A self-powered flexible sensor and its preparation method
By using materials such as nano-zinc oxide and carbon nanotubes in flexible sensors, the piezoelectric properties and tensile resistance of the sensors are enhanced, which solves the problem of weakened conductivity of flexible sensors in soft robot applications and achieves high-performance automatic sensors. Powered flexible sensor.
Patent Information
- Application Number
- CN202210820996.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-13
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-07-13
AI Technical Summary
In the application of soft robots, existing flexible sensors have poor flexibility and poor tensile properties of electrode materials, resulting in weakening or loss of electrode conductivity, and cannot meet the requirements of soft robots for sensor mechanical properties and monitoring performance.
Nano-zinc oxide is used as the piezoelectric material, combined with carbon nanotubes, graphene or carbon powder as the flexible electrode layer. By growing zinc oxide nanosheets and flexible film layers, a self-powered flexible sensor is formed to enhance the piezoelectric performance and resistance of the material. Tensile properties.
It achieves the excellent flexibility and stretch recovery of the flexible sensor, maintains good electrical conductivity and mechanical properties, avoids electrode breakage and loss of electrical conductivity, and meets the mechanical and monitoring performance requirements of the sensor for soft robots.
Smart Images

Figure CN115219571B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrochemical sensors and relates to a self-powered flexible sensor and a preparation method thereof. Background Art
[0002] In the field of soft robotics, the deployment of sensors is often limited by limited lifespan, maintenance costs, and heavy batteries. In recent years, self-powered piezoelectric sensors implanted externally or internally can provide long-term body and environment monitoring behaviors and expand sensory output, greatly meeting the needs of soft robotics and expanding the application range of soft robotics. However, among various commonly used piezoelectric materials, inorganic piezoelectric materials such as BaTiO 3 , lead zirconate titanate (PZT) and lead niobate-lead titanate (PMN-PT), etc., although they have high piezoelectric coefficients, their inherent rigidity limits their application in flexible sensors.
[0003] Since most flexible sensors, such as those using polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyethersulfone (PES), Kapton film or paper as substrates, still cannot meet the flexibility requirements of soft robots in practical applications, there is an obvious defect that does not match the mechanical performance requirements of soft robots. At the same time, since the electrodes of flexible sensors are usually platinum (Pt), copper (Cu) or indium tin oxide (ITO), and are set on polymer films by sputtering, these metal-based electrodes are very easy to break when stretched, which weakens or even completely loses the conductivity of the electrodes.
[0004] Therefore, there is an urgent need for a flexible sensor with excellent flexibility and stretch recovery, stable chemical composition, and superior sensing detection performance to meet the soft robot's requirements for the mechanical properties of flexible sensors, which will promote the development of soft mechanical robots. Summary of the invention
[0005] The purpose of the present invention is to solve the problem in the prior art that the conductivity of the sensor electrode is weakened or even lost due to the poor flexibility of the sensor and the poor tensile properties of the electrode material, and the mechanical properties and monitoring performance requirements of the soft robot for the sensor cannot be met. A self-powered flexible sensor and a preparation method thereof are provided. The sensor has excellent flexibility and tensile recovery, stable chemical composition, and superior sensing and monitoring performance. The micromorphology of the zinc oxide material is changed by introducing metal ions as dopants to enhance the piezoelectric properties of the material, thereby enhancing the mechanoelectric response sensitivity of the self-powered sensor, which can well match the requirements of the soft robot for mechanical properties and monitoring performance.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention provides a self-powered flexible sensor, comprising a first flexible film layer, on which a first flexible electrode layer, a zinc oxide nanosheet layer, a second flexible film layer, a second flexible electrode layer and a third flexible film layer are sequentially arranged; the first flexible electrode layer and the second flexible electrode layer are respectively led out with wires for collecting and deriving electrical signals of the sensor; the first flexible electrode layer and the second flexible electrode layer are carbon nanotube electrode layers, graphene electrode layers or carbon powder electrode layers.
[0008] Preferably, the first flexible film layer, the second flexible film layer and the third flexible film layer are polydimethylsiloxane prepolymer films.
[0009] A method for preparing the self-powered flexible sensor as described above comprises the following steps:
[0010] S1: preparing a first flexible film layer as a flexible substrate;
[0011] S2: preparing a first flexible electrode layer on the surface of the flexible substrate;
[0012] S3: growing a zinc oxide nanosheet layer on the surface of the first flexible electrode layer;
[0013] S4: coating a second flexible film layer on the surface of the zinc oxide nanosheet layer;
[0014] S5: Pressing a second flexible electrode layer on the surface of the second flexible film layer;
[0015] S6: coating a third flexible film layer on the surface of the second flexible electrode layer;
[0016] S7: Connect the wires to the first flexible electrode layer and the second flexible electrode layer to complete the preparation of the self-powered flexible sensor.
[0017] Preferably, the first flexible film layer, the second flexible film layer and the third flexible film layer are prepared by:
[0018] Weighing polydimethylsiloxane prepolymer and polydimethylsiloxane prepolymer curing agent, mixing, and stirring evenly to form a polydimethylsiloxane prepolymer mixed liquid;
[0019] The bubbles in the polydimethylsiloxane prepolymer mixed liquid are discharged, and the bubble-free polydimethylsiloxane prepolymer mixed liquid is coated on the carrier, heated and cured at 65° C. to 85° C. for 10 min to 30 min, washed, and dried to form a flexible film layer.
[0020] Preferably, the mass ratio of the polydimethylsiloxane prepolymer to the polydimethylsiloxane prepolymer curing agent is 10:1.
[0021] Preferably, the preparation method of the first flexible electrode layer and the second flexible electrode layer is:
[0022] Dissolving a surfactant in water to form a surfactant aqueous solution;
[0023] dispersing the carbon material in an aqueous surfactant solution to form a carbon material dispersion;
[0024] The carbon material dispersion is deposited on a filter membrane by vacuum filtration, and allowed to stand at room temperature until the solvent is completely evaporated, and the carbon material on the filter membrane is transferred and bonded to the desired carrier surface, and dried to form a flexible electrode layer.
[0025] Preferably, the surfactant is an alkylbenzene sulfonate, an alkyl sulfonate ester, an alkyl sulfonate, an alkyl sulfate, a fluorinated fatty acid salt, a polysiloxane, a fatty alcohol sulfate, a fatty alcohol polyoxyethylene ether sulfate, an α-olefin sulfonate, a fatty alcohol polyoxyethylene ether phosphate, an alkyl alcohol amide, an alkyl sulfonic acid acetamide, an alkyl succinate sulfonate, an alcoholamine alkylbenzene sulfonate, a cyclopentaneate, an alkylphenol sulfonate or a polyoxyethylene monolaurate.
[0026] Preferably, the mass ratio of the carbon material to the surfactant is: (1:200) to (1:50); the concentration of the surfactant aqueous solution is 2.5 mg / mL to 20 mg / mL.
[0027] Preferably, the specific operation of growing the zinc oxide nanosheet layer on the surface of the first flexible electrode layer is:
[0028] Dissolving zinc acetate and alkali in an ethanol solution to form a first mixed solution;
[0029] Dissolving zinc salt, aluminum salt and hexamethylidene tetramine in an ethanol solution to form a second mixed solution;
[0030] Spin-coat the first mixed solution on the surface of the first flexible electrode layer, dry it, place it in the second mixed solution, and heat it at a constant temperature of 75° C. to 95° C. for 5 h to 6 h;
[0031] The new second mixed liquid is replaced repeatedly, and each time the second mixed liquid is replaced, it is repeatedly placed in a constant temperature heating condition of 75°C to 95°C for 5h to 6h until a densely arranged zinc oxide nanostructure is grown on the surface of the first flexible electrode layer, that is, the growth of the zinc oxide nanosheet layer is completed.
[0032] Preferably, in the first mixed solution, the concentration of zinc acetate is 5mmol / L to 15mmol / L; the concentration of alkali is 20mmol / L to 50mmol / L; in the second mixed solution, the zinc salt is zinc nitrate or zinc chloride, and the concentration of the zinc salt is 20mmol / L to 50mmol / L; the aluminum salt is aluminum nitrate or aluminum chloride, and the concentration of the aluminum salt is 6mmol / L to 8mmol / L; the concentration of hexamethylendetate is 20mmol / L to 50mmol / L.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] The present invention provides a self-powered flexible sensor. The flexible sensor uses nano zinc oxide as a piezoelectric material. The raw material is cheap and easily available. The hexagonal wurtzite structure is the most stable structure under natural conditions. It can generate piezoelectric potential under external tensile / compressive strain, and the piezoelectric tensor is large, the electromechanical coupling coefficient is large, and the piezoelectric performance is good. It can be directly synthesized on a flexible substrate. With the arrangement of a flexible film layer and a flexible electrode layer, the flexibility of the sensor can be improved, the energy consumption can be reduced, and the influence of complex deformations such as long-term torsion, stretching and bending of the sensor on its electrode and overall monitoring performance can be reduced. Secondly, the sensor uses carbon materials including carbon nanotubes, graphene or carbon powder as a flexible electrode layer, which not only has very good electrical conductivity, but also improves the tensile resistance of the flexible electrode, so that it can still maintain very good mechanical properties and electrical conductivity in a stretched state, thereby avoiding the breakage of the sensor electrode due to stretching, or even the loss of conductivity.
[0035] The present invention also provides a method for preparing a self-powered flexible sensor, which can achieve seamless connection and effective integration of rigid piezoelectric ceramic nano zinc oxide with a non-piezoelectric soft material flexible film layer and a flexible electrode layer, which helps to optimize the structural design of piezoelectric devices, analyze the feasibility of using piezoelectric nanomaterials as flexible sensors, and provide a theoretical basis for the application of piezoelectric materials in flexible sensor devices and piezoelectric nanogenerators. The method is simple in process and easy to implement, and can obtain a self-powered flexible sensor with good flexibility and excellent monitoring performance without high-temperature treatment;
[0036] Secondly, the present invention effectively controls the reaction and changes the microscopic morphology of nano zinc oxide crystals through dopants to enhance the piezoelectric output performance, and directly grows the zinc oxide nanoarray on the surface of the first flexible electrode layer to form an elastic piezoelectric film, which further enables the sensor to maintain stability during complex deformation movements such as long-term twisting, stretching, bending, etc.
[0037] The flexible electrode layer is prepared by vacuum filtration method. Compared with traditional metal electrodes, it can maintain better mechanical properties and conductive properties under stretching. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0039] Figure 1 This is a structural diagram of the self-powered flexible sensor of the present invention.
[0040] Figure 2 This is a flow chart of the method for preparing the self-powered flexible sensor of the present invention.
[0041] Figure 3 This is a scanning electron microscope image of the zinc oxide nanosheet layer of the self-powered flexible sensor in an embodiment of the present invention.
[0042] Figure 4 This is a torsion and stretching test diagram of the self-powered flexible sensor in an embodiment of the present invention.
[0043] Figure 5 This is a tensile strength test curve of the self-powered flexible sensor in an embodiment of the present invention.
[0044] Figure 6 Scanning electron microscope images of the self-powered flexible sensor based on the zinc oxide nanosheet piezoelectric structure prepared in the embodiment of the present invention and the traditional self-powered flexible sensor based on the zinc oxide nanowire piezoelectric structure, as well as a comparison diagram of the voltage output curves of the corresponding excitation test under the same conditions.
[0045] Figure 7 It is a bar graph comparing the voltage outputs of the excitation tests of the self-powered flexible sensor based on the piezoelectric structure of zinc oxide nanosheets prepared in the embodiment of the present invention and the traditional self-powered flexible sensor based on the piezoelectric structure of zinc oxide nanowires.
[0046] Among them, a-first flexible film layer, b-first flexible electrode layer, c-zinc oxide nanosheet layer, d-second flexible film layer, e-second flexible electrode layer, f-third flexible film layer. DETAILED DESCRIPTION
[0047] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0048] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0050] In the description of the embodiments of the present invention, it should be noted that if the terms "upper", "lower", "horizontal", "inner", etc. indicate an orientation or positional relationship based on the orientation or positional relationship shown in the drawings, or the orientation or positional relationship in which the product of the invention is usually placed when in use, it is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.
[0051] In addition, if the term "horizontal" appears, it does not mean that the component is required to be absolutely horizontal, but can be slightly tilted. For example, "horizontal" only means that its direction is more horizontal than "vertical", which does not mean that the structure must be completely horizontal, but can be slightly tilted.
[0052] In the description of the embodiments of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal connection of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0053] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0054] See also Figure 1The present invention provides a self-powered flexible sensor, comprising a first flexible film layer a and a third flexible film layer f, wherein a first flexible electrode layer b, a zinc oxide nanosheet layer c, a second flexible film layer d and a second flexible electrode layer e are sequentially arranged between the first flexible film layer a and the third flexible film layer f; the first flexible electrode layer b and the second flexible electrode layer e are respectively led out with wires for collecting and deriving electrical signals of the sensor; the first flexible electrode layer b and the second flexible electrode layer e are carbon nanotube electrode layers, graphene electrode layers or carbon powder electrode layers; the first flexible film layer a, the second flexible film layer d and the third flexible film layer f are polydimethylsiloxane prepolymer films.
[0055] See also Figure 2 The present invention also provides a method for preparing the above-mentioned self-powered flexible sensor, comprising the following steps:
[0056] S1: Prepare a first flexible film layer a as a flexible substrate:
[0057] The specific operation is as follows: weigh the polydimethylsiloxane prepolymer and the polydimethylsiloxane prepolymer curing agent respectively at a mass ratio of 10:1, mix and stir evenly to form a polydimethylsiloxane prepolymer mixed liquid;
[0058] The bubbles in the polydimethylsiloxane prepolymer mixed liquid are discharged, and the bubble-free polydimethylsiloxane prepolymer mixed liquid is coated on the carrier, heated and cured at 65° C. to 85° C. for 10 min to 30 min, washed, and dried to form a flexible film layer.
[0059] S2: On the surface of the flexible substrate, prepare the first flexible electrode layer b:
[0060] The specific operation is as follows: alkylbenzene sulfonate, alkyl sulfonate ester salt, alkyl sulfonate, alkyl sulfate, fluorinated fatty acid salt, polysiloxane, fatty alcohol sulfate, fatty alcohol polyoxyethylene ether sulfate, α-olefin sulfonate, fatty alcohol polyoxyethylene ether phosphate, alkyl alcohol amide, alkyl sulfonic acid acetamide, alkyl succinate sulfonate, alcoholamine alkylbenzene sulfonate, cyclopentaneate, alkylphenol sulfonate or polyoxyethylene monolaurate are dissolved in water as a surfactant to form a surfactant aqueous solution; wherein the concentration of the surfactant aqueous solution is 2.5 mg / mL to 20 mg / mL;
[0061] Dispersing the carbon material in a surfactant aqueous solution to form a carbon material dispersion; the mass ratio of the carbon material to the surfactant is: (1:200) to (1:50);
[0062] The carbon material dispersion is deposited on a filter membrane by vacuum filtration and allowed to stand at room temperature until the solvent is completely evaporated. The carbon material on the filter membrane is transferred and bonded to the desired carrier surface, i.e., the surface of the first flexible film layer a in S1, and dried to form a first flexible electrode layer b.
[0063] S3: growing a zinc oxide nanosheet layer c on the surface of the first flexible electrode layer b;
[0064] The specific operation is: dissolving zinc acetate and alkali in an ethanol solution to form a first mixed solution; in the first mixed solution, the zinc acetate concentration is 5mmol / L to 15mmol / L; the alkali concentration is 20mmol / L to 50mmol / L;
[0065] Dissolving zinc salt, aluminum salt and hexamethonium tetramine in an ethanol solution to form a second mixed solution; in the second mixed solution, the zinc salt is zinc nitrate or zinc chloride, and the concentration of the zinc salt is 20mmol / L to 50mmol / L; the aluminum salt is aluminum nitrate or aluminum chloride, and the concentration of the aluminum salt is 6mmol / L to 8mmol / L; the concentration of hexamethonium tetramine is 20mmol / L to 50mmol / L;
[0066] Spin-coat the first mixed solution on the surface of the first flexible electrode layer b, dry it, place it in the second mixed solution, and heat it at a constant temperature of 75° C. to 95° C. for 5 h to 6 h;
[0067] The new second mixed liquid is replaced repeatedly, and each time the second mixed liquid is replaced, it is repeatedly placed under constant temperature heating at 75°C to 95°C for 5h to 6h until a densely arranged zinc oxide nanosheet structure grows on the surface of the first flexible electrode layer b, that is, the growth of the zinc oxide nanosheet layer c is completed.
[0068] S4: coating a second flexible film layer d on the surface of the zinc oxide nanosheet layer c;
[0069] The specific operation is as follows: spin-coating the polydimethylsiloxane prepolymer mixture prepared in S1 on the surface of the zinc oxide nanosheet layer c, heating and curing at 65°C to 85°C for 10min to 30min, washing, and drying to form a second flexible film layer d;
[0070] S5: Pressing the second flexible electrode layer e on the surface of the second flexible film layer d;
[0071] The specific operation is as follows: the carbon material dispersion prepared in S2 is deposited on the filter membrane by vacuum filtration, and is allowed to stand at room temperature until the solvent is completely evaporated, and the carbon material on the filter membrane is transferred and bonded to the desired carrier surface, i.e., the surface of the second flexible film layer d, and dried to form the second flexible electrode layer e;
[0072] S6: coating a third flexible film layer f on the surface of the second flexible electrode layer e;
[0073] The specific operation is as follows: spin-coating the polydimethylsiloxane prepolymer mixed solution prepared in S1 on the surface of the second flexible electrode layer e, heating and curing at 65° C. to 85° C. for 10 min to 30 min, washing, and drying to form a third flexible film layer f;
[0074] S7: Connect the wires to the first flexible electrode layer b and the second flexible electrode layer e to complete the preparation of the self-powered flexible sensor.
[0075] Example 1
[0076] Prepare a glass sheet of 50 mm × 50 mm × 2 mm required for the test; weigh 10 g of polydimethylsiloxane prepolymer and 1 g of polydimethylsiloxane prepolymer curing agent, the polydimethylsiloxane prepolymer curing agent is a supporting product of polydimethylsiloxane prepolymer, the product name is: SYLGARD TM 184 Silicone Elastomer Base; mixing, stirring at a uniform speed in the same direction to evenly mix the polydimethylsiloxane prepolymer and the polydimethylsiloxane prepolymer curing agent to form a polydimethylsiloxane prepolymer mixed liquid;
[0077] The polydimethylsiloxane prepolymer mixed liquid is placed in a vacuum drying oven and allowed to stand, and vacuumized until all bubbles in the polydimethylsiloxane prepolymer mixed liquid are discharged; the bubble-free polydimethylsiloxane prepolymer mixed liquid is evenly dripped on a pre-prepared glass sheet, and the polydimethylsiloxane prepolymer mixed liquid is spin-coated on the glass sheet using a glue spreader at a speed of 1000 rpm / min and a spin coating time of 1 minute, and the polydimethylsiloxane prepolymer mixed liquid is placed in a constant temperature heating box and heated and cured at 65° C. for 30 minutes, and then cleaned in an ultrasonic cleaner with deionized water, acetone and anhydrous ethanol for 5 minutes to 15 minutes, and dried at 65° C. for use, to form a first flexible film layer a.
[0078] Weigh 1 g of sodium dodecyl sulfate powder and 5 mg of multi-walled carbon nanotube powder, place in 100 mL of deionized water, and sonicate for 20 min to disperse them evenly to form a multi-walled carbon nanotube dispersion;
[0079] A layer of 50nm pore size PTFE filter membrane is placed on the sand core of the vacuum filtration funnel, and the multi-walled carbon nanotube dispersion is poured into the vacuum filtration funnel. After vacuum filtration, a layer of carbon nanotube electrode sheet is deposited on the PTFE filter membrane. The mixture is allowed to stand at room temperature until the solvent is completely evaporated. The multi-walled carbon nanotube material on the filter membrane is transferred and bonded to the surface of the first flexible film layer a, and dried to form a first flexible electrode layer b.
[0080] Weigh 92 mg of zinc acetate and 80 mg of sodium hydroxide respectively, place in 100 mL of anhydrous ethanol solution, and ultrasonically disperse for 20 min until the mixture is uniformly mixed to form a first mixed solution;
[0081] Weigh 470 mg of zinc nitrate, 350 mg of hexamethylidene tetramine and 140 mg of aluminum nitrate respectively, put them into 100 mL of anhydrous ethanol, and ultrasonically disperse them in an ultrasonic cleaning machine for 20 min until they are uniformly mixed to form a second mixed solution;
[0082] The first mixed solution was spin-coated on the surface of the first flexible electrode layer b at a rotation speed of 1000 rpm / min, and dried in a constant temperature heating box at 70°C until completely dry. The surface of the first flexible electrode layer b was placed downward in the second mixed solution, and heated at a constant temperature of 85°C for 5 hours;
[0083] The new second mixed solution was replaced three times, and each time the second mixed solution was replaced, it was repeatedly placed under constant temperature heating at 85° C. for 5 h until a densely arranged zinc oxide nanosheet structure grew on the surface of the first flexible electrode layer b, that is, the growth of the zinc oxide nanosheet layer c was completed.
[0084] On the surface of the zinc oxide nanosheet layer c, a layer of polydimethylsiloxane prepolymer mixed liquid is spin-coated at a rotation speed of 3000 rpm / min for a spin coating time of 2 minutes, heated and cured at 65° C. for 20 minutes, cleaned in an ultrasonic cleaner with deionized water, acetone and anhydrous ethanol for 5 minutes to 15 minutes respectively, and dried at 65° C. to form a second flexible film layer d on the surface of the zinc oxide nanosheet layer c;
[0085] The multi-walled carbon nanotube dispersion is deposited on a filter membrane by vacuum filtration, and allowed to stand at room temperature until the solvent is completely evaporated, and the multi-walled carbon nanotube material on the filter membrane is transferred and bonded to the surface of the second flexible film layer d, and dried to form a second flexible electrode layer e;
[0086] The polydimethylsiloxane prepolymer mixed liquid is spin-coated on the surface of the second flexible electrode layer e at 3000 rpm / min for 2 min, heated and cured at 65° C. for 10 min, washed, and dried to form a third flexible film layer f;
[0087] The first flexible electrode layer b and the second flexible electrode layer e are glued with copper tape and connected with wires to complete the preparation of the self-powered flexible sensor.
[0088] Example 2
[0089] Prepare a glass sheet of 50 mm×50 mm×2 mm required for the test; weigh 10 g of polydimethylsiloxane prepolymer and 1 g of polydimethylsiloxane prepolymer curing agent, mix them, and stir them at a uniform speed in the same direction to make the polydimethylsiloxane prepolymer and the polydimethylsiloxane prepolymer curing agent evenly mixed to form a polydimethylsiloxane prepolymer mixed liquid;
[0090] The polydimethylsiloxane prepolymer mixed liquid is placed in a vacuum drying oven and allowed to stand, and vacuumized until all bubbles in the polydimethylsiloxane prepolymer mixed liquid are discharged; the bubble-free polydimethylsiloxane prepolymer mixed liquid is evenly dripped on a pre-prepared glass sheet, and the polydimethylsiloxane prepolymer mixed liquid is spin-coated on the glass sheet using a glue spreader at a speed of 1000 rpm / min and a spin coating time of 1 minute, and the polydimethylsiloxane prepolymer mixed liquid is placed in a constant temperature heating box and heated and cured at 70° C. for 20 minutes, and then cleaned in an ultrasonic cleaning machine with deionized water, acetone and anhydrous ethanol for 5 minutes to 15 minutes, and dried at 65° C. for use, to form a first flexible film layer a.
[0091] Weigh 0.25 g of sodium dodecylbenzene sulfonate powder and 2.5 mg of multi-walled carbon nanotube powder, place in 100 mL of deionized water, and sonicate for 20 min to disperse them evenly to form a multi-walled carbon nanotube dispersion;
[0092] A layer of 50nm pore size PTFE filter membrane is placed on the sand core of the vacuum filtration funnel, and the multi-walled carbon nanotube dispersion is poured into the vacuum filtration funnel. After vacuum filtration, a layer of carbon nanotube electrode sheet is deposited on the PTFE filter membrane. The mixture is allowed to stand at room temperature until the solvent is completely evaporated. The multi-walled carbon nanotube material on the filter membrane is transferred and bonded to the surface of the first flexible film layer a, and dried to form a first flexible electrode layer b.
[0093] 183.5 mg of zinc acetate and 120 mg of sodium hydroxide were weighed respectively, placed in 100 mL of anhydrous ethanol solution, and ultrasonically dispersed for 30 min until the mixture was uniformly mixed to form a first mixed solution;
[0094] 272.6 mg of zinc chloride, 280.4 mg of hexamethylidene tetramine and 80 mg of aluminum chloride were weighed respectively and placed in 100 mL of anhydrous ethanol, and ultrasonically dispersed in an ultrasonic cleaning machine for 20 min until the mixture was uniformly mixed to form a second mixed solution;
[0095] The first mixed solution was spin-coated on the surface of the first flexible electrode layer b at a rotation speed of 1000 rpm / min, and dried in a constant temperature heating box at 75°C until completely dry. The surface of the first flexible electrode layer b was placed downward in the second mixed solution, and heated at a constant temperature of 75°C for 6 hours;
[0096] The new second mixed solution was replaced three times, and each time the second mixed solution was replaced, it was repeatedly placed under constant temperature heating at 75° C. for 6 hours until a densely arranged zinc oxide nanosheet structure grew on the surface of the first flexible electrode layer b, that is, the growth of the zinc oxide nanosheet layer c was completed.
[0097] On the surface of the zinc oxide nanosheet layer c, a layer of polydimethylsiloxane prepolymer mixed liquid is spin-coated at a rotation speed of 3000 rpm / min for a spin coating time of 2 minutes, heated and cured at 65° C. for 20 minutes, cleaned in an ultrasonic cleaner with deionized water, acetone and anhydrous ethanol for 5 minutes to 15 minutes respectively, and dried at 65° C. to form a second flexible film layer d on the surface of the zinc oxide nanosheet layer c;
[0098] The multi-walled carbon nanotube dispersion is deposited on a filter membrane by vacuum filtration, and allowed to stand at room temperature until the solvent is completely evaporated, and the multi-walled carbon nanotube material on the filter membrane is transferred and bonded to the surface of the second flexible film layer d, and dried to form a second flexible electrode layer e;
[0099] The polydimethylsiloxane prepolymer mixed liquid is spin-coated on the surface of the second flexible electrode layer e at 3000 rpm / min for 2 min, heated and cured at 65° C. for 10 min, washed, and dried to form a third flexible film layer f;
[0100] The first flexible electrode layer b and the second flexible electrode layer e are glued with copper tape and connected with wires to complete the preparation of the self-powered flexible sensor.
[0101] Example 3
[0102] Prepare a glass sheet of 50 mm×50 mm×2 mm required for the test; weigh 20 g of polydimethylsiloxane prepolymer and 2 g of polydimethylsiloxane prepolymer curing agent, mix them, and stir them at a uniform speed in the same direction to make the polydimethylsiloxane prepolymer and the polydimethylsiloxane prepolymer curing agent evenly mixed to form a polydimethylsiloxane prepolymer mixed liquid;
[0103] The polydimethylsiloxane prepolymer mixed liquid is placed in a vacuum drying oven and allowed to stand, and vacuumized until all bubbles in the polydimethylsiloxane prepolymer mixed liquid are discharged; the bubble-free polydimethylsiloxane prepolymer mixed liquid is evenly dripped on a pre-prepared glass sheet, and the polydimethylsiloxane prepolymer mixed liquid is spin-coated on the glass sheet using a glue spreader at a speed of 1000 rpm / min and a spin coating time of 1 minute, and the polydimethylsiloxane prepolymer mixed liquid is placed in a constant temperature heating box and heated and cured at 75° C. for 30 minutes, and then cleaned in an ultrasonic cleaning machine with deionized water, acetone and anhydrous ethanol for 5 minutes to 15 minutes, and dried at 70° C. for use, to form a first flexible film layer a.
[0104] Weigh 0.5 g of polysiloxane and 3.3 mg of carbon powder, place in 100 mL of deionized water, and ultrasonicate for 30 min to disperse them evenly to form a carbon powder dispersion;
[0105] A layer of 50nm pore size PTFE filter membrane is placed on the sand core of the vacuum filtration funnel, and the carbon powder dispersion is poured into the vacuum filtration funnel. After vacuum filtration, a layer of carbon powder electrode sheet is deposited on the PTFE filter membrane. The mixture is allowed to stand at room temperature until the solvent is completely evaporated. The carbon powder material on the filter membrane is transferred and bonded to the surface of the first flexible film layer a, and dried to form a first flexible electrode layer b.
[0106] 128.45 mg of zinc acetate and 160 mg of sodium hydroxide were weighed respectively, placed in 100 mL of anhydrous ethanol solution, and ultrasonically dispersed for 25 min until the mixture was uniformly mixed to form a first mixed solution;
[0107] Weigh 639 mg of zinc nitrate, 420 mg of hexamethylidene tetramine and 149 mg of aluminum nitrate respectively, put them into 100 mL of anhydrous ethanol, and ultrasonically disperse them in an ultrasonic cleaning machine for 30 min until they are uniformly mixed to form a second mixed solution;
[0108] The first mixed solution was spin-coated on the surface of the first flexible electrode layer b at a speed of 1000 rpm / min for 1 min, and then placed in a constant temperature heating box at 65°C to dry until completely dry. The surface of the first flexible electrode layer b was placed downward in the second mixed solution, and heated at a constant temperature of 90°C for 5.5 hours;
[0109] The new second mixed solution was replaced three times, and each time the second mixed solution was replaced, it was repeatedly placed at 90° C. and heated at a constant temperature for 5.5 h until a densely arranged zinc oxide nanosheet structure was grown on the surface of the first flexible electrode layer b, that is, the growth of the zinc oxide nanosheet layer c was completed.
[0110] On the surface of the zinc oxide nanosheet layer c, a layer of polydimethylsiloxane prepolymer mixed liquid is spin-coated at a rotation speed of 3000 rpm / min and a spin coating time of 2 minutes, and heated and cured at 70° C. for 15 minutes, and then cleaned in an ultrasonic cleaning machine with deionized water, acetone and anhydrous ethanol for 5 minutes to 15 minutes, and dried at 65° C. to form a second flexible film layer d on the surface of the zinc oxide nanosheet layer c;
[0111] The carbon powder dispersion is deposited on the filter membrane by vacuum filtration, and is allowed to stand at room temperature until the solvent is completely evaporated, and the carbon powder material on the filter membrane is transferred and bonded to the surface of the second flexible film layer d, and dried to form the second flexible electrode layer e;
[0112] The polydimethylsiloxane prepolymer mixed liquid is spin-coated on the surface of the second flexible electrode layer e at 3000 rpm / min for 2 min, heated and cured at 65° C. for 10 min, washed, and dried to form a third flexible film layer f;
[0113] The first flexible electrode layer b and the second flexible electrode layer e are glued with copper tape and connected with wires to complete the preparation of the self-powered flexible sensor.
[0114] Example 4
[0115] Prepare a glass sheet of 50 mm×50 mm×2 mm required for the test; weigh 10 g of polydimethylsiloxane prepolymer and 1 g of polydimethylsiloxane prepolymer curing agent, mix them, and stir them at a uniform speed in the same direction to make the polydimethylsiloxane prepolymer and the polydimethylsiloxane prepolymer curing agent evenly mixed to form a polydimethylsiloxane prepolymer mixed liquid;
[0116] The polydimethylsiloxane prepolymer mixed liquid is placed in a vacuum drying oven and allowed to stand, and vacuumized until all bubbles in the polydimethylsiloxane prepolymer mixed liquid are discharged; the bubble-free polydimethylsiloxane prepolymer mixed liquid is evenly dripped on a pre-prepared glass sheet, and the polydimethylsiloxane prepolymer mixed liquid is spin-coated on the glass sheet using a glue spreader at a speed of 1000 rpm / min and a spin coating time of 1 minute, and the polydimethylsiloxane prepolymer mixed liquid is placed in a constant temperature heating box and heated and cured at 80° C. for 10 minutes, and then cleaned in an ultrasonic cleaning machine with deionized water, acetone and anhydrous ethanol for 5 minutes to 15 minutes, and dried at 65° C. for use, to form a first flexible film layer a.
[0117] Weigh 2 g of alkylsulfonic acid acetamide and 10 mg of multi-walled carbon nanotube powder, place them in 100 mL of deionized water, and sonicate for 30 min to disperse them evenly to form a multi-walled carbon nanotube dispersion;
[0118] A layer of 50nm pore size PTFE filter membrane is placed on the sand core of the vacuum filtration funnel, and the multi-walled carbon nanotube dispersion is poured into the vacuum filtration funnel. After vacuum filtration, a layer of carbon nanotube electrode sheet is deposited on the PTFE filter membrane. The mixture is allowed to stand at room temperature until the solvent is completely evaporated, and the carbon material on the filter membrane is transferred and bonded to the surface of the first flexible film layer a, and dried to form a first flexible electrode layer b.
[0119] Weigh 220.2 mg of zinc acetate and 280 mg of potassium hydroxide respectively, place in 100 mL of anhydrous ethanol solution, and ultrasonically disperse for 25 min until the mixture is uniformly mixed to form a first mixed solution;
[0120] 757.6 mg of zinc nitrate, 490.6 mg of hexamethylidene tetramine and 170.4 mg of aluminum nitrate were respectively weighed and placed in 100 mL of anhydrous ethanol, and ultrasonically dispersed in an ultrasonic cleaning machine for 30 min until the mixture was uniformly mixed to form a second mixed solution;
[0121] The first mixed solution was spin-coated on the surface of the first flexible electrode layer b at a speed of 1000 rpm / min for 1 min, and then placed in a constant temperature heating box at 68°C to dry until completely dry. The surface of the first flexible electrode layer b was placed downward in the second mixed solution, and heated at a constant temperature of 95°C for 5 h;
[0122] The new second mixed solution was replaced three times, and each time the second mixed solution was replaced, it was repeatedly placed under constant temperature heating at 95° C. for 5 h until a densely arranged zinc oxide nanosheet structure grew on the surface of the first flexible electrode layer b, that is, the growth of the zinc oxide nanosheet layer c was completed.
[0123] On the surface of the zinc oxide nanosheet layer c, a layer of polydimethylsiloxane prepolymer mixed liquid is spin-coated at a rotation speed of 3000 rpm / min and a spin coating time of 2 minutes, and heated and cured at 75° C. for 10 minutes, and then cleaned in an ultrasonic cleaning machine with deionized water, acetone and anhydrous ethanol for 5 minutes to 15 minutes, and dried at 70° C. to form a second flexible film layer d on the surface of the zinc oxide nanosheet layer c;
[0124] The multi-walled carbon nanotube dispersion is deposited on a filter membrane by vacuum filtration, and allowed to stand at room temperature until the solvent is completely evaporated, and the multi-walled carbon nanotube material on the filter membrane is transferred and bonded to the surface of the second flexible film layer d, and dried to form a second flexible electrode layer e;
[0125] The polydimethylsiloxane prepolymer mixed liquid is spin-coated on the surface of the second flexible electrode layer e at 3000 rpm / min for 2 min, heated and cured at 75° C. for 10 min, washed, and dried to form a third flexible film layer f;
[0126] The first flexible electrode layer b and the second flexible electrode layer e are glued with copper tape and connected with wires to complete the preparation of the self-powered flexible sensor.
[0127] Example 5
[0128] Prepare a glass sheet of 50 mm×50 mm×2 mm required for the test; weigh 10 g of polydimethylsiloxane prepolymer and 1 g of polydimethylsiloxane prepolymer curing agent, mix them, and stir them at a uniform speed in the same direction to make the polydimethylsiloxane prepolymer and the polydimethylsiloxane prepolymer curing agent evenly mixed to form a polydimethylsiloxane prepolymer mixed liquid;
[0129] The polydimethylsiloxane prepolymer mixed liquid is placed in a vacuum drying oven and allowed to stand, and vacuumized until all bubbles in the polydimethylsiloxane prepolymer mixed liquid are discharged; the bubble-free polydimethylsiloxane prepolymer mixed liquid is evenly dripped on a pre-prepared glass sheet, and the polydimethylsiloxane prepolymer mixed liquid is spin-coated on the glass sheet using a glue spreader at a speed of 1000 rpm / min and a spin coating time of 1 minute, and the polydimethylsiloxane prepolymer mixed liquid is placed in a constant temperature heating box and heated and cured at 70° C. for 25 minutes, and then cleaned in an ultrasonic cleaning machine with deionized water, acetone and anhydrous ethanol for 5 minutes to 15 minutes, and dried at 65° C. for use, to form a first flexible film layer a.
[0130] Weigh 1.5 g of sodium dodecyl sulfate powder and 12.5 mg of graphene, place in 100 mL of deionized water, and sonicate for 25 min to disperse them evenly to form a graphene dispersion;
[0131] A layer of 50 nm pore size PTFE filter membrane is placed on the sand core of the vacuum filtration funnel, and the graphene dispersion is poured into the vacuum filtration funnel. After vacuum filtration, a layer of graphene electrode sheet is deposited on the PTFE filter membrane. The mixture is allowed to stand at room temperature until the solvent is completely evaporated, and the graphene material on the filter membrane is transferred and bonded to the surface of the first flexible film layer a, and dried to form a first flexible electrode layer b.
[0132] Weigh 275.25 mg of zinc acetate and 140 mg of sodium hydroxide respectively, place in 100 mL of anhydrous ethanol solution, and ultrasonically disperse for 25 min until the mixture is uniformly mixed to form a first mixed solution;
[0133] Weigh 477 mg of zinc chloride, 560.76 mg of hexamethylidene tetramine and 102.7 mg of aluminum chloride respectively, put them into 100 mL of anhydrous ethanol, and ultrasonically disperse them in an ultrasonic cleaning machine for 20 min until they are uniformly mixed to form a second mixed solution;
[0134] The first mixed solution was spin-coated on the surface of the first flexible electrode layer b at a speed of 1000 rpm / min for 1 min, and dried in a constant temperature heating box at 63°C until completely dry. The surface of the first flexible electrode layer b was placed downward in the second mixed solution, and heated at a constant temperature of 80°C for 6 h.
[0135] The new second mixed solution was replaced three times, and each time the second mixed solution was replaced, it was repeatedly placed under constant temperature heating at 80° C. for 6 hours until a densely arranged zinc oxide nanosheet structure grew on the surface of the first flexible electrode layer b, that is, the growth of the zinc oxide nanosheet layer c was completed.
[0136] On the surface of the zinc oxide nanosheet layer c, a layer of polydimethylsiloxane prepolymer mixed liquid is spin-coated at a rotation speed of 3000 rpm / min and a spin coating time of 2 minutes, and heated and cured at 75° C. for 15 minutes, and then cleaned in an ultrasonic cleaning machine with deionized water, acetone and anhydrous ethanol for 5 minutes to 15 minutes, and dried at 65° C. to form a second flexible film layer d on the surface of the zinc oxide nanosheet layer c;
[0137] The graphene dispersion is deposited on the filter membrane by vacuum filtration, and is allowed to stand at room temperature until the solvent is completely evaporated, and the graphene material on the filter membrane is transferred and bonded to the surface of the second flexible film layer d, and dried to form a second flexible electrode layer e;
[0138] The polydimethylsiloxane prepolymer mixed liquid is spin-coated on the surface of the second flexible electrode layer e at 3000 rpm / min for 2 min, heated and cured at 75° C. for 20 min, washed, and dried to form a third flexible film layer f;
[0139] The first flexible electrode layer b and the second flexible electrode layer e are glued with copper tape and connected with wires to complete the preparation of the self-powered flexible sensor.
[0140] Example 6
[0141] Prepare a glass sheet of 50 mm×50 mm×2 mm required for the test; weigh 10 g of polydimethylsiloxane prepolymer and 1 g of polydimethylsiloxane prepolymer curing agent, mix them, and stir them at a uniform speed in the same direction to make the polydimethylsiloxane prepolymer and the polydimethylsiloxane prepolymer curing agent evenly mixed to form a polydimethylsiloxane prepolymer mixed liquid;
[0142] The polydimethylsiloxane prepolymer mixed liquid is placed in a vacuum drying oven and allowed to stand, and vacuumized until all bubbles in the polydimethylsiloxane prepolymer mixed liquid are discharged; the bubble-free polydimethylsiloxane prepolymer mixed liquid is evenly dripped on a pre-prepared glass sheet, and the polydimethylsiloxane prepolymer mixed liquid is spin-coated on the glass sheet using a glue spreader at a speed of 1000 rpm / min and a spin coating time of 1 min, and the polydimethylsiloxane prepolymer mixed liquid is placed in a constant temperature heating box and heated and cured at 85° C. for 10 min, and then cleaned in an ultrasonic cleaner with deionized water, acetone and anhydrous ethanol for 5 min to 15 min in turn, and dried at 60° C. for use, to form a first flexible film layer a.
[0143] Weigh 0.8 g of fatty alcohol polyoxyethylene ether phosphate and 10 mg of multi-walled carbon nanotube powder, place in 100 mL of deionized water, and sonicate for 20 min to disperse them evenly to form a multi-walled carbon nanotube dispersion;
[0144] A layer of 50nm pore size PTFE filter membrane is placed on the sand core of the vacuum filtration funnel, and the multi-walled carbon nanotube dispersion is poured into the vacuum filtration funnel. After vacuum filtration, a layer of carbon nanotube electrode sheet is deposited on the PTFE filter membrane. The mixture is allowed to stand at room temperature until the solvent is completely evaporated. The multi-walled carbon nanotube material on the filter membrane is transferred and bonded to the surface of the first flexible film layer a, and dried to form a first flexible electrode layer b.
[0145] Weigh 92 mg of zinc acetate and 200 mg of sodium hydroxide respectively, place them in 100 mL of anhydrous ethanol solution, and disperse them by ultrasonication for 20 min until they are uniformly mixed to form a first mixed solution;
[0146] 1.065 g of zinc nitrate, 700.1 mg of hexamethylidene tetramine and 149 mg of aluminum nitrate were respectively weighed and placed in 100 mL of anhydrous ethanol, and ultrasonically dispersed in an ultrasonic cleaning machine for 30 min until the mixture was uniformly mixed to form a second mixed solution;
[0147] The first mixed solution was spin-coated on the surface of the first flexible electrode layer b at a speed of 1000 rpm / min for 1 min, and dried in a constant temperature heating box at 65°C until completely dry. The surface of the first flexible electrode layer b was placed downward in the second mixed solution, and heated at a constant temperature of 75°C for 6 h.
[0148] The new second mixed solution was replaced three times, and each time the second mixed solution was replaced, it was repeatedly placed under constant temperature heating at 75° C. for 6 hours until a densely arranged zinc oxide nanosheet structure grew on the surface of the first flexible electrode layer b, that is, the growth of the zinc oxide nanosheet layer c was completed.
[0149] On the surface of the zinc oxide nanosheet layer c, a layer of polydimethylsiloxane prepolymer mixed liquid is spin-coated at a rotation speed of 3000 rpm / min for a spin coating time of 2 minutes, heated and cured at 65° C. for 20 minutes, cleaned in an ultrasonic cleaner with deionized water, acetone and anhydrous ethanol for 5 minutes to 15 minutes respectively, and dried at 65° C. to form a second flexible film layer d on the surface of the zinc oxide nanosheet layer c;
[0150] The multi-walled carbon nanotube dispersion is deposited on a filter membrane by vacuum filtration, and allowed to stand at room temperature until the solvent is completely evaporated, and the multi-walled carbon nanotube material on the filter membrane is transferred and bonded to the surface of the second flexible film layer d, and dried to form a second flexible electrode layer e;
[0151] The polydimethylsiloxane prepolymer mixed liquid is spin-coated on the surface of the second flexible electrode layer e at 3000 rpm / min for 2 min, heated and cured at 65° C. for 10 min, washed, and dried to form a third flexible film layer f;
[0152] The first flexible electrode layer b and the second flexible electrode layer e are glued with copper tape and connected with wires to complete the preparation of the self-powered flexible sensor.
[0153] Example 7
[0154] Prepare a glass sheet of 50 mm×50 mm×2 mm required for the test; weigh 10 g of polydimethylsiloxane prepolymer and 1 g of polydimethylsiloxane prepolymer curing agent, mix them, and stir them at a uniform speed in the same direction to make the polydimethylsiloxane prepolymer and the polydimethylsiloxane prepolymer curing agent evenly mixed to form a polydimethylsiloxane prepolymer mixed liquid;
[0155] The polydimethylsiloxane prepolymer mixed liquid is placed in a vacuum drying oven and allowed to stand, and vacuumized until all bubbles in the polydimethylsiloxane prepolymer mixed liquid are discharged; the bubble-free polydimethylsiloxane prepolymer mixed liquid is evenly dripped on a pre-prepared glass sheet, and the polydimethylsiloxane prepolymer mixed liquid is spin-coated on the glass sheet using a glue spreader at a speed of 1000 rpm / min and a spin coating time of 1 minute, and the polydimethylsiloxane prepolymer mixed liquid is placed in a constant temperature heating box and heated and cured at 85° C. for 20 minutes, and then cleaned in an ultrasonic cleaning machine with deionized water, acetone and anhydrous ethanol for 5 minutes to 15 minutes, and dried at 65° C. for use, to form a first flexible film layer a.
[0156] Weigh 1.25 g of polyoxyethylene monolaurate and 12.5 mg of multi-walled carbon nanotube powder, place in 100 mL of deionized water, and sonicate for 30 min to disperse them evenly to form a multi-walled carbon nanotube dispersion;
[0157] A layer of 50nm pore size PTFE filter membrane is placed on the sand core of the vacuum filtration funnel, and the multi-walled carbon nanotube dispersion is poured into the vacuum filtration funnel. After vacuum filtration, a layer of carbon nanotube electrode sheet is deposited on the PTFE filter membrane. The mixture is allowed to stand at room temperature until the solvent is completely evaporated. The multi-walled carbon nanotube material on the filter membrane is transferred and bonded to the surface of the first flexible film layer a, and dried to form a first flexible electrode layer b.
[0158] 146.8 mg of zinc acetate and 100 mg of sodium hydroxide were weighed respectively, placed in 100 mL of anhydrous ethanol solution, and ultrasonically dispersed for 20 min until the mixture was uniformly mixed to form a first mixed solution;
[0159] 408.9 mg of zinc chloride, 634.05 mg of hexamethylidene tetramine and 149 mg of aluminum nitrate were respectively weighed and placed in 100 mL of anhydrous ethanol, and ultrasonically dispersed in an ultrasonic cleaning machine for 20 min until the mixture was uniformly mixed to form a second mixed solution;
[0160] The first mixed solution was spin-coated on the surface of the first flexible electrode layer b at a speed of 1000 rpm / min for 1 min, and dried in a constant temperature heating box at 70°C until completely dry. The surface of the first flexible electrode layer b was placed downward in the second mixed solution, and heated at a constant temperature of 75°C for 6 h.
[0161] The new second mixed solution was replaced three times, and each time the second mixed solution was replaced, it was repeatedly placed under constant temperature heating at 75° C. for 6 hours until a densely arranged zinc oxide nanosheet structure grew on the surface of the first flexible electrode layer b, that is, the growth of the zinc oxide nanosheet layer c was completed.
[0162] On the surface of the zinc oxide nanosheet layer c, a layer of polydimethylsiloxane prepolymer mixed liquid is spin-coated at a rotation speed of 3000 rpm / min and a spin coating time of 2 minutes, and heated and cured at 75° C. for 15 minutes, and then cleaned in an ultrasonic cleaning machine with deionized water, acetone and anhydrous ethanol for 5 minutes to 15 minutes, and dried at 65° C. to form a second flexible film layer d on the surface of the zinc oxide nanosheet layer c;
[0163] The multi-walled carbon nanotube dispersion is deposited on a filter membrane by vacuum filtration, and allowed to stand at room temperature until the solvent is completely evaporated, and the multi-walled carbon nanotube material on the filter membrane is transferred and bonded to the surface of the second flexible film layer d, and dried to form a second flexible electrode layer e;
[0164] The polydimethylsiloxane prepolymer mixed liquid is spin-coated on the surface of the second flexible electrode layer e at 3000 rpm / min for 2 min, heated and cured at 65° C. for 10 min, washed, and dried to form a third flexible film layer f;
[0165] The first flexible electrode layer b and the second flexible electrode layer e are glued with copper tape and connected with wires to complete the preparation of the self-powered flexible sensor.
[0166] Example 8
[0167] Prepare a glass sheet of 50 mm×50 mm×2 mm required for the test; weigh 10 g of polydimethylsiloxane prepolymer and 1 g of polydimethylsiloxane prepolymer curing agent, mix them, and stir them at a uniform speed in the same direction to make the polydimethylsiloxane prepolymer and the polydimethylsiloxane prepolymer curing agent evenly mixed to form a polydimethylsiloxane prepolymer mixed liquid;
[0168] The polydimethylsiloxane prepolymer mixed liquid is placed in a vacuum drying oven and allowed to stand, and vacuumized until all bubbles in the polydimethylsiloxane prepolymer mixed liquid are discharged; the bubble-free polydimethylsiloxane prepolymer mixed liquid is evenly dripped on a pre-prepared glass sheet, and the polydimethylsiloxane prepolymer mixed liquid is spin-coated on the glass sheet using a glue spreader at a speed of 1000 rpm / min and a spin coating time of 1 minute, and the polydimethylsiloxane prepolymer mixed liquid is placed in a constant temperature heating box and heated and cured at 70° C. for 30 minutes, and then cleaned in an ultrasonic cleaning machine with deionized water, acetone and anhydrous ethanol for 5 minutes to 15 minutes, and dried at 65° C. for use, to form a first flexible film layer a.
[0169] Weigh 1.2 g of sodium naphthenate and 12 mg of multi-walled carbon nanotube powder, place in 100 mL of deionized water, and sonicate for 20 min to disperse them evenly to form a multi-walled carbon nanotube dispersion;
[0170] A layer of 50nm pore size PTFE filter membrane is placed on the sand core of the vacuum filtration funnel, and the multi-walled carbon nanotube dispersion is poured into the vacuum filtration funnel. After vacuum filtration, a layer of carbon nanotube electrode sheet is deposited on the PTFE filter membrane. The mixture is allowed to stand at room temperature until the solvent is completely evaporated. The multi-walled carbon nanotube material on the filter membrane is transferred and bonded to the surface of the first flexible film layer a, and dried to form a first flexible electrode layer b.
[0171] Weigh 92 mg of zinc acetate and 80 mg of sodium hydroxide respectively, place in 100 mL of anhydrous ethanol solution, and ultrasonically disperse for 20 min until the mixture is uniformly mixed to form a first mixed solution;
[0172] Weigh 470 mg of zinc nitrate, 350 mg of hexamethylidene tetramine and 140 mg of aluminum nitrate respectively, put them into 100 mL of anhydrous ethanol, and ultrasonically disperse them in an ultrasonic cleaning machine for 20 min until they are uniformly mixed to form a second mixed solution;
[0173] The first mixed solution was spin-coated on the surface of the first flexible electrode layer b at a rotation speed of 1000 rpm / min, and dried in a constant temperature heating box at 70°C until completely dry. The surface of the first flexible electrode layer b was placed downward in the second mixed solution, and heated at a constant temperature of 85°C for 5 hours;
[0174] The new second mixed solution was replaced three times, and each time the second mixed solution was replaced, it was repeatedly placed under constant temperature heating at 85° C. for 5 h until a densely arranged zinc oxide nanosheet structure grew on the surface of the first flexible electrode layer b, that is, the growth of the zinc oxide nanosheet layer c was completed.
[0175] On the surface of the zinc oxide nanosheet layer c, a layer of polydimethylsiloxane prepolymer mixed liquid is spin-coated at a rotation speed of 3000 rpm / min for a spin coating time of 2 minutes, heated and cured at 65° C. for 20 minutes, cleaned in an ultrasonic cleaner with deionized water, acetone and anhydrous ethanol for 5 minutes to 15 minutes respectively, and dried at 65° C. to form a second flexible film layer d on the surface of the zinc oxide nanosheet layer c;
[0176] The multi-walled carbon nanotube dispersion is deposited on a filter membrane by vacuum filtration, and allowed to stand at room temperature until the solvent is completely evaporated, and the multi-walled carbon nanotube material on the filter membrane is transferred and bonded to the surface of the second flexible film layer d, and dried to form a second flexible electrode layer e;
[0177] The polydimethylsiloxane prepolymer mixed liquid is spin-coated on the surface of the second flexible electrode layer e at 3000 rpm / min for 2 min, heated and cured at 65° C. for 10 min, washed, and dried to form a third flexible film layer f;
[0178] The first flexible electrode layer b and the second flexible electrode layer e are glued with copper tape and connected with wires to complete the preparation of the self-powered flexible sensor.
[0179] Example 9
[0180] Prepare a glass sheet of 50 mm×50 mm×2 mm required for the test; weigh 20 g of polydimethylsiloxane prepolymer and 2 g of polydimethylsiloxane prepolymer curing agent, mix them, and stir them at a uniform speed in the same direction to make the polydimethylsiloxane prepolymer and the polydimethylsiloxane prepolymer curing agent evenly mixed to form a polydimethylsiloxane prepolymer mixed liquid;
[0181] The polydimethylsiloxane prepolymer mixed liquid is placed in a vacuum drying oven and allowed to stand, and vacuumized until all bubbles in the polydimethylsiloxane prepolymer mixed liquid are discharged; the bubble-free polydimethylsiloxane prepolymer mixed liquid is evenly dripped on a pre-prepared glass sheet, and the polydimethylsiloxane prepolymer mixed liquid is spin-coated on the glass sheet using a glue spreader at a speed of 1000 rpm / min and a spin coating time of 1 minute, and the polydimethylsiloxane prepolymer mixed liquid is placed in a constant temperature heating box and heated and cured at 75° C. for 30 minutes, and then cleaned in an ultrasonic cleaning machine with deionized water, acetone and anhydrous ethanol for 5 minutes to 15 minutes, and dried at 70° C. for use, to form a first flexible film layer a.
[0182] Weigh 1 g of sodium alkyl succinate sulfonate and 5 mg of carbon powder, place in 100 mL of deionized water, and ultrasonicate for 30 min to disperse them evenly to form a carbon powder dispersion;
[0183] A layer of 50nm pore size PTFE filter membrane is placed on the sand core of the vacuum filtration funnel, and the carbon powder dispersion is poured into the vacuum filtration funnel. After vacuum filtration, a layer of carbon powder electrode sheet is deposited on the PTFE filter membrane. The mixture is allowed to stand at room temperature until the solvent is completely evaporated. The carbon powder material on the filter membrane is transferred and bonded to the surface of the first flexible film layer a, and dried to form a first flexible electrode layer b.
[0184] 128.45 mg of zinc acetate and 160 mg of sodium hydroxide were weighed respectively, placed in 100 mL of anhydrous ethanol solution, and ultrasonically dispersed for 25 min until the mixture was uniformly mixed to form a first mixed solution;
[0185] Weigh 639 mg of zinc nitrate, 420 mg of hexamethylidene tetramine and 149 mg of aluminum nitrate respectively, put them into 100 mL of anhydrous ethanol, and ultrasonically disperse them in an ultrasonic cleaning machine for 30 min until they are uniformly mixed to form a second mixed solution;
[0186] The first mixed solution was spin-coated on the surface of the first flexible electrode layer b at a speed of 1000 rpm / min for 1 min, and then placed in a constant temperature heating box at 68°C to dry until completely dry. The surface of the first flexible electrode layer b was placed downward in the second mixed solution, and heated at a constant temperature of 90°C for 5.2 h;
[0187] The new second mixed solution was replaced three times, and each time the second mixed solution was replaced, it was repeatedly placed at 90° C. and heated at a constant temperature for 5.2 h until a densely arranged zinc oxide nanosheet structure grew on the surface of the first flexible electrode layer b, that is, the growth of the zinc oxide nanosheet layer c was completed.
[0188] On the surface of the zinc oxide nanosheet layer c, a layer of polydimethylsiloxane prepolymer mixed liquid is spin-coated at a rotation speed of 3000 rpm / min and a spin coating time of 2 minutes, and heated and cured at 70° C. for 15 minutes, and then cleaned in an ultrasonic cleaning machine with deionized water, acetone and anhydrous ethanol for 5 minutes to 15 minutes, and dried at 65° C. to form a second flexible film layer d on the surface of the zinc oxide nanosheet layer c;
[0189] The carbon powder dispersion is deposited on the filter membrane by vacuum filtration, and is allowed to stand at room temperature until the solvent is completely evaporated, and the carbon powder material on the filter membrane is transferred and bonded to the surface of the second flexible film layer d, and dried to form the second flexible electrode layer e;
[0190] The polydimethylsiloxane prepolymer mixed liquid is spin-coated on the surface of the second flexible electrode layer e at 3000 rpm / min for 2 min, heated and cured at 70° C. for 20 min, washed, and dried to form a third flexible film layer f;
[0191] The first flexible electrode layer b and the second flexible electrode layer e are glued with copper tape and connected with wires to complete the preparation of the self-powered flexible sensor.
[0192] See also Figure 3 The zinc oxide nanosheet layer c of the self-powered flexible sensor prepared in Example 1 was characterized by SEM, and it can be seen that the zinc oxide nanosheet layer c successfully grew a dense zinc oxide nanosheet structure.
[0193] See also Figure 4 The prepared self-powered flexible sensor was subjected to strength tests such as stretching and torsion. It was found that the self-powered flexible sensor can maintain a good mechanical structure without breaking after macroscopic bending, stretching and torsion tests.
[0194] See also Figure 5 , stress-strain tests were carried out on the self-powered flexible sensor prepared in Example 1, and it was found that the elastic modulus of the self-powered flexible sensor was small enough and the tensile performance was good.
[0195] See also Figure 6 and Figure 7 Under the same conditions, the traditional flexible sensor and the flexible sensor prepared by the present invention were subjected to excitation tests to test the voltage output. The results showed that as the microscopic morphology of the piezoelectric material was improved from a one-dimensional nanowire structure to a two-dimensional nanosheet structure, the output voltage of the sensor increased from 1V to about 4V, an increase of nearly four times.
[0196] In summary, the self-powered flexible sensor prepared by the present invention has very good conductivity and tensile resistance, so that it can still maintain very good mechanical properties and conductive properties in a stretched state, and can effectively avoid the sensor electrode breakage or even loss of conductivity due to stretching.
[0197] The preferred embodiments of the present invention are only preferred embodiments and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a self-powered flexible sensor, characterized in that: The self-powered flexible sensor comprises a first flexible film layer (a), on which a first flexible electrode layer (b), a zinc oxide nanosheet layer (c), a second flexible film layer (d), a second flexible electrode layer (e) and a third flexible film layer (f) are sequentially arranged; the first flexible electrode layer (b) and the second flexible electrode layer (e) are respectively led out with wires for collecting and deriving electrical signals of the sensor; the first flexible electrode layer (b) and the second flexible electrode layer (e) are carbon nanotube electrode layers, graphene electrode layers or carbon powder electrode layers, and comprises the following steps: S1: preparing a first flexible film layer (a) as a flexible substrate; S2: preparing a first flexible electrode layer (b) on the surface of the flexible substrate; S3: growing a zinc oxide nanosheet layer (c) on the surface of the first flexible electrode layer (b); S4: coating a second flexible film layer (d) on the surface of the zinc oxide nanosheet layer (c); S5: Pressing a second flexible electrode layer (e) on the surface of the second flexible film layer (d); S6: coating a third flexible film layer (f) on the surface of the second flexible electrode layer (e); S7: Connecting the wires to the first flexible electrode layer (b) and the second flexible electrode layer (e) to complete the preparation of the self-powered flexible sensor; The preparation method of the first flexible film layer (a), the second flexible film layer (d) and the third flexible film layer (f) is as follows: Weighing polydimethylsiloxane prepolymer and polydimethylsiloxane prepolymer curing agent, mixing, and stirring evenly to form a polydimethylsiloxane prepolymer mixed liquid; Expelling bubbles from the polydimethylsiloxane prepolymer mixed solution, coating the bubble-free polydimethylsiloxane prepolymer mixed solution on a carrier, heating and curing at 65° C. to 85° C. for 10 min to 30 min, washing, and drying to form a flexible film layer; The preparation method of the first flexible electrode layer (b) and the second flexible electrode layer (e) is: Dissolving a surfactant in water to form a surfactant aqueous solution; dispersing the carbon material in an aqueous surfactant solution to form a carbon material dispersion; The carbon material dispersion is deposited on a filter membrane by vacuum filtration, and allowed to stand at room temperature until the solvent is completely evaporated, and the carbon material on the filter membrane is transferred and bonded to the surface of a desired carrier, and dried to form a flexible electrode layer; The specific operation of growing the zinc oxide nanosheet layer (c) on the surface of the first flexible electrode layer (b) is: Dissolving zinc acetate and alkali in an ethanol solution to form a first mixed solution; wherein the zinc acetate concentration is 5 mmol / L to 15 mmol / L; the alkali concentration is 20 mmol / L to 50 mmol / L; Dissolving zinc salt, aluminum salt and hexamethonium tetramine in an ethanol solution to form a second mixed solution; wherein the zinc salt is zinc nitrate or zinc chloride, and the concentration of the zinc salt is 20 mmol / L to 50 mmol / L; the aluminum salt is aluminum nitrate or aluminum chloride, and the concentration of the aluminum salt is 6 mmol / L to 8 mmol / L; and the concentration of hexamethonium tetramine is 20 mmol / L to 50 mmol / L; Spin-coat the first mixed solution on the surface of the first flexible electrode layer (b), dry it, place it in the second mixed solution, and heat it at a constant temperature of 75° C. to 95° C. for 5 h to 6 h; The second mixed solution is replaced repeatedly for multiple times. Each time the second mixed solution is replaced, it is repeatedly placed under constant temperature heating at 75°C to 95°C for 5 h to 6 h until a densely arranged zinc oxide nanostructure is grown on the surface of the first flexible electrode layer (b), thus completing the growth of the zinc oxide nanosheet layer (c).
2. The method for preparing the self-powered flexible sensor according to claim 1, characterized in that: The mass ratio of the polydimethylsiloxane prepolymer to the polydimethylsiloxane prepolymer curing agent is 10:
1.
3. The method for preparing the self-powered flexible sensor according to claim 1, characterized in that: The surfactant is alkylbenzene sulfonate, alkyl sulfonate ester salt, alkyl sulfonate, alkyl sulfate, fluorinated fatty acid salt, polysiloxane, fatty alcohol sulfate, fatty alcohol polyoxyethylene ether sulfate, α-olefin sulfonate, fatty alcohol polyoxyethylene ether phosphate, alkyl alcohol amide, alkyl sulfonic acid acetamide, alkyl succinate sulfonate, alcoholamine alkylbenzene sulfonate, cyclopentaneate, alkylphenol sulfonate or polyoxyethylene monolaurate.
4. The method for preparing a self-powered flexible sensor according to claim 1, characterized in that: The mass ratio of the carbon material to the surfactant is: (1:200) to (1:50); the concentration of the surfactant aqueous solution is 2.5 mg / mL to 20 mg / mL.
Citation Information
Patent Citations
A method for constructing a flexible strain sensor made of ZnO micro / nano materials
CN102285634A
Preparation method of flexible piezoelectric stress sensor and product thereof
CN110132459A