Epoxy resin and electrodeposition coating

Amino-containing epoxy resins are prepared by reacting epoxy resins with amine compounds with specific components, which solves the problems of insufficient curing and storage stability of electrodeposited coatings at low temperatures, and achieves efficient low-temperature curing and excellent coating performance.

CN115362193BActive Publication Date: 2024-11-08KANSAI PAINT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180024034.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-11-20
Filing Date
2021-03-23
Publication Date
2024-11-08
Estimated Expiration
2041-03-23

AI Technical Summary

Technical Problem

Existing electrodeposited coatings lack sufficient curability and storage stability at low temperatures, and traditional catalysts pose safety and environmental risks, making it difficult to meet the requirements for low-temperature baking and efficient curing.

Method used

Amino-containing epoxy resins are prepared by reacting epoxy resins with amine compounds of specific components. These resins are used in electrodeposition coatings in aqueous media. The resins are modified with ternary or higher phenolic compounds and polyisocyanates with higher or higher trifunctionality to form epoxy resins with high multifunctionality, thereby improving low-temperature curing properties and storage stability.

Benefits of technology

It achieves efficient curing at low temperatures and excellent storage stability, improves the appearance and corrosion resistance of the coating, and meets the requirements of low-temperature baking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0005019488860000021
    Figure FDA0005019488860000021
  • Figure FDA0005019488860000022
    Figure FDA0005019488860000022
  • Figure FDA0005019488860000031
    Figure FDA0005019488860000031
Patent Text Reader

Abstract

The present invention aims to provide an epoxy resin which has excellent curing properties and storage stability when using a low-activity catalyst and at low temperatures, and has excellent coating film appearance characteristics and corrosion resistance when constituting a coating. In addition, the present invention aims to provide an aqueous resin dispersion in which the epoxy resin or a modified product thereof is dispersed in an aqueous medium, an amino-containing epoxy resin obtained by reacting the epoxy resin with an amine compound, and a cationic electrodeposition coating containing the amino-containing epoxy resin. As a solution, an epoxy resin is provided, which is an epoxy resin obtained by reacting at least a compound having one or more epoxy groups and a compound having a functional group reactive with the epoxy group, wherein the epoxy resin satisfies the following conditions (I) and / or (II): (I) the compound having a functional group reactive with the epoxy group is a trivalent or higher phenolic compound and / or a compound containing a trifunctional or higher polyisocyanate; (II) the average multifunctionality (X1) per molecule of the epoxy resin represented by the following formula (1) is greater than 0.30, formula (1): average multifunctionality (X1) = number of ends per molecule of the epoxy resin -2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an epoxy resin and an electrodeposition paint. Specifically, it relates to an epoxy resin obtained by reacting specific components, an epoxy resin having specific characteristics, an aqueous resin dispersion in which any of the above epoxy resins or modified products thereof are dispersed in an aqueous medium, an amino-containing epoxy resin obtained by reacting any of the above epoxy resins with an amine compound, and an electrodeposition paint containing the amino-containing epoxy resin. Background Art

[0002] Epoxy resins have excellent mechanical strength, adhesion, and chemical resistance, and are widely used as film-forming resins for coatings.

[0003] Among coating materials, electrodeposition coatings are widely used for coating metal products (eg, automobile parts, electrical equipment parts, and other industrial equipment) that require these properties because of their excellent coating workability and good corrosion resistance of the formed coating film.

[0004] The electrodeposition coating is provided in the form of a coating film-forming resin which is a cationic resin (e.g., an amino group-containing epoxy resin, etc.) or an anionic resin (e.g., a carboxyl group-containing resin, etc.), a curing agent (e.g., a blocked polyisocyanate compound, etc.), and a curing catalyst dissolved or dispersed in an aqueous medium. The coating composition is used as a coating bath, and electricity is applied to the object to be coated as a cathode or an anode to form a precipitated coating film on the object to be coated, and the precipitated coating film is heated to form a crosslinked and cured coating film.

[0005] In electrodeposition coatings, organotin compounds have been generally used as curing catalysts to promote crosslinking reactions. However, although the catalyst performance of organotin compounds is very high, there may be safety and environmental issues, and their use may be limited, so there has been a demand for a catalyst to replace organotin compounds. As alternatives, bismuth compounds and zinc compounds are considered, but these compounds have problems such as high prices, insufficient catalyst effects, and instability in coatings.

[0006] Furthermore, when an organotin compound catalyst is used, the curing performance must be improved as much as possible.

[0007] Generally, the coating film is formed by crosslinking and curing at a temperature of 160°C or higher. However, depending on the conditions of the drying furnace or the shape of the object to be coated, there may be a portion that is baked at a temperature lower than the target temperature. In addition, in order to reduce energy costs, low-temperature baking at a low temperature (80 to 160°C, preferably 80 to 130°C) has been required.

[0008] In order to perform baking at low temperature, low temperature curable blocked polyisocyanate compounds have been generally used as curing agents. However, the long-term storage stability (bath stability) of the electrodeposition coating with improved reactivity at low temperature is insufficient, resulting in deterioration of the appearance characteristics and corrosion resistance of the coating film.

[0009] Patent Document 1 describes polyfunctionalized epoxy resins. However, these epoxy resins are not used in electrodeposition coatings. Furthermore, the curability, particularly the curability when using a low-activity catalyst, and the storage stability of the coatings have not been studied.

[0010] Patent Documents 2 and 3 describe an electrodeposition coating using an amine-modified epoxy resin obtained by modifying an epoxy resin with an amine, wherein the epoxy resin has been modified with a caprolactone adduct or a phenolic compound. However, the curing characteristics, particularly the low-temperature curing properties and the storage stability of the coating have not been investigated for these electrodeposition coatings.

[0011] Patent document 1: China Patent Application Publication No. 104628995

[0012] Patent Document 2: Japanese Patent Application Publication No. 2016-135848

[0013] Patent Document 3: Japanese Patent Application Publication No. 2001-279168 Summary of the invention

[0014] The present invention aims to provide an epoxy resin which has excellent curing properties and storage stability when using a low-activity catalyst and at low temperatures, and has excellent coating film appearance characteristics and corrosion resistance when constituting a coating. In addition, the present invention provides an aqueous resin dispersion in which the epoxy resin or a modified product thereof is dispersed in an aqueous medium, an amino-containing epoxy resin obtained by reacting the epoxy resin with an amine compound, and a cationic electrodeposition coating containing the amino-containing epoxy resin.

[0015] As a result of intensive studies conducted by the inventors to solve the above-mentioned problems, it has been found that the above-mentioned problems can be solved by an epoxy resin obtained by reacting specific components, an epoxy resin having specific properties, an aqueous resin dispersion obtained by dispersing any of the above-mentioned epoxy resins or modified products thereof in an aqueous medium, an amino-containing epoxy resin obtained by reacting any of the above-mentioned epoxy resins with an amine compound, and a cationic electrodeposition coating containing the amino-containing epoxy resin, thereby completing the present invention.

[0016] The details are as follows.

[0017] Item 1: An epoxy resin obtained by reacting at least a compound having one or more epoxy groups with a compound having a functional group reactive with the epoxy group, wherein the epoxy resin satisfies the following conditions (I) and / or (II):

[0018] (I) the compound having a functional group reactive with an epoxy group is a trivalent or higher phenolic compound and / or contains a trifunctional or higher polyisocyanate,

[0019] (II) the average multifunctionality (X1) per molecule of the epoxy resin represented by the following formula (1) is 0.30 or more,

[0020] Formula (1):

[0021] Average multifunctionality (X1) = number of terminals per molecule of epoxy resin - 2.

[0022] Item 2: The epoxy resin according to Item 1, obtained by reacting at least a compound having one or more epoxy groups with a compound having a functional group reactive with an epoxy group, wherein the epoxy resin is represented by the following formula (1) and has an average multifunctionality (X1) of 0.30 or more,

[0023] Formula (1):

[0024] Average multifunctionality (X1) = number of ends of one epoxy resin molecule - 2

[0025] Furthermore, the average polyfunctional concentration (Y1) represented by the following formula (2) is 0.10 or more,

[0026] Formula (2):

[0027] Average polyfunctional concentration (Y1) = average polyfunctionality of epoxy resin (X1) / weight average molecular weight Mw of epoxy resin × 1000.

[0028] Item 3: The epoxy resin according to Item 1 or Item 2, wherein the trivalent or higher phenol compound comprises a compound represented by the following structural formula (A),

[0029]

[0030] (In the formula, n represents an integer of 1 to 20, p represents an integer of 0 to 4, q represents an integer of 0 to 3, and r represents an integer of 0 to 4; R1 to R3 are each independently a monovalent group; R2 may be different for every n repeating units; when there are multiple R1, R2 and / or R3 in the aromatic ring, they may be the same or different; R1 to R3 may be bonded to each other to form a ring.)

[0031] Item 4: The epoxy resin according to any one of Items 1 to 3, further obtained by reacting a compound having one or more active hydrogen atoms in one molecule other than the trivalent or higher phenol compound.

[0032] Item 5: The epoxy resin according to any one of Items 1 to 4, obtained by reacting a compound represented by the following structural formula (B) with the trivalent or higher phenolic compound, wherein the content ratio (mass ratio) of the trivalent or higher phenolic compound to the compound of structural formula (B) is in the range of 1 / 99 to 99 / 1,

[0033]

[0034] (In the formula, s represents an integer of 0 to 4, t represents an integer of 0 to 4; R4 and R5 are each independently a monovalent group; when there are multiple R4 and / or R5 in the aromatic ring, they may be the same or different; R4 and / or R5 may be bonded to each other to form a ring.)

[0035] Item 6: The epoxy resin according to any one of Items 1 to 5, wherein the trifunctional or higher functional polyisocyanate is an isocyanurate type isocyanate and / or crude MDI (polyphenyl polymethylene polyisocyanate).

[0036] Item 7: An amino group-containing epoxy resin obtained by reacting the epoxy resin according to any one of Items 1 to 6 with an amine compound.

[0037] Item 8: An aqueous resin dispersion obtained by dispersing the epoxy resin or a modified product thereof according to any one of Items 1 to 6 in an aqueous medium.

[0038] Item 9: An anionic electrodeposition paint comprising the epoxy resin or a modified product thereof described in any one of Items 1 to 6 and a curing agent.

[0039] Item 10: A cationic electrodeposition coating comprising the amino-containing epoxy resin described in Item 7 and a curing agent.

[0040] Item 11: A single-layer cationic electrodeposition coating comprising the amino-containing epoxy resin described in Item 7 and a curing agent.

[0041] Item 12: A single-layer cationic electrodeposition coating, comprising the epoxy resin described in any one of Items 1 to 6, and a curing agent, wherein the epoxy resin is obtained by reacting at least a compound having one or more epoxy groups, a trivalent or higher phenolic compound and / or a compound containing a trifunctional or higher polyisocyanate, and an amine compound, wherein the trivalent or higher phenolic compound is a compound represented by the following structural formula (A),

[0042]

[0043] (In the formula, n represents an integer of 1 to 20, p represents an integer of 0 to 4, q represents an integer of 0 to 3, and r represents an integer of 0 to 4; R1 to R3 are each independently a monovalent group; R2 may be different for every n repeating units; when there are multiple R1, R2 and / or R3 in the aromatic ring, they may be the same or different; R1 to R3 may be bonded to each other to form a ring.)

[0044] Item 13: A cationic electrodeposition coating comprising the epoxy resin described in any one of Items 1 to 6, and a curing agent, wherein the epoxy resin is obtained by reacting at least a compound having one or more epoxy groups, a trivalent or higher phenolic compound and / or a compound containing a trifunctional or higher polyisocyanate, and an amine compound, wherein the trivalent or higher phenolic compound is a compound represented by the following structural formula (A),

[0045]

[0046] (In the formula, n represents an integer of 1 to 20, p represents an integer of 0 to 4, q represents an integer of 0 to 3, and r represents an integer of 0 to 4; R1 to R3 are each independently a monovalent group; R2 may be different for every n repeating units; when there are multiple R1, R2 and / or R3 in the aromatic ring, they may be the same or different; R1 to R3 may be bonded to each other to form a ring.)

[0047] When the resin components other than the curing agent are 100% by mass, the content of the amino group-containing epoxy resin is 71% by mass or more.

[0048] Item 14: The cationic electrodeposition coating material according to any one of Items 10 to 13, wherein the compound having one or more epoxy groups is a compound that is not modified with an amine.

[0049] Item 15: A cationic electrodeposition paint according to any one of Items 12 to 14, wherein the epoxy resin is obtained by reacting at least a compound having one or more epoxy groups, a compound containing a trivalent or higher phenolic compound, and a compound having one or more active hydrogen in one molecule other than a trivalent or higher phenolic compound.

[0050] Item 16: The cationic electrodeposition paint according to Item 15, wherein the compound having one or more active hydrogen atoms in one molecule other than the trivalent or higher phenolic compound is a compound represented by the following structural formula (B),

[0051]

[0052] (In the formula, s represents an integer of 0 to 4, t represents an integer of 0 to 4; R4 and R5 are each independently a monovalent group; when there are multiple R4 and / or R5 in the aromatic ring, they may be the same or different; R4 and / or R5 may be bonded to each other to form a ring),

[0053] The content ratio (mass ratio) of the trivalent or higher phenol compound and the compound of the structural formula (B) is in the range of 1 / 99 to 99 / 1.

[0054] Item 17: The cationic electrodeposition coating according to any one of Items 12 to 14, wherein the trifunctional or higher functional polyisocyanate is an isocyanurate type isocyanate and / or crude MDI.

[0055] Item 18: The cationic electrodeposition paint according to any one of Items 10 to 17, further comprising an acrylic resin,

[0056] When the total amount of all epoxy resins and acrylic resins is 100% by mass, the content of the acrylic resin is less than 30% by mass.

[0057] The absolute value of the difference between the solubility parameter SP values ​​of the acrylic resin and the epoxy resin is less than 1.0.

[0058] Item 19: A method for preparing the cationic electrodeposition coating according to any one of Items 10 to 18, comprising the following steps:

[0059] An amino-containing epoxy resin is prepared by reacting an epoxy resin and an amine compound, wherein the epoxy resin is obtained by reacting at least a compound having one or more epoxy groups and a trivalent or higher phenolic compound other than a xylene formaldehyde resin and / or a compound containing a trifunctional or higher polyisocyanate; and

[0060] The amino-containing epoxy resin and a curing agent are mixed to prepare a cationic electrodeposition coating.

[0061] Item 20: A method for preparing a cationic electrodeposition coating according to Item 19, wherein the compound having one or more epoxy groups is a compound that has not been modified by amine, and the prepared cationic electrodeposition coating is a single-layer cationic electrodeposition coating.

[0062] Item 21: A coated product obtained by immersing a coating material in an electrodeposition coating bath containing the cationic electrodeposition coating material according to any one of Items 10 to 18 and performing electrodeposition coating.

[0063] The epoxy resin of the present invention is excellent in curability and storage stability when using a low-activity catalyst and at low temperatures, and is also excellent in coating film appearance characteristics and corrosion resistance when constituting a coating.

[0064] Furthermore, the aqueous resin dispersion and electrodeposition coating of the present invention are excellent in curability, storage stability, coating film appearance characteristics, and corrosion resistance when using a low-activity catalyst and at low temperatures. DETAILED DESCRIPTION

[0065] In the present invention, "epoxy resin" refers to both a resin having an epoxy group and a resin obtained by reacting the epoxy group of the epoxy resin with another functional group-containing compound, and may not contain an epoxy group. In addition, "epoxy group" may be abbreviated as "EP".

[0066] In the present invention, "multifunctional" means the case where the number of functional groups is greater than 2. However, in the present invention, even if there are two or more functional groups generated and / or introduced by the reaction between the terminal epoxy group of the epoxy resin and the compound containing a reactive functional group, the number of functional groups at the terminal portion is still counted as one. Furthermore, the secondary hydroxyl group inside the epoxy resin molecule is not included in the number of the above functional groups due to its low reactivity. In the present invention, the "functional group" in the multifunctional group essentially means a reactive functional group that can react with a curing agent such as a blocked polyisocyanate compound.

[0067] [Epoxy resin]

[0068] <Epoxy Resin of the First Embodiment>

[0069] The epoxy resin of the first aspect of the present invention is obtained by reacting at least a compound having one or more epoxy groups and a trivalent or higher phenol compound and / or a compound containing a trifunctional or higher polyisocyanate.

[0070] During the reaction, a compound having one or more active hydrogen atoms in one molecule other than the trivalent or higher phenol compound and / or a diisocyanate compound may be further reacted as necessary.

[0071] The epoxy resin of the first embodiment of the present invention is excellent in curability, particularly curability when using a low-activity catalyst and curability at low temperatures, storage stability, and coating appearance characteristics and corrosion resistance when the epoxy resin is used to prepare an electrodeposition coating.

[0072] (Compounds having one or more epoxy groups)

[0073] A compound having one or more epoxy groups (epoxy compound) is a compound having at least one epoxy group, preferably two or more epoxy groups in one molecule. In the present invention, the number of epoxy groups in one molecule of the epoxy compound is preferably 2 to 8, more preferably 2 to 6, further preferably 2 to 4, and most preferably two.

[0074] The weight average molecular weight of the epoxy compound is not particularly limited, but preferably has a weight average molecular weight in the range of, for example, at least 300, preferably 400 to 4,000, and more preferably 800 to 2,500. Moreover, the epoxy equivalent of the epoxy compound is also not particularly limited, but suitably has an epoxy equivalent in the range of, for example, at least 160, preferably 180 to 2,500, and more preferably 400 to 1,500. As the epoxy compound, for example, one or more selected from the following: an epoxy compound obtained by a reaction of a polyphenol compound and an epihalohydrin (epichlorohydrin, etc.), an epoxy compound containing a polyalkylene oxide chain in the molecule, dimer acid diglycidyl ester, etc. can be used.

[0075] In the present invention, it is preferable to use an epoxy compound obtained by a reaction between a polyphenol compound and an epihalohydrin.

[0076] As the polyphenol compound reacted with epihalohydrin, known substances can be used without restriction. For example, one or more selected from the following can be used: bis(4-hydroxyphenyl)-2,2-propane [bisphenol A], bis(4-hydroxyphenyl)methane [bisphenol F], bis(4-hydroxycyclohexyl)methane [hydrogenated bisphenol F], 2,2-bis(4-hydroxycyclohexyl)propane [hydrogenated bisphenol A], 4,4'-dihydroxybenzophenone, bis(4-hydroxyphenyl)-1,1-ethane, bis(4-hydroxyphenyl)-1,1-isobutane, bis(4-hydroxy-3-tert-butylphenyl)-2,2-propane, bis(2-hydroxynaphthyl)methane, tetrakis(4-hydroxyphenyl)-1,1,2,2-ethane, 4,4'-dihydroxydiphenyl sulfone, phenol novolac, cresol novolac, etc.

[0077] As the epoxy compound, an epoxy compound containing a polyalkylene oxide chain in the molecule can be used. Generally, such an epoxy compound can be obtained by the following methods: (α) reacting an epoxy compound having at least one (preferably two or more) epoxy group with an alkylene oxide or a polyalkylene oxide to introduce a polyalkylene oxide chain; (β) reacting the above-mentioned polyphenol compound with a polyalkylene oxide having at least one (preferably two or more) epoxy group to introduce a polyalkylene oxide chain. In addition, an epoxy compound already containing a polyalkylene oxide chain can also be used (see, for example, Japanese Patent Application Laid-Open No. 8-337750).

[0078] The alkylene group in the polyalkylene oxide chain is preferably an alkylene group having 2 to 8 carbon atoms, more preferably an ethylene group, a propylene group or a butylene group, and particularly preferably a propylene group.

[0079] Regarding the content of the polyalkylene oxide chain, from the viewpoint of improving stability, appearance characteristics and corrosion resistance when forming an electrodeposition coating, the appropriate content of the polyalkylene oxide constituent component is generally in the range of 1.0 to 15% by mass, preferably in the range of 2.0 to 9.5% by mass, and more preferably in the range of 3.0 to 8.0% by mass, based on the solid content mass of the epoxy resin.

[0080] As the epoxy compound, dimer acid diglycidyl ester can be used. This epoxy compound is obtained by introducing a glycidyl group into a dimer acid obtained by dimerizing an unsaturated fatty acid, and preferably has a linear, branched, and / or cyclic hydrocarbon group having 10 to 150 carbon atoms.

[0081] As the unsaturated fatty acid, any known unsaturated fatty acid may be used without limitation. However, from the viewpoint of flexibility and hydrophobicity of the epoxy compound, a higher unsaturated fatty acid having 11 to 22 carbon atoms is preferably used.

[0082] As the higher unsaturated fatty acid, known substances can be used without limitation. Specifically, for example, one or more selected from the group consisting of oleic acid, linoleic acid, linolenic acid, eicosenoic acid, docosenoic acid, branched-chain octadecenoic acid, branched-chain hexadecenoic acid, and undecenoic acid can be used.

[0083] The epoxy compound is obtained by reacting an epihalohydrin with one or more selected from the group consisting of bis(4-hydroxyphenyl)-2,2-propane [bisphenol A], bis(4-hydroxyphenyl)methane [bisphenol F], bis(4-hydroxycyclohexyl)methane [hydrogenated bisphenol F], 2,2-bis(4-hydroxycyclohexyl)propane [hydrogenated bisphenol A], 4,4'-dihydroxybenzophenone, bis(4-hydroxyphenyl)-1,1-ethane, bis(4-hydroxyphenyl)-1,1-isobutane, bis(4-hydroxy-3-tert-butylphenyl)-2,2-propane, bis(2-hydroxynaphthyl)methane, tetrakis(4-hydroxyphenyl)-1,1,2,2-ethane, 4,4'-dihydroxydiphenyl sulfone, phenol novolac, cresol novolac. In the present invention, it is preferred to use one or more of the epoxy compounds.

[0084] Particularly preferably, there can be mentioned an epoxy compound obtained by the reaction of a polyphenol compound and an epihalohydrin (for example, epichlorohydrin), which is derived from bisphenol A and represented by the following formula, wherein n=0 to 8.

[0085]

[0086] Examples of commercially available products of such epoxy compounds include products sold by Mitsubishi Chemical Corporation under the trade names of jER828EL, jER1002, jER1004, and jER1007.

[0087] In addition, as mentioned above, the secondary hydroxyl groups in the molecule of the epoxy resin in the above formula are not included in the functional groups as multifunctional groups. Moreover, in the modified epoxy resin obtained by reacting the terminal epoxy group of the above formula with a compound containing a reactive functional group, the hydroxyl groups generated by the reaction of the epoxy group are also not included in the functional groups as multifunctional groups in the present invention.

[0088] (Trivalent or higher phenolic compounds)

[0089] The trivalent or higher phenol compound is one or more compounds having three or more hydroxyl groups bonded to an aromatic ring in the molecule.

[0090] As the trivalent phenol compound, for example, one or more selected from the group consisting of pyrogallol, phloroglucinol, hydroxyhydroquinone, 5-methylpyrogallol, gallic acid, 1,8,9-trihydroxyanthracene, 4,4',4"-trihydroxytriphenylmethane, 4,4',4"-ethylenetris(2-methylphenol), 4,4'-(2-hydroxybenzylidene)bis(2,3,6-trimethylphenol), 2,3,4-trihydroxydiphenylmethane, 2,4,6-tris(4-hydroxyphenyl)-1,3,5-triazine, 1,3,5-tris(4-hydroxyphenyl)benzene, 1,1,1-tris(4-hydroxyphenyl)ethane, 1,1,3-tris(4-hydroxyphenyl)propane, 4,4'-[1-[4-[1-(4-hydroxy-3,5-dimethylphenyl)-1-methylethyl]phenyl ]ethylene]bis(2-methylphenol), 4,4'-[1-[4-[1-(4-hydroxyphenyl)-1-methylethyl]phenyl]ethylene]bisphenol, 2,6-bis(4-hydroxy-3,5-dimethylbenzyl)-4-methylphenol, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)propane, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1-[α-methyl-α-(4-hydroxyphenyl)ethyl]-3-[α,α-bis(4-hydroxyphenyl)ethyl]benzene, 1-[α-methyl-α-(4-hydroxyphenyl)ethyl]-4-[α,α-bis(4-hydroxyphenyl)ethyl]benzene, α,α-bis(4-hydroxyphenyl)-4-(4-hydroxy-α,α-dimethylbenzyl)-ethylbenzene, etc.

[0091] As the tetravalent or higher phenolic compound, for example, one or more selected from the following can be used: 2,2'-methylenebis[6-(2-hydroxy-5-methylbenzyl)-p-cresol, 4-[bis(4-hydroxy-3-methylphenyl)methyl]benzene-1,2-diol, 1,1,2,2-tetra(p-hydroxyphenyl)ethane, α,α,α',α"-tetra(4-hydroxyphenyl)-p-xylene, 1,4,9,10-tetrahydroxyanthracene, 2,4,6-tris[(4-hydroxyphenyl)methyl]-1,3-benzenediol, hexahydroxybenzene, 2,3,6,7,10,11-hexahydroxytriphenylene hydrate, etc.

[0092] Furthermore, one or more selected from phenol resins can be used, which are obtained by condensing a phenolic compound (phenol, cresol, bisphenol compound, etc.) component and an aldehyde (formaldehyde, acetaldehyde, benzaldehyde, hydroxy aldehyde, crotonaldehyde, glyoxal, etc.) in the presence of a catalyst. For example, one or more selected from the following: a compound represented by the following structural formula (A), a phenol novolac resin, a cresol novolac resin, a bisphenol novolac resin (bisphenol A novolac resin, etc.), a naphthol novolac resin, a phenol aralkyl resin, a terpene phenolic resin, a dicyclopentadiene phenolic resin, a phenol biphenylene resin, a phenol-modified toluene formaldehyde resin, a co-condensation resin of asphalt or oil and a phenolic compound and formaldehyde, etc. can be used.

[0093]

[0094] (In the formula, n represents an integer of 1 to 20, p represents an integer of 0 to 4, q represents an integer of 0 to 3, and r represents an integer of 0 to 4; R1 to R3 are each independently a monovalent group; R2 may be different for every n repeating units; when there are multiple R1, R2 and / or R3 in the aromatic ring, they may be the same or different; R1 to R3 may be bonded to each other to form a ring.)

[0095] In the present invention, as the trivalent or higher phenolic compound, it is preferred to use one or more of the compounds represented by the above structural formula (A). R1 ​​to R3 in the above structural formula (A) are preferably hydrogen or a carbon-containing organic group. As the carbon-containing organic group, for example, monovalent alkyl groups having 1 to 20 carbon atoms such as methyl, ethyl, propyl, and butyl can be cited.

[0096] (Compounds containing trifunctional or higher polyisocyanates)

[0097] As the compound containing a trifunctional or higher-functional polyisocyanate, one or more kinds of compounds having three or more isocyanate groups in the molecule are used.

[0098] For example, one or more selected from the following can be used: aliphatic triisocyanates, such as 2,6-diisocyanatohexanoic acid 2-isocyanatoethyl ester (lysine ester triisocyanate), 1,6-diisocyanato-3-isocyanatomethylhexane, 1,4,8-triisocyanatooctane, 1,6,11-triisocyanatoundecane, 1,8-diisocyanato-4-isocyanatomethyloctane, 1,3,6-triisocyanatohexane, 2,5,7-trimethyl-1,8-diisocyanato-5-isocyanatomethyloctane, etc.; alicyclic triisocyanates, such as 2,6-diisocyanatohexanoic acid 2-isocyanatoethyl ester (lysine ester triisocyanate), 1,6-diisocyanato-3-isocyanatomethylhexane, 1,4,8-triisocyanatooctane, 1,6,11-triisocyanatoundecane, 1,8-diisocyanato-4-isocyanatomethyloctane, 1,3,6-triisocyanatohexane, 2,5,7-trimethyl-1,8-diisocyanato-5-isocyanatomethyloctane, etc.; triisocyanates, such as 1,3,5-triisocyanatocyclohexane, 1,3,5-trimethylisocyanatocyclohexane, 2-(3-isocyanatopropyl)-2,5-bis(isocyanatomethyl)-bicyclo(2.2.1)heptane, 2-(3-isocyanatopropyl)-2,6-bis(isocyanatomethyl)-bicyclo(2.2.1)heptane, 3-(3-isocyanatopropyl)-2,5-bis(isocyanatomethyl)-bicyclo(2.2.1)heptane, 5-(2-isocyanatoethyl)-2-isocyanatomethyl-3-( 3-isocyanatopropyl)-bicyclo(2.2.1)heptane, 6-(2-isocyanatoethyl)-2-isocyanatomethyl-3-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, 5-(2-isocyanatoethyl)-2-isocyanatomethyl-2-(3-isocyanatopropyl)-bicyclo(2.2.1)-heptane, bicycloheptane triisocyanate, 6-(2-isocyanatoethyl)-2-isocyanatomethyl-2-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, etc.; aromatic aliphatic Triisocyanates, such as 1,3,5-triisocyanatotoluene, etc.; aromatic triisocyanates, such as triphenylmethane-4,4',4"-triisocyanate, 1,3,5-triisocyanatobenzene, 2,4,6-triisocyanatotoluene, etc.; aromatic tetraisocyanates, such as 4,4'-diphenylmethane-2,2',5,5'-tetraisocyanate, etc.; crude compounds of various isocyanates represented by the following structural formula (C), such as crude MDI [polymethylene polyphenyl isocyanate] (polymeric MDI), crude TDI [crude tolylene diisocyanate], etc.; etc.

[0099]

[0100] (In the formula, n represents an integer greater than or equal to 1.)

[0101] Furthermore, for example, one or more selected from the following compounds can be used. The compounds are trimers or isocyanurates and have three or more isocyanate groups in the molecule: aliphatic diisocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate, methylene diisocyanate, 2,6-diisocyanato diisocyanate, ... Methyl hexanoate (common name: lysine diisocyanate), etc.; alicyclic diisocyanates, such as 1,3-cyclopentane diisocyanate, 1,3-cyclopentene diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (common name: isophorone diisocyanate), 4-methyl-1,3-cyclohexene diisocyanate (common name: hydrogenated TDI), 2-methyl-1,3-cyclohexene diisocyanate, 1,3- or 1,4-bis(isocyanatomethyl)cyclohexane (common name: hydrogenated xylene diisocyanate) or its mixture, methylene bis (4,1-cyclohexanediyl) diisocyanate (common name: hydrogenated MDI), norbornane diisocyanate, etc.; aromatic aliphatic diisocyanates, such as methylene bis (4,1-phenylene) diisocyanate (common name: MDI), 1,3- or 1,4-xylene diisocyanate or its mixture, ω,ω'-diisocyanato-1,4-diethylbenzene, 1,3- or 1,4-bis (1-isocyanato-1-methylethyl) benzene (common name: tetramethylxylene diisocyanate) or mixtures thereof; aromatic diisocyanates, such as m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, toluene-2,4-diisocyanate (common name: 2,4-TDI) or 2,6-toluene diisocyanate (common name: 2,6-TDI) or mixtures thereof, 4,4'-toluidine diisocyanate, 4,4'-diphenyl ether diisocyanate, diphenylmethane-2,2'-diisocyanate, diphenylmethane-2,4'-diisocyanate, diphenylmethane-4,4'-diisocyanate, etc.; etc.

[0102] Furthermore, one or more kinds selected from the group consisting of dimers, trimers, biuret, allophanate, uretdione, uretonimine, isocyanurate, oxadiazinetrione and crude compounds of these trifunctional or higher polyisocyanate-containing compounds can be mentioned.

[0103] The compound containing trifunctional or higher polyisocyanate may also be a prepolymer formed by reacting the polyisocyanate or its derivative with a compound having active hydrogen that can react with the polyisocyanate under the condition of excess isocyanate groups. Examples of the compound that can react with the polyisocyanate include one or more selected from the following: polyols, low molecular weight polyester resins, amines, water, active hydrogen-containing resins (acrylic polyols, polyolefin polyols, polyurethane polyols, polyether polyols, polyester polyols), etc.

[0104] The compound containing a trifunctional or higher-functional polyisocyanate may be a compound obtained by blocking the isocyanate group of the above-mentioned polyisocyanate or a derivative thereof with a blocking agent, that is, a blocked polyisocyanate compound.

[0105] As the above-mentioned end-capping agent, for example, the following can be cited: phenols, such as phenol, cresol, xylenol, nitrophenol, ethylphenol, hydroxybiphenyl, butylphenol, isopropylphenol, nonylphenol, octylphenol, methyl hydroxybenzoate, etc.; lactams, such as ε-caprolactam, δ-valerolactam, γ-butyrolactam, β-propiolactam, etc.; aliphatic alcohols, such as methanol, ethanol, propanol, butanol, amyl alcohol, lauryl alcohol, etc.; ethers, such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol monomethyl ether, methoxymethanol, etc.; alcohols, such as benzyl alcohol, glycolic acid, methyl glycolate, ethyl glycolate, butyl glycolate, lactic acid, methyl lactate, ethyl lactate, butyl lactate, hydroxymethyl urea, hydroxymethyl melamine, diacetone alcohol, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, etc.; oximes, such as formamide oxime, acetamide oxime, acetyl oxime, methyl ethyl ketone oxime, diacetyl monooxime, benzophenone oxime, cyclohexanone oxime, etc.; active methylene Bases, such as dimethyl malonate, diethyl malonate, ethyl acetoacetate, methyl acetoacetate, acetylacetone, etc.; thiols, such as butanethiol, tert-butyl mercaptan, hexanethiol, tert-dodecyl mercaptan, 2-mercaptobenzothiazole, thiophenol, methylthiophenol, ethylthiophenol, etc.; amides, such as acetanilide, methoxyacetanilide (acetoanilide), N-acetyltoluidine (acetotoluide), acrylamide, methacrylamide, acetamide, stearamide, benzamide, etc.; imides, Such as succinimide, phthalic acid imide, maleic acid imide, etc.; amines, such as diphenylamine, phenylnaphthylamine, xylidine, N-phenylenediamine, carbazole, aniline, naphthylamine, butylamine, dibutylamine, butylaniline, etc.; ureas, such as urea, thiourea, ethylene urea, ethylene thiourea, diphenyl urea, etc.; carbamates, such as N-phenylcarbamic acid phenyl ester, etc.; imines, such as ethyleneimine, propyleneimine, etc.; sulfites, such as sodium bisulfite, potassium bisulfite, etc.; azole compounds; etc. The above-mentioned azole compounds can be listed as one or more selected from the following: pyrazole or pyrazole derivatives, such as pyrazole, 3,5-dimethylpyrazole, 3-methylpyrazole, 4-benzyl-3,5-dimethylpyrazole, 4-nitro-3,5-dimethylpyrazole, 4-bromo-3,5-dimethylpyrazole, 3-methyl-5-phenylpyrazole, etc.; imidazole or imidazole derivatives, such as imidazole, benzimidazole, 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, etc.; imidazoline derivatives, such as 2-methylimidazoline, 2-phenylimidazoline, etc.; etc.

[0106] When end-capping (reacting with an end-capping agent) is performed, the end-capping can be performed by adding a solvent as needed. As the solvent used in the end-capping reaction, a solvent that is not reactive with the isocyanate group is preferred, for example, ketones such as acetone and methyl ethyl ketone; esters such as ethyl acetate; pyrrolidone solvents such as N-methyl-2-pyrrolidone (NMP) can be cited.

[0107] In the present invention, the compound containing trifunctional or higher polyisocyanate can preferably be selected from one or more of the following: isocyanurates of aliphatic diisocyanates, isocyanurates of aromatic aliphatic diisocyanates, isocyanurates of aromatic diisocyanates, crude compounds of polyisocyanates, etc. It is particularly preferred to use one or more of the following: isocyanurates of hexamethylene diisocyanate, crude MDI (polymeric MDI), and crude TDI.

[0108] (Compounds having more than one active hydrogen in one molecule)

[0109] Examples of the compound having one or more active hydrogen atoms in one molecule other than trivalent or higher phenol compounds include one or more of the following: divalent phenol compounds, polyol compounds, polycarboxylic acid compounds, and compounds having one active hydrogen atoms in one molecule.

[0110] The diphenol compound is a compound having two hydroxyl groups bonded to an aromatic ring in the molecule. As the diphenol compound, for example, one or more selected from the following can be used: bis(4-hydroxyphenyl)-2,2-propane [bisphenol A], bis(4-hydroxyphenyl)methane [bisphenol F], bis(4-hydroxycyclohexyl)methane [hydrogenated bisphenol F], 2,2-bis(4-hydroxycyclohexyl)propane [hydrogenated bisphenol A], 4,4'-dihydroxybenzophenone, bis(4-hydroxyphenyl)-1,1-ethane, bis(4-hydroxyphenyl)-1,1-isobutane, bis(4-hydroxy-3-tert-butyl-phenyl)-2,2-propane, bis(2-hydroxynaphthyl)methane, tetrakis(4-hydroxyphenyl)-1,1,2,2-ethane, 4,4'-dihydroxydiphenyl sulfone, bisphenol, etc.

[0111] In the present invention, when the compound represented by the above structural formula (A) is included as the trivalent or higher phenol compound, it is preferred that the compound represented by the following structural formula (B) is included as the compound having one or more active hydrogen atoms in one molecule.

[0112]

[0113] (In the formula, s represents an integer of 0 to 4, t represents an integer of 0 to 4; R4 and R5 are each independently a monovalent group; when there are multiple R4 and / or R5 in the aromatic ring, they may be the same or different; R4 and / or R5 may be bonded to each other to form a ring.)

[0114] As the polyol compound, for example, one or more selected from the group consisting of alkylene glycols (ethylene glycol, propylene glycol, butylene glycol, 1,6-hexanediol, etc.), glycerin, etc. can be used.

[0115] As the polycarboxylic acid compound, for example, one or more selected from oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, phthalic acid, trimellitic acid, pyromellitic acid, trimesic acid, dimer acid, and anhydrides thereof can be used.

[0116] As the compound having one active hydrogen in one molecule, for example, one or more selected from the following can be used: monophenol compounds (phenol, cresol, nonylphenol, nitrophenol, etc.), monohydric alcohol compounds (hexanol, 2-ethylhexanol, stearyl alcohol, ethylene glycol monobutyl ether, ethylene glycol monohexyl ether, propylene glycol monobutyl ether, propylene glycol monohexyl ether, etc.), monocarboxylic acid compounds (saturated fatty acids and unsaturated fatty acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-ethylhexanoic acid (octanoic acid), caproic acid, capric acid, stearic acid, oleic acid, linoleic acid, etc.), etc.

[0117] Furthermore, one or more selected from hydroxycarboxylic acids (glycolic acid, dimethylolpropionic acid, hydroxyvalproic acid, lactic acid, citric acid, etc.), mercaptoalkanols (mercaptoethanol, etc.), alkanolamines (ethanolamine, etc.), etc. can be used.

[0118] (Diisocyanate compound)

[0119] As the diisocyanate compound, for example, one or more of the following can be cited: aliphatic diisocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate, methylene diisocyanate, dimer acid diisocyanate, 2,6-diisocyanatohexanoic acid methyl ester (common name: lysine diisocyanate), etc.; alicyclic diisocyanates, such as 1,3-cyclopentane diisocyanate, 1,3-cyclopentene diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (common name: isophorone diisocyanate), 4-methyl-1,3-cyclohexene diisocyanate (common name: hydrogenated TDI), 2-methyl-1,3-cyclohexene diisocyanate, 1,3- or 1,4-bis(isocyanatomethyl)cyclohexane (common name: hydrogenated xylylene diisocyanate) or mixtures thereof, methylenebis(4,1-cyclohexyl)diisocyanate diisocyanate (generic name: hydrogenated MDI), norbornane diisocyanate, etc.; aromatic aliphatic diisocyanates, such as methylene bis (4,1-phenylene) diisocyanate (generic name: MDI), 1,3- or 1,4-xylene diisocyanate or a mixture thereof, ω,ω'-diisocyanato-1,4-diethylbenzene, 1,3- or 1,4-bis (1-isocyanato-1-methylethyl) benzene (generic name: tetramethylxylene diisocyanate) or a mixture thereof, etc.; aromatic diisocyanates, such as m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenyl diisocyanate Ester, 1,5-naphthalene diisocyanate, toluene-2,4-diisocyanate (common name: 2,4-TDI) or 2,6-toluene diisocyanate (common name: 2,6-TDI) or a mixture thereof, 4,4'-toluidine diisocyanate, 4,4'-diphenyl ether diisocyanate, diphenylmethane-2,2'-diisocyanate, diphenylmethane-2,4'-diisocyanate, diphenylmethane-4,4'-diisocyanate, etc.; diisocyanate compounds as dimers, trimers, biuret, allophanate, uretdione, uretonimine, oxadiazinetrione, crude compounds of these diisocyanates; etc.

[0120] The diisocyanate compound may be a prepolymer obtained by reacting the diisocyanate or its derivative with a compound having active hydrogen that can react with the diisocyanate under the condition of excess isocyanate groups. Furthermore, it may be a compound in which the isocyanate groups in the diisocyanate or its derivative are blocked by a blocking agent, i.e., a blocked diisocyanate compound.

[0121] As the compound having active hydrogen capable of reacting with the diisocyanate, a compound used in forming a prepolymer containing a trifunctional or higher polyisocyanate compound or a derivative thereof can be used. Also, as the end-capping agent, a compound used in forming a blocked polyisocyanate containing a trifunctional or higher polyisocyanate compound or a derivative thereof can be used.

[0122] In the present invention, as the diisocyanate compound, preferably one or more selected from the following: aliphatic diisocyanates, aromatic aliphatic diisocyanates, aromatic diisocyanates, etc. can be used. Particularly preferably, hexamethylene diisocyanate, xylene diisocyanate, isophorone diisocyanate, monomeric MDI (a compound represented by the following structural formula (C') and n=0) can be used.

[0123]

[0124] (Amount of each ingredient)

[0125] The respective amounts of the "compound having one or more epoxy groups", "trivalent or higher phenolic compounds and / or compounds containing trifunctional or higher polyisocyanates" used in the preparation of the epoxy resin of the first embodiment of the present invention, and the "compound having one or more active hydrogen in one molecule other than trivalent or higher phenolic compounds and / or diisocyanate compounds" used as needed can be appropriately adjusted according to the desired epoxy equivalent, etc.

[0126] For example, based on the total solid content mass of "compounds having one or more epoxy groups", "trivalent or higher phenolic compounds and / or compounds containing trifunctional or higher polyisocyanates", and "compounds having one or more active hydrogen in one molecule other than trivalent or higher phenolic compounds and / or diisocyanate compounds", the blending amount of each component can be in the following range.

[0127] "Compound having one or more epoxy groups": 50 to 99.9% by mass, preferably 65 to 95% by mass, more preferably 65 to 92% by mass.

[0128] "Trivalent or higher phenol compound and / or trifunctional or higher polyisocyanate-containing compound": 0.1 to 50% by mass, preferably 0.2 to 30% by mass, more preferably 0.5 to 20% by mass.

[0129] "Compounds having one or more active hydrogen atoms in one molecule other than trivalent or higher phenol compounds and / or diisocyanate compounds": 0 to 49.9% by mass, preferably 0 to 30% by mass, more preferably 1 to 30% by mass.

[0130] When the content of "a trivalent or higher phenol compound and / or a compound containing a trifunctional or higher polyisocyanate" is less than 0.1% by mass, the multifunctional modification of the epoxy resin may not be sufficient, and a multifunctional and highly reactive epoxy resin may not be obtained. On the other hand, when the content of "a trivalent or higher phenol compound and / or a compound containing a trifunctional or higher polyisocyanate" exceeds 50% by mass, the reactivity of the epoxy resin may be too high, resulting in gelation during synthesis, or the storage stability of the coating may be deteriorated.

[0131] Furthermore, when using “compounds having one or more active hydrogen atoms in one molecule other than trivalent or higher phenolic compounds and / or diisocyanate compounds”, the blending amount of the “trivalent or higher phenolic compounds and / or compounds containing trifunctional or higher polyisocyanates” can be in the following range based on the total solid content mass of the “trivalent or higher phenolic compounds and / or compounds containing trifunctional or higher polyisocyanates” and the “compounds having one or more active hydrogen atoms in one molecule other than trivalent or higher phenolic compounds and / or diisocyanate compounds”.

[0132] "Trivalent or higher phenol compound and / or trifunctional or higher polyisocyanate-containing compound": 0.1 to 99% by mass, preferably 0.5 to 95% by mass, more preferably 0.5 to 90% by mass.

[0133] (First aspect of the method for producing epoxy resin)

[0134] The reaction of the epoxy compound and the trivalent or higher phenol compound can be carried out in a suitable solvent at a temperature of about 80 to 190°C, preferably about 90 to 170°C, for about 1 to 6 hours, preferably about 1 to 5 hours.

[0135] In the present invention, the epoxy resin can be multifunctionalized by a trivalent or higher phenol compound. Also, for example, the chain of the epoxy resin can be extended by a compound having two active hydrogen atoms in one molecule (such as a divalent phenol compound).

[0136] As the solvent used in the reaction, for example, one or more selected from the following can be used: hydrocarbon compounds, such as toluene, xylene, cyclohexane, n-hexane, etc.; ester compounds, such as methyl acetate, ethyl acetate, butyl acetate, etc.; ketone compounds, such as acetone, methyl ethyl ketone, methyl isobutyl ketone, methyl amyl ketone, etc.; amide compounds, dimethylformamide, dimethylformamide, etc.; alcohols, such as methanol, ethanol, n-propanol, isopropanol, etc.; ether alcohol compounds, such as ethylene glycol monobutyl ether, diethylene glycol monoethyl ether, etc.; etc.

[0137] The weight average molecular weight of the epoxy resin of the first embodiment is preferably in the range of usually 500 to 50,000, further preferably in the range of 1,000 to 20,000, and further preferably in the range of 1,500 to 10,000, from the viewpoint of appearance characteristics and corrosion resistance.

[0138] Unless otherwise specified, the weight average molecular weight in this specification is a value obtained by converting the retention time (retention capacity) measured using a gel permeation chromatograph (GPC) into a molecular weight of polystyrene by the retention time (retention capacity) of a standard polystyrene of known molecular weight measured under the same conditions. Specifically, it can be measured under the conditions of using "HLC8120GPC" (trade name, manufactured by Tosoh Corporation) as a gel permeation chromatograph, using "TSKgel G-4000HXL", "TSKgel G-3000HXL", "TSKgel G-2500HXL" and "TSKgel G-2000HXL" (trade names, all manufactured by Tosoh Corporation) as chromatographic columns, tetrahydrofuran as a mobile phase, 40°C as a measurement temperature, 1 mL / min as a flow rate, and RI (differential refractive index detector) as a detector.

[0139] <Epoxy Resin of the Second Embodiment>

[0140] The epoxy resin of the second embodiment of the present invention is an epoxy resin obtained by reacting at least a compound having one or more epoxy groups with a compound having a functional group reactive with an epoxy group, and is an epoxy resin represented by the following formula (1) and having an average multifunctionality (X1) of 0.30 or more per epoxy resin molecule.

[0141] Formula (1):

[0142] Average multifunctionality (X1) = number of ends per epoxy resin molecule - 2

[0143] Examples of the “compound having one or more epoxy groups” used to obtain the epoxy resin of the second embodiment include the “compound having one or more epoxy groups” used to obtain the epoxy resin of the first embodiment.

[0144] Moreover, as the "compound having a functional group reactive with an epoxy group", one or more selected from the following can be listed: a "trivalent or higher phenol compound", a "compound containing a trifunctional or higher polyisocyanate" and a "compound having one or more active hydrogen in one molecule" used to obtain the first embodiment of the epoxy resin.

[0145] Furthermore, the amount of each component added may be the same as that of each component in the epoxy resin of the first embodiment.

[0146] The curability of the epoxy resin of the second embodiment of the present invention, particularly the curability when using a low-activity catalyst and the curability at low temperatures, storage stability, appearance characteristics of the coating film when the epoxy resin is used to prepare an electrodeposition coating, and corrosion resistance are closely related to the multifunctionality of the epoxy resin. In particular, the above characteristics can be optimized by using the average multifunctionality (X1) per epoxy resin molecule as the multifunctionality of the epoxy resin and setting the range thereof to a specific range.

[0147] As methods for making epoxy resins multifunctional, there are the following methods: (1) reacting a multifunctionalizing agent having three or more reactive functional groups that react with epoxy groups with an epoxy resin (having one or more, preferably two or more epoxy groups) (multifunctionalization by a multifunctionalizing agent); (2) multifunctionalizing by reacting a secondary hydroxyl group in an epoxy resin molecule with at least one of the terminal epoxy groups of other epoxy resins (multifunctionalization by incorporation), and any of these methods can be appropriately adopted. From the viewpoint of stably preparing epoxy resins, it is preferred to use at least the above method (1).

[0148] The average multifunctionality (X1) per molecule of epoxy resin can be calculated by the following formula:

[0149] Average multifunctionality (X1) = number of ends of one epoxy resin molecule - 2

[0150] In the formula, "the number of terminals per molecule of epoxy resin" is the number of terminals having an epoxy group or a functional group reactive with an epoxy group in one molecule of epoxy resin.

[0151] For example, when one molecule has three terminals, X is 1, and when the epoxy resin is a linear chain that is not polyfunctionalized at all, X is 0. The larger the average polyfunctionality (X1) value is, the higher the polyfunctionality per molecule is.

[0152] In addition, the polyfunctionalization of the epoxy resin terminal by reacting a polyfunctional modifier (e.g., ketimide of diethylenetriamine and amine compounds such as diethanolamine, and carboxylic acid compounds such as dimethylolpropionic acid) with the epoxy resin terminal is not defined in the "polyfunctionalization" of the present invention because the reactivity is reduced due to steric hindrance. In addition, the secondary hydroxyl group inside the epoxy resin is also not defined in the "polyfunctionalization" of the present invention from the viewpoint of reactivity.

[0153] The term "multifunctionalization" in the present invention means that the main skeleton of the epoxy resin is branched. Furthermore, the term "number of terminals of one molecule of epoxy resin" in the present invention means the number of molecular terminals having functional groups generated by branching of the main skeleton (main chain of the epoxy resin) in the epoxy resin.

[0154] When the epoxy resin is polyfunctionalized by the above method (1) (polyfunctionalization by a polyfunctionalizing agent), the average polyfunctionality (N) per molecule of the epoxy resin by the polyfunctionalizing agent can be calculated by the following formula.

[0155] Average polyfunctionality based on polyfunctional agent (N) = Σ[(valence of each polyfunctional agent - 2) × basic compounding amount of each polyfunctional agent]

[0156] The "basic blending amount" of each polyfunctionalizing agent can be determined by the following method.

[0157] (Calculation method of basic matching)

[0158] Basic compounding amount of each raw material (mol) = compounding amount of each raw material (mol) × basic compounding multiple

[0159] ※The amount of each raw material (mol) = the mass of each raw material (g) / the molecular weight of each raw material

[0160] ※Basic compounding multiple = 2 / (number of epoxy groups (mol) - number of functional groups that react with epoxy groups other than the terminal blocking agent (mol) - number of multifunctional groups based on the multifunctionalizing agent)

[0161] ※Terminal blocking agent: monofunctional amine, acid, etc.

[0162] ※Functional groups that react with epoxy groups: phenolic hydroxyl groups or isocyanate groups with two or more functional groups, amino groups of amines with two or more active hydrogen atoms, etc.

[0163] ※The number of polyfunctional agents based on the polyfunctional agent = (the valence of the polyfunctional agent - 2) × the amount of the polyfunctional agent (mol)

[0164] The above method (2) (multifunctionalization by incorporation) is a method of reacting an epoxy group of an epoxy resin with a secondary hydroxyl group of (another) epoxy resin.

[0165] In this case, the average multifunctionality (M) per molecule of the epoxy resin incorporated can be calculated by the following formula.

[0166] Average multifunctionality based on incorporation (M) = (2-m) / (1-m)-2

[0167] ※m: Excess amount of epoxy groups in the basic formulation

[0168] The excess amount of epoxy groups (excess EP amount) in the basic formulation was calculated as follows.

[0169] ■ Excess amount of EP in the basic compound = Number of EP groups in the basic compound (mol) - Number of functional groups in the basic compound that react with EP groups (mol)

[0170] The excess amount of EP in the epoxy resins of the first to third aspects of the present invention is usually 0 to 5 mmol / g, preferably 0 to 2 mmol / g, and more preferably 0 to 1.5 mmol / g based on the resin solid content.

[0171] Furthermore, the average multifunctionality (X1) per epoxy resin molecule can be calculated from the average multifunctionality (N) based on the multifunctionalizing agent and the average multifunctionality (M) based on incorporation using the following formula.

[0172] Average multifunctionality (X1) = (N+2) × (M+1) - M-2

[0173] Regarding the epoxy resin of the second embodiment of the present invention, the average multifunctionality (X1) per epoxy resin molecule can be 0.30 or more, preferably in the range of 0.30 to 15.00, more preferably in the range of 0.60 to 13.00, further preferably in the range of 0.70 to 10.00, and particularly preferably in the range of 0.90 to 8.00.

[0174] <Third-Part Epoxy Resin>

[0175] The epoxy resin of the third formula of the present invention is an epoxy resin obtained by reacting at least a compound having one or more epoxy groups with a compound having a functional group reactive with an epoxy group. When a plurality of multifunctional epoxy resins are included, the following average multifunctionality (X1) is calculated as the average value of the average multifunctionality of each epoxy resin.

[0176] In the epoxy resin, the average polyfunctionality (X1) of the epoxy resin represented by the following formula (1) is 0.30 or more, and the average polyfunctional concentration (Y1) represented by the following formula (2) is 0.1 or more.

[0177] Formula (1):

[0178] Average multifunctionality (X1) = number of ends of one epoxy resin molecule - 2

[0179] Formula (2):

[0180] Average multifunctional concentration (Y1) = average multifunctionality of epoxy resin (X1) / weight average molecular weight of epoxy resin Mw × 1000

[0181] Examples of the “compound having one or more epoxy groups” used to obtain the epoxy resin of the third embodiment include one or more selected from the “compound having one or more epoxy groups” used to obtain the epoxy resin of the first embodiment.

[0182] Moreover, as the “compound having a functional group reactive with an epoxy group”, one or more selected from the group consisting of “trivalent or higher phenolic compounds”, “compounds containing trifunctional or higher polyisocyanates” and “compounds having one or more active hydrogen atoms in one molecule” used to obtain the first embodiment of the epoxy resin can be listed.

[0183] Furthermore, the amount of each component added may be the same as that of each component in the epoxy resin of the first embodiment.

[0184] For the epoxy resin of the third embodiment of the present invention, its curability, especially curability when using a low-activity catalyst and curability at low temperatures, storage stability, appearance characteristics of the coating film when the epoxy resin is used to prepare an electrodeposition coating, and corrosion resistance are closely related to the average polyfunctional concentration of the epoxy resin in addition to the polyfunctionality of the epoxy resin. In particular, the above characteristics can be optimized by using the average polyfunctionality (X1) and the average polyfunctional concentration (Y1) per molecule of the epoxy resin as the polyfunctionality of the epoxy resin and setting their respective ranges to specific ranges.

[0185] The average multifunctionality (X1) of the epoxy resin represented by the following formula (1) in the epoxy resin of the third embodiment is the same as the average multifunctionality (X1) of the epoxy resin of the second embodiment.

[0186] Formula (1):

[0187] Average multifunctionality (X1) = number of ends of one epoxy resin molecule - 2

[0188] For the epoxy resin of the third formula of the present invention, the average multifunctionality (X1) per epoxy resin molecule can be greater than 0.30, preferably in the range of 0.30 to 15.00, more preferably in the range of 0.60 to 13.00, further preferably in the range of 0.70 to 10.00, and particularly preferably in the range of 0.90 to 8.00.

[0189] For the epoxy resin of the third formula, the average polyfunctional concentration (Y1) of the epoxy resin can be calculated from the average polyfunctionality (X1) of the epoxy resin and the weight average molecular weight Mw of the epoxy resin using the following formula (2).

[0190] Formula (2):

[0191] Average multifunctional concentration (Y1) = average multifunctionality of epoxy resin (X1) / weight average molecular weight of epoxy resin Mw × 1000

[0192] The weight average molecular weight Mw of the epoxy resin is calculated as follows.

[0193] Weight average molecular weight of epoxy resin Mw = Σ(amount of each raw material in the basic formulation (mol) × molecular weight of each raw material)

[0194] The average number of functional groups per trifunctional or higher polyfunctional agent component molecule contained in the polyfunctional agent is calculated by the following formula.

[0195] Average number of functional groups = Σ(content ratio of each multifunctionalizing agent component ÷ molecular weight of each multifunctionalizing agent component × number of functional groups of each multifunctionalizing agent component) / Σ(content ratio of each multifunctionalizing agent component ÷ molecular weight of each multifunctionalizing agent component)

[0196] Moreover, for the epoxy resin of the third formula of the present invention, the average multifunctional concentration (Y1) per gram of solid content of the epoxy resin can be above 0.10 (mmol / g), preferably in the range of 0.10 to 5.00, more preferably in the range of 0.40 to 3.00, and further preferably in the range of 0.40 to 2.00.

[0197] The average polyfunctional concentration (Y1) specifies the degree of polyfunctionality per unit mass. The larger the value of Y1, the more functional groups there are and the higher the reactivity of the resin.

[0198] When the above-mentioned multifunctionality and / or multifunctional concentration is high, gelation or viscosity increase may occur during resin synthesis, and the appearance characteristics of the coating film may deteriorate. In addition, when the above-mentioned multifunctionality and / or multifunctional concentration is low, corrosion resistance and oil-resistant crater resistance (oil-resistant crater resistance) may decrease.

[0199] The epoxy resins of the first to third embodiments may also be resins having terminal functional groups other than epoxy groups, for example, modified epoxy resins having other reactive functional groups at the terminals by reacting the epoxy groups of the multifunctional epoxy resins with a compound containing reactive functional groups after synthesizing the epoxy resins described in the first to third embodiments. However, when the terminal functional groups become multiple by reacting one epoxy group at the terminal of the epoxy resin with a compound containing reactive functional groups (for example, diethanolamine) (in the case of diethanolamine, the epoxy group reacts with the secondary amino group of the diethanolamine to produce two hydroxyl groups derived from the diethanolamine and a hydroxyl group derived from the epoxy group), the "number of multifunctional functional groups" in the present invention is also one as described above.

[0200] The functional group reactive with the epoxy group is not particularly limited as long as it can react with the epoxy group, and examples thereof include a carboxyl group, a primary or secondary amino group, and a hydroxyl group.

[0201] In the above case (modified epoxy resin), the average multifunctionality (X1) and the average multifunctional concentration (Y1) can be calculated in the same manner.

[0202] [Amino-containing epoxy resin]

[0203] The epoxy resin of the present invention may be an amino-containing epoxy resin having an amino group.

[0204] The amino group-containing epoxy resin can be obtained by reacting any one of the epoxy resins of the first to third aspects with an amine compound.

[0205] Examples of the amino group-containing epoxy resin obtained by reacting the epoxy resin of the first embodiment with an amine compound include the following (a) and (b).

[0206] (a) An amino-containing epoxy resin obtained by reacting an epoxy resin with an amine compound, wherein the epoxy resin is obtained by reacting at least a compound having two or more epoxy groups with a compound containing a trivalent or higher phenolic compound, wherein the trivalent or higher phenolic compound contains a compound represented by the following structural formula (A).

[0207]

[0208] (In the formula, n represents an integer of 1 to 20, p represents an integer of 0 to 4, q represents an integer of 0 to 3, and r represents an integer of 0 to 4; R1 to R3 are each independently a monovalent group; R2 may be different for every n repeating units; when there are multiple R1, R2 and / or R3 in the aromatic ring, they may be the same or different; R1 to R3 may be bonded to each other to form a ring.)

[0209] (b) An amino-containing epoxy resin obtained by reacting an epoxy resin with an amine compound, wherein the epoxy resin is obtained by reacting at least a compound having one or more epoxy groups and a trivalent or higher phenolic compound and / or a compound containing a trifunctional or higher polyisocyanate, wherein the trivalent or higher phenolic compound is not a xylene formaldehyde resin.

[0210] As the epoxy compound used when obtaining any of the epoxy resins of the first to third aspects, it is preferred to use a compound that has not been reacted with an amine compound in advance.

[0211] Furthermore, as required, as the epoxy compound used when obtaining any of the first to third forms of epoxy resin, a compound in which an amine compound has been reacted in advance may be used. In this case, the amount of the amine compound used may be appropriately determined so that the amine value of the amino-containing epoxy resin reaches a desired value, and the amount of the amine compound used is preferably 99 mol% or less relative to the total amine compound.

[0212] <Amine compounds>

[0213] The amine compound is not particularly limited as long as it is an amine compound reactive with the epoxy resin. For example, one or more selected from the following can be used: monoalkylamine or dialkylamine, such as monomethylamine, dimethylamine, monoethylamine, diethylamine, dipropylamine, dibutylamine, dihexylamine, dioctylamine, monoisopropylamine, diisopropylamine, monobutylamine, monooctylamine, methylbutylamine, dibutylamine, etc.; alkanolamine, such as monoethanolamine, N-methylethanolamine, N-ethylethanolamine, diethanolamine, mono(2-hydroxypropyl)amine, di(2-hydroxypropyl)amine, N-butylethanolamine, dipropanolamine, monomethylaminoethanol, N-(2-hydroxypropyl)ethylenediamine, 3-methylamino-1,2-propylene glycol, 3-tert-butylamino-1,2-propylene glycol, N-methylglucosamine, N-octylglucosamine, etc.; alkylene polyamines such as polymethylenediamine, polyetherdiamine, ethylenediamine, propylenediamine, butylenediamine, hexamethylenediamine, trimethylhexamethylenediamine, triethylenetetramine, dimethylamino Propylamine, diethylenetriamine, diethylaminopropylamine, bis(4-aminobutyl)amine, etc.; aromatic or alicyclic polyamines, such as phenylenediamine, isophoronediamine, bis(4-amino-3-methylcyclohexyl)methane, meta-phenylenediamine, meta-phenylenediamine, naphthalene diamine, dimethylaminomethylbenzene, etc.; polyamines having a heterocyclic ring, such as piperazine, 1-methylpiperazine, 3-pyrrolidone, 3-piperidinol, 4-pyrrolidone, etc.; epoxy-added polyamines obtained by adding 1 to 30 mol of epoxy-containing compounds to 1 mol of the above polyamines; polyamide polyamines containing one or more primary or secondary amines in the polyamide resin molecule generated by condensation of the above polyamines with aromatic anhydrides, cyclic aliphatic anhydrides, aliphatic anhydrides, halogenated anhydrides and / or dimer acids; ketimines obtained by reacting one or more primary or secondary amines in the above polyamines with a ketone compound; etc.

[0214] As the ketone compound used to prepare the above-mentioned ketimine, as long as it reacts with the primary amine or secondary amine in the above-mentioned polyamine to become a ketimine, and then is hydrolyzed in the aqueous coating composition, it can be used without particular restriction. For example, one or more selected from the following: methyl isopropyl ketone (MIPK), diisobutyl ketone (DIBK), methyl isobutyl ketone (MIBK), diethyl ketone (DEK), ethyl butyl ketone (EBK), ethyl propyl ketone (EPK), dipropyl ketone (DPK), methyl ethyl ketone (MEK), etc. can be used. In the present invention, when ketimine is used, its ketoneization rate is not particularly limited. For example, it is preferably 80% or more.

[0215] The amino-containing epoxy resin can be modified by a modifier as required. Such a modifier is not particularly limited as long as it is a resin or compound reactive with the epoxy resin, and for example, one or more selected from the following can be used: polyols, polyether polyols, polyester polyols, polyamide amines, polycarboxylic acids, fatty acids, polyisocyanate compounds, compounds formed by reaction of polyisocyanate compounds, lactone compounds such as ε-caprolactone, acrylic monomers, compounds formed by polymerization of acrylic monomers, xylene formaldehyde compounds, epoxy compounds, etc.

[0216] The usage ratio of the above-mentioned modifier is not strictly limited and can be appropriately changed according to the application of the coating composition, but from the viewpoint of improving the appearance characteristics and corrosion resistance, the appropriate usage ratio is usually in the range of 0 to 50% by mass, preferably in the range of 0.1 to 30% by mass, and more preferably in the range of 1 to 20% by mass, based on the solid content mass of the amino-containing epoxy resin.

[0217] <Preparation method of amino-containing epoxy resin>

[0218] Regarding the reaction of the first embodiment of the epoxy resin (an epoxy resin obtained by reacting a compound having at least one epoxy group, a trivalent or higher phenolic compound and / or a compound containing a trifunctional or higher polyisocyanate) and an amine compound, the reaction can be carried out, for example, in a suitable solvent at a temperature of about 80°C to about 190°C, preferably about 90°C to about 170°C, for about 1 to 6 hours, preferably about 1 to 5 hours.

[0219] As the solvent used for the reaction, for example, the same solvent as that used for the preparation of the epoxy resin in the first embodiment can be used.

[0220] The weight average molecular weight of the amino group-containing epoxy resin is usually in the range of 1,000 to 50,000, more preferably in the range of 1,300 to 20,000, and particularly preferably in the range of 1,600 to 10,000 from the viewpoint of appearance characteristics and corrosion resistance.

[0221] The amine value of the amino-containing epoxy resin is usually 5 mgKOH / g or more, preferably in the range of 10 to 200 mgKOH / g, and more preferably in the range of 30 to 150 mgKOH / g based on the resin solid content, from the viewpoint of improving water dispersibility and corrosion resistance.

[0222] The amine value in this specification is measured according to JIS K7237-1995. This amine value is the amine value (mgKOH / g) of the total resin solid content.

[0223] In addition, the weight average molecular weight of the amino group-containing epoxy resin is the same as the weight average molecular weight described in the epoxy resin of the first embodiment.

[0224] [Water-based resin dispersion]

[0225] The aqueous resin dispersion of the present invention can be obtained by dispersing one or more epoxy resins selected from any one of the epoxy resins of the first to third aspects and modified products thereof in an aqueous medium.

[0226] For example, it can be obtained by dispersing the epoxy resins of the first to third forms in an aqueous medium. Furthermore, it can be obtained by neutralizing the following amino-containing epoxy resins (i) and / or (ii) with an acid compound and dispersing them in an aqueous medium, wherein the amino-containing epoxy resin (i) is obtained by reacting any one of the epoxy resins of the first to third forms with an amine compound; and the amino-containing epoxy resin (ii) is obtained by using a substance that has been reacted with an amine compound in advance as the epoxy compound used when obtaining any one of the epoxy resins of the first to third forms.

[0227] In the present invention, the "aqueous resin dispersion" refers to a state in which the resin component is not dissolved in the above-mentioned aqueous medium but exists in a particle state.

[0228] The content of one or more epoxy resins selected from any one of the epoxy resins of the first to third aspects and modified products thereof in the aqueous resin dispersion is preferably 50% by mass or more based on the solid content.

[0229] The aqueous resin dispersion is preferably prepared by mixing the epoxy resin of the first to third embodiments and / or its modified product and the curing agent (blocked polyisocyanate compound, etc.) described later and dispersing them in an aqueous medium. In this case, the epoxy resin and / or its modified product is preferably an amino-containing epoxy resin, and the curing agent is preferably a blocked polyisocyanate compound.

[0230] The mixing ratio (mass ratio) of the epoxy resin and / or its modified product and the curing agent is preferably 1 / 99 to 99 / 1, more preferably 30 / 70 to 90 / 10, and even more preferably 40 / 60 to 85 / 15, based on the solid content.

[0231] The aqueous medium used when dispersing one or more epoxy resins selected from any one of the first to third forms of epoxy resins and modified products thereof is a solvent containing water and / or a hydrophilic solvent as a main component (containing 50% by mass or more in the solvent). Other solvents may include, for example, ester solvents, ketone solvents, amide solvents, alcohol solvents, ether alcohol solvents, or mixtures thereof.

[0232] Among them, as the hydrophilic solvent, specifically, for example, one or more selected from the following can be used: ethylene glycol, ethylene glycol monoalkyl ether (for example, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol butyl ether, etc.), diethylene glycol, diethylene glycol monoalkyl ether (for example, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol butyl ether, etc.), glyme solvents (for example, ethylene glycol dimethyl ether, etc.), diethylene glycol dimethyl ether solvents (such as diethylene glycol dimethyl ether, etc.), alcohol solvents (for example, methanol, ethanol, propanol, n-butanol, etc.), propylene glycol, propylene glycol monoalkyl ether (for example, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol butyl ether, etc.), dipropylene glycol, dipropylene glycol monoalkyl ether (for example, dipropylene glycol methyl ether, dipropylene glycol ethyl ether, dipropylene glycol butyl ether, etc.), etc.

[0233] As the acid compound used when dispersing in an aqueous medium, known acid compounds can be used without particular limitation. Specifically, examples include inorganic acids such as hydrochloric acid, nitric acid, phosphoric acid, and aminosulfonic acid; and organic acids including carboxylic acid compounds such as formic acid, acetic acid, propionic acid, and lactic acid. These acid compounds can be used alone or in combination of two or more, among which organic acids can be preferably used, and carboxylic acid compounds are particularly more preferably used.

[0234] The neutralization equivalent is preferably 0.2 to 1.5 equivalents, more preferably 0.5 to 1.0 equivalents, of the acid compound relative to 1 equivalent of the amino group.

[0235] The aqueous resin dispersion of the present invention may contain, in addition to one or more epoxy resins selected from any one of the first to third aspects and modified products thereof and an acid compound, additives such as a neutralizer, an emulsifier, a catalyst, and other resin components as needed.

[0236] When dispersing the amino-containing epoxy resin in the aqueous medium, the aqueous medium may be added while stirring the neutralized amino-containing epoxy resin, or the neutralized amino-containing epoxy resin may be added to the aqueous medium while stirring, or the aqueous medium and the neutralized amino-containing epoxy resin may be mixed and stirred. The dispersion temperature is preferably less than 100° C., more preferably 40 to 99° C., and further preferably 50 to 95° C. The resin solid content concentration of the obtained dispersion is preferably 5 to 80% by mass, and more preferably 10 to 50% by mass.

[0237] [Electrodeposition coating]

[0238] The electrodeposition paint of the present invention may be any of a cationic electrodeposition paint and an anionic electrodeposition paint as long as it contains the epoxy resin.

[0239] The cationic electrodeposition coating preferably contains the epoxy resin of the first to third aspects of the present invention, or an amino-containing epoxy resin obtained by reacting the epoxy resin with an amine compound as a coating film-forming resin component. Furthermore, the cationic electrodeposition coating may also be an electrodeposition coating containing an aqueous resin dispersion, wherein the aqueous resin dispersion is formed by dispersing the epoxy resin of the first to third aspects of the present invention, or an amino-containing epoxy resin obtained by reacting the epoxy resin with an amine compound in an aqueous medium.

[0240] The anionic electrodeposition coating material preferably contains the epoxy resin of the first to third forms of the present invention, or an amino-containing epoxy resin obtained by reacting the epoxy resin with an amine compound as a coating film forming resin component. Furthermore, the anionic electrodeposition coating material may also be an electrodeposition coating material containing an aqueous resin dispersion, wherein the aqueous resin dispersion is formed by dispersing the epoxy resin of the first to third forms of the present invention, or an amino-containing epoxy resin obtained by reacting the epoxy resin with an amine compound in an aqueous medium.

[0241] <Cationic electrodeposition coating>

[0242] The cationic electrodeposition coating of the present invention may also include, as essential components: a coating film-forming resin component containing the epoxy resin of the first to third forms, and a curing agent capable of curing with the epoxy resin. The cationic electrodeposition coating of the present invention may also contain a curing catalyst, a pigment, a solvent such as water, and an additive (surfactant, surface conditioner, curing co-catalyst, neutralizer, etc.) as required. As the above-mentioned epoxy resin, it is preferably an amino-containing epoxy resin (I) obtained by reacting the epoxy resin of the first to third forms with an amine compound.

[0243] Examples of the cationic electrodeposition paint of the present invention include a cationic electrodeposition paint containing the amino group-containing epoxy resin described in the above-mentioned [amino group-containing epoxy resin] and a curing agent.

[0244] Examples of the cationic electrodeposition coating material of the present invention include a single-layer cationic electrodeposition coating material containing the amino group-containing epoxy resin described in the above-mentioned [amino group-containing epoxy resin] and a curing agent.

[0245] Regarding the content of the amino-containing epoxy resin in the cationic electrodeposition coating of the present invention, when the resin components other than the curing agent in the cationic electrodeposition coating are 100 mass %, the content of the amino-containing epoxy resin is preferably 71 mass % or more, more preferably 85 mass % or more.

[0246] The cationic electrodeposition paint of the present invention is preferably a single-layer cationic electrodeposition paint. The single-layer cationic electrodeposition paint is a paint that forms a single-layer coating film having a substantially uniform composition in the thickness direction of the coating film when the coating is subjected to cationic electrodeposition coating and heated and cured.

[0247] For example, the single-layer cationic electrodeposition coating of the present invention is a cationic electrodeposition coating that forms a coating without two-layer separation (or multi-layer separation) when the cross section of the coating after electrodeposition coating is observed through a microscope. In addition, even if there are some deviations in the pigment component or the resin component, the case where no interface between the layers appears when observing the cross section is also a single-layer coating.

[0248] Furthermore, for example, the single-layer cationic electrodeposition paint of the present invention is a cationic electrodeposition paint that does not form a multilayer film having the following concentration gradient by a single electrodeposition coating. The concentration gradient is a concentration gradient in which the corrosion-resistant resin (epoxy resin) is mainly distributed in the lower layer (metal substrate surface side, the same below) and the resin other than the epoxy resin is mainly distributed in the upper layer.

[0249] As the coating film forming resin component other than the amino-containing epoxy resin (I), one or more selected from the following: acrylic resin, epoxy resin other than the epoxy resin of the first to third aspects of the present invention or its modified product (including amino modification), polyurethane resin and melamine resin, etc. can be used.

[0250] When the cationic electrodeposition paint contains an acrylic resin, the content of the acrylic resin in the cationic electrodeposition paint is preferably less than 30% by mass, more preferably less than 15% by mass, and further preferably less than 3% by mass, from the viewpoint of corrosion resistance, etc., when the total amount of all epoxy resins (including modified products) and acrylic resins is 100% by mass.

[0251] Furthermore, from the viewpoint of compatibility of resins and appearance characteristics, the absolute value of the difference in solubility parameter (SP value) between at least one epoxy resin and acrylic resin is preferably less than 1.0, more preferably less than 0.5. By using resins with similar SP values, a coating film without phase separation can be formed.

[0252] Among them, the solubility parameter is generally also called SP value (solubility parameter), which is a scale indicating the hydrophilicity or hydrophobicity of a resin. Moreover, the solubility parameter is an important scale for judging the compatibility between resins. Resins with similar solubility parameter values ​​(the absolute value of the difference in solubility parameter is small) generally have good compatibility.

[0253] The solubility parameter actually measured is a value measured by turbidity titration, and is calculated according to the following formula of KWSUH, JM CORBETT (see Journal of Applied Polymer Science, Vol. 12, 2359-2370 (1968)).

[0254] The actual measured solubility parameter (SP value) = (√Vml·δH+√Vmh·δD) / (√Vml+√Vmh)

[0255] Vml, Vmh, δH and δD are values ​​calculated by applying the titration amount H (mL) and the titration amount D (mL) to the following formula. The titration amount H (mL) is the titration amount at the turbidity point when n-hexane is added to 10 mL of tetrahydrofuran in which 0.5 g (solid content) of the resin is dissolved at a measuring temperature of 20°C and the limit at which a 4-point font can be recognized when looking through a newspaper placed below the bottom from the top of the beaker is set as the turbidity point; the titration amount D (mL) is the titration amount at the turbidity point when deionized water is added to 10 mL of tetrahydrofuran in which 0.5 g (solid content) of the resin is dissolved at a measuring temperature of 20°C.

[0256] Vml=81.1×130.3 / {(1-VH)×130.3+VH×81.1}

[0257] Vmh=81.1×18 / {(1-VD)×18+VD×81.1}

[0258] VH=H / (10+H)

[0259] VD=D / (10+D)

[0260] δH=9.52×10 / (10+H)+7.24×H / (10+H)

[0261] δD=9.52×10 / (10+D)+23.43×D / (10+D)

[0262] In addition, the molecular volume (mL / mol) of each solvent was 81.1 for tetrahydrofuran, 130.3 for n-hexane, and 18 for deionized water, and the SP value of each solvent was 9.52 for tetrahydrofuran, 7.24 for n-hexane, and 23.43 for deionized water.

[0263] The acrylic resin may be used without particular limitation, but a cationic acrylic resin is preferred.

[0264] The cationic acrylic resin can be prepared, for example, by radical copolymerization of an acrylic monomer containing a cationic base and other monomers. In the case of a non-cationic acrylic resin, it can be prepared using only other monomers described below.

[0265] Regarding the above-mentioned cationic base-containing acrylic monomers, specifically, for example, the following can be cited: amino-containing acrylic monomers and quaternary chlorides thereof, such as N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylate, N,N-di-tert-butylaminoethyl (meth)acrylate, etc.; acrylic monomers containing quaternary ammonium bases, such as (meth)acryloyloxyethyltrimethylammonium chloride, (meth)acryloyloxyethyldimethylbenzylammonium chloride, (meth)acryloyloxyethyltrimethylammonium methylsulfate, (meth)acryloyloxyethyldimethylethylethylammonium sulfate, etc.; acrylic monomers containing tertiary sulfonium bases such as 4-(dimethylsulfonyl)phenyl methacrylate, etc., and these can be used alone or in combination of two or more.

[0266] As for the above-mentioned other monomers, any known monomer other than the above-mentioned acrylic monomer containing a cationic base may be used appropriately, and examples thereof include (meth)acrylic acid, styrene, vinyltoluene, aromatic vinyl monomers such as α-methylstyrene, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, adducts of 2-hydroxyethyl (meth)acrylate and caprolactone (for example, products under the trade names of PLACCEL FA-2 and FM-3 manufactured by Daicel Chemical Industry, Ltd.), polyalkylene glycol (meth)acrylate, (meth)acrylamide, etc. These may be used alone or in combination of two or more.

[0267] The acrylic resin can be obtained by subjecting these monomers to a radical copolymerization reaction by a known method.

[0268] The hydroxyl value of the acrylic resin is usually in the range of 0 to 300 mgKOH / g, preferably in the range of 30 to 200 mgKOH / g. The weight average molecular weight of the acrylic resin is usually in the range of 1,000 to 200,000, preferably in the range of 3,000 to 50,000.

[0269] The amine value of the acrylic resin is usually in the range of 0 to 300 mgKOH / g, preferably in the range of 10 to 150 mgKOH / g.

[0270] Furthermore, an acrylic resin can be synthesized by free radical copolymerization of an acrylic monomer containing a reactive functional group and other monomers, and then a cationic base can be introduced into the acrylic resin by reacting the reactive functional group with a compound containing a cationic base. For example, an amine compound containing active hydrogen can be added to the glycidyl group of a copolymer of a polymerizable unsaturated monomer containing glycidyl (meth)acrylate to impart amino groups to the acrylic resin. Examples of the above-mentioned amine compounds include primary monoamines and primary polyamines, secondary monoamines and secondary polyamines, or mixed polyamines of primary and secondary amines, secondary monoamines and secondary polyamines having primary amino groups that have been ketoniated, and hydroxy compounds having primary amino groups that have been ketoniated.

[0271] The cationic electrodeposition coating of the present invention contains the amino group-containing epoxy resin (I), optionally an amino group-containing epoxy resin (II) obtained by reacting an epoxy resin having a functional group number of 2 or less with an amine compound, and a curing agent (particularly a blocked polyisocyanate compound).

[0272] The average multifunctionality (X2) of the amino-containing epoxy resin (I) represented by the following formula (3) may be 0.30 or more, preferably in the range of 0.30 to 15.00, more preferably in the range of 0.60 to 13.00, further preferably in the range of 0.70 to 10.00, and particularly preferably in the range of 0.90 to 8.00.

[0273] A cationic electrodeposition coating represented by the following formula (4) can be used, wherein the average multifunctional concentration (Y2) of the amino-containing epoxy resin contained therein is 0.1 (mmol / g) or more (preferably in the range of 0.1 to 5, more preferably in the range of 0.4 to 3.0, and further preferably in the range of 0.4 to 2.0).

[0274] If necessary, a curing catalyst, a pigment, a solvent such as water, and additives (surfactant, surface conditioner, curing co-catalyst, neutralizer, etc.) may be contained.

[0275] In addition, the above average polyfunctional concentration (Y2) is the average polyfunctional concentration (Y2) of all amino-containing epoxy resins contained in the cationic electrodeposition paint.

[0276] Formula (3):

[0277] Average multifunctionality (X2) = the number of terminals of one molecule of amino-containing epoxy resin (I) - 2

[0278] Formula (4):

[0279] Average polyfunctional concentration of amino-containing epoxy resin contained in cationic electrodeposition coating (Y2) = average polyfunctionality (X2) of amino-containing epoxy resin (I) / weight average molecular weight Mw of amino-containing epoxy resin (I) × 1000 × (amount of amino-containing epoxy resin (I) / amount of all amino-containing epoxy resins)

[0280] (Curing agent)

[0281] The curing agent contained in the cationic electrodeposition coating of the present invention is preferably at least one selected from the group consisting of blocked polyisocyanate compounds and amine resins.

[0282] -Blocked polyisocyanate compound-

[0283] The blocked polyisocyanate compound is an addition reaction product of a polyisocyanate compound and a blocking agent. Furthermore, as required, a compound obtained by reacting an active hydrogen-containing compound other than the blocking agent with the polyisocyanate compound together with the blocking agent may be used.

[0284] As the polyisocyanate compound, known compounds can be used. For example, one or more selected from the following: aromatic, aliphatic or alicyclic polyisocyanate compounds such as toluene diisocyanate, xylene diisocyanate, phenylene diisocyanate, diphenylmethane-2,2'-diisocyanate, diphenylmethane-2,4'-diisocyanate, diphenylmethane-4,4'-diisocyanate, crude MDI [polyphenyl polymethylene polyisocyanate], polymeric MDI, crude TDI, bis(isocyanate methyl) cyclohexane, tetramethylene diisocyanate, hexamethylene diisocyanate, methylene diisocyanate, isophorone diisocyanate, and dimers, trimers, biuret, allophanate, uretdione, uretonimine, isocyanurate, oxadiazinetrione, etc., of these polyisocyanate compounds can be used.

[0285] In particular, aromatic polyisocyanate compounds such as tolylene diisocyanate, xylene diisocyanate, phenylene diisocyanate, diphenylmethane-2,4′-diisocyanate, diphenylmethane-4,4′-diisocyanate, and MDI (preferably crude MDI) are more preferred for corrosion resistance.

[0286] The blocking agent is a substance that is added to the isocyanate group of the polyisocyanate compound to block the isocyanate group. The blocked polyisocyanate compound generated by the addition is relatively stable at room temperature (20±15°C), but the blocking agent is preferably dissociated when heated to the coating baking temperature (for example, about 80°C to about 200°C) to regenerate free isocyanate groups.

[0287] As the end-capping agent, for example, one or more selected from the following can be used: oxime compounds, such as methyl ethyl ketone oxime, cyclohexanone oxime, etc.; phenol compounds, such as phenol, p-tert-butylphenol, cresol, etc.; alcohol compounds, such as n-butanol, 2-ethylhexanol, benzyl alcohol, methylbenzyl alcohol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monoethyl ether, ethylene glycol, propylene glycol, propylene glycol monomethyl ether, methoxymethanol, etc.; lactam compounds, such as ε-caprolactam, γ-butyrolactam etc.; active methylene compounds, such as dimethyl malonate, diethyl malonate, diisopropyl malonate, ethyl acetoacetate, isopropyl acetoacetate, methyl acetoacetate, acetylacetone, etc.; pyrazole compounds, such as pyrazole, 3,5-dimethylpyrazole, 3-methylpyrazole, 4-bromo-3,5-dimethylpyrazole, 4-nitro-3,5-dimethylpyrazole, 4-benzyl-3,5-dimethylpyrazole, methyl-5-methylpyrazole-3-carboxylate, 3-methyl-5-phenylpyrazole, 3,5-dimethylpyrazole-4-carboxyaniline, etc.; thiol compounds, such as butyl mercaptan, tert-butyl mercaptan, hexyl mercaptan, tert-dodecyl mercaptan, 2-mercaptobenzothiazole, thiophenol, methylthiophenol, ethylthiophenol, etc.; amide compounds, such as acetanilide, methoxyacetanilide, N-acetyltoluidine, acrylamide, methacrylamide, acetamide, stearamide, benzamide, etc.; imide compounds, such as succinimide, phthalimide, maleic imide, etc.; amine compounds Compounds such as diphenylamine, phenylnaphthylamine, dimethylaniline, N-phenylenediamine, carbazole, aniline, naphthylamine, butylamine, dibutylamine, butylaniline, etc.; imidazole compounds such as imidazole, 2-ethylimidazole, etc.; urea compounds such as urea, thiourea, ethylene urea, ethylene thiourea, diphenyl urea, etc.; carbamate compounds such as N-phenylcarbamic acid phenyl ester, etc.; imine compounds such as ethyleneimine, propyleneimine, etc.; sulfite compounds such as sodium bisulfite, potassium bisulfite, etc.; etc.

[0288] Among them, the blocking agent is particularly preferably at least one selected from the following: pyrazole compounds, active methylene compounds, oxime compounds, phenol compounds, lactam compounds and alcohol compounds.

[0289] -Amino resin-

[0290] As the amino resin, known substances can be used. For example, one or more selected from various amino resins having alkanol groups (e.g., melamine resin, benzoguanamine resin, urea resin, etc.) and various amino resins containing alkoxyalkyl groups can be used, wherein the various amino resins having alkanol groups are obtained by reacting various amino compounds such as melamine, benzoguanamine, acetoguanamine or urea with various aldehyde compounds (or aldehyde supplying substances) such as formaldehyde or acetaldehyde, and the various amino resins containing alkoxyalkyl groups are obtained by reacting the amino resins having alkanol groups with various lower alcohols such as methanol, ethanol, n-butanol or isobutanol.

[0291] In the cationic electrodeposition coating, regarding the ratio of the amino-containing epoxy resin (including the amino-containing epoxy resin (I) and the amino-containing epoxy resin (II)) and the curing agent, based on the total amount of the amino-containing epoxy resin and the curing agent, the amino-containing epoxy resin is in the range of 30 to 90 parts by mass, preferably 40 to 85 parts by mass, and the curing agent is in the range of 10 to 70 parts by mass, preferably 10 to 60 parts by mass, which also helps to obtain a coating product with good storage stability, excellent appearance characteristics and corrosion resistance. Moreover, as the amine value of all resins contained in the coating, based on the resin solid content, the amine value is more preferably usually in the range of 20 to 150 mgKOH / g. When the ratio deviates from the above range, it will damage any of the properties of the cationic electrodeposition coating and the coating film performance, so it is not advisable.

[0292] (Curing Catalyst)

[0293] The cationic electrodeposition coating of the present invention can use a known curing catalyst as a curing catalyst without limitation. For example, one or more selected from the following can be used: inorganic compounds such as bismuth compounds, zinc compounds, tin compounds, titanium compounds, zirconium compounds, yttrium compounds, etc.; organic compounds such as phosphazene compounds, amine compounds, quaternary salt compounds, etc.; and their composites, etc.

[0294] Furthermore, in order to improve the curability of the coating film, an organic tin compound such as dibutyltin dibenzoate, dioctyltin oxide, or dibutyltin oxide may be used as a catalyst. However, due to current environmental regulations on organic tin compounds, it is preferred not to use organic tin compounds.

[0295] As an alternative catalyst to organic tin compounds, from an environmental perspective, it is more preferred to use one or more selected from the following as a curing catalyst: inorganic compounds, such as zinc compounds, bismuth compounds, titanium compounds, zirconium compounds, yttrium compounds, etc.; organic compounds, such as phosphazene compounds, amine compounds, quaternary salt compounds, etc.; and their complexes, etc., or substantially no curing catalyst is used.

[0296] The cationic electrodeposition paint of the present invention preferably contains a bismuth compound as a curing catalyst from the perspective of environment and safety.

[0297] As a bismuth compound, one or more selected from the following can be used: inorganic bismuth compounds such as metallic bismuth, bismuth chloride, bismuth oxychloride, bismuth bromide, bismuth oxide, bismuth hydroxide, bismuth nitrate, bismuth nitrite, bismuth silicate, bismuth aluminum silicate, bismuth aluminate, bismuth borate, bismuth phosphate, bismuth carbonate, and bismuth oxycarbonate; and organic bismuth compounds such as bismuth formate, bismuth acetate, bismuth salicylate, bismuth citrate, bismuth benzoate, bismuth gallate, bismuth oxalate, bismuth lactate, bismuth oleate, bismuth methoxyacetate, dihydroxymethyl bismuth propionate, dialkyldithiocarbamate bismuth, bismuth toluenesulfonate, and bismuth tribenzenesulfonate.

[0298] The proportion of the curing catalyst in the cationic electrodeposition coating of the present invention is 0.1 to 10 parts by mass, preferably 0.5 to 6 parts by mass, based on 100 parts by mass of the resin solid content.

[0299] (pigment)

[0300] As the pigment that can be used in the cationic electrodeposition paint of the present invention, for example, one or more selected from coloring pigments, rust-proof pigments, extender pigments and the like can be used.

[0301] These pigments are preferably mixed into the coating as a pigment dispersion paste. For example, a pigment dispersion paste prepared by the following process can be used for cationic electrodeposition coatings: a pigment dispersion resin, a pigment, and various additives such as a neutralizer are mixed and dispersed in a dispersion mixer such as a ball mill, a sand mill, or a pebble mill to prepare a pigment dispersion paste.

[0302] As the pigment, known substances can be used without particular limitation. For example, one or more selected from the following can be used: coloring pigments such as titanium oxide, carbon black, red iron oxide, etc.; body pigments such as clay, mica, barite, calcium carbonate, silicon dioxide, etc.; metal compounds having the function of antirust pigments such as zinc phosphate, iron phosphate, aluminum phosphate, calcium phosphate, zinc phosphite, zinc cyanide, zinc oxide, aluminum tripolyphosphate, zinc molybdate, aluminum molybdate, calcium molybdate, aluminum phosphomolybdate, aluminum zinc phosphomolybdate, etc.; etc.

[0303] Furthermore, in the present invention, when silicon dioxide is used, the amount thereof is less than 5% by mass.

[0304] As the pigment dispersing resin, known substances can be used without particular limitation. For example, one or more selected from the following: epoxy resins having hydroxyl groups and cationic groups, acrylic resins having hydroxyl groups and cationic groups, tertiary amine epoxy resins, quaternary ammonium salt epoxy resins, tertiary sulfonium salt epoxy resins, tertiary amine acrylic resins, quaternary ammonium salt acrylic resins, tertiary sulfonium salt acrylic resins, etc. can be used.

[0305] The amount of the pigment to be added is preferably in the range of 1 to 100 parts by mass, particularly preferably in the range of 10 to 50 parts by mass, per 100 parts by mass of the resin solid content in the cationic electrodeposition paint.

[0306] Examples of the cationic electrodeposition paint of the present invention include the following cationic electrodeposition paints (a) or (b).

[0307] (a) A single-layer cationic electrodeposition coating, comprising an amino-containing epoxy resin and a curing agent, wherein the amino-containing epoxy resin is obtained by reacting at least a compound having one or more epoxy groups, a trivalent or higher phenolic compound and / or a compound containing a trifunctional or higher polyisocyanate, and an amine compound, wherein the trivalent or higher phenolic compound is a compound represented by the following structural formula (A).

[0308]

[0309] (In the formula, n represents an integer of 1 to 20, p represents an integer of 0 to 4, q represents an integer of 0 to 3, and r represents an integer of 0 to 4; R1 to R3 are each independently a monovalent group; R2 may be different for every n repeating units; when there are multiple R1, R2 and / or R3 in the aromatic ring, they may be the same or different; R1 to R3 may be bonded to each other to form a ring.)

[0310] (b) A cationic electrodeposition coating, comprising an amino-containing epoxy resin and a curing agent, wherein the amino-containing epoxy resin is obtained by reacting at least a compound having one or more epoxy groups, a trivalent or higher phenolic compound and / or a compound containing a trifunctional or higher polyisocyanate, and an amine compound, wherein the trivalent or higher phenolic compound is a compound represented by the following structural formula (A), and when the resin component other than the blocked polyisocyanate compound is 100% by mass, the content of the amino-containing epoxy resin is 71% by mass or more.

[0311]

[0312] (In the formula, n represents an integer of 1 to 20, p represents an integer of 0 to 4, q represents an integer of 0 to 3, and r represents an integer of 0 to 4; R1 to R3 are each independently a monovalent group; R2 may be different for every n repeating units; when there are multiple R1, R2 and / or R3 in the aromatic ring, they may be the same or different; R1 to R3 may be bonded to each other to form a ring.)

[0313] The compound having one or more epoxy groups constituting the cationic electrodeposition paint of the present invention is preferably a compound that is not modified by amine. Furthermore, the epoxy resin constituting the cationic electrodeposition paint of the present invention is preferably obtained by reacting a compound having one or more epoxy groups, a compound containing a trivalent or higher phenolic compound, and a compound having one or more active hydrogen in one molecule other than a trivalent or higher phenolic compound.

[0314] Among them, the compound having one or more active hydrogen atoms in one molecule other than the trivalent or higher phenol compound is preferably a compound represented by the following structural formula (B), wherein the content ratio (mass ratio) of the trivalent or higher phenol compound and the compound of structural formula (B) is preferably in the range of 1 / 99 to 99 / 1.

[0315]

[0316] (In the formula, s represents an integer of 0 to 4, t represents an integer of 0 to 4; R4 and R5 are each independently a monovalent group; when there are multiple R4 and / or R5 in the aromatic ring, they may be the same or different; R4 and / or R5 may be bonded to each other to form a ring.)

[0317] Furthermore, the trifunctional or higher-functional polyisocyanate is preferably an isocyanurate-type isocyanate and / or crude MDI.

[0318] (Method for preparing cationic electrodeposition coating)

[0319] The cationic electrodeposition coating material of the present invention is not particularly limited as long as the method for preparing the cationic electrodeposition coating material can constitute a cationic electrodeposition coating material containing a predetermined amino group-containing epoxy resin and a curing agent.

[0320] For example, the following method for preparing a cationic electrodeposition coating can be cited, which has the following steps:

[0321] An amino group-containing epoxy resin is prepared by reacting an amine compound with an epoxy resin, wherein the epoxy resin is obtained by reacting at least a compound having one or more epoxy groups, and a trivalent or higher phenolic compound (excluding xylene formaldehyde resin) and / or a compound containing a trifunctional or higher polyisocyanate; and

[0322] The amino-containing epoxy resin and a curing agent are mixed to prepare a cationic electrodeposition coating.

[0323] In the method for preparing the cationic electrodeposition coating of the present invention, the compound having one or more epoxy groups is preferably a compound that is not modified by amine. Furthermore, the prepared cationic electrodeposition coating is preferably a single-layer cationic electrodeposition coating.

[0324] (Cationic electrodeposition coating method and coated product)

[0325] The cationic electrodeposition coating method using the cationic electrodeposition coating material of the present invention comprises the steps of: immersing a coating object in an electrodeposition coating bath composed of the cationic electrodeposition coating material; and applying electricity using the coating object as a cathode.

[0326] A cationic electrodeposition coating product using the cationic electrodeposition coating of the present invention can be obtained by immersing a coating object in an electrodeposition coating bath containing the cationic electrodeposition coating and performing electrodeposition coating.

[0327] Examples of objects to be coated with the cationic electrodeposition paint include automobile bodies, two-wheeled vehicle parts, household appliances, and other appliances, but are not particularly limited as long as they are metal-containing objects.

[0328] Examples of metal plates to be coated include cold-rolled steel plates, alloyed hot-dip galvanized steel plates, electrogalvanized steel plates, double-electrogalvanized iron-plated steel plates, organic composite plated steel plates, Al materials, Mg materials, and the like, as well as metal plates which have been subjected to surface cleaning such as alkaline degreasing and then subjected to surface treatments such as phosphate chemical conversion treatment, chromate treatment, and composite oxide treatment as needed.

[0329] As a cationic electrodeposition coating method, for example, the following method is used: that is, a cationic electrodeposition coating material diluted with deionized water or the like to adjust the solid content concentration to about 5 to 40% by mass, preferably 10 to 25% by mass, and further adjusted to a pH in the range of 4.0 to 9.0, preferably 5.5 to 7.0, is used as a bath, and the object to be coated is usually energized as a cathode under the conditions of adjusting the bath temperature to 15 to 35° C. and the load voltage to 100 to 400 V, preferably 150 to 350 V. After the cationic electrodeposition coating, in order to remove the excess cationic electrodeposition coating material attached to the object to be coated, it is usually washed with ultrafiltrate (UF filtrate), reverse osmosis filtered water (RO water), industrial water, pure water, etc.

[0330] The film thickness of the cationic electrodeposition coating is not particularly limited. Generally speaking, based on the dry coating, it can be set in the range of 5 to 40 μm, preferably in the range of 10 to 30 μm. Moreover, regarding the drying of the coating, the electrodeposition coating can be dried by using a drying device such as an electric hot air dryer or a gas hot air dryer, generally so that the surface temperature of the coated product is higher than 160°C and less than 200°C, but in the present invention, from the viewpoint of saving energy costs, it is preferably less than 160°C, more preferably 80 to 130°C, and particularly preferably 100 to 130°C. The baking time is 10 to 180 minutes, preferably 20 to 50 minutes. A cured coating can be obtained by the above-mentioned drying.

[0331] <Anionic electrodeposition coating>

[0332] The anionic electrodeposition coating of the present invention contains the coating film-forming resin component containing the epoxy resin and the carboxyl-containing resin of the present invention and a curing agent as essential components. It may also contain an epoxy phosphate compound, a curing catalyst, a pigment, a solvent such as water, and additives (surfactant, surface conditioning agent, curing co-catalyst, neutralizing agent, etc.) as needed.

[0333] (Carboxyl resin)

[0334] The carboxyl-containing resin is a resin having at least one carboxyl group in one molecule. The carboxyl-containing resin is preferably a resin further having at least one hydroxyl group. As the carboxyl-containing resin, specifically one or more selected from the following can be used: acrylic resin, polyester resin, polyether resin, polycarbonate resin, polyurethane resin, etc., and acrylic resin is preferably used from the aspect of improving scratch resistance.

[0335] The acrylic resin can be prepared by copolymerizing a mixture of a carboxyl group-containing radically polymerizable unsaturated monomer (a1), a hydroxyl group-containing radically polymerizable unsaturated monomer (a2), and optionally other radically polymerizable unsaturated monomers (a3).

[0336] As the carboxyl group-containing radically polymerizable unsaturated monomer (a1), for example, at least one selected from acrylic acid, methacrylic acid, crotonic acid, itaconic acid, maleic acid, fumaric acid and the like can be used.

[0337] As the above-mentioned hydroxyl-containing free radical polymerizable unsaturated monomer (a2), for example, one or more selected from the following: 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and PLACCEL FM1, PLACCEL FM2, PLACCEL FM3, PLACCEL FA1, PLACCEL FA2, PLACCEL FA3 (all manufactured by Daicel Chemical Industry, Ltd., trade names, caprolactone-modified hydroxy (meth)acrylates) and the like can be used.

[0338] As the above-mentioned other free radical polymerizable unsaturated monomer (a3), it is a free radical polymerizable unsaturated monomer different from the carboxyl group-containing free radical polymerizable unsaturated monomer (a1) and the hydroxyl group-containing free radical polymerizable unsaturated monomer (a2), for example, one or more selected from the following: an alkoxysilyl group-containing unsaturated monomer, such as γ-(meth)acryloxypropyltrimethoxysilane, γ-(meth)acryloxypropylmethyldimethoxysilane, γ-(meth)acryloxypropyltriethoxysilane, vinyltrimethoxysilane, etc.; C1-C1 (meth)acrylate; 18 Alkyl or cycloalkyl esters, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, lauryl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, etc.; aromatic vinyl monomers such as styrene; (meth)acrylamide monomers, such as (meth)acrylamide, N,N-dihydroxymethyl (meth)acrylamide, N,N-dimethoxymethyl (meth)acrylamide, N,N-di-n-butoxymethyl (meth)acrylamide, N-methoxymethyl-N-hydroxymethyl (meth)acrylamide, etc.; by the following formula: CH2=CR 2 -CONH-CH2-OR 1 (In the formula, R 1 represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms, R 2 represents a hydrogen atom or a methyl group); an unsaturated monomer containing an N-hydroxymethyl alkyl ether group represented by

[0339] As the unsaturated monomer containing an N-hydroxymethyl alkyl ether group represented by the above formula, for example, one or more selected from the group consisting of N-hydroxymethyl (meth) acrylamide, N-methoxymethyl (meth) acrylamide, N-ethoxymethyl (meth) acrylamide, N-propoxymethyl (meth) acrylamide, N-isopropoxymethyl (meth) acrylamide, N-butoxymethyl (meth) acrylamide, N-isobutoxymethyl (meth) acrylamide, N-hexyloxymethyl (meth) acrylamide, and N-isohexyloxymethyl (meth) acrylamide can be used.

[0340] In one embodiment, the carboxyl-containing resin is an acrylic resin that can be prepared by copolymerizing a mixture of a carboxyl-containing free radical polymerizable unsaturated monomer (a1), a hydroxyl-containing free radical polymerizable unsaturated monomer (a2), and other free radical polymerizable unsaturated monomers (a3), wherein the carboxyl-containing free radical polymerizable unsaturated monomer (a1) comprises acrylic acid, the hydroxyl-containing free radical polymerizable unsaturated monomer (a2) comprises a hydroxyl (meth)acrylate (e.g., 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, or hydroxybutyl (meth)acrylate), and the other free radical polymerizable unsaturated monomer (a3) ​​comprises one or more C1-C10 (meth)acrylates. 18 Alkyl or cycloalkyl esters. In another embodiment, relative to the above embodiment, as other free radical polymerizable unsaturated monomers (a3), an unsaturated monomer containing an N-hydroxymethyl alkyl ether group is further contained. Moreover, in another embodiment, relative to the above embodiment, as other free radical polymerizable unsaturated monomers (a3), an aromatic vinyl monomer (e.g., styrene) and an unsaturated monomer containing an alkoxysilyl group (e.g., γ-methacryloxypropyltrimethoxysilane) are further contained.

[0341] Regarding the ratio of these free radical polymerizable unsaturated monomers, based on the total amount of the free radical polymerizable unsaturated monomers constituted, it is preferred to include 1 to 20% by mass, preferably 4 to 10% by mass, of a carboxyl group-containing free radical polymerizable unsaturated monomer (a1), 1 to 40% by mass, preferably 5 to 30% by mass, of a hydroxyl group-containing free radical polymerizable unsaturated monomer (a2), and 40 to 98% by mass, preferably 60 to 91% by mass, of other free radical polymerizable unsaturated monomers (a3).

[0342] In particular, in order to improve impact resistance and adhesion of auxiliary materials, the acrylic resin preferably contains 3 to 15 mass %, preferably 5 to 12 mass %, of an unsaturated monomer containing an N-hydroxymethyl alkyl ether group represented by the above formula, based on the total amount of the free radical polymerizable unsaturated monomers.

[0343] The carboxyl resin used in the anionic electrodeposition coating of the present invention can be obtained by the following process: the above-mentioned carboxyl-containing free radical polymerizable unsaturated monomer (a1), the hydroxyl-containing free radical polymerizable unsaturated monomer (a2), any other free radical polymerizable unsaturated monomer (a3) ​​and a polymerization initiator are added and mixed, and then the mixture of free radical polymerizable unsaturated monomers is subjected to a free radical polymerization reaction for about 1 hour to about 24 hours, preferably about 2 hours to about 10 hours in an organic solvent maintained at about 50°C to about 300°C, preferably about 60°C to 250°C, in the presence of an inert gas such as nitrogen.

[0344] As the organic solvent used in the above-mentioned free radical polymerization reaction, for example, one or more selected from the following can be appropriately used: alcohols such as n-propanol, isopropanol, n-butanol, tert-butanol, isobutanol, etc.; ethers such as ethylene glycol monobutyl ether, methyl carbitol, 2-methoxyethanol, 2-ethoxyethanol, 2-isopropanol ethanol, 2-butoxyethanol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, propylene glycol monomethyl ether, etc.; etc. In addition, in addition to this, one or more selected from the following can be selectively used in combination, for example: aromatics such as xylene, toluene, etc.; esters such as acetone, methyl ethyl ketone, 2-pentanone, 2-hexanone, methyl isobutyl ketone, isophorone, cyclohexanone, 2-ethylhexyl acetate, benzyl acetate, cyclohexyl acetate, methyl propionate, ethyl propionate, etc.; etc.

[0345] As the polymerization initiator used in the free radical polymerization reaction, for example, one or more selected from the following: benzoyl peroxide, di-tert-butyl hydroperoxide, tert-butyl hydroperoxide, isopropylbenzene peroxide, isopropylbenzene hydroperoxide, tert-butyl perbenzoate, lauryl peroxide, acetyl peroxide, azodimethylvaleronitrile, azobisisobutyronitrile, etc. can be used.

[0346] The obtained carboxyl group-containing resin (A) preferably has a weight average molecular weight in the range of 5,000 to 100,000, particularly preferably 20,000 to 50,000, an acid value in the range of 5 to 180 mgKOH / g, and a hydroxyl value in the range of 3 to 150 mgKOH / g.

[0347] Here, the weight average molecular weight is a value obtained by converting the weight average molecular weight measured using gel permeation chromatography (GPC) based on the molecular weight of standard polystyrene.

[0348] Specifically, the measurement can be carried out under the following conditions: "HLC8120GPC" (trade name, manufactured by Tosoh Corporation) is used as the gel permeation chromatograph, and four chromatographic columns, namely "TSKgel G-4000HXL", "TSKgel G-3000HXL", "TSKgel G-2500HXL" and "TSKgel G-2000HXL" (trade names, all manufactured by Tosoh Corporation) are used as the chromatographic columns, the mobile phase is tetrahydrofuran, the measurement temperature is 40°C, the flow rate is 1 mL / min, and the detector is RI.

[0349] (Curing agent)

[0350] The curing agent contained in the anionic electrodeposition coating of the present invention can use a conventionally known compound. For example, it is preferably at least one selected from a blocked polyisocyanate compound and an amino resin (melamine resin, benzoguanamine resin, urea resin, etc.). Among them, from the perspective of impact resistance, adhesion of auxiliary materials and scratch resistance, it is preferably one or more selected from a blocked polyisocyanate compound and a melamine resin.

[0351] As the blocked polyisocyanate compound, for example, the blocked polyisocyanate compounds exemplified as the curing agent for the cationic electrodeposition coating of the present invention can be used.

[0352] Moreover, as the blocked polyisocyanate compound, a commercially available product can also be used. As such commercially available products, for example, one or more selected from the following can be used: Bannock D-750, Bannock D-800, Bannock DN-950, Bannock DN-970 or Bannock DN-15-455 (the above are made by DIC Corporation, trade names), Death module L, Death module N, Death module HL, Death module IL or Death module N3390 (the above are made by Bayer Corporation, trade names), Takenate D-102, Takenate D-202, Takenate D-110N or Takenate D-123N (Mitsui Chemicals Corporation, trade names), Coronate L, Coronate HL, Coronate EH or Coronate 203 (Tosoh Corporation, trade names), Duranate 24A-90CX (Asahi Kasei Corporation, trade names), etc.

[0353] As the melamine resin, for example, one or more selected from the following can be used: a partially etherified or fully etherified melamine resin obtained by partially or completely etherifying some or all of the methylol groups of methylolated melamine with a monohydric alcohol having 1 to 8 carbon atoms (for example, methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, 2-ethylbutanol, 2-ethylhexanol, etc.); and the like.

[0354] Furthermore, a commercially available product may be used as the melamine resin. As such commercial products, for example, one or more selected from the following: butylated melamine resins such as Uban 20SE-60, Uban 225 (all manufactured by Mitsui Chemicals Corporation, trade names), SUPER BECKAMINE G840, SUPER BECKAMINE G821 (all manufactured by DIC Corporation, trade names); Sumimal M-100, Sumimal M-40s, Sumimal M-55 (all manufactured by Sumitomo Chemical Co., Ltd., trade names); Cymel 202, Cymel 232, Cymel 235, Cymel 254, Cymel 266, Cymel 272, Cymel 303, Cymel 325, Cymel 327, Cymel 350, Cymel 370 (all manufactured by Allnex Ltd., trade names); Nikalac MS17, Nikalac MS20, MX15, Nikalac MX430, Nikalac MX600 (all of the above are manufactured by Sanwa Chemical Co., Ltd., trade names), Resimene 741 (manufactured by Monsanto Company, trade name) and other methylated melamine resins; Cymel 232S, Cymel 238, Cymel 1130 (all of the above are manufactured by Allnex Ltd., trade names), Sumimal M66B (manufactured by Sumitomo Chemical Co., Ltd., trade name) and other methylated and isobutylated mixed etherified melamine resins; Cymel XV805 (manufactured by Mitsui High-tec Corporation, trade name), Nikalac Ms95 (manufactured by Sanwa Chemical Co., Ltd., trade name) and other methylated and n-butylated mixed etherified melamine resins, etc.

[0355] Regarding the ratio of the carboxyl-containing resin and the curing agent in the anionic electrodeposition coating, based on 100 parts by mass of the total solid content of the carboxyl-containing resin and the curing agent, it includes 50 to 90 parts by mass (preferably 60 to 75 parts by mass) of the carboxyl-containing resin and 10 to 50 parts by mass (preferably 25 to 40 parts by mass) of the curing agent. Such a ratio is preferred from the perspective of impact resistance and scratch resistance.

[0356] (Epoxy phosphate compound)

[0357] The anionic electrodeposition coating material of the present invention may contain an epoxy phosphate compound obtained by adding a phosphoric acid compound to an epoxy resin as required. By adding the epoxy phosphate compound, impact resistance can be improved.

[0358] As the epoxy resin, the epoxy resin of the first embodiment of the present invention can be used. In addition, for example, bisphenol epoxy resin, novolac epoxy resin, modified epoxy resin obtained by reacting epoxy groups or hydroxyl groups in these epoxy resins with a modifier, etc. can be used.

[0359] Examples of the phosphoric acid compound include orthophosphoric acid and pyrophosphoric acid.

[0360] The reaction of the epoxy resin and the phosphoric acid compound can be carried out at 50 to 180° C., preferably 80 to 120° C., in the presence or absence of a catalyst.

[0361] As the epoxy phosphate compound, a commercial product can be used. As such commercial products, for example, one or more selected from the following: XU-8096.07, XU-71899.00, XQ-82908.00, XQ-82919.00, DER620-PP50, DER621-EB50, DER621-PP50 (these are manufactured by Dow Chemical Japan Limited, trade names), Epototo ZX1300, ZX1300-1 (these are manufactured by Nittetsu Chemical & Materials Co., Ltd., trade names), etc. can be used.

[0362] When the anionic electrodeposition coating contains an epoxy phosphate compound, the ratio is in the range of 0.05 to 10.0 parts by mass, preferably in the range of 0.1 to 5.0 parts by mass, and more preferably in the range of 0.5 to 3.0 parts by mass, based on 100 parts by mass of the solid content of the resin containing hydroxyl groups and carboxyl groups and the crosslinking agent. Such a ratio is preferred from the perspectives of coating stability, weather resistance and impact resistance.

[0363] (Curing Catalyst)

[0364] As the curing catalyst contained in the anionic electrodeposition paint of the present invention, any conventionally known curing catalyst can be used without limitation. For example, the curing catalysts listed in the cationic electrodeposition paint of the present invention are suitable.

[0365] Moreover, in the anionic electrodeposition coating of the present invention, as a curing catalyst, for example, one or more selected from the following can be used: n-butylbenzenesulfonic acid, n-pentylbenzenesulfonic acid, n-octylbenzenesulfonic acid, n-dodecylbenzenesulfonic acid, n-octadecylbenzenesulfonic acid, n-dibutylbenzenesulfonic acid, isopropylnaphthalenesulfonic acid, dodecylnaphthalenesulfonic acid, dinonylnaphthalenesulfonic acid, dinonylnaphthalene disulfonic acid, amine neutralizations of these sulfonic acids, etc.

[0366] The proportion of the curing catalyst in the anionic electrodeposition coating of the present invention is 0.1 to 10 parts by mass, preferably 0.5 to 6 parts by mass, based on 100 parts by mass of the resin solid content.

[0367] (pigment)

[0368] In the anionic electrodeposition paint of the present invention, one or more pigments selected from the conventionally known coloring pigments, rust-proof pigments, extender pigments, etc. can be used without limitation. For example, the pigments that can be included in the cationic electrodeposition paint of the present invention are preferred. Similar to the cationic electrodeposition paint of the present invention, these pigments are preferably mixed into the paint after being made into a pigment dispersion paste.

[0369] (Neutralizer)

[0370] In the anionic electrodeposition coating of the present invention, in order to neutralize the carboxyl resin and / or adjust the pH of the anionic electrodeposition coating bath, an alkaline compound may also be contained. Specifically, one or more selected from the following can be used: primary monoamines, such as ethylamine, propylamine, butylamine, benzylamine, monoethanolamine, neopentanolamine, 2-aminopropanol, 3-aminopropanol, etc.; secondary monoamines, such as diethylamine, diethanolamine, di-n-propanolamine or diisopropanolamine, N-methylethanolamine, N-ethylethanolamine, etc.; tertiary monoamines, such as dimethylethanolamine, trimethylamine, triethylamine, triisopropylamine, methyldiethanolamine, dimethylaminoethanol, etc.; and polyamines, such as diethylenetriamine, hydroxyethylaminoethylamine, ethylaminoethylamine, methylaminopropylamine, etc.; etc. Preferably, the ratio of the above alkaline compounds is in the range of 0.1 to 1.2 equivalents, preferably in the range of 0.2 to 0.8 equivalents, based on the neutralization equivalent.

[0371] (Surfactant)

[0372] The anionic electrodeposition coating of the present invention may use a surfactant to improve the water dispersibility and / or coating stability of the carboxyl-containing resin. Specifically, any one of a nonionic surfactant, anionic surfactant, cationic surfactant, and zwitterionic surfactant may be used.

[0373] As the nonionic surfactant, for example, one or more selected from the following can be used: polyoxyethylene alkyl ether, polyoxyethylene alkyl allyl ether, polyoxyethylene derivatives (for example, polyoxyethylene distyrenated phenyl ether, polyoxyethylene tribenzyl phenyl ether, etc.), sorbitan fatty acid ester, polyoxyethylene dehydrated sorbitan fatty acid ester, glycerol fatty acid ester, polyoxyethylene fatty acid ester, polyoxyethylene alkylamine, alkyl alkanolamide, etc.

[0374] As the anionic surfactant, for example, one or more selected from the group consisting of fatty acid salts, alkyl sulfate ester salts, alkylbenzene sulfonates, and alkyl phosphates can be used.

[0375] Examples of the cationic surfactant include alkylamine salts and quaternary ammonium salts. Examples of the zwitterionic surfactant include at least one selected from alkyl betaines and the like.

[0376] The solid content concentration of the anionic electrodeposition coating of the present invention can be set to about 5 to 40% by mass, preferably 10 to 25% by mass, and the pH is adjusted to be in the range of 7.0 to 10.0, preferably 7.5 to 9.5.

[0377] (Cationic electrodeposition coating method)

[0378] The anionic electrodeposition coating method using the anionic electrodeposition paint of the present invention comprises the steps of: immersing a coating object in an electrodeposition bath composed of the anionic electrodeposition paint; and conducting electricity with the coating object as an anode.

[0379] The objects to be coated with the anionic electrodeposition coating include, for example, building materials, household appliances, other appliances, etc., and are not particularly limited as long as they contain metal. For example, building materials, aluminum window frames, doors and windows, balcony substrates, roofing materials, blinds, doors, sliding windows, gaps (door pockets) for retracting and opening panels, sun rooms, etc., and their components can be cited.

[0380] As an anion electrodeposition coating method, for example, the following method is used: that is, a bath of anion electrodeposition paint is prepared, and usually, the bath temperature is adjusted to 15 to 35° C. and the load voltage is 100 to 400 V. The coated object such as aluminum or aluminum alloy is energized in the bath as an anode. After the anion electrodeposition coating, as described above, in order to remove the excess anion electrodeposition paint attached to the aluminum or aluminum alloy, sufficient water washing may be performed or no water washing may be performed.

[0381] The film thickness of the anionic electrodeposition coating is not particularly limited. Generally speaking, based on the dried coating, it can be in the range of 1 to 40 μm, preferably in the range of 5 to 30 μm. Moreover, regarding the drying of the coating, the electrodeposition coating can be dried by using a drying device such as an electric hot air dryer or a gas hot air dryer. Regarding the above-mentioned drying conditions, generally speaking, the drying temperature is usually 140 to 220°C, preferably 170 to 200°C, but in the present invention, from the viewpoint of saving energy costs, it is preferably less than 160°C, more preferably 80 to 130°C, and particularly preferably a temperature of 100 to 130°C. The baking time is 10 to 180 minutes, preferably 20 to 50 minutes. The cured coating can be obtained by the above-mentioned drying.

[0382] Example

[0383] The present invention will be described in more detail below with reference to Examples, but the present invention is not limited to these Examples. In addition, unless otherwise specified, "%" means "mass %" and "part" means "mass part".

[0384] [Amino-containing epoxy resin]

[0385] <Comparative Example 1-1>

[0386] In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen introduction tube and a reflux cooler, 1893.8 parts of bisphenol A type epoxy resin (epoxy compound), 41.6 parts of multifunctionalizing agent α (multifunctionalizing agent), 10.5 parts of compound γ, 603.5 parts of bisphenol A, 1.0 parts of TBAB (tetrabutylammonium bromide; catalyst) and 283.2 parts of methyl isobutyl ketone (solvent) were added, and the materials were reacted at 160°C until the epoxy equivalent reached 592, and the obtained reaction product was diluted with methyl isobutyl ketone until the solid content reached 80%. Next, 386.4 parts of diethanolamine and 185.1 parts of ketimide of diethylenetriamine (containing 10% solvent, hereinafter referred to as "90% product") were added, and the reaction was carried out at 120°C for three hours. Furthermore, methyl isobutyl ketone was added to obtain a multifunctional epoxy resin (A-1) solution having an amino group with a solid content of 75%.

[0387] The obtained epoxy resin (A-1) had an amine value of 92 mgKOH / g, an average multifunctionality (X1) of 0.15, an average multifunctional concentration (Y1) of 0.101, and a solubility parameter of 10.7.

[0388] <Example 1-1>

[0389] In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen introduction tube and a reflux cooler, 1898.7 parts of bisphenol A type epoxy resin (epoxy compound), 83.0 parts of multifunctionalizing agent α (multifunctionalizing agent), 21.0 parts of compound γ, 514.8 parts of bisphenol A, 1.0 parts of TBAB (tetrabutylammonium bromide; catalyst) and 279.7 parts of methyl isobutyl ketone (solvent) were added, and the materials were reacted at 160°C until the epoxy equivalent reached 546, and the obtained reaction product was diluted with methyl isobutyl ketone until the solid content reached 80%. Next, 418.5 parts of diethanolamine and 184.5 parts of ketimide of diethylenetriamine (90% product) were added, and the reaction was carried out at 120°C for three hours. Furthermore, methyl isobutyl ketone was added to obtain a multifunctional epoxy resin (A-2) solution having an amino group with a solid content of 75%.

[0390] The obtained epoxy resin (A-2) had an amine value of 98 mgKOH / g, an average multifunctionality (X1) of 0.30, an average multifunctional concentration (Y1) of 0.202, and a solubility parameter of 10.7.

[0391] <Example 1-2>

[0392] In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen introduction tube and a reflux cooler, 1908.8 parts of bisphenol A type epoxy resin (epoxy compound), 167.6 parts of a multifunctionalizing agent α (multifunctionalizing agent), 42.4 parts of a compound γ, 333.7 parts of bisphenol A, 1.0 parts of TBAB (tetrabutylammonium bromide; catalyst) and 272.5 parts of methyl isobutyl ketone (solvent) were added, and the materials were reacted at 160°C until the epoxy equivalent reached 468, and the obtained reaction product was diluted with methyl isobutyl ketone until the solid content reached 80%. Next, 482.9 parts of diethanolamine and 186.1 parts of a ketimide of diethylenetriamine (90% product) were added, and the reaction was carried out at 120°C for three hours. Furthermore, methyl isobutyl ketone was added to obtain a multifunctional epoxy resin (A-3) solution having an amino group with a solid content of 75%.

[0393] The obtained epoxy resin (A-3) had an amine value of 109 mgKOH / g, an average multifunctionality (X1) of 0.61, an average multifunctional concentration (Y1) of 0.407, and a solubility parameter of 10.7.

[0394] <Examples 1-3>

[0395] In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen introduction tube and a reflux cooler, 1914.7 parts of bisphenol A type epoxy resin (epoxy compound), 219.6 parts of multifunctionalizing agent α (multifunctionalizing agent), 55.6 parts of compound γ, 228 parts of bisphenol A, 1.0 parts of TBAB (tetrabutylammonium bromide; catalyst) and 268.6 parts of methyl isobutyl ketone (solvent) were added, and the materials were reacted at 160°C until the epoxy equivalent reached 434, and the obtained reaction product was diluted with methyl isobutyl ketone until the solid content reached 80%. Next, 519.2 parts of diethanolamine and 181.3 parts of ketimide of diethylenetriamine (90% product) were added, and the reaction was carried out at 120°C for three hours. Furthermore, methyl isobutyl ketone was added to obtain a multifunctional epoxy resin (A-4) solution having an amino group with a solid content of 75%.

[0396] The obtained epoxy resin (A-4) had an amine value of 115 mgKOH / g, an average multifunctionality (X1) of 0.81, an average multifunctional concentration (Y1) of 0.533, and a solubility parameter of 10.8.

[0397] <Examples 1-4>

[0398] In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen introduction tube and a reflux cooler, 1927.7 parts of bisphenol A type epoxy resin (epoxy compound), 353.5 parts of multifunctionalizing agent α (multifunctionalizing agent), 89.5 parts of compound γ, 0.9 parts of TBAB (tetrabutylammonium bromide; catalyst) and 263.4 parts of methyl isobutyl ketone (solvent) were added, and the materials were reacted at 160°C until the epoxy equivalent reached 393, and the obtained reaction product was diluted with methyl isobutyl ketone until the solid content reached 80%. Next, 564.4 parts of diethanolamine and 187.1 parts of ketimide of diethylenetriamine (90% product) were added, and the reaction was carried out at 120°C for three hours. Furthermore, methyl isobutyl ketone was added to obtain a multifunctional epoxy resin (A-5) solution having an amino group with a solid content of 75%.

[0399] The obtained epoxy resin (A-5) had an amine value of 124 mgKOH / g, an average multifunctionality (X1) of 1.50, an average multifunctional concentration (Y1) of 0.858, and a solubility parameter of 10.8.

[0400] <Examples 1-5>

[0401] In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen introduction tube and a reflux cooler, 1928.0 parts of bisphenol A type epoxy resin (epoxy compound), 386.6 parts of multifunctionalizing agent α (multifunctionalizing agent), 97.9 parts of compound γ, 1.0 parts of TBAB (tetrabutylammonium bromide; catalyst) and 268.0 parts of methyl isobutyl ketone (solvent) were added, and the materials were reacted at 160°C until the epoxy equivalent reached 428, and the obtained reaction product was diluted with methyl isobutyl ketone until the solid content reached 80%. Next, 524 parts of diethanolamine and 183.0 parts of ketimide of diethylenetriamine (90% product) were added, and the reaction was carried out at 120°C for three hours. Further, methyl isobutyl ketone was added to obtain a multifunctional epoxy resin (A-6) solution having an amino group and a solid content of 75%.

[0402] The obtained epoxy resin (A-6) had an amine value of 116 mgKOH / g, an average multifunctionality (X1) of 2.02, an average multifunctional concentration (Y1) of 0.939, and a solubility parameter of 10.8.

[0403] <Examples 1-6>

[0404] In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen introduction tube and a reflux cooler, 1928.4 parts of bisphenol A type epoxy resin (epoxy compound), 424.9 parts of multifunctionalizing agent α (multifunctionalizing agent), 107.6 parts of compound γ, 1.0 parts of TBAB (tetrabutylammonium bromide; catalyst) and 273.4 parts of methyl isobutyl ketone (solvent) were added, and the materials were reacted at 160°C until the epoxy equivalent reached 475, and the obtained reaction product was diluted with methyl isobutyl ketone until the solid content reached 80%. Next, 475.5 parts of diethanolamine and 183.2 parts of ketimide of diethylenetriamine (90% product) were added, and the reaction was carried out at 120°C for three hours. Furthermore, methyl isobutyl ketone was added to obtain a multifunctional epoxy resin (A-7) solution having an amino group with a solid content of 75%.

[0405] The obtained epoxy resin (A-7) had an amine value of 108 mgKOH / g, an average multifunctionality (X1) of 3.02, an average multifunctional concentration (Y1) of 1.032, and a solubility parameter of 10.7.

[0406] <Examples 1-7>

[0407] In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen introduction tube and a reflux cooler, 1925.8 parts of bisphenol A type epoxy resin (epoxy compound), 431.2 parts of multifunctionalizing agent β (multifunctionalizing agent), 56.0 parts of compound γ, 1.0 parts of TBAB (tetrabutylammonium bromide; catalyst) and 268.1 parts of methyl isobutyl ketone (solvent) were added, and the materials were reacted at 160°C until the epoxy equivalent reached 429, and the obtained reaction product was diluted with methyl isobutyl ketone until the solid content reached 80%. Next, 523.5 parts of diethanolamine and 182.8 parts of ketimide of diethylenetriamine (90% product) were added, and the reaction was carried out at 120°C for three hours. Furthermore, methyl isobutyl ketone was added to obtain a multifunctional epoxy resin (A-8) solution having an amino group with a solid content of 75%.

[0408] The obtained epoxy resin (A-8) had an amine value of 116 mgKOH / g, an average multifunctionality (X1) of 3.06, an average multifunctional concentration (Y1) of 1.129, and a solubility parameter of 10.7.

[0409] <Example 1-8>

[0410] In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen introduction tube and a reflux cooler, 1928.7 parts of bisphenol A type epoxy resin (epoxy compound), 447.5 parts of multifunctionalizing agent α (multifunctionalizing agent), 113.3 parts of compound γ, 1.0 parts of TBAB (tetrabutylammonium bromide; catalyst) and 276.6 parts of methyl isobutyl ketone (solvent) were added, and the materials were reacted at 160°C until the epoxy equivalent reached 507, and the obtained reaction product was diluted with methyl isobutyl ketone until the solid content reached 80%. Next, 445.3 parts of diethanolamine and 188.0 parts of ketimide of diethylenetriamine (90% product) were added, and the reaction was carried out at 120°C for three hours. Furthermore, methyl isobutyl ketone was added to obtain a multifunctional epoxy resin (A-9) solution having an amino group with a solid content of 75%.

[0411] The obtained epoxy resin (A-9) had an amine value of 103 mgKOH / g, an average multifunctionality (X1) of 4.04, an average multifunctional concentration (Y1) of 1.087, and a solubility parameter of 10.7.

[0412] <Example 1-9>

[0413] In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen introduction tube and a reflux cooler, 1929.1 parts of bisphenol A type epoxy resin (epoxy compound), 485.3 parts of multifunctionalizing agent α (multifunctionalizing agent), 122.8 parts of compound γ, 1.0 parts of TBAB (tetrabutylammonium bromide; catalyst) and 281.9 parts of methyl isobutyl ketone (solvent) were added, and the materials were reacted at 160°C until the epoxy equivalent reached 569, and the obtained reaction product was diluted with methyl isobutyl ketone until the solid content reached 80%. Next, 399.1 parts of diethanolamine and 183.6 parts of ketimide of diethylenetriamine (90% product) were added, and the reaction was carried out at 120°C for three hours. Furthermore, methyl isobutyl ketone was added to obtain a multifunctional epoxy resin (A-10) solution having an amino group with a solid content of 75%.

[0414] The obtained epoxy resin (A-10) had an amine value of 94 mgKOH / g, an average multifunctionality (X1) of 8.00, an average multifunctional concentration (Y1) of 1.179, and a solubility parameter of 10.6.

[0415] <Example 1-10>

[0416] In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen introduction tube and a reflux cooler, 1929.2 parts of bisphenol A type epoxy resin (epoxy compound), 499.7 parts of multifunctionalizing agent α (multifunctionalizing agent), 126.5 parts of compound γ, 1.0 parts of TBAB (tetrabutylammonium bromide; catalyst) and 283.9 parts of methyl isobutyl ketone (solvent) were added, and the materials were reacted at 160°C until the epoxy equivalent reached 597, and the obtained reaction product was diluted with methyl isobutyl ketone until the solid content reached 80%. Next, 381.1 parts of diethanolamine and 182.6 parts of ketimide of diethylenetriamine (90% product) were added, and the reaction was carried out at 120°C for three hours. Furthermore, methyl isobutyl ketone was added to obtain a multifunctional epoxy resin (A-11) solution having an amino group with a solid content of 75%.

[0417] The obtained epoxy resin (A-11) had an amine value of 91 mgKOH / g, an average multifunctionality (X1) of 12.04, an average multifunctional concentration (Y1) of 1.214, and a solubility parameter of 10.5.

[0418] <Example 1-11>

[0419] In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen introduction tube and a reflux cooler, 1651.5 parts of bisphenol A epoxy resin (epoxy compound), 859.1 parts of hexamethylene diisocyanurate (HMDI ヌレート), 5.0 parts of DMBnAm (N,N-dimethylbenzylamine; catalyst) and 273.9 parts of methyl isobutyl ketone (solvent) were added, and the materials were reacted at 160°C until the epoxy equivalent reached 537, and the obtained reaction product was diluted with methyl isobutyl ketone until the solid content reached 80%. Next, 424.5 parts of diethanolamine and 187.2 parts of ketimide of diethylenetriamine (90% product) were added, and the reaction was carried out at 120°C for three hours. Further, methyl isobutyl ketone was added to obtain a multifunctional epoxy resin (A-12) solution having an amino group with a solid content of 75%.

[0420] The obtained epoxy resin (A-12) had an amine value of 99 mgKOH / g, an average multifunctionality (X1) of 1.54, an average multifunctional concentration (Y1) of 0.677, and a solubility parameter of 10.8.

[0421] <Example 1-12>

[0422] In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen introduction tube and a reflux cooler, 1846.4 parts of bisphenol A type epoxy resin (epoxy compound), 413.2 parts of crude MDI, 262.0 parts of monomeric MDI, 5.1 parts of DMBnAm (N,N-dimethylbenzylamine; catalyst) and 280.3 parts of methyl isobutyl ketone (solvent) were added, and the materials were reacted at 160°C until the epoxy equivalent reached 556, and then 47.0 parts of bisphenol A were further added, and the materials were reacted at 160°C until the epoxy equivalent reached 623. The obtained reaction product was diluted with methyl isobutyl ketone until the solid content reached 80%. Next, 367.8 parts of diethanolamine and 183.4 parts of ketimide of diethylenetriamine (90% product) were added, and the reaction was carried out at 120°C for three hours. Furthermore, methyl isobutyl ketone was added to obtain a polyfunctional epoxy resin (A-13) solution having an amino group and having a solid content of 75%.

[0423] The obtained epoxy resin (A-13) had an amine value of 89 mgKOH / g, an average multifunctionality (X1) of 1.52, an average multifunctional concentration (Y1) of 0.592, and a solubility parameter of 10.7.

[0424] <Comparative Example 1-2>

[0425] In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen introduction tube and a reflux cooler, 1914.3 parts of bisphenol A type epoxy resin (epoxy compound), 609.7 parts of bisphenol A, 3.8 parts of dimethylbenzylamine (catalyst) and 280.4 parts of methyl isobutyl ketone (solvent) were added, and the materials were reacted at 160°C until the epoxy equivalent reached 555, and the obtained reaction product was diluted with methyl isobutyl ketone until the solid content reached 80%. Next, 410.9 parts of diethanolamine and 187.5 parts of ketimide of diethylenetriamine (90% product) were added, and the reaction was carried out at 120°C for three hours. Furthermore, methyl isobutyl ketone was added to obtain a multifunctional epoxy resin (A-14) solution having an amino group with a solid content of 75%.

[0426] The obtained epoxy resin (A-14) had an amine value of 97 mgKOH / g, an average multifunctionality (X1) of 0.15, an average multifunctional concentration (Y1) of 0.121, and a solubility parameter of 10.7.

[0427] <Example 1-13>

[0428] In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen introduction tube and a reflux cooler, 2081.6 parts of bisphenol A type epoxy resin (epoxy compound), 292.1 parts of bisphenol A, 3.6 parts of dimethylbenzylamine (catalyst) and 263.7 parts of methyl isobutyl ketone (solvent) were added, and the materials were reacted at 160°C until the epoxy equivalent reached 397, and the obtained reaction product was diluted with methyl isobutyl ketone until the solid content reached 80%. Next, 560.4 parts of diethanolamine and 190.0 parts of ketimide of diethylenetriamine (90% product) were added, and the reaction was carried out at 120°C for three hours. Furthermore, methyl isobutyl ketone was added to obtain a multifunctional epoxy resin (A-15) solution having an amino group with a solid content of 75%.

[0429] The obtained epoxy resin (A-15) had an amine value of 124 mgKOH / g, an average multifunctionality (X1) of 1.50, an average multifunctional concentration (Y1) of 2.133, and a solubility parameter of 10.8.

[0430] <Comparative Examples 1-3>

[0431] In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen introduction tube and a reflux cooler, 1902.4 parts of bisphenol A type epoxy resin (epoxy compound), 28.7 parts of multifunctionalizing agent α (multifunctionalizing agent), 7.3 parts of compound γ, 585.2 parts of bisphenol A, 3.8 parts of dimethylbenzylamine (catalyst) and 280.4 parts of methyl isobutyl ketone (solvent) were added, and the materials were reacted at 160°C until the epoxy equivalent reached 554, and the obtained reaction product was diluted with methyl isobutyl ketone until the solid content reached 80%. Next, 411.6 parts of diethanolamine and 186.9 parts of ketimide of diethylenetriamine (90% product) were added, and the reaction was carried out at 120°C for three hours. Furthermore, methyl isobutyl ketone was added to obtain a multifunctional epoxy resin (A-16) solution having an amino group with a solid content of 75%.

[0432] The obtained epoxy resin (A-16) had an amine value of 97 mgKOH / g, an average multifunctionality (X1) of 0.15, an average multifunctional concentration (Y1) of 0.115, and a solubility parameter of 10.7.

[0433] <Example 1-14>

[0434] In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen introduction tube and a reflux cooler, 1944.2 parts of bisphenol A type epoxy resin (epoxy compound), 300.9 parts of multifunctionalizing agent α (multifunctionalizing agent), 76.2 parts of compound γ, 69.7 parts of bisphenol A, 3.6 parts of dimethylbenzylamine (catalyst) and 265.7 parts of methyl isobutyl ketone (solvent) were added, and the materials were reacted at 160°C until the epoxy equivalent reached 410, and the obtained reaction product was diluted with methyl isobutyl ketone until the solid content reached 80%. Next, 544.4 parts of diethanolamine and 186.0 parts of ketimide (90% product) of diethylenetriamine were added, and the reaction was carried out at 120°C for three hours. Furthermore, methyl isobutyl ketone was added to obtain a multifunctional epoxy resin (A-17) solution having an amino group with a solid content of 75%.

[0435] The obtained epoxy resin (A-17) had an amine value of 120 mgKOH / g, an average multifunctionality (X1) of 1.51, an average multifunctional concentration (Y1) of 0.986, and a solubility parameter of 10.8.

[0436] <Comparative Examples 1-4>

[0437] Into a reaction vessel equipped with a stirrer, a thermometer, a nitrogen inlet pipe and a reflux cooler, 1885.5 parts of bisphenol A type epoxy resin (epoxy compound), 757.8 parts of bisphenol A, 1.1 parts of TBAB (tetrabutylammonium bromide; catalyst) and 293.0 parts of methyl isobutyl ketone (solvent) were added, and the materials were reacted at 160° C. until the epoxy equivalent reached 775, and the obtained reaction product was diluted with methyl isobutyl ketone until the solid content reached 80%.

[0438] Next, 291.7 parts of diethanolamine and 187.1 parts of a ketimide (90% product) of diethylenetriamine and methyl isobutyl ketone were added, and the mixture was reacted for four hours at 120° C. Methyl isobutyl ketone was further added to obtain a non-multifunctional linear epoxy resin solution (A-18) having an amino group and a solid content of 75%.

[0439] The obtained epoxy resin (A-18) had an amine value of 76 mgKOH / g, an average multifunctionality (X1) of 0, an average multifunctional concentration (Y1) of 0, and a solubility parameter of 10.8.

[0440] The ingredients used in preparing the epoxy resin are as follows.

[0441] (Epoxides)

[0442] ■Bisphenol A epoxy resin

[0443] Made by Mitsubishi Chemical Corporation, trade name: jER828EL (number of functional groups: 2, epoxy equivalent: 187, weight average molecular weight: 375).

[0444] (Multifunctional Agent)

[0445] ■Multifunctional agent α

[0446] It is a mixture of compounds having the content ratios shown in Table 1 for each n value relative to the total amount of compounds in the following structural formula (A) where p=q=r=0, R1=R2=R3=H and n is 1 or more. The average number of functional groups is 8.4 and the weight average molecular weight is 878.

[0447] ■Multifunctional agent β

[0448] It is a mixture of compounds having the content ratios shown in Table 1 at various n values ​​relative to the total amount of compounds in the following structural formula (A) where p=q=r=0, R1=R2=R3=H and n is 1 or more. The average number of functional groups is 11.37 and the weight average molecular weight is 1193.

[0449]

[0450] [Table 1]

[0451]

[0452] ■ Hexamethylene diisocyanurate: This is an isocyanurate-modified hexamethylene diisocyanate having a functional group number of 3.93 and a weight average molecular weight of 817.

[0453] ■ Crude MDI: This is a compound represented by the following structural formula (C), wherein n is an integer equal to or greater than 1, the number of NCO functional groups is 4.46, and the weight average molecular weight is 573.

[0454]

[0455] (Compounds having one or more active hydrogen atoms in one molecule, except trivalent or higher phenolic compounds)

[0456] ■Compound γ

[0457] This is a compound (molecular weight: 200) represented by the following structural formula (B) where s=t=0 and R4=R5=H.

[0458]

[0459] (In the formula, s=0, t=0, R4=R5=H)

[0460] ■Bisphenol A

[0461]

[0462] (Diisocyanate compound)

[0463] ■Monomer MDI

[0464] It is a compound represented by the following structural formula (C) with n=0, 2 NCO functional groups and a molecular weight of 250.

[0465]

[0466] [Cationic electrodeposition coating]

[0467] <Preparation of Pigment Dispersing Resin>

[0468] In a beaker equipped with a stirrer, a thermometer, a dropping funnel and a reflux cooler, 390 parts of bisphenol A, 240 parts of PLACCEL 212 (a trade name manufactured by Daicel Chemical Industry, Ltd., polycaprolactone diol, weight average molecular weight of about 1,250) and 0.2 parts of dimethylbenzylamine were added to 1010 parts of bisphenol A type epoxy resin (epoxy equivalent of 190, weight average molecular weight of 350), and the materials were reacted at 130° C. until the epoxy equivalent reached about 1090. Next, 134 parts of dimethylethanolamine and 150 parts of a 90% aqueous lactic acid solution were added, and the materials were reacted at 90° C. until the epoxy group disappeared. Next, propylene glycol monomethyl ether was added to adjust the solid content, and a quaternary ammonium base-containing pigment dispersion resin (R) having a solid content of 60% was obtained.

[0469] <Preparation of Pigment Dispersion Paste>

[0470] (Pigment dispersion paste (P1))

[0471] Add 8.3 parts (solid content is 5 parts) of a pigment dispersing resin (R) containing a quaternary ammonium base with a solid content of 60%, 14.5 parts of titanium oxide, 6.0 parts of refined clay, 0.3 parts of carbon black, 3 parts of bismuth hydroxide and 20.3 parts of deionized water, and disperse in a ball mill for 20 hours to obtain a pigment dispersion paste (P1) with a solid content of 55%.

[0472] (Pigment dispersion paste (P2))

[0473] Add 8.3 parts (solid content is 5 parts) of a pigment dispersing resin (R) containing a quaternary ammonium base with a solid content of 60%, 14.5 parts of titanium oxide, 7.0 parts of refined clay, 0.3 parts of carbon black, 2 parts of dioctyltin oxide and 20.3 parts of deionized water, and disperse in a ball mill for 20 hours to obtain a pigment dispersion paste (P2) with a solid content of 55%.

[0474] <Preparation of Blocked Polyisocyanate Compound (BNCO (B1))>

[0475] 270 parts of Cosmonate M-200 (trade name, manufactured by Mitsui Chemicals Corporation, crude MDI, NCO group content of 31.3%) and 127 parts of methyl isobutyl ketone were added to a reaction container, and the material was heated to 70° C. 236 parts of ethylene glycol monobutyl ether was added dropwise thereto over one hour, and then the material was heated to 100° C., and sampling was performed over time while maintaining the temperature, and infrared absorption spectrum measurement was performed to confirm that the absorption of unreacted isocyanate groups had disappeared, thereby obtaining a blocked polyisocyanate compound (BNCO (B1)) having a resin solid content of 80%.

[0476] <Preparation of acrylic resin>

[0477] (Acrylic resin No.1)

[0478] In a reaction vessel equipped with a stirrer, a cooler, a nitrogen inlet tube, a thermometer, and a dropping funnel, 50 parts of methyl isobutyl ketone were prepared and heated and maintained at 110° C. in a nitrogen atmosphere.

[0479] The following monomer mixture was then added dropwise from the dropping funnel over three hours, and then 0.5 parts of tert-butyl peroctanoate was further added dropwise, and the mixture was kept at 110°C for 1.5 hours. Methyl isobutyl ketone was then added to adjust the solid content to 50%, thereby obtaining an acrylic resin No. 1 solution. The obtained acrylic resin No. 1 had a weight average molecular weight of 12,000, an amine value of 71 mgKOH / g, a hydroxyl value of 43 mgKOH / g, and a solubility parameter of 10.5.

[0480] (Monomer mixture)

[0481] 65 parts of methyl methacrylate

[0482] 5 parts of 2-ethylhexyl methacrylate

[0483] 10 parts of 2-hydroxyethyl methacrylate

[0484] 20 parts of N,N-dimethylaminoethyl methacrylate

[0485] 4 parts of tert-butyl peroctanoate

[0486] (Acrylic resin No.2)

[0487] In a reaction vessel equipped with a stirrer, a cooler, a nitrogen inlet tube, a thermometer, and a dropping funnel, 50 parts of methyl isobutyl ketone were prepared and heated and maintained at 110° C. in a nitrogen atmosphere.

[0488] The following monomer mixture was then added dropwise from the dropping funnel over three hours, and then 0.5 parts of tert-butyl peroctanoate was further added dropwise, and the mixture was kept at 110°C for 1.5 hours. Methyl isobutyl ketone was then added, and the solid content was adjusted to 50% to obtain an acrylic resin No. 2 solution. The obtained acrylic resin No. 2 had a weight average molecular weight of 12,000, an amine value of 71 mgKOH / g, a hydroxyl value of 43 mgKOH / g, and a solubility parameter of 10.1.

[0489] (Monomer mixture)

[0490] 30 parts of methyl methacrylate

[0491] 2-Ethylhexyl Methacrylate 35 parts

[0492] 10 parts of 2-hydroxyethyl methacrylate

[0493] 20 parts of N,N-dimethylaminoethyl methacrylate

[0494] 4 parts of tert-butyl peroctanoate

[0495] (Acrylic resin No.3)

[0496] In a reaction vessel equipped with a stirrer, a cooler, a nitrogen inlet tube, a thermometer, and a dropping funnel, 50 parts of methyl isobutyl ketone were prepared and heated and maintained at 110° C. in a nitrogen atmosphere.

[0497] The following monomer mixture was then added dropwise from the dropping funnel over three hours, and then 0.5 parts of tert-butyl peroctanoate was further added dropwise, and the mixture was kept at 110°C for 1.5 hours. Methyl isobutyl ketone was then added, and the solid content was adjusted to 50% to obtain an acrylic resin No. 3 solution. The obtained acrylic resin No. 3 had a weight average molecular weight of 12,000, an amine value of 71 mgKOH / g, a hydroxyl value of 43 mgKOH / g, and a solubility parameter of 9.7.

[0498] (Monomer mixture)

[0499] 5 parts of methyl methacrylate

[0500] 65 parts of 2-ethylhexyl methacrylate

[0501] 10 parts of 2-hydroxyethyl methacrylate

[0502] 20 parts of N,N-dimethylaminoethyl methacrylate

[0503] 4 parts of tert-butyl peroctanoate

[0504] <Example 2-1>

[0505] 100 parts (solid content) of the amino-containing epoxy resin (A-2) obtained in Example 1-1 and 30 parts (solid content) of the blocked polyisocyanate compound (BNCO) (B1) were mixed, and then 13 parts of 10% acetic acid were added and stirred evenly. Thereafter, deionized water was added dropwise over about 15 minutes while stirring vigorously to obtain an emulsion with a solid content of 34%.

[0506] Next, 294 parts of the above-mentioned emulsion (100 parts solid content), 52.4 parts of the pigment dispersion paste (P1) and deionized water were added to prepare a cationic electrodeposition coating (X-2) having a solid content of 20%. The average multifunctional concentration (Y2) of the cationic electrodeposition coating (X-2) is recorded in Table 2.

[0507] The obtained cationic electrodeposition paint was used for electrodeposition coating, and then heated and cured to obtain an electrodeposition coating film. The surface finish, corrosion resistance (salt water spray), corrosion resistance (salt water immersion), and oil shrinkage resistance of the obtained electrodeposition coating film were evaluated. The results are recorded in Table 2.

[0508] <Example 2-2 to Example 2-21, Comparative Example 2-1 to Comparative Example 2-5>

[0509] In addition to the amino-containing epoxy resin and pigment dispersion paste as shown in Tables 2 to 4, cationic electrodeposition coatings (X-2) to (X-26) having an average multifunctional concentration (Y2) as shown in Tables 2 to 4 and a solid content of 20% were prepared in the same manner as in Example 2-1. In addition, Example 2-12 is an example in which 15 parts of A-5 and 85 parts of A-18 are used as amino-containing epoxy resins, and Example 2-13 is an example in which 40 parts of A-5 and 60 parts of A-18 are used as amino-containing epoxy resins. The average multifunctional concentration (Y2) of Examples 2-12 and 2-13 was calculated by mixing the two epoxy resins and the unit is mmol / g.

[0510] Furthermore, the cationic electrodeposition coating materials of Examples 2-18 to 2-21 and Comparative Example 2-5 also contain an amino group-containing epoxy resin (A-5) and acrylic resins No. 1 to 3.

[0511] The obtained cationic electrodeposition paint is used for electrodeposition coating, and then heat-cured to obtain an electrodeposition coating film.

[0512] The results of observing the cross sections of the electrodeposition coating films showed that all of them were single-layer coating films (without an interface).

[0513] The obtained electrodeposition coating films were evaluated for surface smoothness, corrosion resistance (salt water spray), corrosion resistance (salt water immersion), and oil-induced cratering resistance. The results are collectively recorded in Tables 2 to 4.

[0514] In the present invention, if any one of the four evaluation items is "C", the test result is considered as unqualified.

[0515] In addition, all the resin contents in the table are values ​​of solid content.

[0516] [Table 2]

[0517]

[0518] [Table 3]

[0519]

[0520] [Table 4]

[0521]

[0522] (Note) "Acrylic 1", "Acrylic 2" and "Acrylic 3" in the table represent acrylic resins No. 1 to No. 3, respectively.

[0523] The surface finish, corrosion resistance (salt water spray), corrosion resistance (salt water immersion) and oil shrinkage resistance were evaluated as follows. If any one of the evaluations was "C", the coating (paint) was considered unacceptable.

[0524] (Surface finish)

[0525] A cold rolled steel sheet (0.8 mm × 150 mm × 70 mm) treated with zinc phosphate was electro-deposited at a bath temperature of 28°C and a load voltage such that the cured coating film thickness was 20 μm, and then heat cured at 170°C for 20 minutes to obtain a test plate. Next, the surface roughness value (Ra) defined in JIS B 601 was measured for the coated surface of the test plate using Surftest 301 (manufactured by Mitutoyo Corporation, trade name, surface roughness tester) with a cutoff value of 0.8 mm, and evaluated according to the following criteria. S is the best evaluation, and C is unqualified.

[0526] S: Surface roughness value (Ra) is less than 0.15.

[0527] A: The surface roughness value (Ra) is 0.15 or more and less than 0.25.

[0528] B1: The surface roughness value (Ra) is 0.25 or more and less than 0.35.

[0529] B2: The surface roughness value (Ra) is 0.35 or more and less than 0.45.

[0530] C: The surface roughness value (Ra) is 0.45 or more.

[0531] (Corrosion resistance (salt spray))

[0532] Electrodeposition coating was applied to a cold-rolled steel sheet (0.8 mm × 150 mm × 70 mm) treated with zinc phosphate at a bath temperature of 28°C and a load voltage such that the cured coating film thickness was 20 μm, and the test plate was obtained by heat curing at 170°C for 20 minutes. Next, a cross-cut scratch was made on the coating using a cutter to reach the substrate of the test plate, and a 35°C salt spray test was performed for 840 hours in accordance with JIS Z-2371. Evaluation was performed based on the rust and blister width on one side of the cut portion according to the following evaluation criteria. S is the best evaluation, and C is unqualified.

[0533] S: The maximum width of rust and blister on one side from the cutout portion is 2.0 mm or less, and the corrosion resistance is very excellent.

[0534] A: The maximum width of rust and blister on one side from the cutout portion is more than 2.0 mm and less than 3.0 mm, and the corrosion resistance is good.

[0535] B: The maximum width of rust and blister on one side from the cutout portion is more than 3.0 mm and less than 4.0 mm, and the corrosion resistance is standard.

[0536] C: The maximum width of rust and blistering on one side from the cutout portion is greater than 4.0 mm, indicating poor corrosion resistance.

[0537] (Corrosion resistance (salt water immersion))

[0538] At a bath temperature of 28°C and a load voltage that makes the cured coating film thickness 20μm, a cold-rolled steel sheet (0.8mm×150mm×70mm) treated with zinc phosphate was electroplated and cured at 170°C for 20 minutes to obtain a test plate. Then, after immersing the test plate in a 5% by mass salt solution at 50°C for 600 hours, the test plate was lifted up, the moisture on the coating surface was wiped off, and then a cellophane tape was attached to the coating surface and the tape was instantly peeled off. The peeling rate (%) of the coating was evaluated by this peeling test. S is the best evaluation and C is unqualified.

[0539] S: The peeling rate of the coating film is less than 5% with respect to the test coating film portion.

[0540] A: The peeling rate of the coating film is 5% or more and less than 10% with respect to the test coating film portion.

[0541] B: The peeling rate of the coating film is 10% or more and less than 20% with respect to the test coating film portion.

[0542] C: The peeling rate of the coating film is 20% or more relative to the test coating film portion.

[0543] (Oil shrinkage resistance)

[0544] A cold-rolled steel sheet (0.8 mm×150 mm×70 mm) treated with zinc phosphate was subjected to electrodeposition coating at a bath temperature of 28° C. and a load voltage such that the cured coating film had a thickness of 20 μm, thereby obtaining a wet film.

[0545] The wet film was washed with water and left for 30 minutes. During the baking process, 0.2 ml of rust-proof oil (Nihon Parkerizing Co., Ltd., trade name NOX-RUST320) was evenly scattered and attached. After cooling, the coating surface was observed with the naked eye, the number and size of pits were counted, and the evaluation was performed according to the following evaluation criteria. S is the best evaluation, and C is unqualified.

[0546] S: No pits are generated on the coating film surface.

[0547] A: Less than 10 pits were generated on the coating film surface.

[0548] B: Ten or more pits (all with a diameter of less than 2 mm) are generated on the coating film surface.

[0549] C: Ten or more pits are generated on the coating film surface (the diameter of one or more pits is 2 mm or more).

[0550] As mentioned above, although this invention is demonstrated in detail through embodiment and Example, this invention is not limited to the said embodiment and Example, Various deformation|transformation is possible based on the technical idea of ​​this invention.

[0551] In the present invention, as a polyfunctionalizing agent, compounds (polyfunctionalizing agent α and polyfunctionalizing agent β) in the structural formula (A) where "p=q=r=0, R1=R2=R3=H" are used in the embodiments, but for example, in the case of "p=q=r=1, R1=R2=R3=methyl (-CH3)", it can be confirmed that they have equivalent performance and can be used appropriately.

Claims

1. A cationic electrodeposition coating comprising an amino-containing epoxy resin I and a curing agent, wherein the amino-containing epoxy resin I is obtained by reacting an epoxy resin with an amine compound, wherein: The epoxy resin is an epoxy resin obtained by reacting at least a compound having two or more epoxy groups and a compound having a functional group reactive with the epoxy group, wherein the average multifunctionality X1 per molecule of the epoxy resin represented by the following formula 1 is 0.30 or more and 15.00 or less, Formula 1: Average multifunctionality X1 = number of ends per molecule of epoxy resin - 2, In Formula 1, "the number of terminals per epoxy resin molecule" is the number of terminals having epoxy groups and the number of terminals having functional groups reactive with epoxy groups in one molecule of epoxy resin. The average multifunctionality X2 of the amino-containing epoxy resin I represented by the following formula 3 is 0.30 or more and 15.00 or less, Formula (3): Average multifunctionality X2 = number of terminals of one molecule of amino-containing epoxy resin I - 2 The average multifunctional concentration Y2 represented by the following formula 4 of the amino-containing epoxy resin I contained in the cationic electrodeposition coating is 0.10 mmol / g or more and 5.00 mmol / g or less, Formula (4): Average multifunctional concentration Y2=average multifunctionality X2 of amino-containing epoxy resin I÷weight average molecular weight Mw of amino-containing epoxy resin I×1000×(amount of amino-containing epoxy resin I÷amount of all amino-containing epoxy resins).

2. The cationic electrodeposition paint according to claim 1, wherein: The cationic electrodeposition paint further contains an amino group-containing epoxy resin II obtained by reacting an epoxy resin having a functional group number of 2 or less and an amine compound.

3. The cationic electrodeposition paint according to claim 1, wherein: The average multifunctional concentration Y1 of the epoxy resin represented by the following 2 formula is 0.10 mmol / g or more and 5.00 mmol / g or less, Formula 2: Average multifunctional concentration Y1=average multifunctionality X1 of epoxy resin÷weight average molecular weight Mw of epoxy resin×1000.

4. The cationic electrodeposition paint according to claim 1, wherein: The compound having a functional group reactive with an epoxy group is a trivalent or higher phenolic compound and / or a compound containing a trifunctional or higher polyisocyanate.

5. The cationic electrodeposition paint according to claim 4, wherein: The trivalent or higher phenolic compound comprises a compound represented by the following structural formula (A): In the formula, n represents an integer of 1 to 20, p represents an integer of 0 to 4, q represents an integer of 0 to 3, and r represents an integer of 0 to 4; R1 to R3 are each independently a monovalent group; R2 may be different for each n repeating units; when there are multiple R1, R2 and / or R3 in the aromatic ring, they may be the same as or different from each other; R1 to R3 may be bonded to each other to form a ring.

6. The cationic electrodeposition paint according to claim 4, wherein: The compound having a functional group reactive with an epoxy group further includes a compound having one or more active hydrogen atoms in one molecule other than a trivalent or higher phenol compound.

7. The cationic electrodeposition paint according to claim 4, wherein the compound having a functional group reactive with an epoxy group comprises the trivalent or higher phenol compound and a compound represented by the following structural formula (B), wherein: The content ratio of the trivalent or higher phenolic compound to the compound of the structural formula (B) is in the range of 1 / 99 to 99 / 1, wherein the content ratio is a mass ratio. In the formula, s represents an integer of 0 to 4, t represents an integer of 0 to 4, R4 and R5 are each independently a monovalent group; when there are multiple R4 and / or R5 in the aromatic ring, they may be the same as or different from each other; R4 and / or R5 may be bonded to each other to form a ring.

8. The cationic electrodeposition coating according to claim 4, wherein the trifunctional or higher-functional polyisocyanate is crude MDI.

9. The cationic electrodeposition paint according to claim 1, wherein: The compound having two or more epoxy groups is a compound that is not modified by amine.

10. The cationic electrodeposition paint according to claim 6, wherein: The amino-containing epoxy resin is obtained by reacting at least a compound having two or more epoxy groups, a compound including a trivalent or higher phenol compound, and a compound having one or more active hydrogen atoms in one molecule other than the trivalent or higher phenol compound.

11. The cationic electrodeposition paint according to claim 6, wherein: The compound having one or more active hydrogen atoms in one molecule other than the trivalent or higher phenolic compound is a compound represented by the following structural formula (B): In the formula, s represents an integer of 0 to 4, t represents an integer of 0 to 4; R4 and R5 are each independently a monovalent group; when there are multiple R4 and / or R5 in the aromatic ring, they may be the same or different; R4 and / or R5 may be bonded to each other to form a ring, The content ratio of the trivalent or higher phenol compound to the compound of the structural formula (B) is in the range of 1 / 99 to 99 / 1, wherein the content ratio is a mass ratio.

12. The cationic electrodeposition paint according to claim 1, further comprising an acrylic resin, When the total amount of all epoxy resins and acrylic resins is 100% by mass, the content of the acrylic resin is less than 30% by mass. The absolute value of the difference between the solubility parameter SP values ​​of the acrylic resin and the epoxy resin is less than 1.

0.

13. A coated product obtained by immersing a coating material in an electrodeposition coating bath comprising the cationic electrodeposition coating according to any one of claims 1 to 12 and performing electrodeposition coating.