Laminated films and films with hard coatings

By using a laminated structure containing alicyclic structure polymer and particles in the laminated film and adding a hard coating layer thereon, the problem of reduced performance and insufficient sliding properties of triacetyl cellulose film in high temperature and high humidity environments is solved. Excellent sliding and impact strength under high loads are achieved.

CN115379949BActive Publication Date: 2024-12-06ZEON CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202180028111.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-04-24
Filing Date
2021-04-14
Publication Date
2024-12-06
Estimated Expiration
2041-04-14

AI Technical Summary

Technical Problem

When the existing triacetyl cellulose film is used in high temperature or high humidity environments, the polarization degree is reduced, the polarizer and the protective film are separated, and the sliding property is insufficient, resulting in poor operability, and the long film is prone to sticking and abrasion when wound.

Method used

A laminated film containing an alicyclic structure polymer is adopted, which includes a laminated structure of resin A and resin B. The number average particle size and weight ratio of the fine particles C are within a predetermined range, and the layer (b) is located on the surface and on it. Add a hard coat to improve slippage and impact strength.

Benefits of technology

Excellent sliding and high impact strength under high load conditions are achieved, adhesions and abrasions are reduced, and the operability and durability of the membrane are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115379949B_ABST
    Figure CN115379949B_ABST
Patent Text Reader

Abstract

The present invention provides a laminated film, which has a layer (a) containing resin A and a layer (b) containing resin B and microparticles C, wherein the resin A contains a polymer containing an alicyclic structure, and the resin B contains a polymer containing an alicyclic structure. The layer (b) is located on at least one outermost surface of the laminated film and has a thickness of not less than 1 μm and not more than 5 μm. The number average particle size of the microparticles C is not less than 0.10 μm and not more than 0.80 μm, and the weight ratio of the microparticles C to the resin B is not less than 3 weight % and not more than 10 weight %.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a laminated film and a film with a hard coating layer. Background Art

[0002] A polarizing plate used in a liquid crystal display device or the like generally includes a polarizer and a polarizer protective film for protecting the polarizer. Patent Documents 1 and 2 describe that a film containing triacetyl cellulose or a norbornene resin can be used as a polarizer protective film.

[0003] Furthermore, Patent Document 3 describes that a film containing a norbornene resin and fine particles can be used as a polarizer protective film.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent document 1: Japanese Patent No. 3499974;

[0007] Patent Document 2: Japanese Patent Application Publication No. 2005-181615;

[0008] Patent document 3: Japanese Patent Application Publication No. 2011-011394. Summary of the invention

[0009] Problem that the invention aims to solve

[0010] When a polarizing plate having a triacetyl cellulose film as a polarizer protective film is used for a long time in a high temperature or high humidity environment, the polarization degree may be significantly reduced, the polarizer and the polarizer protective film may be separated, and the transparency may be reduced due to hydrolysis of the triacetyl cellulose.

[0011] In order to reduce the degradation of these properties, when an alicyclic polyolefin resin is used instead of triacetyl cellulose as the material of the polarizer protective film, the slippage of the film is insufficient. The polarizer protective film with insufficient slippage lacks operability and is difficult to be wound into a roll for the purpose of transportation, storage, etc. Therefore, Patent Document 3 proposes a laminated film having a layer containing an alicyclic polyolefin resin and prescribed microparticles on the surface in order to improve the slippage of the film.

[0012] However, when a long laminate film of more than 2000 m is wound into a roll, a large load may be applied near the core, causing blocking and scratching near the core. The laminate film of Patent Document 3 has insufficient slidability when a large load is applied.

[0013] On the other hand, in order to suppress the occurrence of breakage during the conveyance of the laminated film, the laminated film preferably has a high impact strength.

[0014] Therefore, there is a demand for a laminated film having excellent sliding properties when a large load is applied and high impact strength, and a film with a hard coat layer including the laminated film.

[0015] Solutions for solving problems

[0016] The present inventors have conducted intensive research to solve the above-mentioned problems, and as a result, have found that by providing a laminated film comprising: a layer (a) comprising a resin containing a polymer containing an alicyclic structure, and a layer (b) comprising microparticles and a resin containing a polymer containing an alicyclic structure, the number average particle size of the microparticles, the weight ratio of the microparticles and the thickness of layer (b) of the laminated film being within a specified range, the above-mentioned problems can be solved, thereby completing the present invention:

[0017] That is, the present invention provides the following technical solutions.

[0018] [1] A laminated film comprising a layer (a) comprising a resin A, and a layer (b) comprising a resin B and microparticles C, wherein the resin A comprises a polymer containing an alicyclic structure, and the resin B comprises a polymer containing an alicyclic structure, the layer (b) is located on at least one outermost surface of the laminated film, and has a thickness of 1 μm to 5 μm, the number average particle size of the microparticles C is 0.10 μm to 0.80 μm, and the weight ratio of the microparticles C in the layer (b) to the resin B is 3 wt% to 10 wt%.

[0019] [2] The laminated film according to [1], wherein the fine particles C are fine particles of a cross-linked copolymer of methyl methacrylate and styrene.

[0020] [3] The laminated film according to [1], wherein the fine particles C are fine particles containing a crosslinked polymer having an alicyclic structure.

[0021] [4] The laminated film according to any one of [1] to [3], wherein the refractive index nb of the resin B and the refractive index nc of the microparticles C satisfy the following formula (1).

[0022] |nb-nc|≤0.03 (1)

[0023] [5] The laminated film according to [1], wherein the fine particles C are fine particles of silicon dioxide.

[0024] [6] The laminated film according to any one of [1] to [5], wherein the layer (a) contains a UV absorber.

[0025] [7] A film with a hard coating layer, comprising the laminated film according to any one of [1] to [6] and a hard coating layer provided on the laminated film.

[0026] Effects of the Invention

[0027] According to the present invention, there can be provided a laminated film having excellent sliding properties when a large load is applied and high impact strength; and a film with a hard coating layer including the laminated film. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a cross-sectional view schematically showing a laminated film according to one embodiment of the present invention.

[0029] Figure 2 This is a cross-sectional view schematically showing a laminated film according to another embodiment of the present invention. DETAILED DESCRIPTION

[0030] The present invention will be described in detail below by showing embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and can be implemented with arbitrary changes without departing from the scope of the claims of the present invention and their equivalents.

[0031] In the following description, a "long strip" of film refers to a film having a length of more than 5 times the width, preferably 10 times or more, and specifically refers to a film having a length that can be wound into a roll for storage or transportation. The upper limit of the length of the film is not particularly limited, for example, it can be less than 100,000 times relative to the width.

[0032] In the following description, unless otherwise specified, the tilt direction of the long film means an in-plane direction of the film and a direction that is neither parallel to nor perpendicular to the longitudinal direction of the film.

[0033] In the following description, the term "(meth)acrylate" includes "acrylate", "methacrylate" and a combination of these.

[0034] In the following description, the term "(meth)acryl" includes "acryl", "methacryl" and a combination of these.

[0035] [1. Overview of Laminated Film]

[0036] A laminated film according to one embodiment of the present invention comprises a layer (a) comprising a resin A and a layer (b) comprising a resin B and microparticles C, wherein the resin A comprises a polymer containing an alicyclic structure, and the resin B comprises a polymer containing an alicyclic structure. The laminated film may have any layer other than the layer (a) and the layer (b). However, the layer (b) is disposed on the outermost surface of the laminated film, and the layer (b) is exposed on the surface of the laminated film.

[0037] By positioning the layer (b) on the outermost surface of the laminated film, the laminated film can have excellent slidability.

[0038] [1.1.Layer(a)]

[0039] The layer (a) contains the resin A, and the resin A contains an alicyclic structure-containing polymer. When the layer (a) contains the resin A and the resin A contains an alicyclic structure-containing polymer, the heat resistance and moisture resistance of the laminated film can be improved.

[0040] The alicyclic structure-containing polymer refers to a polymer containing an alicyclic structure in the main chain and / or side chain. From the viewpoint of improving the mechanical strength and heat resistance of the laminated film, the alicyclic structure-containing polymer preferably contains an alicyclic structure in the main chain.

[0041] Examples of the alicyclic structure include saturated alicyclic hydrocarbon (cycloalkane) structures, unsaturated alicyclic hydrocarbon (cycloolefin, cycloalkyne) structures, etc. Among them, from the viewpoint of mechanical strength and heat resistance, cycloalkane structures and cycloalkene structures are preferred, and cycloalkane structures are more preferred.

[0042] The number of carbon atoms constituting the alicyclic structure is not particularly limited, and is usually 4 or more, preferably 5 or more, and usually 30 or less, preferably 20 or less, and more preferably 15 or less. When the number of carbon atoms constituting the alicyclic structure is within the above range, the mechanical strength, heat resistance, and moldability of the laminated film are highly balanced, which is preferred.

[0043] The proportion of repeating units containing alicyclic structures in the alicyclic structure-containing polymer can be appropriately selected according to the purpose of use of the laminated film. The proportion of repeating units containing alicyclic structures in 100% by weight of the alicyclic structure-containing polymer is preferably 55% by weight or more, more preferably 70% by weight or more, further preferably 90% by weight or more, and usually 100% by weight or less. When the proportion of repeating units containing alicyclic structures in the alicyclic structure-containing polymer is within the above range, the transparency and heat resistance of the laminated film can be effectively improved.

[0044] Examples of polymers containing alicyclic structures include norbornene polymers, monocyclic cyclic olefin polymers, cyclic conjugated diene polymers, vinyl alicyclic hydrocarbon polymers, and hydrogenated products thereof. Of these, norbornene polymers and hydrogenated products thereof are preferred because of their good transparency and moldability.

[0045] Examples of norbornene-based polymers include: ring-opening polymers of monomers having a norbornene structure and their hydrides; addition polymers of monomers having a norbornene structure and their hydrides. In addition, examples of ring-opening polymers of monomers having a norbornene structure include ring-opening homopolymers of a monomer having a norbornene structure, ring-opening copolymers of two or more monomers having a norbornene structure, and ring-opening copolymers of a monomer having a norbornene structure and any monomer copolymerizable therewith. Furthermore, examples of addition polymers of monomers having a norbornene structure include addition homopolymers of a monomer having a norbornene structure, addition copolymers of two or more monomers having a norbornene structure, and addition copolymers of a monomer having a norbornene structure and any monomer copolymerizable therewith. As these polymers, for example, polymers disclosed in Japanese Patent Publication No. 2002-321302 and the like can be cited.

[0046] Specific examples of norbornene-based polymers and hydrogenated products thereof include “ZEONOR” manufactured by Zeon Corporation; “ARTON” manufactured by JSR Corporation; and “TOPAS” manufactured by Topaz Advanced Polymers Co., Ltd.

[0047] The resin A may contain one type of alicyclic structure-containing polymer alone, or may contain two or more types of alicyclic structure-containing polymers in combination at any ratio.

[0048] In addition, as long as the effect of the present invention is not significantly damaged, resin A can include any polymer except alicyclic structure polymer, and from the viewpoint of significantly exerting the advantages of the present invention, the amount of any polymer is preferably small. The specific amount of any polymer can be different according to factors such as the purpose and thickness of the laminated film. For example, relative to 100 parts by weight of resin A, the ratio of the above-mentioned arbitrary polymer is preferably less than 10 parts by weight, more preferably less than 5 parts by weight, further preferably less than 3 parts by weight, usually more than 0 parts by weight, and can also be 0 parts by weight. Resin A is particularly preferably not including any polymer.

[0049] Furthermore, the resin A may contain any component other than the above-mentioned alicyclic structure-containing polymer, as long as the effect of the present invention is not significantly impaired. Examples of the optional component include stabilizers such as antioxidants, heat stabilizers, and near infrared absorbers; resin modifiers such as lubricants and plasticizers; colorants such as dyes and pigments; and antistatic agents. The resin A may contain one arbitrary component alone, or may contain two or more arbitrary components in combination at any ratio.

[0050] From the viewpoint of significantly exerting the effect of the present invention, the content of the components (the above-mentioned arbitrary polymer and other arbitrary components) other than the resin A containing alicyclic structure polymer is preferably small. The preferred ratio can be different according to factors such as the purpose and thickness of the laminated film. For example, relative to 100 parts by weight of resin A, the ratio of the components other than the alicyclic structure polymer is preferably less than 10 parts by weight, more preferably less than 5 parts by weight, further preferably less than 3 parts by weight, usually more than 0 parts by weight, and can also be 0 parts by weight.

[0051] Layer (a) may contain an ultraviolet absorber in addition to resin A. Thus, the laminated film of the present embodiment can obtain resistance to ultraviolet rays. Therefore, for example, when the laminated film of the present embodiment is used as an optical film such as a polarizer protective film, the laminated film of the present embodiment and the polarizer protected by the laminated film can be effectively protected from degradation caused by ultraviolet rays.

[0052] As the ultraviolet absorber, for example, a benzophenone ultraviolet absorber, a benzotriazole ultraviolet absorber, an acrylonitrile ultraviolet absorber, a hydroxyphenyltriazine ultraviolet absorber, etc. can be used. Among them, as the ultraviolet absorber, preferably used are 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol], 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2,4-di-tert-butyl-6-(5-chlorobenzotriazol-2-yl)phenol, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[(hexyl)oxy]-phenol, 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-dibutoxyphenyl)-1,3,5-triazine, etc. In addition, the ultraviolet absorber may be used alone or in combination of two or more at any ratio.

[0053] As a method for making the layer (a) contain a UV absorber, for example, there is a method of supplying the resin A and the UV absorber to an extruder such as a twin-screw extruder and kneading them to produce a resin for forming the layer (a).

[0054] The weight ratio of the ultraviolet absorber in layer (a) to 100 parts by weight of resin A is preferably 1.0 parts by weight or more, more preferably 3.0 parts by weight or more, preferably 23 parts by weight or less, and more preferably 10 parts by weight or less. When the weight ratio of the ultraviolet absorber is above the lower limit of the above range, ultraviolet rays can be effectively blocked. When the concentration of the ultraviolet absorber is below the upper limit of the above range, point defects caused by poor dispersion of the ultraviolet absorber in the laminated film can be suppressed, and the strength reduction of the laminated film can also be suppressed.

[0055] The thickness of the layer (a) can be arbitrarily set according to the intended use of the laminated film, etc. The thickness of the layer (a) can be, for example, 1 μm or more and 99 μm or less.

[0056] [1.2. Layer (b)]

[0057] The layer (b) is a layer containing a resin B and fine particles C, wherein the resin B contains an alicyclic structure-containing polymer. By making the layer (b) contain the resin B and the resin B contain an alicyclic structure-containing polymer, the heat resistance and moisture resistance of the laminated film of the present embodiment can be improved. Furthermore, generally, the layer (b) contains the resin B and the resin B contains an alicyclic structure-containing polymer, so that the affinity with the layer (a) becomes higher, and thus the bonding strength between the layer (a) and the layer (b) can be improved.

[0058] Examples of the alicyclic structure-containing polymer contained in the resin B include the same examples and preferred examples of the alicyclic structure-containing polymer that can be contained in the resin A. The alicyclic structure-containing polymer contained in the resin A and the alicyclic structure-containing polymer contained in the resin B may be the same as or different from each other.

[0059] As long as the effects of the present invention are not significantly impaired, the resin B may contain any component other than the alicyclic structure-containing polymer. Examples of the optional components include the same examples as the optional components that can be contained in the resin A. The resin B may contain one arbitrary component alone, or may contain two or more arbitrary components in combination at any ratio.

[0060] From the viewpoint of significantly exerting the effect of the present invention, the content of any component other than the alicyclic structure-containing polymer is preferably small in resin B. The specific amount of any component can be different according to factors such as the purpose and thickness of the laminated film. For example, relative to 100 parts by weight of resin B, the proportion of any component is preferably 10 parts by weight or less, more preferably 5 parts by weight or less, further preferably 3 parts by weight or less, usually 0 parts by weight or more, and can also be 0 parts by weight.

[0061] The fine particles C may be inorganic particles, organic particles, or composite particles composed of a combination of an inorganic material and an organic material. The fine particles C may be used alone or in combination of two or more at any ratio.

[0062] In one embodiment, the fine particles C are preferably organic particles, and are more preferably fine particles of an organic polymer from the viewpoint of facilitating adjustment of the refractive index of the fine particles and narrowing the width of the particle size distribution.

[0063] Examples of the organic polymer that can constitute the fine particles C include a crosslinked copolymer of methyl methacrylate and styrene, and an alicyclic structure-containing crosslinked polymer.

[0064] From the viewpoint of easy adjustment of the refractive index, the fine particles C are preferably fine particles of a cross-linked copolymer of methyl methacrylate and styrene.

[0065] From the viewpoint of producing microparticles having a refractive index close to that of the resin B containing the alicyclic structure-containing polymer, the microparticles C are preferably microparticles containing an alicyclic structure crosslinked polymer.

[0066] As described above, the microparticles C can be microparticles of a cross-linked copolymer of methyl methacrylate and styrene. Here, the cross-linked copolymer of methyl methacrylate and styrene refers to a copolymer of methyl methacrylate, styrene, and a cross-linking monomer. Here, as examples of cross-linking monomers, multifunctional monomers containing two or more polymerizable groups per molecule can be cited, and as specific examples, divinylbenzene, ethylene glycol dimethacrylate, 1,3-butanediol dimethacrylate, 1,4-butanediol dimethacrylate, 1,5-pentanediol dimethacrylate, 1,6-hexanediol dimethacrylate, neopentyl glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, and tripropylene glycol dimethacrylate can be cited. The microparticles of the above cross-linked copolymer can be obtained by, for example, suspension polymerization of a monomer mixture containing methyl methacrylate, styrene, and a cross-linking monomer. The weight ratio of methyl methacrylate, styrene, and a cross-linking monomer can be set arbitrarily.

[0067] As the microparticles of the crosslinked copolymer of methyl methacrylate and styrene, microparticles having various average particle diameters are commercially available, and these microparticles can be used. An example of a commercial product of the microparticles is "TECHPOLYMER" manufactured by Sekisui Chemicals Co., Ltd.

[0068] As described above, the microparticles C may also be microparticles of a cross-linked polymer containing an alicyclic structure. Here, the cross-linked polymer containing an alicyclic structure refers to a polymer having a structure formed by cross-linking repeating units containing an alicyclic structure. The examples and preferred examples of the alicyclic structure contained in the cross-linked polymer containing an alicyclic structure, the preferred range of the number of carbon atoms constituting the alicyclic structure, and the preferred range of the proportion of repeating units containing the alicyclic structure are the same as the examples and preferred ranges described for the alicyclic structure-containing polymer in resin A. By making the microparticles C into microparticles of a cross-linked polymer containing an alicyclic structure, the refractive index of the microparticles C can be made close to the refractive index of the resin B containing the alicyclic structure polymer contained in layer (b), and the internal haze of the laminated film can be effectively reduced.

[0069] Examples of crosslinked polymers containing alicyclic structures include norbornene-based crosslinked polymers, monocyclic cyclic olefin-based crosslinked polymers, cyclic conjugated diene-based crosslinked polymers, vinyl alicyclic hydrocarbon-based crosslinked polymers, and hydrogenated products thereof. Among these, norbornene-based crosslinked polymers and hydrogenated products thereof have good transparency and are therefore preferred.

[0070] Examples of norbornene-based crosslinked polymers include: crosslinked polymers of monomer units having a norbornene structure and hydrogenated products thereof; crosslinked products of copolymers of monomers having a norbornene structure and any monomers copolymerizable therewith and hydrogenated products thereof. The copolymer may be a ring-opening copolymer of monomers having a norbornene structure or an addition copolymer.

[0071] As the alicyclic structure-containing crosslinked polymer, for example, particles obtained by crosslinking a monomer having a norbornene structure by suspension polymerization in the presence of a crosslinking agent, particles obtained by crosslinking a polymer having a norbornene structure in the presence of a crosslinking agent, etc. can be used.

[0072] The fine particles C may be inorganic particles. Examples of the inorganic particles include silica particles, synthetic zeolite particles, and glass particles.

[0073] From the viewpoint of making the particle size distribution uniform, the fine particles C are preferably fine particles of silicon dioxide.

[0074] Silica particles having various average particle diameters are commercially available, and these particles can be used. Examples of commercially available products include the "QSG" series manufactured by Shin-Etsu Chemical Co., Ltd., the "SEAHOSTAR" series manufactured by Nippon Shokubai Co., Ltd., and the "ADMANANO" series manufactured by Yaduma Technology Co., Ltd.

[0075] The number average particle size of the microparticle C is usually 0.10 μm or more, preferably 0.20 μm or more, usually 0.80 μm or less, preferably 0.50 μm or less. When the number average particle size is above the above lower limit, the slip of the laminated film can be sufficient. By making the number average particle size below the above upper limit, the internal haze of the laminated film can be reduced. In addition, when the melt containing resin B and microparticle C is passed through a polymer filter, the clogging of the polymer filter can be reduced. Therefore, the reduction in the productivity of the laminated film can be suppressed.

[0076] When the fine particles C are organic particles, the number average particle size of the fine particles C is preferably 0.1 μm or more, more preferably 0.2 μm or more, and is preferably 0.8 μm or less, more preferably 0.5 μm or less.

[0077] When the fine particles C are inorganic particles, the number average particle size of the fine particles C is preferably 0.1 μm or more, preferably 0.5 μm or less, and more preferably 0.3 μm or less.

[0078] The number average particle size of the fine particles C is a value measured by a laser diffraction scattering method using a particle size distribution analyzer.

[0079] The volume proportion of coarse particles with a particle size of 1 μm or more in the microparticles C is preferably small. Thus, when the melt containing resin B and microparticles C is passed through a polymer filter, the clogging of the polymer filter can be further reduced, so the productivity of the laminated film is further improved. The volume proportion of coarse particles with a particle size of 1 μm or more in the microparticles C is preferably 1% or less, more preferably 0.1% or less, usually 0% or more, preferably 0%, and can also be 0.01% or more. In the calculation of the proportion of coarse particles, the upper limit of the particle size of the coarse particles is not particularly limited, for example, it can be 1 mm or less. However, in normal manufacturing, particles with a particle size exceeding 1 mm can be completely removed, so even if particles exceeding 1 mm are included in the calculation, the preferred range of the proportion of coarse particles is the same as the above-mentioned value.

[0080] By classifying the fine particles C by sieving or the like to remove coarse particles, the volume ratio of the coarse particles in the fine particles C can be reduced.

[0081] The refractive index nb of the resin B and the refractive index nc of the fine particles C preferably satisfy the following formula (1).

[0082] |nb-nc|≤0.03 (1)

[0083] When the refractive index nb and the refractive index nc satisfy the above formula (1), the internal haze of the laminated film can be further reduced.

[0084] The value of |nb-nc| is more preferably 0.02 or less, further preferably 0.01 or less, and is usually 0 or more, ideally 0, but may be 0.005 or more.

[0085] The refractive index can be measured by the method described in Examples using light having a wavelength of 589 nm.

[0086] The value of |nb-nc| can be reduced by, for example, making the microparticles C microparticles of an organic polymer, adjusting the type and amount of the raw material of the organic polymer, etc. For example, the value of |nb-nc| can be reduced by using a monomer common to the raw material of the polymer contained in the resin B as the raw material of the organic polymer.

[0087] In layer (b), the weight ratio of the microparticles C to the resin B is usually 3 wt % or more, preferably 4 wt % or more, and usually 10 wt % or less, preferably 9 wt % or less, and more preferably 8 wt % or less.

[0088] When the weight ratio of the microparticles C to the resin B is less than the above lower limit, when the laminated film is a long strip of film exceeding 2000 m in length and a large load is applied near the core when it is rolled up, the film sometimes has insufficient slipperiness, resulting in adhesion near the core, causing defects such as scratches.

[0089] By microparticle C relative to resin B weight ratio is below the above-mentioned upper limit, the surface roughness of layer (b) becomes appropriate, and the increase of the external haze of laminated film is suppressed. As a result, when laminated film is used as the structural unit of image display device, the visibility of image display device can be improved. In addition, when any additional layer such as hard coating is stacked on laminated film, the adhesion of layer (b) and the additional layer becomes good. In addition, by microparticle C relative to resin B weight ratio is below the above-mentioned upper limit, it is advantageous in terms of manufacturing cost. And then, when manufacturing the material for constituting layer (b), microparticle C can be suppressed from being poorly dispersed to resin B.

[0090] The layer (b) may contain an ultraviolet absorber in addition to the resin B and the fine particles C. From the viewpoint of suppressing the bleeding of the ultraviolet absorber, the weight ratio of the ultraviolet absorber in the layer (b) relative to 100 parts by weight of the resin B is preferably 2 parts by weight or less, more preferably 1 part by weight or less, and is usually 0 parts by weight or more, and may be 0 parts by weight or 0.1 parts by weight or more.

[0091] The thickness of the layer (b) is usually 1 μm or more, preferably 1.5 μm or more, and usually 5 μm or less, preferably 3 μm or less.

[0092] By making the thickness of layer (b) more than the above lower limit, when layer (b) is formed by extrusion molding such as coextrusion, thickness control can be easily performed. In addition, by making the thickness of layer (b) less than the above upper limit, the slidability of layer (b) containing microparticles C and the strength reduction of layer (b) are balanced, the strength of the laminated film can be made good, and when carrying the laminated film, the laminated film can be suppressed from breaking, so that the operability of the laminated film becomes excellent. Here, in the case where the laminated film has a multilayer layer (b), the thickness of each layer (b) is preferably within the above range.

[0093] The ratio of the thickness of layer (b) to the thickness of layer (a) (the thickness of layer (b) / the thickness of layer (a)) is preferably less than 0.32, more preferably less than 0.25, and further preferably less than 0.11. By making the above ratio less than the above upper limit, the strength of the laminated film can be further improved. In addition, the above ratio is preferably more than 0.02, more preferably more than 0.04. By making the above ratio more than the above lower limit, the thickness control of the laminated film can be better performed. Here, in the case where the laminated film has a multilayer layer (b), the thickness of each layer (b) is preferably within the above range.

[0094] [1.3. Layer structure of laminated film]

[0095] The laminated film of one embodiment of the present invention has layer (a) and layer (b). The laminated film can be a laminated film formed by only two layers of layer (a) and layer (b). However, as described above, the laminated film can also have any layer in addition to layer (a) and layer (b). Any layer can be one layer, or two or more layers. In addition, when there are more than two layers of any layer, any layer can be a layer with the same thickness, material, etc., or a layer with different thickness, material, etc. In addition, as long as layer (b) is configured on at least one outermost surface, the position of any layer can be set arbitrarily. From the viewpoint of thinning the laminated film, the laminated film preferably does not have a layer other than layer (a) and layer (b).

[0096] The laminated film may have two layers (b). When the laminated film has two layers (b), the laminated film is usually a laminated film having layer (b), layer (a) and layer (b) in sequence, and usually layer (b) is arranged on both surfaces of the laminated film, and the two layers (b) are exposed on both surfaces of the laminated film, respectively.

[0097] From the viewpoint of suppressing the bleeding of additives such as ultraviolet absorbers that may be contained in layer (a) and further improving the slip properties, the laminated film preferably has two layers (b), and has a first layer (b), layer (a), and second layer (b) in this order.

[0098] When the laminate film has two layers (b), the two layers (b) may be made of the same material and have the same thickness, or may be made of the same material but with different thicknesses, or may be made of materials with different types of components, weight ratios of components, etc. When the laminate film has two layers (b), the manufacturing can be facilitated and the curling of the laminate film can be suppressed. Therefore, the two layers (b) are preferably made of the same material and have the same thickness.

[0099] The laminated film may include a plurality of layers (a). When the laminated film includes a plurality of layers (a), the plurality of layers (a) may be composed of materials different in the types of components, weight ratios of the components, etc.

[0100] Hereinafter, the layer structure of the laminated film according to the embodiment of the present invention will be described using the drawings.

[0101] Figure 1The cross-sectional view schematically shows a laminated film according to an embodiment of the present invention. The laminated film 100 according to the present embodiment comprises a layer (a) 110 and a layer (b) 120 arranged in contact with a surface 110U of the layer (a). The layer (b) 120 is arranged on the outermost surface of the laminated film 100, and the surface 120U of the layer (b) 120 is exposed.

[0102] Figure 2 The cross-sectional view schematically shows another embodiment of the laminated film of the present invention. The laminated film 200 of the present embodiment has layer (b) 221, layer (a) 210 and layer (b) 222 in sequence. Layer (b) 221 is configured in a manner in contact with one surface 210U of layer (a) 210. Layer (b) 222 is configured in a manner in contact with another surface 210D of layer (a) 210. Layer (b) 221 and layer (b) 222 are respectively configured on the outermost surface of the laminated film 200, and the surface 221U of layer (b) 221 and the surface 222D of layer (b) 222 are exposed.

[0103] [1.4. Thickness, length, and physical properties of laminated films]

[0104] (thickness)

[0105] The thickness of the laminated film can be set to any thickness, and can be preferably 10 μm or more and 100 μm or less, and more preferably 10 μm or more and 80 μm or less. Since the laminated film has a layer (a) and a layer (b) containing a resin, and the resin contains an alicyclic structure-containing polymer, the heat resistance and moisture resistance of the laminated film can be improved. Therefore, even if the thickness of the laminated film is reduced as in the above range, the heat resistance and moisture resistance of the laminated film can be sufficient.

[0106] (Length of laminated film)

[0107] The laminated film may be in the form of a sheet or a long strip. The laminated film of this embodiment can reduce defects such as adhesion and scratches near the winding core, and therefore, it is preferably in the form of a long strip and a roll. In the case where the laminated film is a long strip, the length of the laminated film may exceed 2000m. Even in the case where the laminated film of this embodiment is wound into a roll in this way, it is possible to reduce defects such as adhesion and scratches near the winding core as described above.

[0108] (UV transmittance)

[0109] The laminated film preferably has a low ultraviolet transmittance. The transmittance of ultraviolet rays at a wavelength of 380 nm of the laminated film is preferably 4% or less, more preferably 1% or less, usually 0% or more, and may also be 0%. A laminated film having an ultraviolet transmittance below the above upper limit can be preferably used as a protective film for a structural unit of an image display device (particularly a structural unit of an organic electroluminescent element, a polarizer, etc.). The ultraviolet transmittance can be measured using a spectrophotometer.

[0110] By making any of the layers constituting the laminated film contain an ultraviolet absorber, the ultraviolet transmittance of the laminated film can be reduced.

[0111] In the layers constituting the laminated film, layer (a) may contain a UV absorber, layer (b) may contain a UV absorber, both layer (a) and layer (b) may contain a UV absorber, and any layer other than layer (a) and layer (b) may contain a UV absorber. In the case where the laminated film is a film containing a UV absorber, preferably layer (a) contains a UV absorber, and layer (b) does not contain a UV absorber.

[0112] (Sliding property: static friction coefficient)

[0113] The laminate film has excellent sliding properties. The sliding properties can be evaluated by using a friction tester according to JIS K7125 with a load of 1 kg to obtain the static friction coefficient of the laminate film. The static friction coefficient of the laminate film obtained by the method described in the items of the examples is preferably 0.4 or more, preferably 0.8 or less, and more preferably 0.7 or less.

[0114] By making the coefficient of static friction of the laminated film measured at a load of 1 kg to be above the above lower limit, the sliding property of the laminated film can be moderate, and the operability when winding the laminated film can be made more excellent. In addition, by making the coefficient of static friction of the laminated film measured at a load of 1 kg to be below the above upper limit, when the laminated film is rolled up like a long film with a length of more than 2000m, even if a large load is applied near the winding core, it is possible to reduce the occurrence of defects such as adhesion near the winding core and abrasion.

[0115] (Internal haze)

[0116] The laminated film according to one embodiment of the present invention has low internal haze.

[0117] The internal haze of the laminated film is preferably less than 0.7%, more preferably less than 0.6%, further preferably less than 0.5%, particularly preferably less than 0.2%, usually more than 0.0%, and ideally 0.0%. By making the internal haze of the laminated film low, the laminated film can be preferably used as a structural unit of an image display device requiring fine display performance. The internal haze of the laminated film can be measured using a haze meter by the method described in the items of the examples.

[0118] (Impact strength: 50% destructive energy)

[0119] The laminated film of one embodiment of the present invention has high impact strength. The impact strength of the film can be evaluated by measuring 50% destruction energy according to JIS K7124-1 by the method described in the item of the examples. 50% destruction energy refers to the energy used to destroy 50% of the number of film sheets as a sample.

[0120] The 50% breaking energy of the laminated film is preferably 0.03 J or more, more preferably 0.04 J or more, and although a larger value is more preferred, it may be 0.5 J or less.

[0121] Since the 50% breaking energy of the laminated film is large, the occurrence of breakage of the laminated film can be suppressed during transportation of the laminated film, thereby making the handling property of the laminated film excellent.

[0122] [1.5. Method for producing laminated film]

[0123] The laminated film of one embodiment of the present invention can be manufactured by any method. The laminated film can be appropriately manufactured by a molding method utilizing coextrusion, such as a coextrusion T-die method, a coextrusion inflation method, a coextrusion lamination method, etc.; a film lamination molding method such as dry lamination; a coating molding method such as a resin solution constituting layer (b) is applied to a film constituting layer (a), and other known methods. Among them, from the viewpoint of manufacturing efficiency and preventing volatile components such as solvents from remaining in the film, a molding method utilizing coextrusion is preferably used. Among the molding methods utilizing coextrusion, a coextrusion T-die method is preferred. As examples of the coextrusion T-die method, a feed head method and a multi-manifold method can be cited.

[0124] The material constituting the layer (a) included in the laminated film can be produced by, for example, supplying the resin A and, if necessary, any optional components such as a UV absorber to an extruder such as a twin-screw extruder and kneading them.

[0125] The material constituting the layer (b) included in the laminated film can be produced by, for example, supplying the resin B, the fine particles C, and, if necessary, any optional components to an extruder such as a twin-screw extruder and kneading them.

[0126] When a laminated film is produced by a co-extrusion molding method, the material constituting layer (a) and the material constituting layer (b) are supplied to an extruder such as a uniaxial extruder, extruded together from a die head to form a molten resin layer, and the extruded molten resin layer is cooled on a cooling drum. Thus, the laminated film can be produced continuously.

[0127] After the laminated film is manufactured by a molding method such as coextrusion, it can also be subjected to any process such as stretching. For example, after coextrusion, the laminated film can also be subjected to any stretching process such as longitudinal uniaxial stretching, transverse uniaxial stretching, longitudinal and transverse simultaneous biaxial stretching, successive biaxial stretching, and oblique stretching. Therefore, the laminated film can be an unstretched film without stretching, or a stretched film that has been stretched, but from the perspectives of not being easy to interfere with the polarized light of the image display device, not being easy to fall off particles during film manufacturing, and not being easy to cause cohesion damage near the surface layer of the laminated film, and being able to ensure the bonding strength of the laminated film with other components, the unstretched film is preferred.

[0128] [2. Film with hard coating]

[0129] The film with a hard coating layer of one embodiment of the present invention comprises the above-mentioned laminated film and a hard coating layer arranged on the above-mentioned laminated film. The film with a hard coating layer is preferably directly provided with a hard coating layer on the laminated film, and preferably no other layer exists between the laminated film and the hard coating layer. By providing a hard coating layer on the laminated film, it is possible to form a film having at least one function of scratch resistance, anti-glare, antistatic property, and low reflectivity. The film with a hard coating layer may have a plurality of hard coating layers, for example, the film with a hard coating layer may have two hard coating layers, and hard coating layers are respectively provided on the two surfaces of the laminated film.

[0130] Examples of the composition for forming the hard coat layer include compositions containing an active energy ray-curable resin that can be cured by active energy rays. Examples of the active energy rays include ultraviolet rays and electron beams.

[0131] As the active energy ray-curable resin, a resin which shows a hardness of "HB" or higher in a pencil hardness test specified in JIS K5600-5-4 after curing is preferably used.

[0132] Examples of active energy ray-curable resins include silicone, melamine, epoxy, acrylic, polyurethane (meth) acrylate, and multifunctional (meth) acrylate. Among them, polyurethane (meth) acrylate UV-curable resins and / or multifunctional (meth) acrylate UV-curable resins are preferred from the viewpoints of good bonding strength, toughness, and excellent productivity. These can be used alone or in combination of two or more in any ratio.

[0133] The polyfunctional (meth)acrylate-based resin is a resin containing polyfunctional (meth)acrylate.

[0134] The polyfunctional (meth)acrylate is a compound having two or more (meth)acryloyl groups in one molecule. Specific examples of the multifunctional (meth)acrylate include: di(meth)acrylates of diols such as 1,4-butanediol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 2-methyl-1,8-octanediol di(meth)acrylate, 2-butyl-2-ethyl-1,3-propanediol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, and tripropylene glycol di(meth)acrylate; polyethylene glycol di(meth)acrylate; polypropylene glycol di(meth)acrylate; di(meth)acrylate of tris(2-hydroxyethyl)isocyanurate ester; di(meth)acrylate of a diol obtained by adding 4 or more ethylene oxide or propylene oxide to 1 mol of neopentyl glycol; di(meth)acrylate of a diol obtained by adding 2 mol of ethylene oxide or propylene oxide to 1 mol of bisphenol A; trimethylolpropane tri(meth)acrylate; ethylene oxide-modified trimethylolpropane tri(meth)acrylate; propylene oxide-modified trimethylolpropane tri(meth)acrylate; ditrimethylolpropane tri(meth)acrylate; ditrimethylolpropane tetra(meth)acrylate, tris(2-(meth)acryloyloxyethyl)isocyanurate; pentaerythritol tri(meth)acrylate; pentaerythritol tetra(meth)acrylate; dipentaerythritol tri(meth)acrylate; dipentaerythritol tetra(meth)acrylate; dipentaerythritol penta(meth)acrylate; dipentaerythritol hexa(meth)acrylate. These multifunctional (meth)acrylates may be used alone or in combination of two or more in any ratio. In addition, among these multifunctional (meth)acrylates, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, pentaerythritol tetra(meth)acrylate, and pentaerythritol tri(meth)acrylate are preferred because the scratch resistance of the cured coating film (hard coating) of the composition containing the active energy ray-curable resin is improved.

[0135] The urethane (meth)acrylate-based resin is a resin containing urethane (meth)acrylate.

[0136] The urethane (meth)acrylate can be obtained by reacting polyisocyanate with a (meth)acrylate having a hydroxyl group.

[0137] Examples of the polyisocyanate include aliphatic polyisocyanates and aromatic polyisocyanates. Aliphatic polyisocyanates are preferred because they can reduce coloration of a cured coating film of a composition containing an active energy ray-curable resin.

[0138] The above-mentioned aliphatic polyisocyanate is a compound whose parts other than the isocyanate group are composed of aliphatic hydrocarbons. As specific examples of aliphatic polyisocyanates, there can be mentioned: linear or branched aliphatic polyisocyanates such as hexamethylene diisocyanate, lysine diisocyanate, and lysine triisocyanate; alicyclic polyisocyanates such as norbornane diisocyanate, isophorone diisocyanate, methylenebis(4-cyclohexyl isocyanate), 1,3-bis(isocyanatomethyl)cyclohexane, 2-methyl-1,3-diisocyanatocyclohexane, and 2-methyl-1,5-diisocyanatocyclohexane. In addition, as the above-mentioned aliphatic polyisocyanate, a trimer obtained by trimerizing the above-mentioned linear or branched aliphatic polyisocyanate or alicyclic polyisocyanate can also be used. In addition, these aliphatic polyisocyanates can be used alone or in combination of two or more in any ratio.

[0139] Among the above-mentioned aliphatic polyisocyanates, hexamethylene diisocyanate as a diisocyanate of a straight-chain aliphatic hydrocarbon, norbornane diisocyanate as an alicyclic diisocyanate, and isophorone diisocyanate are preferred in order to improve the scratch resistance of the hard coat layer.

[0140] The (meth)acrylate is a compound having a hydroxyl group and a (meth)acryloyl group. Specific examples of the (meth)acrylate include mono(meth)acrylates of diols such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 1,5-pentanediol mono(meth)acrylate, 1,6-hexanediol mono(meth)acrylate, neopentyl glycol mono(meth)acrylate, and hydroxypivalate neopentyl glycol mono(meth)acrylate; mono(meth)acrylates or di(meth)acrylates of triols such as trimethylolpropane di(meth)acrylate, ethylene oxide (EO)-modified trimethylolpropane (meth)acrylate, propylene oxide (PO)-modified trimethylolpropane di(meth)acrylate, glycerol di(meth)acrylate, and bis(2-(meth)acryloyloxyethyl)hydroxyethyl isocyanurate; and mono(meth)acrylates having hydroxyl groups obtained by modifying a part of these alcoholic hydroxyl groups with ε-caprolactone. esters and di(meth)acrylates; compounds having a monofunctional hydroxyl group and a trifunctional or higher (meth)acryloyl group, such as pentaerythritol tri(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, and dipentaerythritol penta(meth)acrylate, or polyfunctional (meth)acrylates having a hydroxyl group obtained by further modifying the compound with ε-caprolactone; (meth)acrylates having an oxyalkylene chain, such as dipropylene glycol mono(meth)acrylate, diethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, and polyethylene glycol mono(meth)acrylate; (meth)acrylates having an oxyalkylene chain of a block structure, such as polyethylene glycol-polypropylene glycol mono(meth)acrylate, and polyoxybutylene-polyoxypropylene mono(meth)acrylate; (meth)acrylates having an oxyalkylene chain of a random structure, such as poly(ethylene glycol-tetramethylene glycol) mono(meth)acrylate and poly(propylene glycol-tetramethylene glycol) mono(meth)acrylate. These (meth)acrylates may be used alone or in combination of two or more in any ratio.

[0141] In the above-mentioned polyurethane (meth) acrylate, from the viewpoint of improving the scratch resistance of the cured coating film (hard coating) of the composition containing the active energy ray curable resin, it is preferred to have four or more (meth) acryloyl groups in one molecule. Since the above-mentioned polyurethane (meth) acrylate has four or more (meth) acryloyl groups in one molecule, as the above-mentioned (meth) acrylate, it is preferred to have two or more (meth) acryloyl groups in one molecule. As such (meth) acrylate, for example: trimethylolpropane di(meth) acrylate, ethylene oxide modified trimethylolpropane di(meth) acrylate, propylene oxide modified trimethylolpropane di(meth) acrylate, glycerol di(meth) acrylate, bis(2-(meth) acryloyloxyethyl) hydroxyethyl isocyanurate, pentaerythritol tri(meth) acrylate, ditrimethylolpropane tri(meth) acrylate, dipentaerythritol penta(meth) acrylate. Relative to one of the above-mentioned aliphatic polyisocyanates, these (meth) acrylates can be used one or more. Among these (meth)acrylates, pentaerythritol tri(meth)acrylate and dipentaerythritol penta(meth)acrylate are preferred from the viewpoint of improving the scratch resistance of the hard coat layer.

[0142] The composition for forming the hard coating layer may contain a solvent for dissolving or dispersing the active energy ray-curable resin. Examples of the solvent include alcohols such as methanol, ethanol, isopropanol, n-butanol, and isobutanol; glycols and glycol derivatives such as ethylene glycol, ethylene glycol monobutyl ether, ethylene glycol monoethyl acetate, diethylene glycol, diethylene glycol monobutyl ether, and diacetone glycol; aromatic hydrocarbons such as toluene and xylene; aliphatic hydrocarbons such as n-hexane and n-heptane; esters such as ethyl acetate and butyl acetate; ketones such as methyl ethyl ketone and methyl isobutyl ketone; oximes such as methyl ethyl ketoxime; and combinations of two or more of these.

[0143] When the active energy ray-curable resin is cured by ultraviolet rays, the composition for forming the hard coat layer may further contain a photopolymerization initiator.

[0144] When anti-glare property is imparted to the hard coat, it is preferred to control the concavo-convex shape of the hard coat surface by mixing particles in the composition for forming the hard coat. As examples of the particles used, in addition to the particles exemplified as particles C, aluminum oxide particles, zirconium oxide particles, titanium dioxide particles, tin oxide particles, antimony-doped tin oxide (ATO) particles, zinc oxide particles can also be cited. From the viewpoint of improving anti-glare property and scratch resistance at the same time, it is usually preferred to use inorganic particles with a hardness higher than that of organic particles.

[0145] The average particle size of the particles is preferably 1 nm to 2.0 μm, more preferably 100 nm to 2.0 μm.

[0146] The concavoconvex shape of the hard coat surface preferably satisfies any of the following formulas: Here, the average inclination angle of the concavoconvex shape is θa, the skewness of the concavoconvex structure is Sk, the arithmetic mean roughness is Ra, and the ten-point average roughness of the concavoconvex shape is Rz.

[0147] 0.01°≤θa≤0.10°

[0148] |Sk|≤0.5

[0149] 0.02μm≤Ra≤0.10μm

[0150] Rz<0.5μm

[0151] From the viewpoint of imparting antistatic properties to the hard coat layer, the composition for forming the hard coat layer may contain an antistatic agent. Examples of the antistatic agent include conductive particles such as tin oxide particles and ATO particles; conductive polymers such as polythiophene; and surfactants.

[0152] From the viewpoint of imparting low reflectivity to the hard coating layer, the composition for forming the hard coating layer preferably comprises: low refractive index particles such as hollow silica and magnesium fluoride; fluorine-based resin as a low refractive index resin; and / or a fluorine-based resin containing silica or magnesium fluoride. The refractive index of the hard coating layer comprising these is 1.45 or less, and particularly preferably 1.42 or less. The lower limit of the refractive index is not particularly limited, and can be, for example, 1.00 or more.

[0153] The composition for forming the hard coat layer may contain various additives (for example, a polymerization inhibitor, an antioxidant, an ultraviolet absorber, a light stabilizer, a defoaming agent, and a leveling agent) in addition to the active energy ray-curable resin and the above-mentioned components.

[0154] The thickness of the hard coat layer is preferably 3 μm or more and 20 μm or less, and more preferably 5 μm or more and 13 μm or less.

[0155] (Method for producing film with hard coat layer)

[0156] The method for producing a film with a hard coating layer is arbitrary and can be produced by a conventionally known method. As an example of a method for producing a film with a hard coating layer, there can be cited a method of performing the following steps: (1) preparing the above-mentioned laminated film comprising layer (a) and layer (b), (2) then applying a composition to form a hard coating layer on the laminated film, and forming a coating layer on the laminated film, (3) then, as required, performing a drying step for drying the coating layer and / or a curing step for curing the coating layer as required.

[0157] Example

[0158] The present invention will be described in detail below with reference to the following examples, but the present invention is not limited to the following examples and can be implemented with any modifications without departing from the scope of the claims and their equivalents.

[0159] In the following description, "%" and "parts" indicating amounts are based on weight unless otherwise specified. In addition, the operations described below are performed under normal temperature and pressure conditions unless otherwise specified.

[0160] [Evaluation method]

[0161] (Thickness of each layer of the film)

[0162] The film was sliced ​​into 0.05 μm thick slices using a microtome ("RV-240" manufactured by Yamato Koki Co., Ltd.), and the cross-section was observed under a microscope to measure the thickness of each layer.

[0163] (Glass transition temperature of resin)

[0164] The glass transition temperature of the resin was measured by differential scanning calorimetry using "DSC7020" manufactured by Hitachi, Ltd. The measurement was performed under a nitrogen atmosphere at a heating rate of 20° C. / min and a holding time of 30 min.

[0165] (Refractive Index)

[0166] The refractive index of the resin or microparticles is measured by the Baker method (JIS K7142). The refractive index is measured by immersing the resin particles or microparticles in a liquid with a known refractive index to confirm the outline of the resin particles or microparticles. As the light source of the microscope, sodium D line with a wavelength of 589nm is used as monochromatic light.

[0167] (Number average particle size of microparticles)

[0168] The number average particle size of the fine particles is measured by the following method.

[0169] A water slurry having a fine particle concentration of 2% by weight was prepared, and the slurry was measured by a laser diffraction scattering method using "LMS-3000" manufactured by Shinshin Enterprise Co., Ltd.

[0170] (Static friction coefficient of film)

[0171] The static friction coefficient of the film obtained in each example was measured using a friction tester ("TR-2" manufactured by Toyo Seiki Seisaku-sho Co., Ltd.) in accordance with JIS K7125. The measurement was performed under the conditions of a test piece size of 140 mm × 65 mm, a load of 1 kg, and a speed of 500 mm / min. The smaller the static friction coefficient, the greater the sliding property of the film.

[0172] (UV transmittance of film)

[0173] The light transmittance at a wavelength of 380 nm was measured using a spectrophotometer ("V-7200DS" manufactured by JASCO Corporation).

[0174] (Measurement of internal haze)

[0175] In a quartz cell having a height of 55 mm, a length of 40 mm, and a width of 14 mm, a zinc bromide aqueous solution (refractive index: 1.53) prepared by diluting zinc bromide with pure water was added.

[0176] A quartz cell was set in a haze meter ("NDH7000" manufactured by Nippon Denshoku Co., Ltd.), and the haze was measured and zero-point calibration was performed.

[0177] Next, the film obtained in each example was cut into a rectangular shape, and the cut film piece was inserted into the above-mentioned quartz cell. The quartz cell with the film piece inserted was set in a haze meter ("NDH7000" manufactured by Nippon Denshoku Co., Ltd.), and the internal haze of the film was measured.

[0178] (Impact strength of film)

[0179] According to JIS K7124-1, a 5.5g spherical hammer is used to measure the energy required to break 50% of the number of film pieces (50% breaking energy). The greater the 50% breaking energy, the greater the impact strength of the film. It is predicted that the greater the impact strength of the film, the more the breakage during the transport of the film can be suppressed.

[0180] [Example 1]

[0181] (Preparation of Materials for Layer (a))

[0182] 100 parts by weight of "ZEONOR 1600" (glass transition temperature 160°C, refractive index 1.53) manufactured by Zeon Co., Ltd. as resin A and 5 parts by weight of a UV absorber ("ADK STAB LA-31" (2,2'-methylenebis[6-(2H-benzotriazole-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol] manufactured by Adecco Co., Ltd.) were supplied to a co-rotating twin-screw kneader ("HK-25D" manufactured by PACCAR Co., Ltd., Φ=25 mm, L / D=41) and kneaded at a kneading temperature of 280°C to obtain resin (a) for layer (a). "ZEONOR 1600" is a resin containing an alicyclic structure-containing polymer (norbornene-based polymer). "ADK STAB LA-31" is a benzotriazole-based UV absorber.

[0183] (Preparation of Materials for Layer (b1) and Layer (b2))

[0184] 100 parts by weight of "ZEONOR 1600" manufactured by Zeon Co., Ltd. as resin B (glass transition temperature 160°C, refractive index 1.53) and 4 parts by weight of polymer beads "TECHPOLYMER" manufactured by Sekisui Chemicals Co., Ltd. (number average particle size 0.5 μm, refractive index 1.53) as fine particles C were supplied to a co-rotating twin-screw kneader ("HK-25D" manufactured by PACCAR Co., Ltd., Φ=25 mm, L / D=41) and kneaded at a kneading temperature of 280°C to obtain resin (b) for layer (b1) and layer (b2). "TECHPOLYMER" is fine particles of a cross-linked copolymer of methyl methacrylate and styrene.

[0185] (Manufacturing of laminated film)

[0186] Three types of three-layer multilayer extruders (manufactured by Collin) with feed heads are used to manufacture laminated films by coextrusion. The feed head has a structure capable of forming a laminate having a three-layer structure of layer (b1) / layer (a) / layer (b2). Resin (a) is used as the resin of layer (a), and resin (b) is used as the resin of layer (b1) and layer (b2). The laminated molten resin is discharged from the die head of the extruder onto a cooling drum and cooled to obtain a laminated film having layer (b1), layer (a) and layer (b2) in sequence. The extrusion processing temperature is 285°C, and the temperature of the cooling drum is 118°C. The extrusion conditions are adjusted so that the thickness of layer (b1) and layer (b2) is 2μm, the thickness of layer (a) is 36μm, and the total thickness of the laminated film is 40μm.

[0187] [Example 2]

[0188] A laminated film was produced in the same manner as in Example 1 except that the following matters were changed.

[0189] In (Preparation of Materials for Layer (b1) and Layer (b2)), the polymer beads "TECHPOLYMER" were used in an amount of 8 parts by weight.

[0190] [Example 3]

[0191] A laminated film was produced in the same manner as in Example 1 except that the following matters were changed.

[0192] In (Preparation of materials for layer (b1) and layer (b2)), 10 parts by weight of silica particles ("QSG-100" manufactured by Shin-Etsu Chemical Co., Ltd., number average particle size 0.1 μm, refractive index 1.43) were used instead of 4 parts by weight of polymer beads "TECHPOLYMER".

[0193] [Example 4]

[0194] A laminated film was produced in the same manner as in Example 1 except that the following matters were changed.

[0195] In (Preparation of materials for layer (b1) and layer (b2)), 10 parts by weight of silica particles ("QSG-170" manufactured by Shin-Etsu Chemical Co., Ltd., number average particle size 0.17 μm, refractive index 1.43) were used instead of 4 parts by weight of polymer beads "TECHPOLYMER".

[0196] [Comparative Example 1]

[0197] A laminated film was produced in the same manner as in Example 1 except that the following matters were changed.

[0198] In (Preparation of materials for layer (b1) and layer (b2)), polymer beads "TECHPOLYMER" were not used.

[0199] [Comparative Example 2]

[0200] A laminated film was produced in the same manner as in Example 1 except that the following matters were changed.

[0201] In (Preparation of Materials for Layer (b1) and Layer (b2)), the polymer beads "TECHPOLYMER" were used in an amount of 1 part by weight.

[0202] In (Production of Laminated Film), extrusion conditions were adjusted so that the thickness of each layer (b1) and layer (b2) was 10 μm, the thickness of layer (a) was 20 μm, and the total thickness of the laminated film was 40 μm.

[0203] [Comparative Example 3]

[0204] A laminated film was produced in the same manner as in Example 1 except that the following matters were changed.

[0205] In (Preparation of Materials for Layer (b1) and Layer (b2)), the polymer beads "TECHPOLYMER" were used in an amount of 8 parts by weight.

[0206] In (Production of Laminated Film), extrusion conditions were adjusted so that the thickness of each layer (b1) and layer (b2) was 10 μm, the thickness of layer (a) was 20 μm, and the total thickness of the laminated film was 40 μm.

[0207] [Comparative Example 4]

[0208] A laminated film was produced in the same manner as in Example 1 except that the following matters were changed.

[0209] In (Preparation of Materials for Layer (b1) and Layer (b2)), the polymer beads "TECHPOLYMER" were used in an amount of 8 parts by weight.

[0210] In (Production of Laminated Film), extrusion conditions were adjusted so that the thicknesses of layer (b1) and layer (b2) were 7 μm, the thickness of layer (a) was 26 μm, and the total thickness of the laminated film was 40 μm.

[0211] [Comparative Example 5]

[0212] A laminated film was produced in the same manner as in Example 1 except that the following matters were changed.

[0213] In (Preparation of materials for layer (b1) and layer (b2)), 6 parts by weight of silica particles ("QSG-030" manufactured by Shin-Etsu Chemical Co., Ltd., number average particle size 0.03 μm, refractive index 1.43) were used instead of 4 parts by weight of polymer beads "TECHPOLYMER".

[0214] [Comparative Example 6]

[0215] A laminated film was produced in the same manner as in Example 1 except that the following matters were changed.

[0216] In (Preparation of materials for layer (b1) and layer (b2)), 0.5 parts by weight of silica particles (manufactured by DIC Corporation, number average particle size 0.30 μm, refractive index 1.43) were used instead of 4 parts by weight of polymer beads "TECHPOLYMER".

[0217] [Comparative Example 7]

[0218] A laminated film was produced in the same manner as in Example 1 except that the following matters were changed.

[0219] In (Preparation of materials for layer (b1) and layer (b2)), 2.5 parts by weight of silica particles (manufactured by DIC Corporation, number average particle size 0.30 μm, refractive index 1.43) were used instead of 4 parts by weight of polymer beads "TECHPOLYMER".

[0220] [Comparative Example 8]

[0221] A laminated film was produced in the same manner as in Example 1 except that the following matters were changed.

[0222] ·In (Preparation of materials for layer (b1) and layer (b2)), 2 parts by weight of polymer beads "TECHPOLYMER" manufactured by Sekisui Chemicals Co., Ltd. (number average particle size 0.72 μm, refractive index 1.53) are used instead of 4 parts by weight of polymer beads "TECHPOLYMER" (number average particle size 0.5 μm, refractive index 1.53).

[0223] In (Production of Laminated Film), extrusion conditions were adjusted so that the thicknesses of layer (b1) and layer (b2) were 8 μm, the thickness of layer (a) was 16 μm, and the total thickness of the laminated film was 32 μm.

[0224] [result]

[0225] The results are shown in the table below.

[0226] The abbreviations in the following table have the following meanings.

[0227] "ZNR1600": "ZEONOR1600" manufactured by Japan Zeon Co., Ltd.

[0228] "LA-31": ADK STAB LA-31 manufactured by ADK Co., Ltd.

[0229] "nb": refractive index of resin B

[0230] "nc": refractive index of particle C

[0231] In the evaluation of the static friction coefficient in the following table, “cannot be measured” means that the static friction coefficient could not be determined because the static friction coefficient was larger than the measurable range in the measurement conditions.

[0232] [Table 1]

[0233] Table 1

[0234]

[0235] [Table 2]

[0236] Table 2

[0237]

[0238] [Table 3]

[0239] Table 3

[0240]

[0241] From the above results, we can know the following things.

[0242] The laminated film of Comparative Example 1 in which the layer (b1) and the layer (b2) did not contain the fine particles C had poor slidability, small 50% fracture energy, and insufficient impact strength of the film.

[0243] The laminated films of Comparative Examples 2 to 4 and 8, in which the thickness of the layer (b1) and the layer (b2) were respectively larger than 5 μm, had small 50% fracture energy and insufficient impact strength of the films.

[0244] The laminated films of Comparative Examples 2, 6, 7, and 8, in which the weight ratio of the fine particles C was less than 3% by weight, had poor slidability.

[0245] The laminated film of Comparative Example 5 in which the number average particle size of the fine particles C was less than 0.10 μm had poor slidability, small 50% fracture energy, and insufficient impact strength of the film.

[0246] The laminated film of the example was excellent in slidability, had a high 50% breaking energy of 0.03 J or more, and had sufficient impact strength. In addition, the internal haze was less than 0.7%, which was good.

[0247] Description of Reference Numerals

[0248] 100: Laminated film

[0249] 110: Layer(a)

[0250] 110U: Surface

[0251] 120: Layer (b)

[0252] 120U: Surface

[0253] 200: Laminated film

[0254] 210: Layer(a)

[0255] 210U: Surface

[0256] 210D: Face

[0257] 221: Layer (b)

[0258] 221U: Surface

[0259] 222: Layer (b)

[0260] 222D: Face

Claims

1. A laminated film comprising a layer containing a resin A and a layer containing a resin B and fine particles C, wherein the resin A contains an alicyclic structure-containing polymer and the resin B contains an alicyclic structure-containing polymer, The layer containing the resin B and the fine particles C is located on at least one outermost surface of the laminated film and has a thickness of 1 μm to 5 μm. The ratio of the thickness of the layer containing resin B and fine particles C to the thickness of the layer containing resin A, i.e., the thickness of the layer containing resin B and fine particles C / the thickness of the layer containing resin A is 0.04 or more and 0.11 or less, The number average particle size of the microparticles C is 0.10 μm or more and 0.80 μm or less, The weight ratio of the fine particles C to the resin B in the layer including the resin B and the fine particles C is 3% by weight or more and 10% by weight or less.

2. The laminated film according to claim 1, wherein The microparticles C are microparticles of a cross-linked copolymer of methyl methacrylate and styrene.

3. The laminated film according to claim 1, wherein The microparticles C are microparticles containing alicyclic cross-linked polymers.

4. The laminated film according to any one of claims 1 to 3, wherein The refractive index nb of the resin B and the refractive index nc of the microparticles C satisfy the following formula (1): |nb-nc|≤0.03(1).

5. The laminated film according to claim 1, wherein The microparticles C are microparticles of silicon dioxide.

6. The laminated film according to any one of claims 1 to 3 and 5, wherein The layer containing resin A contains an ultraviolet absorber. 7 . A film with a hard coating layer, comprising the laminated film according to claim 1 and a hard coating layer provided on the laminated film.

Citation Information

Patent Citations

  • Polymer resin laminated material containing alicyclic structure

    JP2002321302A

  • Optical laminate

    JP2005181615A

  • Laminated film and method of manufacturing the same, and polarization plate

    JP2011011394A

  • Method of manufacturing optical laminate

    JP2015161910A

  • Light diffusing film, polarizing plate, image display device and production method of light diffusing film

    US20120105769A1