A flame retardant insulating material and its preparation method and application

By using a composite flame retardant insulating agent of phosphazene flame retardant, phosphorus-containing silicon organic flame retardant and modified mica in PVC wire trough, the problem of reduced flame retardant and insulation performance after plasticizer is solved, and efficient Flame retardant and insulating effect, and has green environmental protection and impact resistance properties.

CN115322437BActive Publication Date: 2024-10-25HUNAN LIANSU TECH IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210950583.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-09
Publication Date
2024-10-25
Estimated Expiration
2042-08-09

AI Technical Summary

Technical Problem

The flame retardant and insulation properties of existing PVC wire ducts are reduced after plasticizer is added, and toxic gases are produced when burned, posing health and environmental hazards.

Method used

A composite flame retardant insulating agent composed of phosphazene flame retardant, phosphorus-containing silicon organic flame retardant and modified mica is used. Flame retardant substances are generated through the decomposition of phosphazene flame retardant, and the migration of silicon element forms a protective layer. Modification Mica improves insulation and works synergistically to improve flame retardant and insulating properties.

Benefits of technology

It has achieved improvements in flame retardant performance and insulation performance, and at the same time has green environmental protection and impact resistance properties, meeting standard requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115322437B_ABST
    Figure CN115322437B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of chemical materials, and specifically relates to a flame-retardant insulating material and a preparation method and application thereof. The present invention adds a composite flame-retardant insulating agent composed of a phosphazene flame retardant, a phosphorus-containing silicon organic flame retardant and modified mica to the formula. Through the synergistic effect of the phosphazene flame retardant, the phosphorus-containing silicon organic flame retardant and the modified mica, the flame-retardant insulating PVC wire trough prepared by the insulating flame-retardant material of the present invention has good insulation effect, excellent flame-retardant performance, and is green and environmentally friendly. In addition, the flame-retardant insulating PVC wire trough of the present invention also has excellent impact resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of chemical materials, and more specifically, relates to a flame retardant insulating material and a preparation method and application thereof. Background Art

[0002] Polyvinyl chloride has the advantages of good chemical stability, flame retardancy and self-extinguishing, high insulation and so on, and is widely used in the plastics industry. However, due to its poor plasticizing performance, it is often necessary to add plasticizers and other auxiliary agents to assist processing, resulting in a decrease in its flame retardant and insulation performance. In order to solve the problem of decreased flame retardancy and insulation due to processing aids, some flame retardants and insulating agents are generally added to the formula. For example, Chinese patent application CN105038026A discloses a flame retardant and smoke suppression PVC wire trough and its preparation method, which achieves the effect of flame retardancy and smoke suppression by adding a composite flame retardant composed of three flame retardants, namely, molybdenum flame retardant, antimony flame retardant and halogen flame retardant, to the formula. However, halogen flame retardants are used in the formula. On the one hand, halogen flame retardants will produce toxic gases when burned, which poses health and environmental hazards; on the other hand, the formula only solves the problem of decreased flame retardancy, but does not solve the problem of decreased insulation performance. Therefore, it is urgent to provide a flame retardant and insulating material that can simultaneously solve the problem of decreased flame retardancy and insulation performance after adding plasticizers and other auxiliary agents to polyvinyl chloride materials, and is green and environmentally friendly. Summary of the invention

[0003] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the existing PVC wire troughs that cannot simultaneously improve the flame retardant and insulating properties and produce toxic gases that harm human health and the environment when burned, and to provide a flame retardant insulating material with good flame retardant and insulating properties and green and environmentally friendly.

[0004] The purpose of the present invention is to provide a composite flame retardant insulating agent.

[0005] Another object of the present invention is to provide a flame retardant insulating PVC wire duct.

[0006] Another object of the present invention is to provide a method for preparing a flame retardant insulating PVC wire duct.

[0007] Another object of the present invention is to provide an application of a composite flame retardant insulating agent or insulating material in the preparation of an insulating flame retardant product.

[0008] The above purpose of the present invention is achieved through the following technical solutions:

[0009] A composite flame retardant insulating agent is composed of a phosphazene flame retardant, a phosphorus silicon organic flame retardant and modified mica in a mass ratio of 1-10:1-6:1-5.

[0010] Preferably, the mass ratio of the phosphazene flame retardant, the phosphorus-containing silicon organic flame retardant and the modified mica is 5-10:3-6:1.5-4.

[0011] Preferably, the phosphazene flame retardant is selected from one or more of hexaphenoxy cyclotriphosphazene, hexa(allylamino)cyclotriphosphazene and hexa(phenylamino)cyclotriphosphazene.

[0012] Preferably, the phosphorus-containing silicon organic flame retardant is selected from one or more of tris(1-oxo-2,6,7-trioxa-1-phosphabicyclo[2.2.2]octane-4-methyleneoxy)phenylsilane (PPSi) or tetrakis(1-oxo-2,6,7-trioxa-1-phosphabicyclo[2.2.2]octane-4-methyleneoxy)silane (TPSi).

[0013] Preferably, the sedimentation volume of the light calcium carbonate is ≥2.5 mL / g and the whiteness is ≥90.

[0014] Preferably, the heat stabilizer is selected from one or more of a calcium zinc stabilizer, a composite lead salt stabilizer and an organic tin stabilizer.

[0015] Preferably, the impact modifier is selected from one or more of chlorinated polyethylene (CPE), acrylic polymer (ACR) and methyl methacrylate-butadiene-styrene terpolymer (MBS).

[0016] Preferably, the lubricant is selected from one or more of paraffin wax, polyethylene wax (PE wax), stearic acid and chlorinated polyethylene wax (CPE wax).

[0017] Preferably, the polyvinyl chloride resin is SG-5 type PVC resin.

[0018] Preferably, the processing aid is methyl methacrylate-acrylate graft polymer (ACR).

[0019] Preferably, the modified mica is modified by a silane coupling agent.

[0020] More preferably, the preparation method of the modified mica comprises:

[0021] Grind and disperse the grinding balls and mica, add silane coupling agent and grind evenly, then add paraffin or sebacic acid to react completely to obtain the product.

[0022] Preferably, the silane coupling agent is γ-aminopropyltriethoxysilane (KH550), γ-(2,3-epoxypropyloxy)propyltrimethoxysilane (KH560) or γ-methacryloxypropyltrimethoxysilane (KH570).

[0023] Preferably, the mass ratio of the grinding balls to mica is 8 to 10:1.

[0024] Preferably, the mass ratio of the silane coupling agent to mica is 40-60:1.

[0025] Preferably, the grinding time after adding the silane coupling agent is 10 to 20 minutes.

[0026] Preferably, the flame retardant insulating material further comprises a pigment.

[0027] More preferably, the pigment is titanium dioxide.

[0028] The present invention further protects a flame retardant insulating material, comprising 5 to 25 parts of the above composite flame retardant insulating agent and the following components calculated by weight:

[0029]

[0030] The present invention creatively selects a mixture of phosphazene flame retardant, phosphorus-containing silicon organic flame retardant and modified mica as a composite flame retardant insulating agent. Among them, the bond energy of PON and other substances contained in the phosphazene flame retardant is lower than the CC bond energy in the polyvinyl chloride resin. It first decomposes in the heating stage to generate flame retardants such as pyrophosphoric acid and polyphosphoric acid, which can inhibit combustion; and in the process of combustion and pyrolysis, it generates an expanded and dense carbon layer covering the surface of the polyvinyl chloride material, which plays a role in isolating heat and air to protect the inside of the polyvinyl chloride material. In the combustion environment, the silicon element present in the phosphorus-containing silicon organic flame retardant further improves the thermal stability of the phosphorus-containing residual carbon formed by the phosphorus element. This is because the silicon with strong stability migrates to the surface of the polyvinyl chloride during the combustion process, forming a protective layer to inhibit the further degradation of the carbon layer at high temperature, thereby achieving the purpose of protecting the internal material. The addition of modified mica further improves the insulation of the polyvinyl chloride material; at the same time, it also has good transparency, excellent strippability, chemical stability, reducibility, and the ability to maintain the above-mentioned excellent physical and chemical properties under high temperature. The phosphazene flame retardant, the phosphorus silicon organic flame retardant and the modified mica have a synergistic effect, so that the flame-retardant insulating PVC wire duct prepared by the insulating flame-retardant material of the present invention has good insulation effect, excellent flame-retardant performance, and is green and environmentally friendly. In addition, the flame-retardant insulating PVC wire duct of the present invention also has excellent impact resistance.

[0031] The present invention further protects a flame-retardant insulating PVC wire duct, which is prepared from the flame-retardant insulating material.

[0032] The present invention further provides a method for preparing a flame retardant insulating PVC wire duct, comprising the following steps:

[0033] S1. Heat and stir the components according to the amount, and stir and cool when the temperature reaches 110 to 120 ° C. When the temperature is cooled to 30 to 40 ° C, stop stirring to obtain the initial product;

[0034] S2. The primary product obtained in step S1 is plasticized and molded at 160-205°C.

[0035] The present invention further protects the use of the above insulating material in preparing insulating flame-retardant products.

[0036] The present invention has the following beneficial effects:

[0037] The present invention adds a composite flame retardant insulating agent composed of a phosphazene flame retardant, a phosphorus-containing silicon organic flame retardant and modified mica into the formula. Through the synergistic effect of the phosphazene flame retardant, the phosphorus-containing silicon organic flame retardant and the modified mica, the flame retardant insulating PVC wire duct prepared by the insulating flame retardant material of the present invention has good insulation effect, excellent flame retardant performance, is green and environmentally friendly, and the flame retardant insulating PVC wire duct of the present invention also has excellent impact resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a picture of the flame-proof insulated PVC wire duct obtained in Example 1 of the present invention after impact.

[0039] Figure 2 This is a picture of the flame-insulated PVC wire duct obtained in Comparative Example 1 of the present invention after impact. DETAILED DESCRIPTION

[0040] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0041] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0042] Preparation of modified mica (D-KP):

[0043] Weigh 500g of grinding balls in a grinding chamber, add 50g of mica while stirring, grind and disperse for 10min, then add 1g of KH550 dropwise under high-speed grinding and grind for 15min, then add 1g of paraffin (P) dropwise and react for 30min to obtain D-KP modified mica.

[0044] Preparation of modified mica (D-KS):

[0045] Weigh 500g of grinding balls in a grinding chamber, add 50g of mica while stirring, grind and disperse for 10min, then add 1g of KH550 dropwise under high-speed grinding and grind for 15min, then add 1g of sebacic acid (S) dropwise and react for 30min to obtain D-KS modified mica.

[0046] Example 1 Preparation of flame-retardant insulating PVC wire trough

[0047] By weight, 100 parts of polyvinyl chloride resin, 12 parts of light calcium carbonate, 5 parts of calcium zinc heat stabilizer, 10 parts of composite flame retardant insulating agent (hexaphenoxy cyclotriphosphazene: PPSi: D-KP modified mica = 6:3:1.5), 6 parts of CPE impact modifier, 1 part of ACR processing aid, 1.2 parts of PE wax and 2 parts of titanium dioxide are put into the hot mixing cylinder of the high-speed mixing unit, and after starting high-speed stirring, when the temperature of the hot mixing cylinder reaches 120°C, the materials are discharged into the cold mixing cylinder for stirring and cooling, and when the temperature drops to 40°C, the materials are put into a conical twin-screw extruder for plasticization at 161-196°C and molding at 173-205°C.

[0048] Example 2 Preparation of flame-retardant insulating PVC wire trough

[0049] By weight, 100 parts of polyvinyl chloride resin, 12 parts of light calcium carbonate, 5.5 parts of calcium zinc heat stabilizer, 17 parts of composite flame retardant insulating agent (hexaphenoxy cyclotriphosphazene: PPSi: D-KP modified mica = 8:4:2), 10 parts of CPE impact modifier, 1 part of ACR processing aid, 1.2 parts of PE wax, 0.3 parts of paraffin wax and 2 parts of titanium dioxide are put into the hot mixing cylinder of the high-speed mixing unit, and after starting high-speed stirring, when the temperature of the hot mixing cylinder reaches 110°C, the materials are discharged into the cold mixing cylinder for stirring and cooling, and when the temperature drops to 40°C, the materials are put into a conical twin-screw extruder for plasticization at 161-196°C and molding at 173-205°C.

[0050] Example 3 Preparation of flame retardant insulating PVC wire trough

[0051] By weight, 100 parts of polyvinyl chloride resin, 12 parts of light calcium carbonate, 4.5 parts of calcium zinc heat stabilizer, 15 parts of composite flame retardant insulating agent (hexa(allylamino)cyclotriphosphazene: PPSi: D-KS modified mica=8:5:3), 7 parts of CPE impact modifier, 1.2 parts of ACR processing aid, 1 part of PE wax, 0.5 parts of paraffin wax and 2 parts of titanium dioxide are put into the hot mixing cylinder of the high-speed mixing unit, and after starting high-speed stirring, when the temperature of the hot mixing cylinder reaches 120°C, the materials are discharged into the cold mixing cylinder for stirring and cooling, and when the temperature drops to 30°C, the materials are put into a conical twin-screw extruder for plasticization at 161-196°C and molding at 173-205°C.

[0052] Example 4 Preparation of flame retardant insulating PVC wire trough

[0053] By weight, 100 parts of polyvinyl chloride resin, 8 parts of light calcium carbonate, 3 parts of calcium zinc heat stabilizer, 5 parts of composite flame retardant insulating agent (hexa(phenylamino)cyclotriphosphazene: PPSi: D-KS modified mica = 9:6:3), 3.5 parts of CPE impact modifier, 0.8 parts of ACR processing aid, 0.5 parts of PE wax, 0.5 parts of paraffin wax and 1 part of titanium dioxide are put into the hot mixing cylinder of the high-speed mixing unit, and after starting high-speed stirring, when the temperature of the hot mixing cylinder reaches 120°C, the materials are discharged into the cold mixing cylinder for stirring and cooling, and when the temperature drops to 40°C, the materials are put into a conical twin-screw extruder for plasticization at 161-196°C and molding at 173-205°C.

[0054] Example 5 Preparation of flame retardant insulating PVC wire trough

[0055] By weight, 100 parts of polyvinyl chloride resin, 10 parts of light calcium carbonate, 3.5 parts of calcium zinc heat stabilizer, 18 parts of composite flame retardant insulating agent (hexaphenoxy cyclotriphosphazene: PPSi: D-KP modified mica = 5:3:5), 5 parts of CPE impact modifier, 1 part of ACR processing aid, 0.2 parts of PE wax and 2 parts of titanium dioxide are put into the hot mixing cylinder of the high-speed mixing unit, and after starting high-speed stirring, when the temperature of the hot mixing cylinder reaches 120°C, the materials are discharged into the cold mixing cylinder for stirring and cooling, and when the temperature drops to 40°C, the materials are put into a conical twin-screw extruder for plasticization at 161-196°C and molding at 173-205°C.

[0056] Example 6 Preparation of flame retardant insulating PVC wire trough

[0057] By weight, 100 parts of polyvinyl chloride resin, 16 parts of light calcium carbonate, 8 parts of calcium zinc heat stabilizer, 25 parts of composite flame retardant insulating agent (hexaphenoxy cyclotriphosphazene: TPSi: D-KP modified mica = 7:5:3), 10 parts of CPE impact modifier, 3 parts of ACR processing aid, 2 parts of PE wax, 1 part of paraffin wax and 2 parts of titanium dioxide are put into the hot mixing cylinder of the high-speed mixing unit, and after starting high-speed stirring, when the temperature of the hot mixing cylinder reaches 120°C, the materials are discharged into the cold mixing cylinder for stirring and cooling, and when the temperature drops to 40°C, the materials are put into a conical twin-screw extruder for plasticization at 161-196°C and molding at 173-205°C.

[0058] Comparative Example 1 Preparation of flame-retardant insulating PVC wire trough

[0059] By weight, 100 parts of polyvinyl chloride resin, 12 parts of light calcium carbonate, 5 parts of calcium zinc heat stabilizer, 10 parts of composite flame retardant insulating agent (hexaphenoxy cyclotriphosphazene: PPSi: D-KP modified mica = 6:3:0.5), 6 parts of CPE impact modifier, 1 part of ACR processing aid, 1.2 parts of PE wax and 2 parts of titanium dioxide are put into the hot mixing cylinder of the high-speed mixing unit, and after starting high-speed stirring, when the temperature of the hot mixing cylinder reaches 120°C, the materials are discharged into the cold mixing cylinder for stirring and cooling, and when the temperature drops to 40°C, the materials are put into a conical twin-screw extruder for plasticization at 161-196°C and molding at 173-205°C.

[0060] The only difference from Example 1 is that the mass fraction ratio of hexaphenoxycyclotriphosphazene:PPSi:D-KP modified mica is changed from 6:3:1.5 in Example 1 to 6:3:0.5.

[0061] Comparative Example 2 Preparation of flame-retardant insulating PVC wire trough

[0062] By weight, 100 parts of polyvinyl chloride resin, 12 parts of light calcium carbonate, 5.5 parts of calcium zinc heat stabilizer, 10 parts of composite flame retardant insulating agent (hexaphenoxy cyclotriphosphazene: PPSi: D-KP modified mica = 6: 0.5: 1.5), 6 parts of CPE impact modifier, 1 part of ACR processing aid, 1.2 parts of PE wax and 2 parts of titanium dioxide are put into the hot mixing cylinder of the high-speed mixing unit, and after starting high-speed stirring, when the temperature of the hot mixing cylinder reaches 120°C, the materials are discharged into the cold mixing cylinder for stirring and cooling, and when the temperature drops to 40°C, the materials are put into a conical twin-screw extruder for plasticization at 161-196°C and molding at 173-205°C.

[0063] The only difference from Example 1 is that the mass fraction ratio of hexaphenoxycyclotriphosphazene:PPSi:D-KP modified mica is changed from 6:3:1.5 in Example 1 to 6:0.5:1.5.

[0064] Comparative Example 3 Preparation of flame-retardant insulating PVC wire trough

[0065] By weight, 100 parts of polyvinyl chloride resin, 12 parts of light calcium carbonate, 5 parts of calcium zinc heat stabilizer, 10 parts of composite flame retardant insulating agent (hexaphenoxy cyclotriphosphazene: PPSi: D-KP modified mica = 6:7:1), 6 parts of CPE impact modifier, 1 part of ACR processing aid, 1.2 parts of PE wax and 2 parts of titanium dioxide are put into the hot mixing cylinder of the high-speed mixing unit. After starting high-speed stirring, when the temperature of the hot mixing cylinder reaches 120°C, the materials are discharged into the cold mixing cylinder for stirring and cooling. When the temperature drops to 40°C, the materials are put into a conical twin-screw extruder for plasticization at 161-196°C and molding at 173-205°C.

[0066] The only difference from Example 1 is that the mass fraction ratio of hexaphenoxycyclotriphosphazene:PPSi:D-KP modified mica is changed from 6:3:1.5 in Example 1 to 6:7:1.

[0067] Comparative Example 4 Preparation of flame-retardant insulating PVC wire trough

[0068] By weight, 100 parts of polyvinyl chloride resin, 12 parts of light calcium carbonate, 5 parts of calcium zinc heat stabilizer, 10 parts of composite flame retardant insulating agent (hexaphenoxy cyclotriphosphazene: PPSi: D-KP modified mica = 12:3:2), 6 parts of CPE impact modifier, 1 part of ACR processing aid, 1.2 parts of PE wax and 2 parts of titanium dioxide are put into the hot mixing cylinder of the high-speed mixing unit. After starting high-speed stirring, when the temperature of the hot mixing cylinder reaches 120°C, the materials are discharged into the cold mixing cylinder for stirring and cooling. When the temperature drops to 40°C, the materials are put into a conical twin-screw extruder and plasticized at 161-196°C and molded at 173-205°C.

[0069] The only difference from Example 1 is that the mass fraction ratio of hexaphenoxycyclotriphosphazene:PPSi:D-KP modified mica is changed from 6:3:1.5 in Example 1 to 12:3:2.

[0070] Comparative Example 5 Preparation of flame-retardant insulating PVC wire trough

[0071] By weight, 100 parts of polyvinyl chloride resin, 12 parts of light calcium carbonate, 5 parts of calcium zinc heat stabilizer, 10 parts of composite flame retardant insulating agent (hexaphenoxy cyclotriphosphazene: PPSi: D-KP modified mica = 3:3:0.5), 6 parts of CPE impact modifier, 1 part of ACR processing aid, 1.2 parts of PE wax and 2 parts of titanium dioxide are put into the hot mixing cylinder of the high-speed mixing unit, and after starting high-speed stirring, when the temperature of the hot mixing cylinder reaches 120°C, the materials are discharged into the cold mixing cylinder for stirring and cooling, and when the temperature drops to 40°C, the materials are put into a conical twin-screw extruder for plasticization at 161-196°C and molding at 173-205°C.

[0072] The only difference from Example 1 is that the mass fraction ratio of hexaphenoxycyclotriphosphazene:PPSi:D-KP modified mica is changed from 6:3:1.5 in Example 1 to 3:3:0.5.

[0073] Comparative Example 6 Preparation of flame-retardant insulating PVC wire trough

[0074] By weight, 100 parts of polyvinyl chloride resin, 12 parts of light calcium carbonate, 5 parts of calcium zinc heat stabilizer, 10 parts of composite flame retardant insulating agent (hexaphenoxy cyclotriphosphazene: PPSi: D-KP modified mica = 12: 0.5: 3), 6 parts of CPE impact modifier, 1 part of ACR processing aid, 1.2 parts of PE wax and 2 parts of titanium dioxide are put into the hot mixing cylinder of the high-speed mixing unit, and after starting high-speed stirring, when the temperature of the hot mixing cylinder reaches 120°C, the materials are discharged into the cold mixing cylinder for stirring and cooling, and when the temperature drops to 40°C, the materials are put into a conical twin-screw extruder for plasticization at 161-196°C and molding at 173-205°C.

[0075] The only difference from Example 1 is that the mass fraction ratio of hexaphenoxycyclotriphosphazene:PPSi:D-KP modified mica is changed from 6:3:1.5 in Example 1 to 12:0.5:3.

[0076] Comparative Example 7 Preparation of Flame Retardant Insulated PVC Wire Tray

[0077] By weight, 100 parts of polyvinyl chloride resin, 12 parts of light calcium carbonate, 5 parts of calcium zinc heat stabilizer, 10 parts of composite flame retardant insulating agent (hexaphenoxy cyclotriphosphazene: PPSi=6:3), 6 parts of CPE impact modifier, 1 part of ACR processing aid, 1.2 parts of PE wax and 2 parts of titanium dioxide are put into the hot mixing cylinder of the high-speed mixing unit. After starting high-speed stirring, when the temperature of the hot mixing cylinder reaches 120°C, the materials are discharged into the cold mixing cylinder for stirring and cooling. When the temperature drops to 40°C, the materials are put into a conical twin-screw extruder and plasticized at 161-196°C and molded at 173-205°C.

[0078] The only difference from Example 1 is that no modified mica is added to the composite flame retardant insulating agent.

[0079] Comparative Example 8 Preparation of Flame Retardant Insulated PVC Wire Tray

[0080] By weight, 100 parts of polyvinyl chloride resin, 12 parts of light calcium carbonate, 5 parts of calcium zinc heat stabilizer, 10 parts of composite flame retardant insulating agent (PPSi: D-KP modified mica = 3:1.5), 6 parts of CPE impact modifier, 1 part of ACR processing aid, 1.2 parts of PE wax and 2 parts of titanium dioxide are put into the hot mixing cylinder of the high-speed mixing unit. After starting high-speed stirring, when the temperature of the hot mixing cylinder reaches 120°C, the materials are discharged into the cold mixing cylinder for stirring and cooling. When the temperature drops to 40°C, the materials are put into a conical twin-screw extruder for plasticization at 161-196°C and molding at 173-205°C.

[0081] The only difference from Example 1 is that no phosphazene flame retardant is added to the composite flame retardant insulating agent.

[0082] Comparative Example 9 Preparation of flame-retardant insulating PVC wire trough

[0083] By weight, 100 parts of polyvinyl chloride resin, 12 parts of light calcium carbonate, 5 parts of calcium zinc heat stabilizer, 10 parts of composite flame retardant insulating agent (hexaphenoxy cyclotriphosphazene: D-KP modified mica = 6:1.5), 6 parts of CPE impact modifier, 1 part of ACR processing aid, 1.2 parts of PE wax and 2 parts of titanium dioxide are put into the hot mixing cylinder of the high-speed mixing unit, and after starting high-speed stirring, when the temperature of the hot mixing cylinder reaches 120°C, the materials are discharged into the cold mixing cylinder for stirring and cooling, and when the temperature drops to 40°C, the materials are put into a conical twin-screw extruder for plasticization at 161-196°C and molding at 173-205°C.

[0084] The only difference from Example 1 is that no silicon-phosphorus-containing organic flame retardant is added to the composite flame retardant insulating agent.

[0085] Comparative Example 10

[0086] By weight, 100 parts of polyvinyl chloride resin, 12 parts of light calcium carbonate, 5 parts of calcium zinc heat stabilizer, 10 parts of composite flame retardant insulating agent (hexaphenoxy cyclotriphosphazene: polydimethylsilane (PDMS): D-KP modified mica = 6:3:1.5), 6 parts of CPE impact modifier, 1 part of ACR processing aid, 1.2 parts of PE wax and 2 parts of titanium dioxide are put into the hot mixing cylinder of the high-speed mixing unit, and after starting high-speed stirring, when the temperature of the hot mixing cylinder reaches 120°C, the materials are discharged into the cold mixing cylinder for stirring and cooling, and when the temperature drops to 40°C, the materials are put into a conical twin-screw extruder for plasticization at 161-196°C and molding at 173-205°C.

[0087] The only difference from Example 1 is that the silicon-phosphorus organic flame retardant in the composite flame retardant insulating agent is replaced with polydimethylsilane (PDMS) in the organosilicon flame retardant.

[0088] Comparative Example 11

[0089] By weight, 100 parts of polyvinyl chloride resin, 12 parts of light calcium carbonate, 5 parts of calcium zinc heat stabilizer, 10 parts of composite flame retardant insulating agent (hexaphenoxy cyclotriphosphazene: tricresyl phosphate: D-KP modified mica = 6:3:1.5), 6 parts of CPE impact modifier, 1 part of ACR processing aid, 1.2 parts of PE wax and 2 parts of titanium dioxide are put into the hot mixing cylinder of the high-speed mixing unit, and after starting high-speed stirring, when the temperature of the hot mixing cylinder reaches 120°C, the materials are discharged into the cold mixing cylinder for stirring and cooling, and when the temperature drops to 40°C, the materials are put into a conical twin-screw extruder for plasticization at 161-196°C and molding at 173-205°C.

[0090] The only difference from Example 1 is that the silicon-phosphorus organic flame retardant in the composite flame retardant insulating agent is replaced with tricresyl phosphate in the organic phosphorus flame retardant.

[0091] Experimental Example: Performance Test of Flame-retardant Insulated PVC Wire Trays Prepared in Examples 1 to 6 and Comparative Examples 1 to 11

[0092] The flame retardant insulating PVC wire ducts prepared in Examples 1 to 6 and Comparative Examples 1 to 11 were tested according to GB / T 1614-2000 "Flame Retardant Insulated Polyvinyl Chloride Wire Ducts and Accessories", and the test results are shown in Tables 1 to 3.

[0093] Table 1: Performance results of flame retardant insulating PVC wire ducts obtained in Examples 1 to 6

[0094]

[0095] Table 2: Performance results of flame retardant insulating PVC wire ducts obtained in Comparative Examples 1 to 6

[0096]

[0097] Table 3: Performance results of flame retardant insulating PVC wire ducts obtained in Comparative Examples 7 to 11

[0098]

[0099]

[0100] As can be seen from Table 1, the flame retardant insulating PVC wire ducts obtained in Examples 1 to 6 were tested according to GB / T1614-2000 "Flame Retardant Insulated Polyvinyl Chloride Wire Ducts and Accessories". The results show that the oxygen index of the wire ducts in each example is greater than 32%, the smoke density SDR is less than 75, and the insulation resistance is greater than 1.0*10 8 The withstand voltage will not break down within 1 minute, and the flame retardant insulation performance fully meets the standard requirements.

[0101] like Figure 1 As shown, the flame-retardant insulated PVC wire duct obtained in Example 1 has no visible breakage or cracks after impact, and its physical and mechanical impact properties meet the standard requirements.

[0102] It can be seen from Table 2 that for the flame-retardant insulating PVC wire ducts obtained in Comparative Examples 1 to 6, when the ratio of any one of the phosphazene flame retardant, phosphorus-containing silicon flame retardant and modified mica in the composite flame retardant is not within the range defined by the present invention, the PVC wire ducts prepared by such composite flame retardant insulating agent cannot simultaneously meet the requirements of having a higher oxygen index, a lower smoke density, a higher insulation resistance and good voltage resistance and mechanical properties.

[0103] like Figure 2 As shown, the flame-insulated PVC wire duct obtained in Comparative Example 1 has obvious visible breakage and cracks after impact, and the physical and mechanical impact resistance cannot meet the standard requirements.

[0104] It can be seen from Table 3 that for the flame-retardant insulating PVC wire ducts obtained in Comparative Examples 7 to 11, when any one of the phosphazene flame retardant, phosphorus-silicon organic flame retardant, and modified mica is missing, some of their properties will be affected and fail to meet the standard performance requirements.

[0105] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A composite flame retardant insulating agent, characterized in that: The composite flame retardant insulating agent is composed of a phosphazene flame retardant, a phosphorus-silicon organic flame retardant and modified mica in a mass ratio of 5-10:3-6:1.5-4; The phosphazene flame retardant is selected from one or more of hexaphenoxy cyclotriphosphazene, hexa(allylamino)cyclotriphosphazene and hexa(phenylamino)cyclotriphosphazene; The phosphorus-silicon organic flame retardant is selected from one or both of tris(1-oxo-2,6,7-trioxa-1-phosphabicyclo[2.2.2]octane-4-methyleneoxy)phenylsilane and tetrakis(1-oxo-2,6,7-trioxa-1-phosphabicyclo[2.2.2]octane-4-methyleneoxy)silane; The modified mica is obtained by modification with a silane coupling agent.

2. The composite flame retardant insulating agent according to claim 1, characterized in that: The silane coupling agent is one of γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane or γ-methacryloxypropyltrimethoxysilane.

3. A flame retardant insulating material, characterized in that: The invention comprises 5 to 25 parts of the composite flame retardant insulating agent according to claim 1 or 2 and the following components calculated by weight: 100 parts of polyvinyl chloride resin; Light calcium carbonate 5-25 parts; Heat stabilizer 2~8 parts; Impact modifier 2~10 parts; Processing aid 0.3~3 parts; 0.5~3 parts of lubricant.

4. A flame retardant insulating PVC wire trough, characterized in that: Prepared from the flame-retardant insulating material described in claim 3.

5. The method for preparing the flame-retardant insulating PVC wire duct according to claim 4, characterized in that: The steps include: S1. Heat and stir the components according to the amount, and stir and cool when the temperature reaches 110-120°C. Stop stirring when the temperature is cooled to 30-40°C to obtain the initial product; S2. The primary product obtained in step S1 is plasticized and molded at 160-205°C.

6. Use of the composite flame retardant insulating agent according to claim 1 or 2 or the insulating material according to claim 3 in the preparation of insulating flame retardant products.