combining the modified sulfur with an aggregate and a hardener.

11. The method of claim 10, wherein the hardener is magnesium oxide or cement.

Citation Information

Patent Citations

  • Modified sulfur, method for preparing same, apparatus for preparing same, and use thereof

    CN105492381A