DP field effect tube preparation method and DP field effect tube
By preparing a P-well layer deeper than the groove gate in the field effect tube and forming a DP structure, the oxide layer breakdown problem caused by a high electric field at the groove gate position is solved, and the short-circuit resistance is significantly improved.
Patent Information
- Application Number
- CN202210932886.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-04
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-08-04
AI Technical Summary
High electric fields are prone to appear at the gate gate position in conventional field effect tubes, resulting in the gate oxide layer being easily broken down and has poor short-circuit resistance.
By preparing a P-well layer deeper than the groove gate, and making the P-well layer cover the corners of the groove gate and the P-well layers on both sides of the groove gate are not connected, a DP structure is formed, which improves the reliability of the gate oxide layer and the field effect tube Short circuit resistance.
It effectively improves the reliability of the gate oxide layer and the short-circuit resistance of the field effect tube, and prevents the corners of the groove gate from being broken down.
Smart Images

Figure CN115376922B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor technology, and in particular to a DP field effect transistor preparation method and a DP field effect transistor. Background Art
[0002] In the related art, a high electric field is easily generated at the trench gate position in a conventional field effect transistor, and the gate oxide layer is easily broken down without effective shielding, resulting in poor short-circuit resistance. Summary of the invention
[0003] The present application aims to solve at least one of the technical problems existing in the prior art. To this end, the present application proposes a method for preparing a DP field effect transistor, by preparing a P well layer deeper than a trench gate, and making the P well layer cover the corner of the trench gate and the P well layers on both sides of the trench gate are not connected, so as to form a DP (Double P-shield) structure, thereby improving the reliability of the gate oxide layer and the short circuit resistance of the field effect transistor.
[0004] The present application also proposes a DP field effect transistor prepared using the above-mentioned DP field effect transistor preparation method.
[0005] According to the first aspect of the present application, the DP field effect transistor preparation method includes: etching an epitaxial wafer to form a groove gate; injecting P-type impurities on both sides of the groove gate to form a P-well layer; pushing the P-well layer through a push-junction process to make the depth of the P-well layer greater than the depth of the groove gate; wherein the P-well layer covers the corners of the groove gate and the P-well layers on both sides of the groove gate are not connected; and injecting N-type impurities on both sides of the groove gate to form an N-type source region.
[0006] The DP field effect transistor preparation method according to the embodiment of the present application has at least the following beneficial effects: by preparing a P-well layer deeper than the groove gate, and at the same time making the P-well layer cover the corners of the groove gate and the P-well layers on both sides of the groove gate are not connected, a DP structure is formed, thereby improving the reliability of the gate oxide layer and the short-circuit resistance of the field effect transistor.
[0007] According to some embodiments of the present application, the step of etching the epitaxial wafer to form a groove gate specifically includes: setting a protective layer on the epitaxial wafer; etching the protective layer to form a groove window; etching the epitaxial wafer at the position of the groove window to form a groove; depositing a gate oxide layer and a filling layer on the epitaxial wafer respectively; etching the gate oxide layer and the filling layer outside the groove to form the groove gate.
[0008] According to some embodiments of the present application, a material of the gate oxide layer includes silicon dioxide or silicon oxynitride.
[0009] According to some embodiments of the present application, the material of the filling layer is polysilicon.
[0010] According to some embodiments of the present application, the step of pushing the P-well layer through a push-junction process so that the depth of the P-well layer is greater than the depth of the trench gate specifically includes: heating the furnace tube to a preset initial temperature; placing the epitaxial wafer in the heated furnace tube; heating the furnace tube to a first temperature at a preset heating rate, and introducing oxygen at a first flow rate; wherein the first temperature is higher than the initial temperature; maintaining the temperature in the furnace tube according to a preset maintenance time, and introducing oxygen at a second flow rate; wherein the second flow rate is less than the first flow rate; cooling the furnace tube at a preset cooling rate, and maintaining the introduction of oxygen at the second flow rate; when the temperature of the furnace tube drops to the initial temperature, stopping the introduction of oxygen and taking out the epitaxial wafer.
[0011] According to some embodiments of the present application, during the process of pushing the knot on the P-well layer through a push-knot process, the method further includes: in the push-knot process, introducing a protective gas into the furnace tube at a third flow rate; wherein the third flow rate is greater than the first flow rate.
[0012] According to some embodiments of the present application, a depth of the N-type source region is less than a depth of the trench gate.
[0013] According to some embodiments of the present application, after the step of injecting N-type impurities on both sides of the groove gate to form an N-type source region, the method further includes: setting an anti-oxidation layer on the groove gate; setting a metal layer on the top and bottom surfaces of the epitaxial wafer; wherein the metal layer on the top surface of the epitaxial wafer covers the anti-oxidation layer.
[0014] According to the DP field effect transistor of the second aspect embodiment of the present application, the DP field effect transistor is prepared by the DP field effect transistor preparation method described in the first aspect embodiment; the DP field effect transistor includes: an epitaxial wafer; a groove gate, the groove gate is etched on the epitaxial wafer; a P-well layer, the P-well layer is arranged on both sides of the groove gate, and the depth of the P-well layer is greater than the depth of the groove gate; an N-type source region, the N-type source region is arranged on both sides of the groove gate, and the depth of the P-well layer is greater than the depth of the groove gate; an anti-oxidation layer, the anti-oxidation layer is arranged on the groove gate; a metal layer, the metal layer is arranged on the top and bottom surfaces of the epitaxial wafer, and the metal layer on the top surface of the epitaxial wafer covers the anti-oxidation layer.
[0015] The DP field effect transistor according to the embodiment of the present application has at least the following beneficial effects: the DP field effect transistor is prepared by the DP field effect transistor preparation method of the first aspect embodiment, the DP field effect transistor is provided with a P-well layer deeper than the groove gate, and at the same time, the P-well layer covers the corners of the groove gate and the P-well layers on both sides of the groove gate are not connected, thereby improving the reliability of the gate oxide layer and the short-circuit resistance of the field effect transistor.
[0016] According to some embodiments of the present application, the trench gate includes a corner surface, and the P-well layer wraps the corner surface.
[0017] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The present application is further described below with reference to the accompanying drawings and embodiments, wherein:
[0019] Figure 1 This is a flow chart of an embodiment of the method for preparing a DP field effect transistor of the present application;
[0020] Figure 2 for Figure 1 The flowchart of step S100 is shown as an embodiment;
[0021] Figure 3 for Figure 1 The flowchart of step S300 is shown as an embodiment;
[0022] Figure 4 for Figure 1 The flowchart of another embodiment of step S300 is shown;
[0023] Figure 5 A flow chart of another embodiment of the method for preparing a DP field effect transistor of the present application;
[0024] Figure 6 This is a schematic structural diagram of an embodiment of a DP field effect transistor of the present application. DETAILED DESCRIPTION
[0025] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.
[0026] In the description of the present application, it should be understood that descriptions involving orientation, such as up, down, front, back, left, right, etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0027] In the description of this application, "several" means more than one, "more" means more than two, "greater than", "less than", "exceed", etc. are understood to exclude the number itself, and "above", "below", "within", etc. are understood to include the number itself. If there is a description of "first" or "second", it is only used for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.
[0028] In the description of this application, unless otherwise clearly defined, terms such as setting, installing, connecting, etc. should be understood in a broad sense, and technicians in the relevant technical field can reasonably determine the specific meanings of the above terms in this application based on the specific content of the technical solution.
[0029] The DP field effect tube preparation method of the embodiment of the present application can be used to prepare a DP field effect tube. In the related art, a high electric field is easily generated at the trench gate position of a conventional field effect tube, and the gate oxide layer is easily broken down without effective shielding, and the short circuit resistance is poor.
[0030] Based on this, the present application proposes a DP field effect transistor preparation method and a DP field effect transistor, by preparing a P-well layer deeper than the groove gate, and at the same time making the P-well layer cover the corners of the groove gate and the P-well layers on both sides of the groove gate are not connected, so as to form a DP structure, thereby improving the reliability of the gate oxide layer and the short-circuit resistance of the field effect transistor.
[0031] Reference Figure 1 The DP field effect transistor preparation method of the embodiment of the present application includes but is not limited to steps S100 to S400:
[0032] S100, etching the epitaxial wafer to form a trench gate;
[0033] S200, implanting P-type impurities on both sides of the trench gate to form a P-well layer;
[0034] S300, pushing the P-well layer through a pushing-junction process, so that the depth of the P-well layer is greater than the depth of the trench gate; wherein the P-well layer covers the corners of the trench gate and the P-well layers on both sides of the trench gate are not connected;
[0035] S400 , N-type impurities are implanted on both sides of the trench gate to form an N-type source region.
[0036] In steps S100 to S400 shown in the embodiment of the present application, a DP structure is formed by preparing a P-well layer deeper than the trench gate, and at the same time making the P-well layer cover the corners of the trench gate and the P-well layers on both sides of the trench gate are not connected, thereby improving the reliability of the gate oxide layer and the short-circuit resistance of the field effect transistor.
[0037] In step S100 of some embodiments, a trench gate is etched on an epitaxial wafer. In this embodiment, the epitaxial wafer is composed of a silicon substrate and a silicon epitaxial layer. In other embodiments, the components of the epitaxial wafer are not specifically limited. Also, there is no specific limitation on the tool or equipment for etching.
[0038] In step S200 of some embodiments, a P-well layer is formed on both sides of the trench gate by injecting P-type impurities. In an exemplary embodiment, the P-type impurities may be boron. There is no specific limitation on the tools or equipment used for injecting P-type impurities.
[0039] In step S300 of some embodiments, the DP structure is formed by making the P-well layer cover the corners of the trench gate and the P-well layers on both sides of the trench gate are disconnected, thereby enhancing the short-circuit resistance of the field effect transistor.
[0040] In step S400 of some embodiments, N-type impurities are implanted on both sides of the trench to form an N-type source region, which is the source region of the field effect transistor. There is no specific limitation on the tools or equipment used to implant the N-type impurities.
[0041] In some embodiments, reference Figure 2 , etching the epitaxial wafer to form a trench gate, specifically including but not limited to steps S110 to S150:
[0042] S110, providing a protective layer on the epitaxial wafer;
[0043] S120, etching the protective layer to form a groove window;
[0044] S130, etching the epitaxial wafer at the position of the groove window to form a groove;
[0045] S140, depositing a gate oxide layer and a filling layer on the epitaxial wafer respectively;
[0046] S150, etching the gate oxide layer and the filling layer outside the trench to form a trench gate.
[0047] In the step S110 to step S150 shown in the embodiment of the present application, a trench window is constructed to form a trench shape of a trench gate, and a gate oxide layer and a filling layer are deposited separately and the redundant gate oxide layer and filling layer outside the trench are etched to ensure that the gate oxide layer thickness of the trench gate is uniform.
[0048] In step S110 of some embodiments, the protective layer is an inorganic thin film material, the main components of which include silicon nitride, silicon dioxide, etc.
[0049] In step S120 of some embodiments, the protective layer is etched using a photolithography process to form a groove window, and there is no specific limitation on the tool or equipment for forming the groove window.
[0050] In step S130 of some embodiments, the epitaxial wafer is etched at the position of the trench window by a silicon etching process to form a trench. There is no specific limitation on the tool or equipment for forming the trench.
[0051] In step S140 of some embodiments, in the field effect transistor, in order to effectively suppress the short channel effect and maintain a good subthreshold slope, the gate oxide layer thickness should decrease in the same proportion as the channel length. The filling layer is used to fill the trench.
[0052] In step S150 of some embodiments, the redundant gate oxide layer and the filling layer outside the trench are removed to form a trench gate structure. There is no specific limitation on the tool or equipment for etching the gate oxide layer and the filling layer.
[0053] It should be noted that the material of the gate oxide layer includes silicon dioxide and silicon oxynitride. In an exemplary embodiment, when the thickness of the prepared gate oxide layer is less than 45 nm, hafnium oxide is selected as the material of the gate oxide layer.
[0054] In some embodiments, the material of the filling layer is polycrystalline silicon. Polycrystalline silicon is a form of elemental silicon. When molten elemental silicon solidifies under supercooling conditions, silicon atoms are arranged in a diamond lattice to form many crystal nuclei. If these crystal nuclei grow into grains with different crystal plane orientations, these grains will combine and crystallize into polycrystalline silicon.
[0055] In some embodiments, reference Figure 3 The step of pushing the P-well layer through a pushing-junction process so that the depth of the P-well layer is greater than the depth of the trench gate specifically includes but is not limited to steps S310 to S360:
[0056] S310, heating the furnace tube to a preset initial temperature;
[0057] S320, placing the epitaxial wafer in a heated furnace tube;
[0058] S330, heating the furnace tube to a first temperature at a preset heating rate, and introducing oxygen at a first flow rate; wherein the first temperature is higher than the initial temperature;
[0059] S340, maintaining the temperature in the furnace tube according to a preset maintenance time, and introducing oxygen at a second flow rate; wherein the second flow rate is less than the first flow rate;
[0060] S350, cooling the furnace tube at a preset cooling rate, and maintaining the introduction of oxygen at a second flow rate;
[0061] S360, when the temperature of the furnace tube drops to the initial temperature, stop introducing oxygen and take out the epitaxial wafer.
[0062] In step S310 and step S320 of some embodiments, the initial temperature of the furnace tube is 800°C.
[0063] In step S330 of some embodiments, the preset heating rate is 5°C / min, the first temperature is 1150°C, and the first flow rate is 7L / min. Therefore, the furnace tube is heated to the first temperature of 1150°C at the preset heating rate of 5°C / min, and oxygen is introduced at the first flow rate of 7L / min during the process.
[0064] In step S340 of some embodiments, the furnace temperature is maintained at 1150° C., the preset maintenance time is 120 min, and the second flow rate is 100 mL / min. Therefore, oxygen is introduced at a second flow rate of 100 mL / min during this process.
[0065] In step S350 of some embodiments, the preset cooling rate is 3°C / min, and the furnace tube is cooled at the preset cooling rate of 3°C / min, and oxygen is kept flowing at a second flow rate of 100 mL / min during this process.
[0066] In step S360 of some embodiments, when the temperature of the furnace tube drops to 800° C., the introduction of oxygen is stopped and the epitaxial wafer is taken out.
[0067] In steps S310 to S360 shown in this embodiment, by selecting a specific temperature and air flow rate ratio, while ensuring that the depth of the P-well layer meets the requirements, a good wrapping morphology can be formed on the corners of the groove gate to avoid incomplete wrapping or the phenomenon that the P-well layers on both sides of the groove gate are connected. In this embodiment, there is no specific restriction on the tools or equipment for implementing the push-junction process. A P-well layer deeper than the groove gate is prepared by the push-junction method, and at the same time, the P-well layer covers the corners of the groove gate and the P-well layers on both sides of the groove gate are not connected, forming a DP structure, thereby improving the reliability of the gate oxide layer and the short-circuit resistance of the field effect transistor.
[0068] In some embodiments, reference Figure 4 In the process of pushing the junction of the P well layer by the pushing junction process, the method further includes but is not limited to step S370:
[0069] S370, in the push-knot process, introducing protective gas into the furnace tube at a third flow rate; wherein the third flow rate is greater than the first flow rate.
[0070] In step S370 of some embodiments, the third flow rate is 13 L / min, and the protective gas is introduced into the furnace tube at a third flow rate of 13 L / min, and the protective gas can be nitrogen. Nitrogen is introduced at a flow rate higher than that of oxygen to protect the preparation of the DP field effect tube during the push-in process, so that the preparation of the DP field effect tube is more stable.
[0071] In some embodiments, the depth of the N-type source region is less than the depth of the trench gate. In this embodiment, the depth of the N-type source region is limited to be less than the depth of the trench gate, so that the P-well layer can wrap around the corners of the trench gate to perform electric field shielding on both sides of the trench gate to prevent the corners of the trench gate from being broken down.
[0072] In some embodiments, reference Figure 5 After the step of implanting N-type impurities on both sides of the trench gate to form an N-type source region, the method further includes but is not limited to steps S500 and S600:
[0073] S500, providing an anti-oxidation layer on the trench gate;
[0074] S600, providing a metal layer on the top and bottom surfaces of the epitaxial wafer; wherein the metal layer on the top surface of the epitaxial wafer is covered with an anti-oxidation layer.
[0075] In the step S500 and step S600 shown in the embodiment of the present application, the anti-oxidation layer is provided to prevent the device from absorbing moisture and realize the anti-oxidation function, and the metal layer has a protective effect. It should be noted that in the actual production and preparation process, borophosphosilicate glass deposition, flattening treatment, lead hole lithography and other process steps are required to form a complete field effect tube device.
[0076] Reference Figure 6 The DP field effect transistor of the embodiment of the present application is prepared by the DP field effect transistor preparation method of any of the above embodiments; the DP field effect transistor includes: an epitaxial wafer, a groove gate, a P-well layer, an N-type source region, an anti-oxidation layer and a metal layer, the groove gate is etched on the epitaxial wafer; the P-well layer is arranged on both sides of the groove gate, and the depth of the P-well layer is greater than the depth of the groove gate; the N-type source region is arranged on both sides of the groove gate, and the depth of the P-well layer is greater than the depth of the groove gate; the anti-oxidation layer is arranged on the groove gate; the metal layer is arranged on the top and bottom surfaces of the epitaxial wafer, and the metal layer on the top surface of the epitaxial wafer covers the anti-oxidation layer.
[0077] In some embodiments, the trench gate includes a corner surface, and the P-well layer wraps the corner surface. By preparing a P-well layer deeper than the trench gate, and making the P-well layer wrap the corner of the trench gate and the P-well layers on both sides of the trench gate are not connected, a DP structure is formed, thereby improving the reliability of the gate oxide layer and the short-circuit resistance of the field effect transistor.
[0078] In the description of the present application, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples" or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0079] The embodiments of the present application are described in detail above in conjunction with the accompanying drawings, but the present application is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present application. In addition, the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.
Claims
1. DP field effect tube preparation method, It is characterized in that include: Etching the epitaxial wafer to form a trench gate; The step of etching the epitaxial wafer to form a groove gate specifically includes: providing a protective layer on the epitaxial wafer; etching the protective layer to form a groove window; etching the epitaxial wafer at the position of the groove window to form a groove; depositing a gate oxide layer and a filling layer on the epitaxial wafer respectively; etching the gate oxide layer and the filling layer outside the groove to form the groove gate; wherein the material of the gate oxide layer includes silicon dioxide and silicon oxynitride; the thickness of the gate oxide layer and the length of the groove decrease in the same proportion to suppress the short channel effect; Implanting P-type impurities on both sides of the trench gate to form a P-well layer; The P-well layer is pushed through a push-junction process so that the depth of the P-well layer is greater than the depth of the groove gate; the step of pushing the P-well layer through a push-junction process so that the depth of the P-well layer is greater than the depth of the groove gate specifically includes: heating the furnace tube at a preset initial temperature; placing the epitaxial wafer in the heated furnace tube; heating the furnace tube to a first temperature at a preset heating rate, and introducing oxygen at a first flow rate; the first temperature is higher than the initial temperature; maintaining the temperature in the furnace tube according to a preset maintenance time, and introducing oxygen at a second flow rate; the second flow rate is less than the first flow rate; cooling the furnace tube at a preset cooling rate, and maintaining the introduction of oxygen at the second flow rate; when the temperature of the furnace tube drops to the initial temperature, stopping the introduction of oxygen and taking out the epitaxial wafer; wherein the P-well layer covers the corners of the groove gate and the P-well layers on both sides of the groove gate are not connected; N-type impurities are implanted on both sides of the trench gate to form an N-type source region.
2. The method for preparing a DP field effect transistor according to claim 1, It is characterized in that The material of the filling layer is polysilicon.
3. The method for preparing a DP field effect transistor according to claim 1, It is characterized in that In the process of pushing the junction of the P-well layer by a pushing junction process, the method further comprises: In the push-knot process, protective gas is introduced into the furnace tube at a third flow rate; wherein the third flow rate is greater than the first flow rate.
4. The method for preparing a DP field effect transistor according to any one of claims 1 to 2, It is characterized in that The depth of the N-type source region is smaller than the depth of the trench gate.
5. The method for preparing a DP field effect transistor according to any one of claims 1 to 2, It is characterized in that After the step of implanting N-type impurities on both sides of the trench gate to form an N-type source region, the method further includes: Disposing an anti-oxidation layer on the groove gate; A metal layer is disposed on the top and bottom surfaces of the epitaxial wafer; wherein the metal layer on the top surface of the epitaxial wafer covers the anti-oxidation layer.
6. A DP field effect tube, It is characterized in that The DP field effect transistor is prepared by the DP field effect transistor preparation method according to any one of claims 1 to 5; the DP field effect transistor comprises: Epitaxial wafer; A groove gate, wherein the groove gate is etched on the epitaxial wafer; A P-well layer, the P-well layer is arranged on both sides of the trench gate, and the depth of the P-well layer is greater than the depth of the trench gate; An N-type source region, wherein the N-type source region is disposed on both sides of the trench gate, and the depth of the P-well layer is greater than the depth of the trench gate; an anti-oxidation layer, the anti-oxidation layer being disposed on the groove gate; the groove gate comprising a corner surface, the P-well layer wrapping the corner surface; A metal layer is disposed on the top and bottom surfaces of the epitaxial wafer, and the metal layer on the top surface of the epitaxial wafer covers the anti-oxidation layer.