A microporous rubber-metal composite plate and its preparation process

By adopting the preparation process of microporous rubber layer in rubber metal composite plates, and using microcrystalline glass microtubes and flame burning technology, the problem of poor permeability after pore formation is solved, and high permeability is achieved Permeable microporous rubber metal composite board.

CN115416330BActive Publication Date: 2024-11-29NAN YANG TIAN YI MI FENG ZHI PIN YOU XIAN GONG SI
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211129020.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-16
Publication Date
2024-11-29
Estimated Expiration
2042-09-16

AI Technical Summary

Technical Problem

The rubber metal composite plate has poor permeability during the pore formation process, resulting in poor permeability of micropores, affecting its performance after adhesion.

Method used

The preparation process of microporous rubber layer includes mixing rubber powder, polyethylene glycol, carbon ash, sulfur, calcium carbonate and stearic acid and mixing, building a microcrystalline glass microtube framework, and burning through flames and The pressing roller extrusion connects the microporous rubber layer to the composite metal substrate to form a microporous rubber metal composite plate with high permeability and permeability.

Benefits of technology

The micropore permeability and permeability of the rubber layer are significantly improved, so that the composite plate has better sealing and vibration-absorbing properties after bonding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003850151480000071
    Figure BDA0003850151480000071
  • Figure BDA0003850151480000101
    Figure BDA0003850151480000101
Patent Text Reader

Abstract

The present invention provides a microporous rubber-metal composite plate and a preparation process thereof, belonging to the technical field of composite materials, comprising a microporous rubber layer and a composite metal substrate, wherein the microporous rubber layer comprises rubber powder, polyethylene glycol, carbon ash, sulfur, calcium carbonate and stearic acid; the present invention can greatly enhance the permeability and permeability of the micropores after the rubber is opened, and enables the rubber layer to have higher permeability and permeability after being connected with the composite metal plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite materials, and in particular to a microporous rubber-metal composite plate and a preparation process thereof. Background Art

[0002] Metal composite plates are composite materials formed by metallurgically bonding metals with different properties at the interface using various composite technologies. Through appropriate material selection and reasonable structural design, metal composite plates can greatly improve the thermal expansion, strength, toughness, wear resistance, corrosion resistance, electrical properties, magnetic properties and many other properties of single metal materials, and are therefore widely used in industrial fields such as petroleum, chemical, shipbuilding, metallurgy, electricity, water conservancy, transportation, environmental protection, food, and pharmaceuticals. In addition to its structural and functional characteristics, metal composite plates can also save the use of precious metals and significantly reduce the cost of various equipment materials. Metal-rubber composite materials are based on metal plates, with a layer of elastomeric rubber coating applied on both sides or one side of the metal plate. This composite material has both the high elasticity and excellent compressibility of rubber elastomers and the high strength of metal core plates, so it has excellent sealing performance and vibration resistance and heat resistance. It can play a role in protection, sealing, impact resistance, vibration reduction, and heat resistance in different occasions. In particular, its structure and excellent sealing properties have made it widely used in sealing fields such as motor vehicles;

[0003] However, due to the material problem, rubber is not easy to mature in technical means such as pore forming, the pore density is small, and the pore filtration performance is poor. After being adhered to the composite metal plate, the permeability and filtration performance of its micropores are even worse. Summary of the invention

[0004] In view of this, the present invention provides a microporous rubber-metal composite plate and its preparation process, which can not only greatly enhance the permeability and permeability of the micropores after the rubber is opened, but also make the rubber layer and the composite metal plate have higher permeability and permeability after being connected.

[0005] To solve the above technical problems, the present invention provides a microporous rubber-metal composite plate, comprising a microporous rubber layer and a composite metal substrate, wherein the microporous rubber layer comprises rubber powder, polyethylene glycol, carbon ash, sulfur, calcium carbonate and stearic acid.

[0006] Furthermore, the specific steps of preparing the composite board are:

[0007] S1. Preparation of the microporous rubber layer base material, the rubber powder is mixed with polyethylene glycol, carbon ash, sulfur, calcium carbonate and stearic acid, and is put into an internal mixer for heating and mixing to obtain a liquid microporous rubber layer base material, and after mixing, the heat is kept and heated, and stirring is maintained;

[0008] S2. Construction of the microporous rubber layer skeleton, cutting the micro-glass micro-tubes and laying them flat in the square groove to be poured, pouring the liquid micro-porous rubber layer base material in S1 into the square groove, and letting it stand and cool to obtain a lamellar micro-porous rubber layer, and polishing the micro-glass micro-tubes on the surface of the micro-porous rubber layer;

[0009] S3. Pretreatment of the composite metal substrate, performing micro-hole drilling on the surface of the composite metal substrate and cleaning and polishing the surface of the metal plate;

[0010] S4. connecting the composite metal substrate and the microporous rubber layer, heating the polished surface of the microporous rubber layer, adhering and connecting the composite metal plate and the heated microporous rubber layer, inserting microcrystalline glass microtubes into the micropores on the composite metal substrate, and continuously heating the composite metal plate so that the microcrystalline glass tubes are inserted into the microporous rubber layer;

[0011] S5. Post-processing of the composite metal substrate, using a pair of pressure rollers to repeatedly roll the connected composite metal substrate and the microporous rubber layer, causing the microcrystalline glass tube to break.

[0012] Furthermore, the mixing times in S1 is 2 to 4 times.

[0013] Furthermore, the temperature of the heat preservation heating is 260-280°C.

[0014] Furthermore, the diameter of the microcrystalline glass tube in S2 is 0.05 to 0.10 mm.

[0015] Furthermore, the thickness of the lamellar microporous rubber layer in S2 is 3 to 7 cm.

[0016] Furthermore, the thickness of the glass-ceramic microtubes laid in S2 is higher than the depth of the square frame grooves.

[0017] Furthermore, the size of the micropores on the surface of the composite metal substrate in S3 is 0.10 to 0.20 mm.

[0018] Furthermore, the heating method in S4 is to heat the composite metal plate by flame burning.

[0019] The beneficial effects of the above technical solution of the present invention are as follows:

[0020] After using the microcrystalline glass tube, according to the contact between the tube walls of the microcrystalline glass tube, a pair of pressure rollers are used in the subsequent steps for repeated rolling, so that interconnected pores are generated in the rubber layer. In addition, due to the support of the microcrystalline glass tube when the rubber layer is fixed, the permeability between the micropores is improved, and a more stable microporous channel is generated after solidification. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described in combination with the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.

[0022] Embodiment 1

[0023] According to weight, 4000g of rubber powder, 280g of polyethylene glycol, 500g of carbon ash, 200g of sulfur, 600g of calcium carbonate and 500g of stearic acid are weighed, mixed and added into an internal mixer for mixing at a mixing temperature of 300°C. After mixing, a second mixing is performed, and after the second mixing, the mixture is allowed to stand for 8 hours, and a third mixing is performed to obtain a liquid microporous rubber layer base material, and the temperature is maintained at 270°C and stirred to prevent surface film formation;

[0024] Then, a square frame groove is built around a horizontal, smooth, clean flat plate, and microcrystalline glass tubes with a diameter of 0.08 mm are selected. The microcrystalline glass tubes are randomly scattered and cross-laid inside the square frame groove, and the microporous rubber layer base material that has been kneaded three times is poured into the square frame groove. The microporous rubber layer base material in the square frame groove is heated from the top of the square frame groove using an electric heating wire or an open flame until the outside of the microcrystalline glass tube in the square frame groove is filled with the microporous rubber layer base material, and the microcrystalline glass tube is exposed on the upper part of the microporous rubber layer base material, and the exposed microcrystalline glass tube is crushed and polished using a grinding tool, so that a plurality of micropores are leaked on the microporous rubber layer base material;

[0025] Take out an iron-aluminum alloy metal plate of the same size as the square groove, and use a punching tool to punch holes on the surface of the iron-aluminum alloy metal plate. The punching density is 500,000 holes / m 2 ,After the drilling is completed, the surface of the metal plate is ground and polished;

[0026] Use a flame spray gun to heat the polished surface of the microporous rubber layer to melt the rubber on the surface of the microporous rubber layer, align the metal plates, and connect and bond them so that the microporous rubber layer is located on the upper part of the metal plates. Then use a flame spray gun to heat the lower surface of the metal plates so that the rubber can be penetrated by the microcrystalline glass tubes. Then use rows of microcrystalline glass tubes to pass through the micropores on the surface of the metal plates and make the microcrystalline glass tubes collide with the microcrystalline glass tubes in the microporous rubber layer.

[0027] Then, a pair of upper and lower pressing rollers are used to insert the bonded metal plate and the microporous rubber layer between the two pressing rollers for extrusion, so that the microcrystalline glass is broken, the holes in the microporous rubber layer are cross-linked with each other, and the irregular debris between the glass is connected, and has permeability.

[0028] Embodiment 2

[0029] According to weight, 4000g of rubber powder, 280g of polyethylene glycol, 500g of carbon ash, 200g of sulfur, 600g of calcium carbonate and 500g of stearic acid are weighed, mixed and added into an internal mixer for mixing at a mixing temperature of 300°C. After mixing, a second mixing is performed, and after the second mixing, the mixture is allowed to stand for 8 hours, and a third mixing is performed to obtain a liquid microporous rubber layer base material, and the temperature is maintained at 270°C and stirred to prevent surface film formation;

[0030] Then, a square frame groove is built around a horizontal, smooth, clean flat plate, and microcrystalline glass tubes with a diameter of 0.05 mm are selected. The microcrystalline glass tubes are randomly scattered and cross-laid inside the square frame groove, and the microporous rubber layer base material that has been kneaded three times is poured into the square frame groove. The microporous rubber layer base material in the square frame groove is heated from the top of the square frame groove using an electric heating wire or an open flame until the outside of the microcrystalline glass tube in the square frame groove is filled with the microporous rubber layer base material, and the microcrystalline glass tube is exposed on the upper part of the microporous rubber layer base material, and the exposed microcrystalline glass tube is crushed and polished using a grinding tool, so that a plurality of micropores are leaked on the microporous rubber layer base material;

[0031] Take out an iron-aluminum alloy metal plate of the same size as the square groove, and use a punching tool to punch holes on the surface of the iron-aluminum alloy metal plate. The punching density is 500,000 holes / m 2 ,After the drilling is completed, the surface of the metal plate is ground and polished;

[0032] Use a flame spray gun to heat the polished surface of the microporous rubber layer to melt the rubber on the surface of the microporous rubber layer, align the metal plates, and connect and bond them so that the microporous rubber layer is located on the upper part of the metal plates. Then use a flame spray gun to heat the lower surface of the metal plates so that the rubber can be penetrated by the microcrystalline glass tubes. Then use rows of microcrystalline glass tubes to pass through the micropores on the surface of the metal plates and make the microcrystalline glass tubes collide with the microcrystalline glass tubes in the microporous rubber layer.

[0033] Then, a pair of upper and lower pressing rollers are used to insert the bonded metal plate and the microporous rubber layer between the two pressing rollers for extrusion, so that the microcrystalline glass is broken, the holes in the microporous rubber layer are cross-linked with each other, and the irregular debris between the glass is connected, and has permeability.

[0034] Embodiment 3

[0035] According to weight, 4000g of rubber powder, 280g of polyethylene glycol, 500g of carbon ash, 200g of sulfur, 600g of calcium carbonate and 500g of stearic acid are weighed, mixed and added into an internal mixer for mixing at a mixing temperature of 300°C. After mixing, a second mixing is performed, and after the second mixing, the mixture is allowed to stand for 8 hours, and a third mixing is performed to obtain a liquid microporous rubber layer base material, and the temperature is maintained at 270°C and stirred to prevent surface film formation;

[0036] Then, a square frame groove is built around a horizontal, smooth, clean flat plate, and microcrystalline glass tubes with a diameter of 0.06 mm are selected. The microcrystalline glass tubes are randomly scattered and cross-laid inside the square frame groove, and the microporous rubber layer base material that has been kneaded three times is poured into the square frame groove. The microporous rubber layer base material in the square frame groove is heated from the top of the square frame groove using an electric heating wire or an open flame until the outside of the microcrystalline glass tube in the square frame groove is filled with the microporous rubber layer base material, and the microcrystalline glass tube is exposed on the upper part of the microporous rubber layer base material, and the exposed microcrystalline glass tube is crushed and polished using a grinding tool, so that a plurality of micropores are leaked on the microporous rubber layer base material;

[0037] Take out an iron-aluminum alloy metal plate of the same size as the square groove, and use a punching tool to punch holes on the surface of the iron-aluminum alloy metal plate. The punching density is 500,000 holes / m 2 ,After the drilling is completed, the surface of the metal plate is ground and polished;

[0038] Use a flame spray gun to heat the polished surface of the microporous rubber layer to melt the rubber on the surface of the microporous rubber layer, align the metal plates, and connect and bond them so that the microporous rubber layer is located on the upper part of the metal plates. Then use a flame spray gun to heat the lower surface of the metal plates so that the rubber can be penetrated by the microcrystalline glass tubes. Then use rows of microcrystalline glass tubes to pass through the micropores on the surface of the metal plates and make the microcrystalline glass tubes collide with the microcrystalline glass tubes in the microporous rubber layer.

[0039] Then, a pair of upper and lower pressing rollers are used to insert the bonded metal plate and the microporous rubber layer between the two pressing rollers for extrusion, so that the microcrystalline glass is broken, the holes in the microporous rubber layer are cross-linked with each other, and the irregular debris between the glass is connected, and has permeability.

[0040] Embodiment 4

[0041] According to weight, 4000g of rubber powder, 280g of polyethylene glycol, 500g of carbon ash, 200g of sulfur, 600g of calcium carbonate and 500g of stearic acid are weighed, mixed and added into an internal mixer for mixing at a mixing temperature of 300°C. After mixing, a second mixing is performed, and after the second mixing, the mixture is allowed to stand for 8 hours, and a third mixing is performed to obtain a liquid microporous rubber layer base material, and the temperature is maintained at 270°C and stirred to prevent surface film formation;

[0042] Then, a square frame groove is built around a horizontal, smooth, clean flat plate, and microcrystalline glass tubes with a diameter of 0.07 mm are selected, and the microcrystalline glass tubes are randomly scattered and cross-laid inside the square frame groove, and the microporous rubber layer base material that has been kneaded three times is poured into the square frame groove, and the microporous rubber layer base material in the square frame groove is heated from the top of the square frame groove using an electric heating wire or an open flame until the outside of the microcrystalline glass tube in the square frame groove is filled with the microporous rubber layer base material, and the microcrystalline glass tube is exposed on the upper part of the microporous rubber layer base material, and the exposed microcrystalline glass tube is crushed and polished using a grinding tool, so that a plurality of micropores are leaked on the microporous rubber layer base material;

[0043] Take out an iron-aluminum alloy metal plate of the same size as the square groove, and use a punching tool to punch holes on the surface of the iron-aluminum alloy metal plate. The punching density is 500,000 holes / m 2 ,After the drilling is completed, the surface of the metal plate is ground and polished;

[0044] Use a flame spray gun to heat the polished surface of the microporous rubber layer to melt the rubber on the surface of the microporous rubber layer, align the metal plates, and connect and bond them so that the microporous rubber layer is located on the upper part of the metal plates. Then use a flame spray gun to heat the lower surface of the metal plates so that the rubber can be penetrated by the microcrystalline glass tubes. Then use rows of microcrystalline glass tubes to pass through the micropores on the surface of the metal plates and make the microcrystalline glass tubes collide with the microcrystalline glass tubes in the microporous rubber layer.

[0045] Then, a pair of upper and lower pressing rollers are used to insert the bonded metal plate and the microporous rubber layer between the two pressing rollers for extrusion, so that the microcrystalline glass is broken, the holes in the microporous rubber layer are cross-linked with each other, and the irregular debris between the glass is connected, and has permeability.

[0046] Embodiment 5

[0047] According to weight, 4000g of rubber powder, 280g of polyethylene glycol, 500g of carbon ash, 200g of sulfur, 600g of calcium carbonate and 500g of stearic acid are weighed, mixed and added into an internal mixer for mixing at a mixing temperature of 300°C. After mixing, a second mixing is performed, and after the second mixing, the mixture is allowed to stand for 8 hours, and a third mixing is performed to obtain a liquid microporous rubber layer base material, and the temperature is maintained at 270°C and stirred to prevent surface film formation;

[0048] Then, a square frame groove is built around a horizontal, smooth, clean flat plate, and microcrystalline glass tubes with a diameter of 0.10 mm are selected. The microcrystalline glass tubes are randomly scattered and cross-laid inside the square frame groove, and the microporous rubber layer base material that has been kneaded three times is poured into the square frame groove. The microporous rubber layer base material in the square frame groove is heated from the top of the square frame groove using an electric heating wire or an open flame until the outside of the microcrystalline glass tube in the square frame groove is filled with the microporous rubber layer base material, and the microcrystalline glass tube is exposed on the upper part of the microporous rubber layer base material, and the exposed microcrystalline glass tube is crushed and polished using a grinding tool, so that a plurality of micropores are leaked on the microporous rubber layer base material;

[0049] Take out an iron-aluminum alloy metal plate of the same size as the square groove, and use a punching tool to punch holes on the surface of the iron-aluminum alloy metal plate. The punching density is 500,000 holes / m 2 ,After the drilling is completed, the surface of the metal plate is ground and polished;

[0050] Use a flame spray gun to heat the polished surface of the microporous rubber layer to melt the rubber on the surface of the microporous rubber layer, align the metal plates, and connect and bond them so that the microporous rubber layer is located on the upper part of the metal plates. Then use a flame spray gun to heat the lower surface of the metal plates so that the rubber can be penetrated by the microcrystalline glass tubes. Then use rows of microcrystalline glass tubes to pass through the micropores on the surface of the metal plates and make the microcrystalline glass tubes collide with the microcrystalline glass tubes in the microporous rubber layer.

[0051] Then, a pair of upper and lower pressing rollers are used to insert the bonded metal plate and the microporous rubber layer between the two pressing rollers for extrusion, so that the microcrystalline glass is broken, the holes in the microporous rubber layer are cross-linked with each other, and the irregular debris between the glass is connected, and has permeability.

[0052]

[0053] Embodiment 6

[0054] According to weight, 4000g of rubber powder, 280g of polyethylene glycol, 500g of carbon ash, 200g of sulfur, 600g of calcium carbonate and 500g of stearic acid are weighed, mixed and added into an internal mixer for mixing at a mixing temperature of 300°C. After mixing, a second mixing is performed, and after the second mixing, the mixture is allowed to stand for 8 hours, and a third mixing is performed to obtain a liquid microporous rubber layer base material, and the temperature is maintained at 270°C and stirred to prevent surface film formation;

[0055] Then, a square frame groove is built around a horizontal, smooth, clean flat plate, and microcrystalline glass tubes with a diameter of 0.08 mm are selected. The microcrystalline glass tubes are randomly scattered and cross-laid inside the square frame groove, and the microporous rubber layer base material that has been kneaded three times is poured into the square frame groove. The microporous rubber layer base material in the square frame groove is heated from the top of the square frame groove using an electric heating wire or an open flame until the outside of the microcrystalline glass tube in the square frame groove is filled with the microporous rubber layer base material, and the microcrystalline glass tube is exposed on the upper part of the microporous rubber layer base material, and the exposed microcrystalline glass tube is crushed and polished using a grinding tool, so that a plurality of micropores are leaked on the microporous rubber layer base material;

[0056] Take out an iron-aluminum alloy metal plate of the same size as the square slot, and use a punching tool to punch holes on the surface of the iron-aluminum alloy metal plate. The punching density is 300,000 holes / m 2 ,After the drilling is completed, the surface of the metal plate is ground and polished;

[0057] Use a flame spray gun to heat the polished surface of the microporous rubber layer to melt the rubber on the surface of the microporous rubber layer, align the metal plates, and connect and bond them so that the microporous rubber layer is located on the upper part of the metal plates. Then use a flame spray gun to heat the lower surface of the metal plates so that the rubber can be penetrated by the microcrystalline glass tubes. Then use rows of microcrystalline glass tubes to pass through the micropores on the surface of the metal plates and make the microcrystalline glass tubes collide with the microcrystalline glass tubes in the microporous rubber layer.

[0058] Then, a pair of upper and lower pressing rollers are used to insert the bonded metal plate and the microporous rubber layer between the two pressing rollers for extrusion, so that the microcrystalline glass is broken, the holes in the microporous rubber layer are cross-linked with each other, and the irregular debris between the glass is connected, and has permeability.

[0059] Embodiment 7

[0060] According to weight, 4000g of rubber powder, 280g of polyethylene glycol, 500g of carbon ash, 200g of sulfur, 600g of calcium carbonate and 500g of stearic acid are weighed, mixed and added into an internal mixer for mixing at a mixing temperature of 300°C. After mixing, a second mixing is performed, and after the second mixing, the mixture is allowed to stand for 8 hours, and a third mixing is performed to obtain a liquid microporous rubber layer base material, and the temperature is maintained at 270°C and stirred to prevent surface film formation;

[0061] Then, a square frame groove is built around a horizontal, smooth, clean flat plate, and microcrystalline glass tubes with a diameter of 0.08 mm are selected. The microcrystalline glass tubes are randomly scattered and cross-laid inside the square frame groove, and the microporous rubber layer base material that has been kneaded three times is poured into the square frame groove. The microporous rubber layer base material in the square frame groove is heated from the top of the square frame groove using an electric heating wire or an open flame until the outside of the microcrystalline glass tube in the square frame groove is filled with the microporous rubber layer base material, and the microcrystalline glass tube is exposed on the upper part of the microporous rubber layer base material, and the exposed microcrystalline glass tube is crushed and polished using a grinding tool, so that a plurality of micropores are leaked on the microporous rubber layer base material;

[0062] Take out an iron-aluminum alloy metal plate of the same size as the square groove, and use a punching tool to punch holes on the surface of the iron-aluminum alloy metal plate. The punching density is 400,000 holes / m 2 ,After the drilling is completed, the surface of the metal plate is ground and polished;

[0063] Use a flame spray gun to heat the polished surface of the microporous rubber layer to melt the rubber on the surface of the microporous rubber layer, align the metal plates, and connect and bond them so that the microporous rubber layer is located on the upper part of the metal plates. Then use a flame spray gun to heat the lower surface of the metal plates so that the rubber can be penetrated by the microcrystalline glass tubes. Then use rows of microcrystalline glass tubes to pass through the micropores on the surface of the metal plates and make the microcrystalline glass tubes collide with the microcrystalline glass tubes in the microporous rubber layer.

[0064] Then, a pair of upper and lower pressing rollers are used to insert the bonded metal plate and the microporous rubber layer between the two pressing rollers for extrusion, so that the microcrystalline glass is broken, the holes in the microporous rubber layer are cross-linked with each other, and the irregular debris between the glass is connected, and has permeability.

[0065] Embodiment 8

[0066] According to weight, 4000g of rubber powder, 280g of polyethylene glycol, 500g of carbon ash, 200g of sulfur, 600g of calcium carbonate and 500g of stearic acid are weighed, mixed and added into an internal mixer for mixing at a mixing temperature of 300°C. After mixing, a second mixing is performed, and after the second mixing, the mixture is allowed to stand for 8 hours, and a third mixing is performed to obtain a liquid microporous rubber layer base material, and the temperature is maintained at 270°C and stirred to prevent surface film formation;

[0067] Then, a square frame groove is built around a horizontal, smooth, clean flat plate, and microcrystalline glass tubes with a diameter of 0.08 mm are selected. The microcrystalline glass tubes are randomly scattered and cross-laid inside the square frame groove, and the microporous rubber layer base material that has been kneaded three times is poured into the square frame groove. The microporous rubber layer base material in the square frame groove is heated from the top of the square frame groove using an electric heating wire or an open flame until the outside of the microcrystalline glass tube in the square frame groove is filled with the microporous rubber layer base material, and the microcrystalline glass tube is exposed on the upper part of the microporous rubber layer base material, and the exposed microcrystalline glass tube is crushed and polished using a grinding tool, so that a plurality of micropores are leaked on the microporous rubber layer base material;

[0068] Take out an iron-aluminum alloy metal plate of the same size as the square slot, and use a punching tool to punch holes on the surface of the iron-aluminum alloy metal plate. The punching density is 600,000 holes / m 2 ,After the drilling is completed, the surface of the metal plate is ground and polished;

[0069] Use a flame spray gun to heat the polished surface of the microporous rubber layer to melt the rubber on the surface of the microporous rubber layer, align the metal plates, and connect and bond them so that the microporous rubber layer is located on the upper part of the metal plates. Then use a flame spray gun to heat the lower surface of the metal plates so that the rubber can be penetrated by the microcrystalline glass tubes. Then use rows of microcrystalline glass tubes to pass through the micropores on the surface of the metal plates and make the microcrystalline glass tubes collide with the microcrystalline glass tubes in the microporous rubber layer.

[0070] Then, a pair of upper and lower pressing rollers are used to insert the bonded metal plate and the microporous rubber layer between the two pressing rollers for extrusion, so that the microcrystalline glass is broken, the holes in the microporous rubber layer are cross-linked with each other, and the irregular debris between the glass is connected, and has permeability.

[0071] Embodiment 9

[0072] According to weight, 4000g of rubber powder, 280g of polyethylene glycol, 500g of carbon ash, 200g of sulfur, 600g of calcium carbonate and 500g of stearic acid are weighed, mixed and added into an internal mixer for mixing at a mixing temperature of 300°C. After mixing, a second mixing is performed, and after the second mixing, the mixture is allowed to stand for 8 hours, and a third mixing is performed to obtain a liquid microporous rubber layer base material, and the temperature is maintained at 270°C and stirred to prevent surface film formation;

[0073] Then, a square frame groove is built around a horizontal, smooth, clean flat plate, and microcrystalline glass tubes with a diameter of 0.08 mm are selected. The microcrystalline glass tubes are randomly scattered and cross-laid inside the square frame groove, and the microporous rubber layer base material that has been kneaded three times is poured into the square frame groove. The microporous rubber layer base material in the square frame groove is heated from the top of the square frame groove using an electric heating wire or an open flame until the outside of the microcrystalline glass tube in the square frame groove is filled with the microporous rubber layer base material, and the microcrystalline glass tube is exposed on the upper part of the microporous rubber layer base material, and the exposed microcrystalline glass tube is crushed and polished using a grinding tool, so that a plurality of micropores are leaked on the microporous rubber layer base material;

[0074] Take out an iron-aluminum alloy metal plate of the same size as the square slot, and use a punching tool to punch holes on the surface of the iron-aluminum alloy metal plate. The punching density is 700,000 holes / m 2 ,After the drilling is completed, the surface of the metal plate is ground and polished;

[0075] Use a flame spray gun to heat the polished surface of the microporous rubber layer to melt the rubber on the surface of the microporous rubber layer, align the metal plates, and connect and bond them so that the microporous rubber layer is located on the upper part of the metal plates. Then use a flame spray gun to heat the lower surface of the metal plates so that the rubber can be penetrated by the microcrystalline glass tubes. Then use rows of microcrystalline glass tubes to pass through the micropores on the surface of the metal plates and make the microcrystalline glass tubes collide with the microcrystalline glass tubes in the microporous rubber layer.

[0076] Then, a pair of upper and lower pressing rollers are used to insert the bonded metal plate and the microporous rubber layer between the two pressing rollers for extrusion, so that the microcrystalline glass is broken, the holes in the microporous rubber layer are cross-linked with each other, and the irregular debris between the glass is connected, and has permeability.

[0077]

[0078] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A microporous rubber-metal composite plate, characterized in that: The invention comprises a microporous rubber layer and a composite metal substrate, wherein the microporous rubber layer comprises rubber powder, polyethylene glycol, carbon ash, sulfur, calcium carbonate and stearic acid; The specific steps of preparing the composite board are: S1. Preparation of the microporous rubber layer base material, the rubber powder is mixed with polyethylene glycol, carbon ash, sulfur, calcium carbonate and stearic acid, and is put into an internal mixer for heating and mixing to obtain a liquid microporous rubber layer base material, and after mixing, the heat is kept and heated, and stirring is maintained; S2. Construction of the microporous rubber layer skeleton, cutting the micro-glass micro-tubes and laying them flat in the square groove to be poured, pouring the liquid micro-porous rubber layer base material in S1 into the square groove, and letting it stand and cool to obtain a lamellar micro-porous rubber layer, and polishing the micro-glass micro-tubes on the surface of the micro-porous rubber layer; S3. Pretreatment of the composite metal substrate, performing micro-hole drilling on the surface of the composite metal substrate and cleaning and polishing the surface of the metal plate; S4. connecting the composite metal substrate and the microporous rubber layer, heating the polished surface of the microporous rubber layer, adhering and connecting the composite metal plate and the heated microporous rubber layer, inserting microcrystalline glass microtubes into the micropores on the composite metal substrate, and continuously heating the composite metal plate so that the microcrystalline glass tubes are inserted into the microporous rubber layer; S5. Post-processing of the composite metal substrate, using a pair of pressure rollers to repeatedly roll the connected composite metal substrate and the microporous rubber layer, causing the microcrystalline glass tube to break.

2. A microporous rubber-metal composite plate as claimed in claim 1, characterized in that: The number of mixing times in S1 is 2 to 4 times.

3. The microporous rubber-metal composite plate according to claim 1, characterized in that: The temperature of the insulation heating is 260~280℃.

4. The microporous rubber-metal composite plate according to claim 1, characterized in that: The diameter of the microcrystalline glass tube in S2 is 0.05~0.10mm.

5. The microporous rubber-metal composite plate according to claim 1, characterized in that: The thickness of the lamellar microporous rubber layer in S2 is 3~7cm.

6. The microporous rubber-metal composite plate according to claim 1, characterized in that: The thickness of the glass-ceramic microtubes laid in S2 is higher than the depth of the square frame grooves.

7. The microporous rubber-metal composite plate according to claim 1, characterized in that: The size of the micropores on the surface of the composite metal substrate in S3 is 0.10~0.20mm.

8. The microporous rubber-metal composite plate according to claim 1, characterized in that: The heating method in S4 is to heat the composite metal plate by flame burning.

Citation Information

Patent Citations

  • High compensation nature compound seal pad

    CN204533520U