Conductive silver paste for heterojunction battery and preparation method thereof
By optimizing the composition and preparation method of silver paste, the problem of viscosity and tensile strength imbalance in heterojunction solar cells was solved, improving printability and battery performance, and achieving efficient electrode interconnection and battery efficiency.
Patent Information
- Application Number
- CN202210920045.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-01
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-08-01
AI Technical Summary
In the prior art, the viscosity of the silver paste used in heterojunction cells cannot be balanced with the tensile force after electrode interconnection, which affects printability and cell performance.
A combination of flake and spherical silver powder is used, along with 0.2–0.45 wt% of glass powder with a thermal expansion coefficient of 50–100 × 10⁻⁷/℃ and a particle size of 1.5–3.5 μm. A mixture of phenolic epoxy resin and alicyclic epoxy resin is used as the inorganic binder, and thixotropic agents and dispersants are added. The viscosity and printability of the silver paste are adjusted through a specific preparation method.
It achieves good printing results for silver paste, reduces resistivity, improves solderability and battery electrical performance, reduces post-printing depressions and collapses, and ensures good electrode bonding.
Smart Images

Figure CN115240898B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solar cell pastes, and more specifically, relates to a conductive silver paste for heterojunction cells and a preparation method thereof. Background Art
[0002] With the advancement of science and technology, battery technology is iterating towards N-type and developing towards a high-efficiency route. Due to the problems of light-induced degradation, photothermal degradation, and potential-induced degradation of p-type batteries, their conversion efficiency is greatly limited. However, the efficiency potential of heterojunction batteries exceeds 28%, which is much higher than that of traditional p-type batteries. Compared with the high-temperature silver paste on traditional P-type batteries, N-type HIT (heterojunction) batteries require the use of low-temperature silver paste due to the sensitivity of the internal amorphous silicon layer to temperature, so as not to damage the thin film structure of the HJT battery. Therefore, the demand for battery silver paste is also changing.
[0003] Patent No. CN109273137B provides a low-temperature conductive silver paste for solar HIT cells and a preparation method thereof. A low-viscosity carrier resin is prepared by mixing acrylic modified epoxy resin and diethylene glycol butyl ether acetate, thereby improving the viscosity of the silver paste to 260-300 Pa·s. Patent No. CN111145934B provides a room-temperature storable silver paste for heterojunction (HIT) solar cells and a preparation method thereof. 1-Fluoro-2,4,6-trimethylpyridine boron tetrafluoride is used to make the viscosity of the silver paste 133.5 Pa·s, which can be stored for a long time at room temperature.
[0004] Generally, glass powder is only added to high-temperature conductive silver paste, and the addition ratio is generally 1-2wt%. If the ratio of glass powder added is too high or too low, it will increase the defects of printing effect; if the thermal expansion coefficient of glass powder added is too high or too low, Isc (short circuit current) will be too low during printing, and the screen will stick to the screen when cleaning after printing, making it difficult to clean the screen.
[0005] However, in the prior art, the viscosity of the silver paste and the tension after the electrodes are interconnected still cannot maintain a balance, and the printability of the silver paste is affected. Summary of the invention
[0006] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.
[0007] In order to achieve these purposes and other advantages according to the present invention, a conductive silver paste for a heterojunction battery is provided, comprising 88.4 to 89.55 parts by weight of a conductive phase, 0.2 to 0.45 parts by weight of an inorganic binder phase and 10 to 11.4 parts by weight of an organic vehicle.
[0008] Preferably, the conductive phase is flaky silver powder and spherical silver powder, and the weight ratio of flaky silver powder to spherical silver powder is 25-38:50-65, further 29.6:59.4;
[0009] The particle size of the flaky silver powder is 2-7 um, and the particle size of the spherical silver powder is 1-4 um.
[0010] Preferably, the inorganic binder phase is glass powder, the addition ratio of the glass powder accounts for 0.2-0.45wt% of the total weight of the conductive silver paste, and the thermal expansion coefficient of the glass powder used is 50×10 -7 / ℃~100×10 -7 / ℃, particle size is 1.5~3.5um.
[0011] Preferably, the organic carrier comprises epoxy resin, a curing agent, a solvent, a thixotropic agent and a dispersant.
[0012] Preferably, the epoxy resin is one or more of alicyclic epoxy resin, phenolic epoxy resin and bisphenol F epoxy resin, and the tensile strength of the phenolic epoxy resin is 55 to 67 MPa;
[0013] When the epoxy resin is selected from alicyclic epoxy resin and phenolic epoxy resin, the weight ratio of the alicyclic epoxy resin to the phenolic epoxy resin is 1:2-3.
[0014] Preferably, the curing agent is one or more of tetraethylenepentamine, hexahydromethylphthalic anhydride, and trimethylhexamethylenediamine.
[0015] Preferably, the thixotropic agent is fumed silica and / or calcium silicate.
[0016] Preferably, in the organic vehicle, the weight ratio of epoxy resin, curing agent, thixotropic agent and dispersant is 6-9:2.1-2.7:0.45-1:0.45-0.52.
[0017] Preferably, the solvent is at least one of diethylene glycol butyl ether acetate and terpineol.
[0018] A method for preparing a conductive silver paste for a heterojunction battery comprises the following steps:
[0019] Step 1, preparing an organic carrier, the specific method includes: pouring epoxy resin, curing agent, thixotropic agent and dispersant into a reaction kettle, adding solvent to a volume of 1.3 to 2 times the original volume, controlling the temperature of the reaction kettle at 30 to 40° C., stirring at a speed of 1500 r / min, stirring for 2 to 3 hours until a uniform viscous liquid is formed, and then filtering with a 250-mesh filter to obtain an organic carrier;
[0020] Step 2: silver paste mixing, the specific method includes: adding the conductive phase, the inorganic adhesive and the organic carrier into a double planetary stirring kettle, controlling the temperature within 40°C, the stirring speed is 100r / min, the dispersion plate speed is 150r / min, and stirring for 4h to obtain a uniform slurry;
[0021] Step three, three-roll grinding and filtering, the specific method includes: grinding the evenly stirred slurry in step two, grinding twice with a grinding gap of 80um and 60um; grinding twice with a grinding gap of 60um and 30um; grinding twice with a grinding gap of 40um and 20um. After grinding, use a scraper fineness meter to test the fineness to be less than 10um, and obtain a conductive silver paste.
[0022] The present invention at least has the following beneficial effects: the thermal expansion coefficient of the silver paste system is (50-100)×10 -7 / ℃, glass powder with a particle size of 1.5 to 3.5um, is conducive to ensuring good printing effect while reducing the resistivity of silver paste. Phenolic epoxy resin and alicyclic epoxy resin with a tensile strength of 55 to 67MPa are added to the organic carrier, and the weight ratio of alicyclic epoxy resin and phenolic epoxy resin in the epoxy resin is controlled to be 1: (2 to 3), which not only reduces the viscosity of the conductive silver paste, improves the fluidity of the silver paste, and improves the weldability of the silver paste, so that the silver paste has good bonding after interconnection with the electrode, but also unexpectedly improves the printing effect of the silver paste, so that the obtained silver paste has less depression after screen printing, and the degree of collapse of the fine grid is reduced. The silver paste provided by the present invention has excellent viscosity, tension, thixotropic index, solid content, printing effect and resistivity. The viscosity is 60-120 Pa·s, the thixotropic index is 3.5-5.0, the solid content is 91-94.5wt%, the tension is 1.59-2.82N, the printing speed is 300-400mm / s, and the laying speed is 600-800mm / s. It has good printing effect. When used for batteries, especially the front and back sides of batteries with 9BB PVD film sources, the electrical performance of the batteries is excellent.
[0023] Generally, glass powder is only added to high temperature conductive silver paste, and the addition ratio is generally 1-2wt%. In the present application, the applicant found that the thermal expansion coefficient of adding 0.2-0.45wt% of glass powder to the silver paste system is (50-100)×10 -7 / ℃, glass powder with a particle size of 1.5 to 3.5um is beneficial to ensure good printing effect while reducing the resistivity of silver paste.
[0024] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a SEM scanning electron microscope image of the conductive silver paste obtained in Example 1. DETAILED DESCRIPTION
[0026] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0027] It should be understood that terms such as “having”, “including” and “comprising” used herein do not specify the existence or addition of one or more other elements or combinations thereof.
[0028] The raw materials for preparing the compositions in the examples are all commercially available, wherein the sources of the flaky silver powders in Examples 1 and 3 are different. The flaky silver powder in Example 1 is purchased from BROFO, with the item number Brofos-Ag-P05 and a particle size of 5 μm. The flaky silver powder in Example 3 is purchased from BROFO, with the item number Brofos-Ag-P01 and a particle size of 1 μm. The spherical silver powder is purchased from BROFO, with the item number Brofos-Ag-W02 and a particle size of 2 μm. The glass powder is purchased from Guizhou Baibo, with the item number BYB552 and a thermal expansion coefficient of (80-90)×10 -7 / ℃, particle size 2.5um, phenolic epoxy resin purchased from Sumitomo of Japan, model E 16521A, tensile strength 62MPa, alicyclic epoxy resin purchased from Synasia, model Syna Epoxy S-100, fumed silica purchased from Hubei Huifu Nanomaterials Co., Ltd., model HL-300, dispersant purchased from BYK, model BYK-111.
[0029] Example 1
[0030] This embodiment provides a conductive silver paste for a heterojunction battery, the raw materials of which include 89 kg of electric phase, 0.34 kg of glass powder and 10.66 kg of organic carrier.
[0031] The conductive phase is flaky silver powder and spherical silver powder. In the conductive phase, the weight ratio of flaky silver powder to spherical silver powder is 29.6:59.4. The flaky silver powder is purchased from BROFO, item number Brofos-Ag-P05, and the particle size is 5 um.
[0032] The inorganic binder phase is glass powder.
[0033] The raw materials of the organic carrier include resin, curing agent, solvent, thixotropic agent and dispersant. In the organic carrier, the weight ratio of epoxy resin, curing agent, thixotropic agent and dispersant is 7.4:2.3:0.5:0.46.
[0034] The epoxy resin is alicyclic epoxy resin and phenolic epoxy resin. In the epoxy resin, the weight ratio of alicyclic epoxy resin to phenolic epoxy resin is 1:2.5.
[0035] The curing agent is tetraethylenepentamine.
[0036] The thixotropic agent is fumed silica.
[0037] The organic carrier also includes a solvent, and the solvent is diethylene glycol butyl ether acetate.
[0038] The present embodiment also provides a method for preparing a conductive silver paste for a heterojunction battery, the method is as follows: Step 1, preparing an organic carrier, the specific method comprising: pouring an epoxy resin, a curing agent, a thixotropic agent and a dispersant into a reaction kettle, adding a solvent to a volume that is 1.5 times the original volume, controlling the temperature of the reaction kettle at 30-40° C., stirring at a speed of 1500 r / min, stirring for 3 hours until a uniform viscous liquid is formed, and then filtering with a 250-mesh filter to obtain an organic carrier;
[0039] Step 2: silver paste mixing, the specific method includes: adding the conductive phase, the inorganic adhesive and the organic carrier into a double planetary stirring kettle, controlling the temperature within 40°C, the stirring speed is 100r / min, the dispersion plate speed is 150r / min, and stirring for 4h to obtain a uniform slurry;
[0040] Step three, three-roll grinding and filtering, the specific method includes: grinding the evenly stirred slurry in step two, grinding twice with a grinding gap of 80um and 60um; grinding twice with a grinding gap of 60um and 30um; grinding twice with a grinding gap of 40um and 20um. After grinding, use a scraper fineness meter to test the fineness to be less than 10um, and obtain a conductive silver paste.
[0041] Example 2
[0042] This embodiment provides a conductive silver paste for heterojunction batteries. Different from Embodiment 1, the raw materials of the conductive silver paste for heterojunction batteries include 88.5 kg of conductive phase, 0.5 kg of inorganic binder phase and 11 kg of organic carrier.
[0043] This embodiment also provides a method for preparing a conductive silver paste for a heterojunction battery, which is the same as that of Embodiment 1.
[0044] Example 3
[0045] This embodiment provides a conductive silver paste for a heterojunction battery. The difference from Embodiment 1 is that the source of the flaky silver powder is different. The flaky silver powder is purchased from BROFO with the item number Brofos-Ag-P01 and a particle size of 1 um. In the conductive phase, the weight ratio of the flaky silver powder to the spherical silver powder is 27:54.
[0046] This embodiment also provides a method for preparing a conductive silver paste for a heterojunction battery, which is the same as that of Embodiment 1.
[0047] Example 4
[0048] This embodiment provides a conductive silver paste for heterojunction batteries. Different from Embodiment 1, the raw materials of the conductive silver paste for heterojunction batteries include 89 kg of conductive phase, 0.1 kg of inorganic binder phase and 10 kg of organic carrier.
[0049] This embodiment also provides a method for preparing a conductive silver paste for a heterojunction battery, which is the same as that of Embodiment 1.
[0050] Example 5
[0051] This embodiment provides a conductive silver paste for a heterojunction battery. The difference from Embodiment 1 is that in the epoxy resin, the weight ratio of the alicyclic epoxy resin to the phenolic epoxy resin is 1:1.
[0052] This embodiment also provides a method for preparing a conductive silver paste for a heterojunction battery, which is the same as that in Example 1.
[0053] Performance test: Viscosity test: The conductive silver paste obtained in Examples 1-5 was tested using a viscosity tester. The results are shown in Table 1:
[0054] Table 1
[0055] Example Viscosity (Pa·s, 25℃) 1 90 2 95 3 104 4 155 5 172
[0056] It can be seen from Table 1 that the viscosity of the conductive silver paste prepared in Example 1 is significantly lower than that in Examples 2-5.
[0057] Solid content test: The conductive silver paste obtained in Examples 1-5 was tested using a muffle furnace. The results are shown in Table 2:
[0058] Table 2
[0059] Example Solid content (wt%) 1 92 2 91 3 89 4 85 5 87
[0060] It can be seen from Table 2 that the solid content of the conductive silver paste prepared in Example 1 can reach 92%, which is significantly higher than that of Examples 2-5.
[0061] Tensile test: Using 9BB PVD film source, the conductive silver paste obtained in Examples 1-5 was tested according to YS / T 612-2014. The results are shown in Table 3:
[0062] Table 3
[0063] Example Cell front tension (N) 1 2.91 2 2.85 3 2.78 4 2.37 5 2.33
[0064] It can be seen from Table 3 that the glass powder usage in Example 1 accounts for 0.34wt% and the weight ratio of alicyclic epoxy resin to phenolic epoxy resin in epoxy resin is 1:2.5. All of them adopt the technical solution provided by the present invention, and the positive tensile force of the battery cell of the conductive silver paste prepared is better than that of Examples 2-5.
[0065] SEM test: The conductive silver paste obtained in Example 1 was tested using a SEM scanning electron microscope. The results are as follows Figure 1 ,from Figure 1 It can be seen that the conductive silver paste prepared in this embodiment is densely filled and has relatively good conductivity.
[0066] Battery efficiency test: The conductive silver paste obtained in Examples 1-5 was tested using a photovoltaic device of model JEC 2A. The battery cells were made of 9BB PVD source and cured at 180°C for 38 minutes. The results are shown in Table 4:
[0067] Table 4
[0068]
[0069] It can be seen from Table 4 that using 9BB PVD sheet source as the battery sheet, the conductive silver pastes prepared in Examples 1-5 all have very high charge and discharge efficiency Eta, short circuit current Isc and fill factor FF. Among them, the conductive silver paste prepared in Example 1 with a glass powder content of 0.34wt%, has a charge and discharge efficiency Eta, short circuit current Isc and fill factor FF that are significantly better than those of Examples 2-4.
[0070] The number of devices and processing scales described here are used to simplify the description of the present invention. Applications, modifications and variations of the present invention will be obvious to those skilled in the art.
[0071] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.
Claims
1. A conductive silver paste for heterojunction batteries, characterized in that: It comprises 88.4-89.55 parts by weight of a conductive phase, 0.2-0.45 parts by weight of an inorganic binder phase and 10-11.4 parts by weight of an organic carrier; The conductive phase is flaky silver powder and spherical silver powder, and the weight ratio of the flaky silver powder to the spherical silver powder is 25-38:50-65; The particle size of the flaky silver powder is 2-7 um, and the particle size of the spherical silver powder is 1-4 um; The inorganic binder phase is glass powder, and the addition ratio of glass powder accounts for 0.2-0.45wt% of the total weight of the conductive silver paste. The thermal expansion coefficient of the glass powder used is 50×10 -7 / ℃~100×10 -7 / ℃, particle size is 1.5~3.5 um; The organic carrier comprises epoxy resin, curing agent, solvent, thixotropic agent and dispersant; The epoxy resin is one or more of alicyclic epoxy resin, phenolic epoxy resin and bisphenol F epoxy resin, and the tensile strength of the phenolic epoxy resin is 55-67 MPa; When the epoxy resin is selected from alicyclic epoxy resin and phenolic epoxy resin, the weight ratio of alicyclic epoxy resin to phenolic epoxy resin is 1:2~3; The curing agent is one or more of tetraethylenepentamine, hexahydromethylphthalic anhydride, and trimethylhexamethylenediamine; The thixotropic agent is fumed silica and / or calcium silicate.
2. The conductive silver paste for heterojunction battery according to claim 1, characterized in that: In the organic carrier, the weight ratio of epoxy resin, curing agent, thixotropic agent and dispersant is 6-9:2.1-2.7:0.45-1:0.45-0.
52.
3. The conductive silver paste for heterojunction battery according to claim 1, characterized in that: The solvent is at least one of diethylene glycol butyl ether acetate and terpineol.
4. A method for preparing a conductive silver paste for a heterojunction battery according to any one of claims 1 to 3, characterized in that: The following steps are involved: Step 1, preparing an organic carrier, the specific method includes: pouring epoxy resin, curing agent, thixotropic agent and dispersant into a reaction kettle, adding solvent to a volume of 1.3 to 2 times the original volume, controlling the temperature of the reaction kettle at 30 to 40° C., stirring at a speed of 1500 r / min, stirring for 2 to 3 hours until a uniform viscous liquid is formed, and then filtering with a 250-mesh filter to obtain an organic carrier; Step 2: silver paste mixing, the specific method includes: adding the conductive phase, the inorganic binder phase and the organic carrier into a double planetary stirring kettle, controlling the temperature within 40° C., stirring at a speed of 100 r / min, a dispersion plate speed of 150 r / min, and stirring for 4 hours to obtain a uniform slurry; Step three, three-roll grinding and filtering, the specific method includes: grinding the evenly stirred slurry in step two, grinding twice with a grinding gap of 80um and 60um; grinding twice with a grinding gap of 60um and 30um; grinding twice with a grinding gap of 40um and 20um. After grinding, use a scraper fineness meter to test the fineness to be less than 10um, and obtain a conductive silver paste.