A compatibilizer for PP / PS alloy
By using PP/PS alloys with combinations of styrene-butadiene block copolymers and ethylene-butene elastomers and combining auxiliary agents, the problem of poor compatibility of PP/PS alloys is solved, and the problem of it is significantly improved. Mechanical properties and impact resistance, suitable for a variety of industrial applications.
Patent Information
- Application Number
- CN202211049932.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-30
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-08-30
AI Technical Summary
The poor compatibility of PP/PS alloys leads to poor mechanical properties and easy peeling, which makes it difficult to meet the industry's demand for materials.
Styrene-butadiene block copolymer (SBS) is used as the first main material, combined with ethylene-butene elastomer (POE) or other elastomer as the second main material, and combined with graft modifier and reagent , antioxidants, lubricants and other auxiliary materials are blended into the extruder to prepare compatible agents to improve the toughness and impact resistance of PP/PS alloys.
It significantly improves the toughness and impact resistance of PP/PS alloys, improves the interface bonding performance, expands its application range, and is suitable for travel boxes, brackets, building materials and other fields.
Smart Images

Figure BDA0003823393280000031 
Figure BDA0003823393280000032 
Figure BDA0003823393280000041
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a PP / PS alloy compatibilizer used in the fields of suitcases, brackets, building materials, electrical appliances, etc. Background Art
[0002] At present, the research and development of organic alloys is a relatively active research field in organic polymer research. The research of organic alloys can combine the favorable properties of different polymer materials and expand new application fields, thereby meeting the actual industrial demand for materials. Compared with the research and development of polymers, the research and development of organic alloys has low research and development costs, low risks, and low expenses. In addition, organic alloys have excellent performance and can often develop properties that neither homopolymer has.
[0003] At present, the commonly used compatibilizer components in PP / PS alloys are SBS, Vistamaxx (PP-based elastomer), POE, etc. SBS is a styrene-butadiene-styrene block copolymer, which is a material with large output and low cost among SBCs, which is conducive to industrial production. It has the properties of both plastics and rubber and can improve the impact resistance of organic alloys. Vistamaxx is a commonly used propylene-based elastomer with good coating properties, good compatibility with various materials and excellent processability. POE is a copolymer of ethylene and octene. It is a thermoplastic elastomer with excellent properties and is widely used in nylon (PA) and polypropylene (PP) polymer materials.
[0004] PP / PS alloy is mainly composed of PP / PS blend modification, but the compatibility between the two is poor. It is difficult to disperse them in each other's components when they are directly melt-blended. The dispersed phase of the blend formed is relatively rough, has poor mechanical properties, and is more prone to peeling. Therefore, solving the compatibility and interfacial adhesion between PP and PS is the key to the preparation of PP / PS alloy. Summary of the invention
[0005] In order to overcome the shortcomings of the prior art, the inventors have discovered through extensive research that styrene-butadiene block copolymer (SBS) can effectively increase the toughness and impact resistance of PP / PS alloys and reduce peeling. It can not only increase the interfacial bonding performance of PP / PS alloys, but also increase the toughness and impact resistance of the alloy, and has obvious price advantages.
[0006] To this end, the object of the present invention is to provide a compatibilizer for PP / PS alloy, which is composed of 90 to 100 parts by weight of a main material and 0 to 10 parts by weight of an auxiliary material; wherein:
[0007] The main material comprises at least 50 parts by weight of a first main material component and at least 20 parts by weight of a second main material component; the first main material component is a styrene-butadiene-styrene copolymer, and the second main material component is an elastomer; specifically, the content of the second main material component is less than or equal to the content of the first main material component;
[0008] The auxiliary materials include a grafting modifier, a co-reactant, an initiator, an antioxidant, a lubricant, methyl silicone oil, and linear low-density polyethylene powder (LLDPE powder).
[0009] Furthermore, in a preferred embodiment, the first main ingredient component comprises 50 to 80 parts by weight of styrene-butadiene-styrene block copolymer, the second main ingredient component comprises 20 to 50 parts by weight of a second main ingredient component, and the second main ingredient component is selected from one or more of ethylene-butene elastomer (POE), Vistamaxx (propylene-based elastomer), hydrogenated styrene-butadiene block copolymer (SEBS), metallocene (mPE) or a variety of elastomer compound copolymers.
[0010] Further, in a preferred embodiment, the graft modifier is selected from one or more of acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, crotonic acid, citraconic acid, maleic anhydride (MAT), itaconic anhydride, crotonic anhydride and citraconic anhydride.
[0011] Furthermore, in a preferred embodiment, the co-reactant is a monoolefin monomer selected from one or both of styrene (St) and divinylbenzene (DVB).
[0012] Further, in a preferred embodiment, the initiator is a peroxide initiator, selected from one or more of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane (DTBH), dicumyl peroxide (DCP) and dibenzoyl peroxide (BPO).
[0013] Furthermore, in a preferred embodiment, the antioxidant is selected from one or more of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (antioxidant 1010), tris(2,4-di-tert-butyl)phenyl phosphite antioxidant 168), β(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, and 2,6-di-tert-butyl-p-cresol.
[0014] Furthermore, in a preferred embodiment, the lubricant is selected from one or more of pentaerythritol stearate (PETS), silicone powder, and polyethylene wax.
[0015] Further, in a preferred embodiment, the following components are included by weight:
[0016]
[0017] Further, in a preferred embodiment, the following components are included by weight:
[0018]
[0019]
[0020] 2 to 7 parts of low-density polyethylene powder; specifically, by weight, comprising the following components:
[0021]
[0022] In some preferred embodiments, specifically, the following components are included by weight:
[0023]
[0024] Furthermore, in a preferred embodiment, the PP / PS alloy is selected from one or more polymer materials of general-purpose polystyrene, high-impact polystyrene, polypropylene, organic alloys and mixtures thereof.
[0025] In another aspect, the present invention provides a method for preparing a compatibilizer for PP / PS alloy, comprising blending a main material and an auxiliary material in an extruder to obtain the compatibilizer.
[0026] Furthermore, in a preferred embodiment, the extruder is a twin-screw extruder.
[0027] Furthermore, in a preferred embodiment, when methyl silicone oil is added to the auxiliary material components, the methyl silicone oil is first mixed with the main material until the surface is wetted and then mixed with other auxiliary material components.
[0028] On the other hand, the present invention also provides the above PP / PS alloy material, wherein the PP / PS alloy material is prepared with the participation of the above compatibilizer.
[0029] The present invention has the following beneficial effects:
[0030] 1. The present invention uses styrene-butadiene block copolymer as the first main material, elastomeric material as the second main material, and auxiliary materials to obtain the PP / PS alloy compatibilizer, which is used for PP / PS alloy materials. Compared with PP and PS materials, the PP / PS alloy material has better toughness and impact resistance and has a broader application market;
[0031] 2. The PP / PS alloy compatibilizer of the present invention can increase the toughness and impact resistance of the product, and effectively improve the poor compatibility problem in the PP / PS system, improve the interface bonding performance, and meet industrial needs;
[0032] 3. The PP / PS alloy compatibilizer of the present invention can be used in the fields of suitcases, brackets, building materials, electrical appliances, etc., including but not limited to PP / PS alloy materials. DETAILED DESCRIPTION
[0033] The experimental methods in the following examples are conventional methods unless otherwise specified. The raw materials involved in the following examples are common commercial products and can be purchased from the market unless otherwise specified; the detection methods are conventional detection methods unless otherwise specified.
[0034] The compatibilizer of the present invention comprises a main ingredient and an auxiliary ingredient.
[0035] Main material: comprising a first main material component, the first main material component is styrene-butadiene-styrene block copolymer (SBS), and its content can be 50, 55, 60, 65, 70, 75, 80 parts by weight (calculated by weight).
[0036] In the present invention, the content of SBS is preferably 50 to 80 parts by weight, more preferably 55 to 75 parts by weight, particularly preferably 60 to 65 parts by weight.
[0037] In addition to the above-mentioned first main ingredient component, the compatibilizer according to the present invention may also include a second main ingredient component, which may be an elastomeric substance commonly used in existing industrial production, such as: ethylene-propylene copolymer (POE); it may also be Vistamaxx (propylene-based elastomer), hydrogenated styrene-butadiene block copolymer, metallocene or a variety of elastomer compound copolymers.
[0038] The content of the second main ingredient component according to the present invention can be 20, 25, 30, 35, 40, 45, 50 parts by weight (parts by weight).
[0039] In the present invention, the content of the second main ingredient component is preferably 20 to 50 parts by weight, more preferably 30 to 40 parts by weight, and particularly preferably 35 to 40 parts by weight.
[0040] According to the present invention, the content of the second main ingredient component is less than or equal to the content of the first main ingredient component.
[0041] Auxiliary materials: including grafting modifier, co-reactant, initiator, lubricant, antioxidant, LLDPE powder and methyl silicone oil.
[0042] According to the present invention, the graft modifier can be selected from acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, crotonic acid, citraconic acid, maleic anhydride, itaconic anhydride, crotonic anhydride and citraconic anhydride; preferably one or more of maleic anhydride, itaconic anhydride, crotonic anhydride and citraconic anhydride; particularly preferably maleic anhydride (MAH).
[0043] The amount of the graft modifier according to the present invention can be 0, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2 parts by weight (by weight). The amount of the graft modifier is preferably 0 or 0.5 to 1.0 parts by weight, more preferably 0 or 0.6 to 0.8 parts by weight.
[0044] According to the present invention, the co-reactant is a monoolefin monomer, preferably selected from styrene (St) and divinylbenzene (DVB). The amount of the co-reactant according to the present invention can be 0, 0.1, 0.2, 0.3, 0.4, 0.5 parts by weight, and the content of the co-reactant is preferably 0 to 0.5 parts by weight, more preferably 0 or 0.3 to 0.4 parts by weight (by weight).
[0045] According to the present invention, the initiator is a peroxide initiator, preferably selected from 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane (DTBH), dicumyl peroxide (DCP) and dibenzoyl peroxide (BPO). The amount of the initiator according to the present invention can be 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10 parts by weight (by weight). The amount of the initiator is preferably 0 to 0.07 parts by weight, more preferably 0 to 0.05 parts by weight, and particularly preferably 0 or 0.2 to 0.5 parts by weight.
[0046] In addition, the auxiliary materials according to the present invention may also include LLDPE powder and silicone oil. LLDPE powder is mainly used for the preparation of auxiliary materials, which can dilute MAH and initiator, and the product stability is better when mixed with the main material. Silicone oil (preferably methyl silicone oil) can be mixed with the main material until its surface is wetted and then mixed with other granular materials.
[0047] According to the present invention, the amount of silicone oil used may be 0.1 to 0.5 parts by weight, preferably 0.2 to 0.4 parts by weight, and particularly preferably 0.3 parts by weight.
[0048] According to the present invention, the amount of LLDPE powder used is 0 to 10.0 parts by weight, preferably 0 to 7.0 parts by weight, and particularly preferably 0 or 3.5 to 6 parts by weight.
[0049] In the present invention, the graft modifier, co-reactant, initiator, antioxidant, lubricant and LLDPE powder may not be added, and the four auxiliary material components of the graft modifier, co-reactant, initiator and LLDPE powder should be added or not added at the same time in the test plan.
[0050] In another aspect, the present invention provides a method for preparing a compatibilizer for PP / PS alloy, comprising blending a main material and an auxiliary material in an extruder to obtain the compatibilizer; the extruder is a twin-screw extruder. When the compatibilizer includes an auxiliary material component to which silicone oil is added, the silicone oil should be first mixed with the main material until the surface is wetted, and then mixed with other auxiliary material components.
[0051] The compatibilizer according to the present invention can be used for PP / PS alloy materials, and the alloy materials can be polymer materials such as polypropylene (PP), general-purpose polypropylene (GPPS), high-impact polystyrene (HIPS), organic alloys and mixtures thereof. For example, white pollution often occurs in waste industrial products and domestic garbage. A large amount of PP and PS resin materials in waste resin materials can be purified and reprocessed as raw materials to make PP / PS alloys, which are used in the manufacture of some relatively low-end life products, including cement formwork for construction sites. Based on the needs of reducing costs and performance, some lightweight household appliances that require lower density and certain mechanical properties, such as suitcase pull rods, selfie sticks, crutches, brackets, etc., also need to use the PP / PS alloy and its compatibilizer.
[0052] The present invention is described in further detail below in conjunction with embodiments:
[0053] Raw materials and equipment:
[0054] All raw materials used in the embodiments, for example: PP, SBS, SEBS, Vistamaxx, POE, mPE, GPPS, HIPS, GPPS, and modified materials of Ganzhou Nengzhiguang New Materials Co., Ltd.
[0055] The equipment used in the examples is as follows:
[0056] Twin-screw extruder, model HK26, purchased from Keya Machinery Co., Ltd.;
[0057] Injection molding machine, model MA900Ⅲ, purchased from Haitian Plastic Machinery Group Co., Ltd.;
[0058] The micro electronic universal testing machine, model CMT4204, was purchased from Meters Systems Co., Ltd.
[0059] The performance tests performed in the examples were performed as follows:
[0060] The tensile strength and elongation at break tests were carried out according to GB / T10470-1992, with sample size of 150×10×4mm and tensile rate of 50mm / min;
[0061] The flexural strength and flexural modulus tests were carried out according to GB / T3356-1996, with sample size of 80×10×4mm and tensile rate of 2mm / min;
[0062] The notched impact strength test was carried out according to GB / T1843-1996, the sample size was 80×10×4mm, and the notch depth was 2mm.
[0063] Preparation method of compatibilizer:
[0064] According to the proportions of the components of Comparative Example 1 and Examples 1-5 shown in Table 1, the main material components and the auxiliary material components were mixed and poured into a twin-screw extruder for blending, wherein the main speed of the extruder was 330 r / min and the feeding speed was 20 Hz. After blending, extrusion and pelletizing were performed for subsequent use.
[0065] Table 1: Proportions of the main ingredients and auxiliary ingredients of the compatibilizer (unit: parts)
[0066]
[0067] Preparation of injection molded samples:
[0068] The sample proportions of injection molded parts of Comparative Examples 3-5 and Examples 6-10 are shown in Table 2. PP, HIPS, and GPPS were dried in a vacuum oven at 80°C for 2 hours, and then blended with 5 parts by weight of the compatibilizer prepared above at 30, 45, and 20 parts by weight, respectively, and poured into a twin-screw extruder. The process parameter settings of the extruder are shown in Table 3.
[0069] Table 2: Proportions of injection molded samples (unit: parts)
[0070]
[0071]
[0072] Table 3: Extruder process parameters for injection molded sample preparation
[0073]
[0074] The sample obtained from the extruder was dried in a dryer at 70°C for 2 hours. Finally, the dried material was poured into an injection molding machine and molded into an injection molded sample at a temperature of 190-210°C, using an injection pressure of 75MPa and a holding pressure of 75MPa. The injection molded sample was required to have neither skirt nor shrinkage.
[0075] Performance Test:
[0076] The injection molded samples of Comparative Examples 3-5 and Examples 6-10 prepared above were left to stand for more than 2 hours to avoid the influence of internal stress on the measurement. Then, the tensile strength, elongation at break, flexural strength, flexural modulus and impact strength were measured using a micro electronic universal testing machine. Each test data is the average value of three sets of parallel test results, and the results are shown in Table 4.
[0077] Table 4: Mechanical properties test results of injection molded samples
[0078]
[0079] From the above performance test results, it can be seen that the compatibilizer prepared by the present invention has excellent mechanical properties and impact resistance and excellent overall performance when used in alloy materials. In comparative example 3, without using a compatibilizer, the impact strength of the PP / PS alloy material without adding a compatibilizer is only 8.881 KJ / m 2 , tensile strength 15.18MPa, elongation at break 30.22%, which are worse than those of the present invention; in comparative examples 4 and 5, both SBS compounded Vistamaxx and SBS compounded POE have significantly improved tensile strength, elongation at break and impact strength after adding the compatibilizer, indicating that the main ingredient ratio of the present invention is reasonable; adding appropriate auxiliary materials can further improve the mechanical properties and impact resistance; in addition, the peeling phenomenon of the products using the compatibilizer of the present invention is improved.
[0080] Finally, it should be emphasized that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various changes and modifications. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
[0081] In addition, the numerical ranges expressed by endpoints herein include all values and endpoints contained in the range.
[0082] In addition, the preferred technical solutions according to the present invention can be combined with the basic technical solutions of the present invention alone or in any combination. All such combined technical solutions are included in the protection scope of the present invention.
Claims
1. A compatibilizer for PP / PS alloy, characterized in that: In parts by weight, the compatibilizer is composed of 92 parts by weight of main material and 8 parts by weight of auxiliary material; wherein, The main material comprises at least 50 parts by weight of a first main material component and at least 20 parts by weight of a second main material component; the first main material component is styrene-butadiene-styrene copolymer, and the second main material component is Vistamaxx; The auxiliary materials include a grafting modifier, a co-reactant, an initiator, an antioxidant, a lubricant, methyl silicone oil, and linear low-density polyethylene powder; The grafting modifier is maleic anhydride; The co-reactant is styrene; The initiator is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane; The antioxidant is a mixture of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and tris(2,4-di-tert-butyl)phenyl phosphite in a mass ratio of 1:1; The lubricant is a mixture of pentaerythritol stearate and silicone powder in a mass ratio of 5:
3.
2. The compatibilizer for PP / PS alloy according to claim 1, characterized in that: The first main material component comprises 50 to 80 parts by weight of styrene-butadiene-styrene block copolymer, and the second main material component comprises 20 to 50 parts by weight of Vistamaxx.
3. The compatibilizer for PP / PS alloy according to claim 1, characterized in that: By weight, it includes the following components: 50 to 80 parts of the first main ingredient component; 20 to 50 parts of the second main ingredient component; Graft modifier 0.5 to 1.0 part; 0.05 to 0.2 parts of co-reactant; Initiator 0.03 to 0.07 parts; Lubricant 0.3 to 0.5 parts; 0.3 to 0.5 parts of antioxidant; Methyl silicone oil 0.2 to 0.5 parts; 2 to 7 parts of low density polyethylene powder.
4. The compatibilizer for PP / PS alloy according to claim 1, characterized in that: The main raw material of the PP / PS alloy is a mixture of high-impact polystyrene and polypropylene.
5. A PP / PS alloy material, characterized in that: The PP / PS alloy material is prepared by the compatibilizer described in any one of claims 1 to 4.
Citation Information
Patent Citations
Modified polypropylene composite material of high gloss and low shrinkage and preparation method thereof
CN102250413A
In-situ compatibilization polyolefin / polystyrene alloy and preparation method and application thereof
CN102643484A
Phase solvent and its aplication in composite and preparation process of said composite
CN1560101A