A method for solving the uneven wall thickness stretching during the inflation process of hydrogen storage bottles
By setting up multiple independent heating air chambers and special algorithms during the blow molding of hydrogen cylinders, adjusting the heating degree of the air chamber, combined with the binomial distributed heating method of the spoiler rod, the problem of uneven stretching of the wall thickness of the hydrogen storage bottle is solved. , achieving improved wall thickness uniformity and production efficiency.
Patent Information
- Application Number
- CN202211055209.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-30
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-08-30
AI Technical Summary
The wall thickness stretching of the hydrogen storage bottle during blow molding is uneven, resulting in dangerous accidents that may occur during the vehicle driving. The conventional radial wall thickness adjustment cost is high and the service life is low, and the unstable material flow affects product quality. .
The hydrogen cylinder blow molding air ring with multiple independent heating air chambers is set up between the hydrogen cylinder tube blank exit mold and the mold, and the air outlet temperature and heating degree of the air chamber are adjusted through a special algorithm, combining the two spoiler rods The nickel distribution heating method is used to adjust the spacing between the air ring and the mold to achieve uniform stretching of the wall thickness.
Through multiple independent heating air chambers and algorithm-adjusted heating methods, the fluidity of the wall thickness position is improved, the uniformity of the wall thickness of the blow-molded product is achieved, the hot air interference is reduced, and the product quality and production efficiency are improved.
Smart Images

Figure CN115416261B_ABST
Abstract
Description
Technical field:
[0001] The invention belongs to the technical field of blow molding equipment, and more specifically relates to a method for solving the problem of uneven wall thickness stretching during the inflation process of a hydrogen storage bottle. Background technology:
[0002] After the liquid plastic is sprayed out, the wind force blown out by the machine is used to blow the plastic body to a mold cavity of a certain shape to make a product. This machine is called a blow molding machine.
[0003] There are two types of hydrogen storage bottles for new energy vehicles, metal and polymer. With the advancement of technology, polymer blow molding hydrogen storage bottles are becoming more and more widely used. However, the requirements for hydrogen storage bottles are different from other blow molding products, because there will inevitably be bumps and shocks during vehicle driving. Therefore, the wall thickness of hydrogen storage bottles is required to be uniform. Conventional rotational molding has a slightly uniform wall thickness but low production efficiency.
[0004] If the wall thickness of the hydrogen storage bottle used in new energy vehicles is uneven, dangerous accidents may occur due to uneven force during the vehicle's driving, when there are bumps and shocks.
[0005] Among them, hollow blow molding will inevitably cause uneven wall thickness due to different blowing and stretching ratios of various parts. This is because during hollow blow molding, the injected blank is round, which causes the blank to be flattened to a certain extent when the mold is closed. When it is blown by the blow needle, the asymmetry of the structure causes different blowing and stretching ratios of various parts, resulting in uneven wall thickness; conventional radial wall thickness adjustment is not only expensive and has a short service life, but also causes local deformation and unstable material flow, which will have a certain impact on product quality. Summary of the invention:
[0006] In order to solve the above problems and overcome the shortcomings of the prior art, the present invention provides a method for solving the problem of uneven wall thickness stretching during the inflation of a hydrogen storage bottle, which can effectively solve the problem of uneven wall thickness stretching during the inflation of a hydrogen storage bottle.
[0007] The specific technical solution of the present invention to solve the above technical problems is: a method for solving the uneven wall thickness stretching during the inflation of hydrogen storage bottles, comprising:
[0008] 1. Equipment connection and debugging;
[0009] The fixing ring of the hydrogen cylinder blow molding air ring is assembled and sleeved on the extension of the hydrogen cylinder tube blank ejection port, and fixed by bolts. The fixing ring is rotatably connected with the extension of the hydrogen cylinder tube blank ejection port, and the length of the adjusting screw is adjusted according to the process requirements to adjust the distance between the air ring body and the hydrogen cylinder tube blank ejection port;
[0010] 2. Preparation and wall thickness test of hydrogen storage bottles in the control group;
[0011] The fan and the heating rod on the air ring body are turned off, and the blank is extruded from the hydrogen bottle blank out of the die, and falls into the mold after passing through the hydrogen bottle blow molding air ring, and is blown after the mold is closed. The obtained hydrogen storage bottle is used as a control group for wall thickness detection, and the coordinates of the X-axis and Y-axis in the horizontal direction of the wall thickness are determined;
[0012] 3. Use the wall thickness test of the control group to obtain the difference of uneven wall thickness stretching and determine the coordinates of the X-axis and Y-axis of the wall thickness in the horizontal direction. According to the algorithm feedback, adjust the outlet air temperature of multiple independent air chambers in the air ring body; adjust the outlet air temperature of multiple independent air chambers in the air ring body by adjusting the temperature of the heating rod;
[0013] Fourth, determine the actual thickness and position of the blank by determining the coordinates of the X-axis and Y-axis in the horizontal direction of the wall thickness. Based on the algorithm in step three, rotate the fixed ring to adjust the degree of heating of the wind chamber at different positions of the blank, thereby improving the fluidity of the wall thickness position. During the blow molding process, the wall thickness position of the blank will be stretched larger than other positions of the blank, thereby achieving a more uniform wall thickness of the blow-molded product.
[0014] Furthermore, in step three, the wall thickness detection is used to obtain the difference of uneven wall thickness stretching, and the coordinates of the X-axis and Y-axis of the wall thickness in the horizontal direction are determined, and the air outlet temperatures of multiple independent air chambers in the air ring body are adjusted according to the algorithm feedback; the algorithm is: the standard thickness of the hydrogen storage bottle is 5mm;
[0015] When the thickness of the hydrogen storage bottle is 5mm, the outlet temperature of the corresponding independent air chamber is 210±0.5℃;
[0016] When the thickness of the hydrogen storage bottle is 6mm, the outlet temperature of the corresponding independent air chamber is 215±0.5℃;
[0017] When the thickness of the hydrogen storage bottle is 7mm, the outlet temperature of the corresponding independent air chamber is 218±0.5℃;
[0018] When the thickness of the hydrogen storage bottle is 8mm, the outlet temperature of the corresponding independent air chamber is 220±0.5℃;
[0019] When the thickness of the hydrogen storage bottle is less than 5 mm, the die gap should be adjusted to increase the overall thickness.
[0020] Furthermore, the hydrogen cylinder blow molding air ring is arranged between the hydrogen cylinder tube blank ejection die opening and the mold.
[0021] Furthermore, the blow-molded wind ring of the hydrogen cylinder includes a hollow annular wind ring body, a preset number of independent wind chambers are arranged in the wind ring body, an air outlet is arranged on the inner side of the wind chamber, an air inlet is arranged on the outer side of the wind chamber, a fan is connected to the air inlet, a heating rod and a spoiler rod are plugged in the wind chamber, and the heating temperatures of the preset number of independent wind chambers are different.
[0022] Furthermore, the spoiler rods are arranged on the outside of the heating rods, and the spoiler rods are arranged in a binomial distribution form.
[0023] Furthermore, the upper end surface of the air ring body is provided with an adjusting screw for adjusting the distance between the air ring body and the exit opening of the hydrogen bottle tube blank. The upper end of the adjusting screw is fixed on a fixing ring, which is composed of two semicircular rings. A slide groove is provided on the inner side wall of the fixing ring. The extension of the exit opening of the hydrogen bottle tube blank cooperates with the slide groove through a sliding connection.
[0024] Furthermore, the upper end surface of the fixing ring is also provided with inverted teeth, and the side wall of the hydrogen bottle tube blank leaving the die is provided with an elastic sheet that cooperates with the inverted teeth.
[0025] The beneficial effects of the present invention are:
[0026] The present invention creatively arranges a hydrogen cylinder blow molding air ring with multiple independent heating air chambers between the hydrogen cylinder tube blank exit die and the mold, and uses a special algorithm to adjust the heating degree of the air chambers on different positions of the blank, thereby improving the fluidity of the wall thickness position. During the blow molding process, the wall thickness position of the blank will be stretched larger than other positions of the blank, thereby achieving the purpose of more uniform wall thickness of the blow-molded product;
[0027] The inventive spoiler rod of the present invention is disposed on the outside of the heating rod and is arranged in a binomial distribution form. The principles of fluid mechanics and dynamics are utilized and combined with the principle of binomial distribution probability to concentrate the hot air in the middle. This heating method is relatively gentle and is conducive to positioning and centralized heating. At the same time, the hot air volume and temperature on both sides are relatively low, reducing the interference of different independent wind chambers.
[0028] The fixing ring creatively arranged in the present invention is rotatably connected with the extension of the hydrogen cylinder tube blank ejection outlet, and the length of the adjusting screw can be adjusted according to process requirements to adjust the distance between the air ring body and the hydrogen cylinder tube blank ejection outlet. The operation is convenient and adjustment is facilitated, and the stability is good. Description of the drawings:
[0029] Attached Figure 1 It is a schematic diagram of the present invention;
[0030] Attached Figure 2 It is a schematic diagram of the present invention without a fixing ring;
[0031] Attached Figure 3It is a cross-sectional schematic diagram of the present invention; in the accompanying drawings:
[0032] 1. Hydrogen cylinder tube blank exiting the die, 2. inverted teeth, 3. fan, 4. elastic sheet, 5. fixing ring, 6. heating rod, 7. spoiler rod, 8. adjusting screw, 9. air ring body, 10. air inlet, 11. air outlet, 12. slideway. Specific implementation method:
[0033] In the description of the present invention, specific details are only for a full understanding of the embodiments of the present invention, but those skilled in the art should know that the implementation of the present invention is not limited to these details. In addition, well-known structures and functions are not described or shown in detail to avoid blurring the key points of the embodiments of the present invention. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0034] Specific implementation of the present invention:
[0035] The hydrogen cylinder blow molding air ring is arranged between the hydrogen cylinder tube blank ejection port and the mold.
[0036] Furthermore, the blow-molded wind ring of the hydrogen cylinder includes a hollow annular wind ring body, a preset number of independent wind chambers are arranged in the wind ring body, an air outlet is arranged on the inner side of the wind chamber, an air inlet is arranged on the outer side of the wind chamber, a fan is connected to the air inlet, a heating rod and a spoiler rod are plugged in the wind chamber, and the heating temperatures of the preset number of independent wind chambers are different.
[0037] As a preferred embodiment of the present invention, the spoiler rod is arranged on the outside of the heating rod, and the spoiler rod can also be arranged in a binomial distribution form, aiming to arrange the spoiler rod in a binomial distribution form, utilizing the principles of fluid mechanics and dynamics, combined with the principle of binomial distribution probability, to concentrate the hot air more concentratedly in the middle. This heating method is relatively mild and is conducive to positioning and centralized heating. At the same time, the hot air volume and temperature on both sides are relatively low, reducing the interference of different independent wind chambers.
[0038] Furthermore, an adjusting screw for adjusting the distance between the air ring body and the ejection opening of the hydrogen bottle tube blank is provided on the upper end surface of the air ring body, and the upper end of the adjusting screw is fixed on the fixing ring, which is composed of two semicircular rings, and a slide groove is provided on the inner side wall of the fixing ring, and the extension of the ejection opening of the hydrogen bottle tube blank is matched with the slide groove through a sliding connection, and the upper end surface of the fixing ring is also provided with a reverse tooth, and the side wall of the ejection opening of the hydrogen bottle tube blank is provided with an elastic sheet matched with the reverse tooth, so as to enable the fixing ring to be rotatably connected and matched with the extension of the ejection opening of the hydrogen bottle tube blank, and the length of the adjusting screw can also be adjusted according to the process requirements to adjust the distance between the air ring body and the ejection opening of the hydrogen bottle tube blank, which is convenient to operate and facilitates adjustment, and has good stability;
[0039] When using, the specific operations are as follows:
[0040] 1. Equipment connection and debugging;
[0041] The fixing ring 5 of the blow molding air ring of the hydrogen cylinder is assembled and sleeved on the extension of the hydrogen cylinder tube blank ejection opening 1, the assembled fixing ring 5 is fixed by bolts, the fixing ring 5 is rotatably connected and matched with the extension of the hydrogen cylinder tube blank ejection opening 1, the length of the adjusting screw 8 is adjusted according to the process requirements, and the distance between the air ring body 9 and the hydrogen cylinder tube blank ejection opening 1 is adjusted;
[0042] Preparation and wall thickness testing of hydrogen storage bottles in control group 2;
[0043] The fan 3 and the heating rod 6 on the air ring body 9 are turned off, and the blank is extruded from the hydrogen bottle tube blank out of the die opening 1, and falls into the mold after passing through the hydrogen bottle blow molding air ring, and is blown after the mold is closed. The obtained hydrogen storage bottle is used as a control group for wall thickness detection; and the coordinates of the X-axis and Y-axis in the horizontal direction of the wall thickness are determined;
[0044] Third, the wall thickness detection is used to obtain the difference of uneven wall thickness stretching, and the coordinates of the X-axis and Y-axis of the wall thickness in the horizontal direction are determined, and the outlet air temperature of multiple independent air chambers in the air ring body 9 is adjusted according to the algorithm feedback; as an embodiment of the present invention, wherein: the standard thickness of the hydrogen storage bottle is selected to be 5mm;
[0045] When the thickness of the hydrogen storage bottle is 5mm, the outlet temperature of the corresponding independent air chamber is 210±0.5℃;
[0046] When the thickness of the hydrogen storage bottle is 6mm, the outlet temperature of the corresponding independent air chamber is 215±0.5℃;
[0047] When the thickness of the hydrogen storage bottle is 7mm, the outlet temperature of the corresponding independent air chamber is 218±0.5℃;
[0048] When the thickness of the hydrogen storage bottle is 8mm, the outlet temperature of the corresponding independent air chamber is 220±0.5℃;
[0049] When the thickness of the hydrogen storage bottle is less than 5 mm, the die gap should be adjusted to increase the overall thickness.
[0050] Fourth, according to the coordinates of the X-axis and Y-axis in the horizontal direction of the wall thickness, the actual thickness and position of the blank are determined. Based on the algorithm of step three, the fixed ring 5 is rotated to adjust the heating degree of the wind chamber to different positions of the blank, and the air outlet temperature of the wind chamber is adjusted according to the algorithm of step three, so as to improve the fluidity of the wall thickness position. During the blow molding process, the wall thickness position of the blank will be stretched larger than other positions of the blank, thereby achieving the purpose of more uniform wall thickness of the blow-molded product.
[0051] The principle is: a hydrogen cylinder blow molding air ring with multiple independent heating air chambers is set between the hydrogen cylinder tube exiting the die and the mold, and a special algorithm is used to adjust the heating degree of the air chamber to different positions of the billet, thereby improving the fluidity of the wall thickness position. During the blow molding process, the wall thickness position of the billet will be stretched larger than other positions of the billet, thereby achieving the purpose of more uniform wall thickness of the blow-molded product.
[0052] In summary, the present invention creatively arranges a hydrogen cylinder blow molding air ring with multiple independent heating air chambers between the hydrogen cylinder tube blank exit die and the mold, and uses a special algorithm to adjust the heating degree of the air chambers to different positions of the blank, thereby improving the fluidity of the wall thickness position. During the blow molding process, the wall thickness position of the blank will be stretched larger than other positions of the blank, thereby achieving the purpose of more uniform wall thickness of the blow-molded product;
[0053] The inventive spoiler rod of the present invention is disposed on the outside of the heating rod and is arranged in a binomial distribution form. The principles of fluid mechanics and dynamics are utilized and combined with the principle of binomial distribution probability to concentrate the hot air in the middle. This heating method is relatively gentle and is conducive to positioning and centralized heating. At the same time, the hot air volume and temperature on both sides are relatively low, reducing the interference of different independent wind chambers.
[0054] The fixing ring creatively arranged in the present invention is rotatably connected with the extension of the hydrogen cylinder tube blank ejection outlet, and the length of the adjusting screw can be adjusted according to process requirements to adjust the distance between the air ring body and the hydrogen cylinder tube blank ejection outlet. The operation is convenient and adjustment is facilitated, and the stability is good.
Claims
1. A method for solving the uneven wall thickness stretching during the inflation of hydrogen storage bottles. Features include:
1. Equipment connection and debugging; The fixing ring (5) of the blow-molded air ring of the hydrogen cylinder is assembled and sleeved on the extension of the hydrogen cylinder tube blank ejection opening (1), the assembled fixing ring (5) is fixed by bolts, the fixing ring (5) is rotatably connected and matched with the extension of the hydrogen cylinder tube blank ejection opening (1), the length of the adjusting screw (8) is adjusted according to process requirements, and the distance between the air ring body (9) and the hydrogen cylinder tube blank ejection opening (1) is adjusted; (ii) Preparation and wall thickness testing of hydrogen storage bottles in the control group; The fan (3) and the heating rod (6) on the air ring body (9) are turned off, and the blank is extruded from the hydrogen bottle tube blank out of the die opening (1), and after passing through the hydrogen bottle blow molding air ring, it falls into the mold, and after the mold is closed, it is blown and molded. The obtained hydrogen storage bottle is used as a control group to test the wall thickness; and the coordinates of the X-axis and Y-axis in the horizontal direction of the wall thickness are determined; (iii) using the wall thickness test of the control group to obtain the difference in uneven wall thickness stretching and determine the coordinates of the X-axis and Y-axis of the wall thickness in the horizontal direction, and adjusting the outlet air temperature of the multiple independent air chambers in the air ring body (9) according to the algorithm feedback; adjusting the outlet air temperature of the multiple independent air chambers in the air ring body (9) by adjusting the temperature of the heating rod (6); the algorithm is: the standard thickness of the hydrogen storage bottle is 5 mm; When the thickness of the hydrogen storage bottle is 5mm, the outlet temperature of the corresponding independent air chamber is 210±0.5℃; When the thickness of the hydrogen storage bottle is 6mm, the outlet temperature of the corresponding independent air chamber is 215±0.5℃; When the thickness of the hydrogen storage bottle is 7mm, the outlet temperature of the corresponding independent air chamber is 218±0.5℃; When the thickness of the hydrogen storage bottle is 8mm, the outlet temperature of the corresponding independent air chamber is 220±0.5℃; When the thickness of the hydrogen storage bottle is less than 5mm, the die gap should be adjusted to increase the overall thickness; (iv) determining the actual thickness and position of the blank by determining the coordinates of the X-axis and Y-axis in the horizontal direction of the wall thickness, and based on the algorithm of step three, rotating the fixed ring (5) to adjust the degree of heating of the wind chamber at different positions of the blank, thereby improving the fluidity of the wall thickness position. During the blow molding process, the wall thickness position of the blank will be stretched larger than other positions of the blank, thereby achieving the purpose of more uniform wall thickness of the blow-molded product.
2. The method for solving the uneven wall thickness stretching during the inflation of the hydrogen storage bottle according to claim 1, Features It comprises a hydrogen cylinder blow molding air ring, wherein the hydrogen cylinder blow molding air ring is arranged between a hydrogen cylinder tube blank ejection die opening (1) and a mold.
3. The method for solving the uneven wall thickness stretching during the inflation of the hydrogen storage bottle according to claim 1, Features The blow-molded air ring for the hydrogen cylinder comprises a hollow annular air ring body (9), a preset number of independent air chambers are arranged inside the air ring body (9), an air outlet (11) is arranged inside the air chamber, an air inlet (10) is arranged outside the air chamber, the air inlet (10) is connected to a fan (3), a heating rod (6) and a spoiler rod (7) are inserted in the air chamber, and the heating temperatures of the preset number of independent air chambers are different.
4. The method for solving the uneven wall thickness stretching during the inflation of the hydrogen storage bottle according to claim 3, Features The spoiler rods (7) are arranged on the outside of the heating rod (6), and the spoiler rods (7) are arranged in a binomial distribution form.
5. The method for solving the problem of uneven wall thickness stretching during the inflation of hydrogen storage bottles according to claim 3, Features The upper end surface of the air ring body (9) is provided with an adjusting screw (8) for adjusting the distance between the air ring body (9) and the hydrogen bottle tube blank ejection opening (1), the upper end of the adjusting screw (8) is fixed on a fixing ring (5), the fixing ring (5) is composed of two semicircular rings, the inner side wall of the fixing ring (5) is provided with a slide groove (12), and the extension of the hydrogen bottle tube blank ejection opening (1) is matched with the slide groove (12) through a sliding connection.
6. The method for solving the problem of uneven wall thickness stretching during the inflation of hydrogen storage bottles according to claim 3, Features The upper end surface of the fixing ring (5) is also provided with inverted teeth (2), and the side wall of the hydrogen bottle tube blank from the die opening (1) is provided with an elastic sheet (4) that cooperates with the inverted teeth (2).