Silicon-based long-wavelength semiconductor optical amplifier chip for optical communication and preparation method thereof
By growing specific hierarchical structures and process processing on silicon substrates, a silicon-based long-wavelength semiconductor optical amplification chip is formed, which solves the problem that the existing technology cannot amplify laser light sources above 1600nm, realizes cost reduction and integration convenience, and is suitable for high-speed coherence Communication and gas sensing fields.
Patent Information
- Application Number
- CN202110457348.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-04-27
AI Technical Summary
The prior art is difficult to realize a long-wavelength semiconductor optical amplification chip with silicon as the substrate, and cannot directly amplify laser light sources with a wavelength of more than 1600 nm, and additional heat sinks are required in practical applications, which increases the cost of use and integration difficulty.
An intermediate layer, an N-InGaAsP light field expansion layer, a lower waveguide layer, a strain-combined multi-quantum well, an upper waveguide layer, a P-InP space layer, a P-InGaAsP transition layer, is adopted, P-InGaAs ohmic contact layer forms a phylum ridge waveguide structure, and the SiNO passivation layer is deposited by PECVD and electron beam evaporation Ti/Pt/Au to form an ohmic contact alloy. Combined with MOCVD and PECVD processes, heat treatment and deposition are carried out to form optical communications. Silicon-based long-wavelength semiconductor optical amplification chip.
It realizes direct amplification of laser light sources with wavelengths above 1600nm, reducing the cost of use, and without additional heat sinks, making it easy to integrate with lasers, modulators, etc., and is suitable for high-speed coherent communication, lidar and gas sensing fields.
Smart Images

Figure CN115249945B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a silicon-based long-wavelength semiconductor light amplification chip for optical communication and a preparation method thereof. Background Art
[0002] The large capacity and high-speed development of information technology requires that communication networks have the characteristics of fast and flexible switching, recombination, and high signal-to-noise ratio. Semiconductor optical amplifiers are widely used in signal transmission amplification, linear relay, and receiving amplification in optical communication links due to their small size, low power consumption, easy integration, and long life. They can significantly improve signal quality and signal-to-noise ratio. At the same time, semiconductor optical amplifier chips combined with special packaging processes can also achieve the characteristics of widely tunable lasers, and their laser light sources can be used in unmanned laser radars, high-speed coherent communications, and other fields. Laser light sources with wavelengths exceeding 1600nm can be used in atmospheric sensing, methane detection, and other fields.
[0003] The integration of semiconductor groups III and V based on silicon substrate is the key to the next generation of optoelectronic integration and is the inevitable trend for the development of optoelectronic integration towards systematization, miniaturization, low power consumption and low cost. Summary of the invention
[0004] The purpose of the present invention is to provide a silicon-based long-wavelength semiconductor optical amplifier chip for optical communication and a preparation method thereof, so as to realize a long-wavelength semiconductor optical amplifier chip with silicon as a substrate, which can directly amplify laser light sources with a wavelength above 1600nm and can be used in the fields of high-speed coherent communication, laser radar, gas sensing, etc. In addition, the optical communication long-wavelength semiconductor optical amplifier chip prepared on the silicon substrate does not require an additional heat sink in actual applications, thereby reducing the cost of use, and is convenient for further integration with lasers, modulators, etc. in actual optoelectronic integration.
[0005] To achieve the above-mentioned purpose, the technical solution of the present invention is: a silicon-based long-wavelength semiconductor optical amplifier chip for optical communication, comprising a substrate and an intermediate layer, an N-InGaAsP optical field expansion layer, a lower waveguide layer, a strained combination multiple quantum well, an upper waveguide layer, a P-InP space layer, a P-InGaAsP transition layer, and a P-InGaAs ohmic contact layer grown in sequence from bottom to top on the substrate; the intermediate layer is a GaAs layer and an InP layer in sequence from bottom to top; wherein the P-InGaAs ohmic contact layer is etched downward to the N-InGaAsP optical field expansion layer to form an inverted mesa ridge waveguide structure.
[0006] In one embodiment of the present invention, a P-InP protective layer is also grown on the P-InGaAs ohmic contact layer, and the P-InP protective layer is also corroded accordingly.
[0007] In one embodiment of the present invention, the periphery of the inverted mesa ridge waveguide structure and the surface of the N-InGaAsP extension layer are coated with a passivation layer.
[0008] In one embodiment of the present invention, the ridge top of the inverted mesa ridge waveguide structure and the surface passivation layer of the N-InGaAsP extension layer are provided with openings, and Ti / Pt / Au metal is evaporated by electron beam to form ohmic contacts and alloys.
[0009] In one embodiment of the present invention, the substrate is a silicon substrate.
[0010] The present invention also provides a method for preparing the silicon-based long-wavelength semiconductor optical amplifier chip for optical communication described above, wherein the surface of the Si substrate is heat-treated in the MOCVD cavity, and an N-GaAs transition layer is grown; then the surface of the epitaxial wafer is heat-treated by MOCVD to cause a mass transport process on the surface of the material, and then an N-InP transition layer is grown, and then the surface of the wafer is heat-treated by MOCVD and an N-InP buffer layer is grown; then an N-InGaAsP optical field expansion layer is grown; then an undoped lower SCH layer, i.e., a lower waveguide layer, is grown, and then a strain-compensated InGaAsP multiple quantum well, i.e., a strain-combined multiple quantum well, is grown, and a thickness-varying combination is used. Quantum wells are used to broaden the gain spectrum width of the material; then an undoped upper SCH layer, a P-InP space layer, a P-InGaAsP transition layer, and a P-InGaAs ohmic contact layer are grown; then, a dielectric layer is deposited by PECVD, and a curved ridge waveguide structure is formed by photolithography. A bromine solution is used for isotropic etching, and the etching depth reaches the N-InGaAsP light field expansion layer to form an inverted mesa ridge waveguide structure; SiNO is deposited by PECVD as a passivation layer, and holes are opened on the ridge top of the inverted mesa ridge waveguide structure and the surface passivation layer of the N-InGaAsP light field expansion layer, and Ti / Pt / Au metal is evaporated by electron beam to form ohmic contacts and alloys.
[0011] In one embodiment of the present invention, a P-InGaAs ohmic contact layer is also grown with a P-InP protective layer, and before the dielectric layer is grown, the P-InP protective layer is also corroded by hydrochloric acid.
[0012] In one embodiment of the present invention, the prepared chip is dissociated, and the dissociated bar strips are bombarded with Ar ions on the coating end surface before the optical film is evaporated.
[0013] In one embodiment of the present invention, the specific implementation process of the method is as follows: a silicon substrate is placed in an MOCVD chamber, and heat-treated at 500°C in an AsH3 atmosphere for 15 minutes to grow 500nm N-GaAs doped 3e18; then, the surface of the epitaxial wafer is heat-treated at 500°C in an MOCVD chamber in a PH3 atmosphere for 20 minutes to allow mass transport to occur on the surface of the material, improve the material regrowth interface, grow 500nm N-InP doped 3e18, and then heat-treat the surface of the material at 500°C for 20 minutes to grow 300nm The N-InP buffer layer is doped with 1e18; then a 2μm thick N-InGaAsP optical field expansion layer is grown, PL=1050nm, doped with 5e17; then 40nm undoped InGaAsP is grown, PL=1100nm, and 40nm undoped InGaAsP is grown, PL=1200nm as the lower waveguide layer; then compressively strained quantum wells with thicknesses of 10nm, 7nm, and 4nm are grown in sequence, and the PL of the quantum well with a thickness of 10nm is 1650nm. The corresponding 7nm and 4nm quantum wells are combined to form a broadened material gain spectrum due to different ground state electron energy levels, with a barrier thickness of 10nm and a PL wavelength of 1200nm; then 40nm undoped InGaAsP is grown, PL=1200nm, and 40nm undoped InGaAsP is grown, PL=1100nm as the upper waveguide layer; then 2200nm P-InP is grown, and the doping concentration changes gradually from 5e17 to 2e18; 50nm is grown P-InGaAsP transition layer, doping concentration 5e18; grow 300nm P-InGaAs electrical contact layer, doping concentration 2e19; grow 20nm P-InP protective layer; hydrochloric acid etch the P-InP protective layer, PECVD deposit 250nm SiO2 dielectric layer on the surface of the epitaxial wafer, photolithography to form a curved ridge waveguide structure pattern, BOE etch the dielectric layer outside the waveguide, then stand in Br2:HBr:H2O solution at 0℃ for isotropic etching to form a ridge waveguide, the etching depth is 3.0μm, and the N-InGaAsP optical field expansion layer is etched, and the ridge top dielectric layer is removed by BOE; PECVD deposit 400nm SiNO on the surface of the wafer as a passivation layer to play a role in resisting water vapor on the surface of the wafer, photolithography holes are opened on the top of the ridge waveguide and the surface of the N-InGaAsP optical field expansion layer, and then electron beam evaporates Ti / Pt / Au to form the P / N ohmic contacts of the chip respectively, and the P / N type electrodes are all located on the surface of the chip.
[0014] In one embodiment of the present invention, the prepared chip is dissociated, and the dissociated bars are bombarded with Ar ions on the dissociation cavity surface in an electron beam evaporation device before the high-reflection and high-transmittance films on the dissociation cavity surface are evaporated. By controlling the cleaning time of the Ar ions and the bombardment ability of the Ar ions, the oxide layer of the material in the quantum well region of the dissociation cavity surface is cleaned, thereby improving the reliability of the chip; at the same time, the ion bombardment forms a certain roughness on the dissociation cavity surface, reducing the optical feedback gain of the cavity surface, thereby further suppressing the FP mode of the spectrum, improving the spectrum ripple, and increasing the flatness and width of the gain spectrum.
[0015] Compared with the prior art, the present invention has the following beneficial effects: the present invention realizes a long-wavelength semiconductor optical amplifier chip with silicon as a substrate, which can directly amplify laser light sources with a wavelength above 1600nm, and can be used in high-speed coherent communication, laser radar, gas sensing and other fields. In addition, the optical communication long-wavelength semiconductor optical amplifier chip prepared on the silicon substrate does not require an additional heat sink in actual applications, thereby reducing the cost of use, and is convenient for further integration with lasers, modulators, etc. in actual optoelectronic integration. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 Figure 1 is the epitaxial structure diagram of the material, where 1 is the silicon substrate; 2 is the intermediate layer for improving the material growth quality, which are GaAs and InP layers from bottom to top; 3 is the N-InGaAsP light field expansion layer; 4 is the lower waveguide layer; 5 is the strained combination multiple quantum well; 6 is the upper waveguide layer; 7 is the P-InP space layer; 8 is the P-InGaAsP transition layer; and 9 is the P-InGaAs ohmic contact layer.
[0017] Figure 2 This is the structure diagram of the ridge waveguide after etching, and the etching depth reaches the N-InGaAsP light field expansion layer.
[0018] Figure 3 is the conduction band energy band and optical near-field distribution of the material. DETAILED DESCRIPTION
[0019] The technical solution of the present invention is described in detail below in conjunction with the accompanying drawings.
[0020] The present invention discloses a silicon-based long-wavelength semiconductor optical amplifier chip for optical communication, comprising a substrate and an intermediate layer, an N-InGaAsP optical field expansion layer, a lower waveguide layer, a strained composite multi-quantum well, an upper waveguide layer, a P-InP space layer, a P-InGaAsP transition layer, and a P-InGaAs ohmic contact layer grown sequentially from bottom to top on the substrate; the intermediate layer is a GaAs layer and an InP layer sequentially from bottom to top; wherein the P-InGaAs ohmic contact layer is etched downward to the N-InGaAsP optical field expansion layer to form an inverted mesa ridge waveguide structure. A P-InP protective layer is also grown on the P-InGaAs ohmic contact layer, and the P-InP protective layer is also etched accordingly.
[0021] The present invention also provides a method for preparing the silicon-based long-wavelength semiconductor optical amplifier chip for optical communication described above, wherein the surface of the Si substrate is heat-treated in the MOCVD cavity, and an N-GaAs transition layer is grown; then the surface of the epitaxial wafer is heat-treated by MOCVD to cause a mass transport process on the surface of the material, and then an N-InP transition layer is grown, and then the surface of the wafer is heat-treated by MOCVD and an N-InP buffer layer is grown; then an N-InGaAsP optical field expansion layer is grown; then an undoped lower SCH layer, i.e., a lower waveguide layer, is grown, and then a strain-compensated InGaAsP multiple quantum well, i.e., a strain-combined multiple quantum well, is grown, and a thickness-varying combination is used. Quantum wells are used to broaden the gain spectrum width of the material; then, an undoped upper SCH layer, a P-InP space layer, a P-InGaAsP transition layer, and a P-InGaAs ohmic contact layer are grown; then, a dielectric layer is deposited by PECVD, a curved ridge waveguide structure is formed by photolithography, and a bromine solution is used for isotropic etching, and the etching depth reaches the N-InGaAsP light field expansion layer to form an inverted mesa ridge waveguide structure; SiNO is deposited by PECVD as a passivation layer, and holes are opened on the ridge top of the inverted mesa ridge waveguide structure and the surface passivation layer of the N-InGaAsP light field expansion layer, and Ti / Pt / Au metal is evaporated by electron beam to form an ohmic contact and alloy. The P-InGaAs ohmic contact layer is also grown with a P-InP protective layer, and before the dielectric layer is grown, the P-InP protective layer is also etched with hydrochloric acid.
[0022] The following is the specific implementation process of the present invention.
[0023] like Figure 1 , 2As shown, the present invention is a silicon-based long-wavelength semiconductor optical amplifier chip for optical communication, comprising a substrate and an intermediate layer, an N-InGaAsP optical field expansion layer, a lower waveguide layer, a strained combination multi-quantum well, an upper waveguide layer, a P-InP space layer, a P-InGaAsP transition layer, and a P-InGaAs ohmic contact layer grown sequentially from bottom to top on the substrate; the intermediate layer is a GaAs layer and an InP layer sequentially from bottom to top; wherein the P-InGaAs ohmic contact layer is etched downward to the N-InGaAsP optical field expansion layer to form an inverted mesa ridge waveguide structure. A P-InP protective layer is also grown on the P-InGaAs ohmic contact layer, and the P-InP protective layer is also etched accordingly.
[0024] For semiconductor optical amplifier chips, the output power of the chip has the following relationship, where P sat is the chip saturation output optical power, d is the quantum well thickness, w is the active area width, Г is the light field confinement factor, h is Planck constant, v is the photon frequency, a is the differential gain, τ s is the carrier lifetime.
[0025]
[0026] While optimizing the material structure to achieve high-power output, the most direct way is to reduce the light confinement factor of the quantum well. Here we use the N-type to add a light field expansion layer to adjust the light field. The first choice is that light field expansion can reduce the chip's light divergence angle and improve coupling efficiency; secondly, because the light field loss in N-type materials is lower than that in P-type materials, it can reduce the internal loss of light propagating in the material; at the same time, the N expansion layer reduces the light confinement factor of the quantum well, thereby improving the chip's saturated light output power.
[0027] The laser is further subjected to conventional wet etching to prepare a ridge-type process, forming an inverted mesa structure to reduce the ohmic contact resistance, and a SiNO passivation layer is used to achieve non-airtight operation of the chip.
[0028] On the cavity surface of the optical chip, the cavity surface oxide layer is removed by ion bombardment to improve the reliability of long-term operation. In addition, due to the roughening of the cavity surface under the bombardment, the gain of the cavity surface feedback is reduced, thereby improving the width and flatness of the light output spectrum.
[0029] The present invention realizes a long-wavelength semiconductor light amplifier chip with silicon as a substrate, which can directly amplify laser light sources with wavelengths above 1600nm and can be used in high-speed coherent communications, laser radar, gas sensing and other fields.
[0030] Figure 3 is the conduction band energy band and optical near-field distribution of the material.
[0031] The specific preparation process of the chip of the present invention is as follows:
[0032] 1. Place the silicon substrate in the MOCVD chamber and heat treat it at 500℃ in AsH3 atmosphere for 15min to grow 500nm N-GaAs doped 3e18; then heat treat the surface of the epitaxial wafer in the MOCVD chamber at 500℃ in PH3 atmosphere for 20min to make the mass transport process occur on the surface of the material, improve the material regrowth interface, grow 500nm N-InP doped 3e18, then heat treat the surface of the material at 500℃ for 20min to grow 300nm The N-InP buffer layer is doped with 1e18; then a 2μm thick N-InGaAsP optical field expansion layer is grown, with PL=1050nm and doped with 5e17; 40nm undoped InGaAsP is grown, with PL=1100nm, and 40nm undoped InGaAsP is grown, with PL=1200nm as the lower waveguide layer; then compressively strained quantum wells with thicknesses of 10nm, 7nm, and 4nm are grown in sequence, and the PL of the quantum well with a thickness of 10nm is 1650nm. The corresponding 7nm and 4nm quantum wells are combined to form a broadened material gain spectrum due to different ground state electron energy levels, with a barrier thickness of 10nm and a PL wavelength of 1200nm; then 40nm undoped InGaAsP is grown, with PL=1200nm, and 40nm undoped InGaAsP is grown, with PL=1100nm as the upper waveguide layer; then 2200nm P-InP is grown, with the doping concentration gradiently changing from 5e17 to 2e18; 50nm is grown P-InGaAsP transition layer, doping concentration 5e18; grow 300nm P-InGaAs electrical contact layer, doping concentration 2e19; grow 20nm P-InP protective layer.
[0033] 2. The P-InP protective layer is etched with hydrochloric acid, and a 250nm SiO2 dielectric layer is deposited on the surface of the epitaxial wafer by PECVD. The waveguide pattern as described in the figure above is formed by photolithography. The dielectric layer outside the waveguide is etched by BOE, and then a ridge waveguide is formed by isotropic etching in a Br2:HBr:H2O solution at 0°C. The etching depth is 3.0μm, and the N-InGaAsP optical field expansion layer is etched. The ridge top dielectric layer is removed by BOE; 400nm SiNO is deposited on the surface of the wafer by PECVD as a passivation layer to resist water vapor on the surface of the wafer. Holes are opened by photolithography on the top of the ridge waveguide and the surface of the N-InGaAsP optical field expansion layer, and then Ti / Pt / Au are evaporated by electron beam to form the P / N ohmic contacts of the chip respectively. The P / N type electrodes are both located on the surface of the chip.
[0034] 3. Dissociate the prepared chip, and bombard the dissociated cavity surface with Ar ions before evaporating the high-reflection and high-transmittance films on the dissociation cavity surface in the electron beam evaporation equipment. By controlling the cleaning time and bombardment ability of the Ar ions, the oxide layer of the material in the quantum well area of the dissociation cavity surface can be cleaned, thereby improving the reliability of the chip. At the same time, the ion bombardment forms a certain roughness on the dissociation cavity surface, reducing the optical feedback gain of the cavity surface, thereby further suppressing the FP mode of the spectrum, improving the spectral ripple, and increasing the flatness and width of the gain spectrum.
[0035] The chip is prepared after the optical film is evaporated. The optical communication long-wavelength semiconductor optical amplifier chip prepared on the silicon substrate of the present invention does not require an additional heat sink in practical applications, thereby reducing the cost of use. At the same time, it is convenient for further integration with lasers, modulators, etc. in actual optoelectronic integration.
[0036] The above are preferred embodiments of the present invention. Any changes made according to the technical solution of the present invention, as long as the resulting functions do not exceed the scope of the technical solution of the present invention, belong to the protection scope of the present invention.
Claims
1. A method for preparing a silicon-based long-wavelength semiconductor optical amplifier chip for optical communication, characterized in that: The silicon-based long-wavelength semiconductor optical amplifier chip for optical communication comprises a substrate and an intermediate layer, an N-InGaAsP optical field expansion layer, a lower waveguide layer, a strained combination multi-quantum well, an upper waveguide layer, a P-InP space layer, a P-InGaAsP transition layer, and a P-InGaAs ohmic contact layer grown sequentially from bottom to top on the substrate; the intermediate layer is a GaAs layer and an InP layer sequentially from bottom to top; wherein the P-InGaAs ohmic contact layer is etched downward to the N-InGaAsP optical field expansion layer to form an inverted mesa ridge waveguide structure; the method for preparing the silicon-based long-wavelength semiconductor optical amplifier chip for optical communication comprises the following steps: heat-treating the surface of the Si substrate in an MOCVD cavity and growing the N-GaAs transition layer; then heat-treating the surface of the epitaxial wafer by MOCVD to cause a mass transport process to occur on the surface of the material, then growing the N-InP transition layer, then heat-treating the surface of the wafer by MOCVD and growing the N-InP buffer layer; then growing the N-InGaAsP optical field expansion layer ; Then, an undoped lower SCH layer, i.e., a lower waveguide layer, is grown, and then strain-compensated InGaAsP multiple quantum wells, i.e., strain-combined multiple quantum wells, are grown, and the thickness-varied combined quantum wells are used to broaden the material gain spectrum width; Then, an undoped upper SCH layer, a P-InP space layer, a P-InGaAsP transition layer, and a P-InGaAs ohmic contact layer are grown; Then, a dielectric layer is deposited by PECVD, a curved ridge waveguide structure is formed by photolithography, and a bromine solution is used for isotropic etching, and the etching depth reaches the N-InGaAsP light field expansion layer to form an inverted mesa ridge waveguide structure; SiNO is deposited by PECVD as a passivation layer, and holes are opened on the ridge top of the inverted mesa ridge waveguide structure and the surface passivation layer of the N-InGaAsP light field expansion layer, and Ti / Pt / Au metal is evaporated by electron beam to form an ohmic contact and an alloy; The P-InGaAs ohmic contact layer is also grown with a P-InP protective layer, and before the dielectric layer is grown, the P-InP protective layer is also corroded by hydrochloric acid.
2. The method for preparing a silicon-based long-wavelength semiconductor optical amplifier chip for optical communication according to claim 1, characterized in that: A P-InP protective layer is also grown on the P-InGaAs ohmic contact layer, and the P-InP protective layer is also corroded accordingly.
3. The method for preparing a silicon-based long-wavelength semiconductor optical amplifier chip for optical communication according to claim 1, characterized in that: The periphery of the inverted mesa ridge waveguide structure and the surface of the N-InGaAsP extension layer are coated with a passivation layer.
4. The method for preparing a silicon-based long-wavelength semiconductor optical amplifier chip for optical communication according to claim 3, characterized in that: The ridge top of the inverted mesa ridge waveguide structure and the surface passivation layer of the N-InGaAsP extension layer are provided with openings, and Ti / Pt / Au metal is evaporated by electron beam to form ohmic contact and alloy.
5. The method for preparing a silicon-based long-wavelength semiconductor optical amplifier chip for optical communication according to claim 1, characterized in that: The substrate is a silicon substrate.
6. The method for preparing a silicon-based long-wavelength semiconductor optical amplifier chip for optical communication according to claim 1, characterized in that: The prepared chip is dissociated, and the dissociated bar strips are bombarded with Ar ions on the coating end surface before the optical film is evaporated.
7. The method for preparing a silicon-based long-wavelength semiconductor optical amplifier chip for optical communication according to claim 1, characterized in that: The specific implementation process of the method is as follows: a silicon substrate is placed in an MOCVD chamber, and heat-treated at 500°C in an AsH3 atmosphere for 15 minutes to grow 500nm N-GaAs doped 3e18; then the surface of the epitaxial wafer is heat-treated at 500°C in an MOCVD chamber in a PH3 atmosphere for 20 minutes to allow mass transport to occur on the surface of the material, improve the material regrowth interface, grow 500nm N-InP doped 3e18, and then the surface of the material is heat-treated at 500°C for 20 minutes to grow 300nm The N-InP buffer layer is doped with 1e18; then a 2μm thick N-InGaAsP optical field expansion layer is grown, PL=1050nm, doped with 5e17; then 40nm undoped InGaAsP is grown, PL=1100nm, and 40nm undoped InGaAsP is grown, PL=1200nm as the lower waveguide layer; then compressively strained quantum wells with thicknesses of 10nm, 7nm, and 4nm are grown in sequence, and the PL of the quantum well with a thickness of 10nm is 1650nm. The corresponding 7nm and 4nm quantum wells are combined to form a broadened material gain spectrum due to different ground state electron energy levels, with a barrier thickness of 10nm and a PL wavelength of 1200nm; then 40nm undoped InGaAsP is grown, PL=1200nm, and 40nm undoped InGaAsP is grown, PL=1100nm as the upper waveguide layer; then 2200nm P-InP is grown, and the doping concentration changes gradually from 5e17 to 2e18; 50nm is grown P-InGaAsP transition layer, doping concentration 5e18; grow 300nm P-InGaAs electrical contact layer, doping concentration 2e19; grow 20nm P-InP protective layer; hydrochloric acid etch the P-InP protective layer, PECVD deposit 250nm SiO2 dielectric layer on the surface of the epitaxial wafer, photolithography form a curved ridge waveguide structure pattern, BOE etch the dielectric layer outside the waveguide, then stand in Br2:HBr:H2O solution at 0℃ and isotropically etch to form a ridge waveguide, the etching depth is 3.0μm, and the N-InGaAsP optical field expansion layer is etched, and the ridge top dielectric layer is removed by BOE; PECVD deposit 400nm SiNO on the surface of the wafer as a passivation layer to play a role in resisting water vapor on the surface of the wafer, photolithography opens holes on the top of the ridge waveguide and the surface of the N-InGaAsP optical field expansion layer, and then electron beam evaporates Ti / Pt / Au to form the P / N ohmic contacts of the chip respectively, and the P / N type electrodes are all located on the surface of the chip.
8. The method for preparing a silicon-based long-wavelength semiconductor optical amplifier chip for optical communication according to claim 7, characterized in that: The prepared chip is dissociated, and the dissociated bars are bombarded with Ar ions on the dissociation cavity surface in an electron beam evaporation device before the high-reflection and high-transmittance films on the dissociation cavity surface are evaporated. By controlling the cleaning time and bombardment ability of the Ar ions, the oxide layer of the material in the quantum well area of the dissociation cavity surface is cleaned, thereby improving the reliability of the chip. At the same time, the ion bombardment forms a certain roughness on the dissociation cavity surface, reducing the optical feedback gain of the cavity surface, thereby further suppressing the FP mode of the spectrum, improving the spectrum ripple, and increasing the flatness and width of the gain spectrum.