A low-absorbency matte surface cloth and its preparation process and application

By coating the surface of the fiberglass cloth with Teflon coating, the surface tension is reduced and a uniform coating is formed, which solves the problem of cracking of the fiberglass mesh cloth at high temperatures, improves adhesion and heat resistance, and is suitable for a variety of applications. The composite application of materials ensures production continuity.

CN115216972BActive Publication Date: 2024-10-15GUANGDONG SHUO CHENG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111571429.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-21
Publication Date
2024-10-15
Estimated Expiration
2041-12-21

AI Technical Summary

Technical Problem

The existing glass fiber mesh cloth is prone to cracking under high temperature conditions, which affects the production continuity of printed circuit boards. Moreover, the cost of the graphene mixture is high and is not suitable for large-scale promotion.

Method used

The low-adsorption matte surface of Teflon coating and glass fiber cloth is coated by a mixture of polytetrafluoroethylene suspension, polyether siloxane, cetyl alcohol ester and epoxy silane coupling agent. , reduce the surface tension of fiberglass cloth, improve the adhesion of Teflon coating, and form a uniform coating through multiple baking to avoid cracking during high-temperature baking.

Benefits of technology

It achieves good adhesion between the fiberglass cloth and the paint, avoids adhesion to the steel plate, improves heat resistance and anti-adhesion, is suitable for composite applications of a variety of materials, and ensures the continuity of the production process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a low-adsorbability matte surface cloth, and the raw materials for preparation include: glass fiber grey cloth, Teflon coating, and the thickness ratio of the glass fiber grey cloth to the Teflon coating is (1-5): (0.4-0.8). The present invention has good heat resistance and anti-sticking properties by coating 3-5 layers of Teflon coating on the surface of the glass fiber grey cloth, and can be applied to a variety of rubber pressing pads and metal product surfaces, and can avoid adhesion to steel plates, affecting the continuous progress of the production process. And through the synergistic effect of polyether siloxane and 3-(2,3-epoxypropoxy)propyltrimethoxysilane, the surface tension of the glass fiber grey cloth is reduced, and the adhesion of the water-based Teflon coating on the surface of the glass fiber grey cloth is increased. At the same time, by introducing hexadecyl alcohol ester, the dispersibility of the fluorocarbon emulsion is increased, so that it is easy to form a film on the surface of the grey cloth, and the film layer is prevented from cracking and falling off during high-temperature baking.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a low-adsorbability matte surface cloth and a preparation process thereof, and relates to B32B, and in particular to the field of flat layered products. Background Art

[0002] With the rapid development of electronic information technology and the communications industry, the printed circuit board industry has continued to rise along with the development of the electronics industry. The main substrate of the printed circuit board is a copper-clad laminate, which is made of multiple layers of materials pressed between a hot plate and a steel plate under high temperature and high pressure conditions. In order to reduce the temperature difference between each layer, a pressing buffer pad needs to be added, which needs to have good high temperature resistance and the property of not sticking to the steel plate. At present, there are glass fiber mesh cloths on the market that are used as pressing pads after being glued by dipping, but the adhesion between the glass fiber mesh cloth and the coating is low, and it is easy to crack under high temperature conditions, affecting continuous production and operation.

[0003] Chinese invention patent CN201810182422.3 discloses a two-dimensional material modified glass fiber composite material, which combines glass fiber with a graphene mixture to improve the thermal conductivity and mechanical properties of the composite material. However, the cost of using the graphene mixture is high and it is not suitable for large-scale promotion. Chinese invention patent CN201910677059.7 discloses a production method for electronic grade glass fiber cloth. By optimizing the formula of the glass fiber cloth sizing agent, the stability of the sizing agent on the surface of the glass fiber cloth is improved, and the stability of the electronic substrate is improved. However, the stirring speed and stirring time during the stirring process need to be strictly controlled, and the reaction conditions are strict and difficult to control. Summary of the invention

[0004] In order to reduce the adhesion between the surface cloth and the steel plate and improve the adhesion between the glass fiber grey cloth and the coating, the first aspect of the present invention provides a low-adsorbability matte surface cloth, the preparation raw materials include: glass fiber grey cloth, Teflon coating, the Teflon coating is cured to form a Teflon coating, and the thickness ratio of the glass fiber grey cloth to the Teflon coating is (1-5): (0.4-0.8).

[0005] As a preferred embodiment, the thickness ratio of the glass fiber grey cloth to the Teflon coating is (2-4): (0.5-0.7).

[0006] As a preferred implementation, the thickness ratio of the glass fiber grey cloth to the Teflon coating is 3:0.6.

[0007] As a preferred embodiment, the Teflon coating includes, by weight: 55-70 parts of fluorocarbon emulsion, 0.1-0.5 parts of polysiloxane, 1-5 parts of alcohol ester solution, 1-3 parts of silane coupling agent, 1-5 parts of thickener, and 10-30 parts of water.

[0008] As a preferred embodiment, the Teflon coating includes, by weight: 57-63 parts of fluorocarbon emulsion, 0.2-0.4 parts of polysiloxane, 2-4 parts of alcohol ester solution, 1.5-2.5 parts of silane coupling agent, 2-4 parts of thickener, and 15-25 parts of water.

[0009] As a preferred embodiment, the Teflon coating includes, by weight: 60 parts of fluorocarbon emulsion, 0.3 parts of polysiloxane, 3 parts of alcohol ester solution, 2 parts of silane coupling agent, 3 parts of thickener, and 20 parts of water.

[0010] As a preferred embodiment, the polysiloxane is selected from one or a combination of amino polysiloxane, epoxy polysiloxane, polyether siloxane, carboxyl polysiloxane, alcohol hydroxyl-modified polysiloxane, and mercapto-modified polysiloxane.

[0011] As a preferred embodiment, the polysiloxane is polyether siloxane.

[0012] As a preferred embodiment, the alcohol ester solution is selected from one or a combination of dodecyl alcohol ester, hexadecanol ester, propylene glycol methyl ether acetate, and hexylene glycol butyl ether acetate.

[0013] As a preferred embodiment, the alcohol ester solution is hexadecyl alcohol ester.

[0014] As a preferred embodiment, the silane coupling agent is selected from one or a combination of epoxy silane coupling agents, amino silane coupling agents, vinyl silane coupling agents, alkyl silane coupling agents, phenyl silane coupling agents, and chlorine-containing silane coupling agents.

[0015] As a preferred embodiment, the silane coupling agent is an epoxy silane coupling agent.

[0016] As a preferred embodiment, the epoxy silane coupling agent is selected from one or a combination of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-(2,3-epoxypropoxy)propyltriethoxysilane, 3-(2,3-epoxypropoxy)propylmethyldiethoxysilane, and 3-(2,3-epoxypropoxy)propylmethyldimethoxysilane.

[0017] As a preferred embodiment, the epoxy silane coupling agent is 3-(2,3-epoxypropoxy)propyltrimethoxysilane.

[0018] The surface tension of the fabric prepared from glass fiber is relatively large. If a simple fluorocarbon emulsion is used for coating, the adhesion to the glass fiber fabric is poor and it is not easy to coat and form a film. During the experiment, the applicant found that the adhesion and film-forming properties of the Teflon coating and the glass fiber fabric can be improved by mixing and coating a polytetrafluoroethylene suspension, polyether siloxane, hexadecyl alcohol ester and epoxy silane coupling agent. The possible reason is that the synergistic effect of polyether siloxane and epoxy silane coupling agent can reduce the surface tension of the glass fiber fabric, form a hydrophilic layer on the surface of the glass fiber fabric, and increase the adhesion of the water-based Teflon coating on the surface of the glass fiber fabric. Hexadecyl alcohol ester can increase the dispersibility of the fluorocarbon emulsion, make the fluorocarbon emulsion easy to flow on the surface of the glass fiber fabric, and form a film to form a uniform Teflon coating on the surface. When baking at high temperature, it can avoid the formation of a dry outside and wet inside state that causes the coating to crack and fall off.

[0019] The applicant found during the experiment that coating one side of the glass fiber grey cloth can prevent the surface cloth from adhering to the steel plate, while the other side can be composited with a variety of materials, thus avoiding the problem that the glass fiber is difficult to composite with other materials after double-sided dip coating.

[0020] As a preferred embodiment, the thickener is selected from cellulose ether thickeners, inorganic thickeners, high molecular polymer thickeners, and natural high molecular derivative thickeners.

[0021] As a preferred embodiment, the thickener is a high molecular polymer thickener.

[0022] As a preferred embodiment, the thickener is polyvinyl pyrrolidone.

[0023] As a preferred embodiment, the preparation method of the Teflon coating comprises the following steps: adding fluorocarbon emulsion, polysiloxane, alcohol ester solution, silane coupling agent, and thickener into 20 parts by weight of water and mixing them evenly.

[0024] The second aspect of the present invention provides a process for preparing a low-adsorbability matte surface cloth, comprising the following steps:

[0025] (1) Pretreatment: Bake the glass fiber cloth to remove moisture and dewax at a temperature of 250-280°C;

[0026] (2) Base coating: Apply Teflon coating evenly to the surface of glass fiber cloth;

[0027] (3) Pre-baking: Set the temperature to 330-340°C for pre-baking;

[0028] (4) Secondary coating and baking, the baking temperature is 340-350°C;

[0029] (5) coating again and baking at a temperature of 350-360° C., and repeating step (5) 3-5 times to obtain the product.

[0030] As a preferred embodiment, the coating amount of Teflon coating in step 2 is 0.5-0.8 kg / m 2 .

[0031] As a preferred embodiment, step (1) is performed independently, and steps (2) to (5) are performed continuously, and the machine operating speed during the continuous process is 0.5 to 1 m / min.

[0032] The third aspect of the present invention provides an application of a low-adsorbability matte surface cloth, which is applied to the surface of a rubber material or a metal material, preferably, to the surface of a rubber pressing pad or a metal pressing pad.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] (1) The low-adsorbability matte surface cloth of the present invention has good heat resistance and anti-stickiness by coating 3-5 layers of Teflon coating on the surface of the glass fiber grey cloth. It can be applied to a variety of rubber pressing pads and metal product surfaces to avoid adhesion to steel plates and affecting the continuous progress of the production process.

[0035] (2) The low-adsorbability matte surface fabric of the present invention reduces the surface tension of the glass fiber grey fabric and increases the adhesion of the water-based Teflon coating on the surface of the glass fiber grey fabric through the synergistic effect of polyether siloxane and 3-(2,3-epoxypropoxy)propyltrimethoxysilane.

[0036] (3) The low-absorption matte surface cloth of the present invention increases the dispersibility of the fluorocarbon emulsion by introducing hexadecyl alcohol ester and synergizing with 3-(2,3-epoxypropoxy)propyltrimethoxysilane, making it easy to form a film on the surface of the grey cloth, thereby avoiding cracking and falling off of the film layer during high-temperature baking. DETAILED DESCRIPTION

[0037] The present invention is described in detail below by way of examples. It is necessary to point out here that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by professionals and technicians in this field based on the content of the present invention above still belong to the scope of protection of the present invention.

[0038] In addition, unless otherwise stated, all raw materials used were commercially available.

[0039] Example 1

[0040] A low-adsorbability matte surface cloth, the preparation raw materials of which include: glass fiber grey cloth, Teflon coating, the Teflon coating is formed after curing, and the thickness ratio of the glass fiber grey cloth to the Teflon coating is 3:0.6.

[0041] In parts by weight, the Teflon coating includes: 60 parts of fluorocarbon emulsion, 0.3 parts of polysiloxane, 3 parts of alcohol ester solution, 2 parts of silane coupling agent, 3 parts of thickener, and 20 parts of water.

[0042] The fluorocarbon emulsion was purchased from Shandong Dongyue with the brand name JF-4DC; the polysiloxane was polyether siloxane with the model name HY-6085, purchased from Beijing Maier Chemical Technology Co., Ltd. The alcohol ester solution was hexadecyl alcohol ester. The silane coupling agent was 3-(2,3-epoxypropoxy)propyltrimethoxysilane, purchased from Qufu Chenguang Chemical Co., Ltd. The thickener was polyvinyl pyrrolidone with the model name PVP-90, purchased from Shandong Xuguang Chemical Co., Ltd.

[0043] The preparation method of the Teflon coating comprises the following steps: adding fluorocarbon emulsion, polysiloxane, alcohol ester solution, silane coupling agent and thickener to 20 parts by weight of water and mixing them evenly to obtain the coating.

[0044] A preparation process of a low-adsorbability matte surface cloth comprises the following steps:

[0045] (1) Pretreatment: The glass fiber cloth is baked to remove moisture and dewax at a baking temperature of 265°C;

[0046] (2) Base coating: Apply Teflon coating evenly to the surface of glass fiber cloth, with a coating amount of 0.7 kg / m 2 ;

[0047] (3) Pre-baking: Set the temperature to 335°C for pre-baking;

[0048] (4) Secondary coating and baking at a temperature of 345°C;

[0049] (5) coating again and baking at a temperature of 355° C. Repeat step (5) 5 times to obtain the product.

[0050] Steps (2) to (5) are carried out continuously at a machine speed of 0.8 m / min.

[0051] Example 2

[0052] A low-adsorbability matte surface cloth, a preparation process and an application thereof, wherein the specific steps are the same as those in Example 1, except that the alcohol ester solution is dodecanol ester.

[0053] Example 3

[0054] A low-adsorbability matte surface cloth, a preparation process and an application thereof, wherein the specific steps are the same as those of Example 1, except that the thickener is hydroxyethyl cellulose.

[0055] Example 4

[0056] A low-adsorbability matte surface cloth, a preparation process and an application thereof, wherein the specific steps are the same as those in Example 1, except that the baking temperature in step 2 is 345°C.

[0057] Performance Testing

[0058] 1. Abrasion resistance test: The matte surface fabrics prepared in Examples 1-4 were subjected to an abrasion resistance test by rubbing them using a horizontal abrasion machine to test how many times the surface fabrics were rubbed before being damaged.

[0059] 2. Friction coefficient: Test the dynamic friction coefficient according to GB10006 test standard.

[0060] 3. High temperature adhesion: The adhesion between glass fiber cloth and Teflon coating is tested at 250℃ according to GB / T5210-1985 test standard.

[0061] Examples 1-4 were tested according to the above standards, and the test results are shown in Table 1.

[0062] Table 1

[0063] Abrasion resistance / times Dynamic friction coefficient Adhesion N / cm Example 1 >1000 ≤0.04 9.15 Example 2 980 0.06 8.35 Example 3 990 0.071 8.43 Example 4 975 0.065 7.12

Claims

1. A low-absorbency matte surface fabric, characterized in that: The preparation raw materials include: glass fiber grey cloth, Teflon coating, and the Teflon coating is formed after being cured. The thickness ratio of the glass fiber grey cloth to the Teflon coating is (1-5): (0.4-0.8); In parts by weight, the Teflon coating includes: 55-70 parts of fluorocarbon emulsion, 0.1-0.5 parts of polysiloxane, 1-5 parts of alcohol ester solution, 1-3 parts of silane coupling agent, 1-5 parts of thickener, and 10-30 parts of water; The polysiloxane is polyether siloxane; the alcohol ester solution is hexadecanol ester; the silane coupling agent is 3-(2,3-epoxypropoxy)propyltrimethoxysilane; The thickener is polyvinyl pyrrolidone.

2. A process for preparing the low-adsorbability matte surface fabric according to claim 1, characterized in that: The following steps are involved: (1) Pretreatment: Bake the glass fiber cloth to remove moisture and dewax at a temperature of 250-280°C; (2) Base coating: Apply Teflon coating evenly to the surface of glass fiber cloth; (3) Pre-baking: Set the temperature to 330-340°C for pre-baking; (4) Secondary coating and baking, the baking temperature is 340-350℃; (5) Coat again and bake at a temperature of 350-360°C. Repeat step (5) 3-5 times to obtain the product.

3. The process for preparing the low-adsorbability matte surface fabric according to claim 2, characterized in that: The coating amount of Teflon coating in step (2) is 0.5-0.8 kg / m 2 .

4. The process for preparing the low-adsorbability matte surface fabric according to claim 2, characterized in that: The step (1) is performed independently, and the steps (2) to (5) are performed continuously.

5. An application of the low-absorption matte surface fabric according to claim 1, characterized in that: Applicable to the surface of rubber and metal materials.

6. The use of the low-absorption matte surface fabric according to claim 5, characterized in that: Applied to the surface of rubber or metal press pads.