A high-strength, high-thermal-conductivity, low-roughness graphene / copper composite material and preparation method thereof
By using specific electrodeposition solution formulas and processes in the preparation of graphene/copper composite materials, combined with asynchronous rolling and recrystallization annealing, the problems of coarse grains and insufficient performance of the material are solved, and high thermal conductivity and low roughness are achieved. The preparation of graphene/copper composite materials with high strength and excellent mechanical properties can meet the efficient heat dissipation needs of electronic components.
Patent Information
- Application Number
- CN202211070041.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-02
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-09-02
AI Technical Summary
During the preparation process of existing graphene/copper composite materials, the grains are coarse, easy to crack and warp, and the performance has not been significantly improved. The thermal conductivity is insufficient, making it difficult to meet the efficient heat dissipation needs of electronic components.
A well-proportioned electrodeposition solution formula is used, including copper sulfate pentahydrate, 2-mercaptobenzimidazole and jenna green. The composite material is prepared by alternating pulse electrodeposition method, and is subjected to asynchronous rolling and recrystallization annealing to form a dense , flat layered structure.
A graphene/copper composite material with high thermal conductivity, low roughness and excellent mechanical properties has been obtained. The thermal conductivity can reach 1180W/m·k, the tensile strength can reach up to 524MPa, and the surface roughness can reach up to 0.3±0.1μm. , to meet the needs in the field of heat conduction.
Smart Images

Figure HDA0003829446640000011 
Figure HDA0003829446640000012 
Figure HDA0003829446640000013
Abstract
Description
Technical Field
[0001] The present invention relates to the field of heat conduction materials, and in particular to a high-strength, high-thermal-conductivity, low-roughness graphene / copper composite material and a preparation method thereof. Background Art
[0002] As the characteristic dimensions of electronic components such as integrated circuits gradually decrease, the power dissipation and heat generation of electronic components are increasing. Therefore, the thermal conductivity and heat dissipation capacity of electronic components has become a key issue that needs to be solved urgently.
[0003] Copper-based composite materials have been widely used in structural materials, electronic equipment, and aerospace fields due to their good thermal and electrical conductivity, wear resistance, and excellent mechanical properties.
[0004] At present, the preparation of graphene metal-based composite materials mainly includes powder metallurgy, hydrothermal method, chemical vapor deposition method and electrochemical deposition method. Powder metallurgy is simple to operate, but the mold is single and the controllability is poor; the hydrothermal method has high equipment requirements and great technical difficulty; although the coating prepared by chemical vapor deposition is dense and uniform, the coating is thin, which is not conducive to practical application. The electrochemical deposition method is a method of preparing composite materials through redox reaction in a solution of a specific proportion. This method has a simple process, low cost and good product quality, but in the preparation process, the selection of the plate, the adjustment of the process parameters and the ratio of the components of the electrodeposition liquid will directly affect the organization and performance of the prepared composite materials. The existing process formula and parameter control prepared graphene / copper composite materials have coarse grains, are prone to cracking and warping, and the performance is not significantly improved compared to pure copper. Summary of the invention
[0005] In order to solve the technical problems pointed out in the background technology, the present invention provides a low-roughness composite material with high thermal conductivity and excellent mechanical properties and a preparation method thereof. The purpose of the present invention is to provide an electrodeposition solution of a graphene / copper composite material with reasonable ratio, green environmental protection, cost saving, and controllable coating thickness, as well as the required process method and parameters, and after a suitable rolling annealing process, a graphene / copper composite material with excellent performance is obtained.
[0006] The technical solution of the present invention is:
[0007] The graphene / copper composite material was prepared by electrodeposition as follows:
[0008] (1) Preparing an electrodeposition solution of a graphene / copper composite material, the composition according to mass concentration is:
[0009] Electrodeposition solution A: copper sulfate pentahydrate 60-240 g / L, 2-mercaptobenzimidazole 40-80 mg / L, Cl- (provided by hydrochloric acid) 40-80 mg / L, graphene (Gr) 0-0.45 g / L, and the balance is deionized water.
[0010] Electrodeposition solution B: copper sulfate pentahydrate 60-240 g / L, Janus green (JGB) 10-30 mg / L, graphene (Gr) 0-0.45 g / L, and the balance is deionized water.
[0011] The preparation method of the electrodeposition solution is as follows: the graphene solution is dispersed by ultrasonication, and then dispersed by a high-speed homogenizer at a speed of 5000 r / min; 2-mercaptobenzimidazole and Cl are added respectively. - After mechanically stirring with Janus Green (JGB), it was mixed with a copper sulfate pentahydrate solution, and then stirred with an electric stirrer and dispersed with a high-speed homogenizer to obtain graphene / copper-2-mercaptobenzimidazole / Cl- and graphene / copper-Jannac Green composite electrodeposition solutions.
[0012] Among them, under the low pH conditions of acidic copper plating, chloride will be adsorbed on the cathode copper with a high coverage rate of 2-mercaptobenzimidazole and continue to move to the surface. The adsorbed chloride ions will not hinder the deposition of copper, and can even attract copper ions and serve as a channel for electron transfer, accelerating the electrochemical reaction, which is beneficial to obtaining a denser copper layer to a certain extent; in addition, Cl- can synergize with 2-mercaptobenzimidazole to optimize and improve the density and surface roughness of the composite foil.
[0013] JGB can effectively improve the dispersion of graphene and reduce agglomeration. The higher energy gap of JGB molecules and their adsorption on the cathode surface require a higher overpotential for copper ion deposition, which promotes nucleation and refines grains, thereby optimizing the deposition rate and surface roughness of the composite foil.
[0014] (2) Use metallographic sandpaper to polish the anode (copper plate) and cathode (titanium plate) to remove oil stains and oxide film, and then activate the plates with 10% dilute hydrochloric acid solution for 5 to 20 minutes.
[0015] (3) Using the prepared deposition solution for deposition, with a titanium plate as the substrate, pulse electrodeposition was adopted, first depositing in a deposition solution containing 2-mercaptobenzimidazole and Cl- for 10 min, then depositing in a deposition solution containing janna green for 10 min, repeating twice, and depositing for a total of 40 min.
[0016] The process parameters are: pulse width ratio of 3:1 to 6:1 (positive / negative), pulse voltage of 1 to 2.5V / 0.5 to 1V, and pulse current frequency of 500Hz. The process environment is: deposition liquid temperature of 25 to 45°C, and deposition liquid pH of 1.0 to 3.0. Changes in deposition liquid temperature, pH, current density and other parameters will affect the deposition rate and quality of the material.
[0017] (4) The prepared graphene / copper composite material is subjected to asynchronous rolling and recrystallization annealing treatment, and the process conditions are: speed ratio 1.0-2.0, final deformation 10-30%, annealing temperature 150-300° C., and annealing time 15-120 min.
[0018] The copper sulfate-graphene composite deposition liquid used in the invention has a reasonable composition ratio and can be recycled, which not only saves costs but is also environmentally friendly; the graphene / copper composite material prepared by using the deposition liquid has a flat and smooth surface and a uniform and dense structure.
[0019] By using the alternating electrodeposition process, the composite material can form a layered structure with a unique two-dimensional structure and excellent performance, which has a better improvement effect on the performance of the graphene-reinforced composite material.
[0020] Asynchronous rolling can effectively reduce the recrystallization temperature of copper, which is beneficial to nucleation during annealing, and can form shear bands, refine grains, and improve the mechanical properties of materials. Appropriate annealing process parameters can effectively improve the comprehensive properties of composite materials.
[0021] The main advantages of the present invention are:
[0022] (1) The present invention provides a method for preparing a graphene / copper composite material, namely, alternating pulse electrodeposition + asynchronous rolling + recrystallization annealing, which has a simple process, low cost, and the electrolyte can be repeatedly used. In addition, the prepared composite material is flat and dense, and has excellent mechanical properties, thermal conductivity and surface roughness.
[0023] (2) The present invention provides a new type of deposition liquid formula: the addition of 2-mercaptobenzimidazole and jana green can effectively improve the wettability between the matrix and the reinforcement phase and improve the bonding strength; at the same time, it is beneficial to improve the surface quality of the deposition layer and improve the surface flatness of the coating. The composite material prepared by the present invention is used in the field of thermal conductive materials to improve the heat dissipation efficiency of the material. In addition, the pulse electrodeposition technology can also be used to make heat dissipation films and heat dissipation lines of electronic components, such as internal heat dissipation plates of electronic equipment, GPU chips, etc.
[0024] (3) The present invention provides an asynchronous rolling and recrystallization annealing process, which can effectively optimize and improve the tensile strength, thermal conductivity and surface roughness of the material. The tensile strength of the composite coating can reach up to 524MPa, the thermal conductivity can reach up to 1180W / m·k, and the surface roughness can reach 0.3±0.1μm, which better meets the needs of the thermal conduction field. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A three-dimensional image of the surface morphology of the deposited graphene / copper composite material of Example 3 of the present invention;
[0026] Figure 2 This is a three-dimensional image of the surface morphology of the graphene / copper composite material after asynchronous rolling + annealing in Example 3 of the present invention;
[0027] Figure 3 This is a surface scanning electron microscope image of the deposited graphene / copper composite material of Example 3 of the present invention. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below in conjunction with embodiments: These embodiments are only used to illustrate the present invention and are not used to limit the scope of the invention.
[0029] Example 1
[0030] The composition ratio of the graphene / copper composite electrodeposition solution is:
[0031] Electrodeposition solution A: 60 g / L copper sulfate pentahydrate, 40 mg / L 2-mercaptobenzimidazole, 40 mg / L Cl- (provided by hydrochloric acid), 0.05 g / L graphene (Gr), and the balance is deionized water.
[0032] The preparation method of the electrodeposition solution is as follows: ultrasonically dispersing the graphene solution, and then dispersing it with a high-speed homogenizer at a speed of 5000r / min; adding 2-mercaptobenzimidazole and Cl-, mechanically stirring, and mixing with a copper sulfate pentahydrate solution, and then stirring with an electric stirrer and dispersing with a high-speed homogenizer to obtain a graphene / copper-2-mercaptobenzimidazole / Cl- composite electrodeposition solution.
[0033] Electrodeposition solution B: copper sulfate pentahydrate 60g / L, Janus green (JGB) 10mg / L, graphene (Gr)
[0034] 0.05g / L, the balance is deionized water.
[0035] The preparation method of the electrodeposition solution is as follows: ultrasonically dispersing the graphene solution, and then dispersing it with a high-speed homogenizer at a speed of 5000r / min; adding Janus Green (JGB) and mechanically stirring it, mixing it with a copper sulfate pentahydrate solution, and then stirring it with an electric stirrer and dispersing it with a high-speed homogenizer to obtain a graphene / copper-Janus Green composite electrodeposition solution.
[0036] Use metallographic sandpaper to polish the anode (copper plate) and cathode (titanium plate) to remove oil stains and oxide film, and then activate the plates with 10% dilute hydrochloric acid solution for 10 minutes.
[0037] The pulse electrodeposition method was adopted. The deposition was first carried out in a deposition solution containing 2-mercaptobenzimidazole and Cl- for 10 minutes, and then in a deposition solution containing JGB for 10 minutes. The cycle was repeated twice and the total deposition was 40 minutes. The process environment of the deposition solution was: temperature 25℃, PH=3; the electrodeposition process parameters were: pulse width ratio 3:1 (positive / negative), pulse voltage 2.5V / 0.6V, and pulse current frequency 500Hz. The deposition layer prepared under this condition and the process conditions had a uniform thickness of about 20μm, a small amount of protruding particles on the surface, general flatness, general density, and a surface roughness of 2.8±0.1μm; the process parameters of rolling annealing were: speed ratio 1.2, final deformation of 10%, annealing temperature 150℃, annealing time 15min, and the tensile strength of the obtained composite coating was 341MPa, the thermal conductivity was 440W / m·k, and the surface roughness was 1.2±0.1μm.
[0038] Example 2
[0039] Electrodeposition solution A: 100 g / L copper sulfate pentahydrate, 50 mg / L 2-mercaptobenzimidazole, 50 mg / L Cl- (provided by hydrochloric acid), 0.15 g / L graphene (Gr), and the balance is deionized water.
[0040] Electrodeposition solution B: copper sulfate pentahydrate 100 g / L, Janus green (JGB) 20 mg / L, graphene (Gr) 0.15 g / L, and the balance is deionized water.
[0041] Use metallographic sandpaper to polish the anode (copper plate) and cathode (titanium plate) to remove oil stains and oxide film, and then activate the plates with 10% dilute hydrochloric acid solution for 10 minutes.
[0042] The pulse electrodeposition method was adopted. The deposition was first carried out in a deposition solution containing 2-mercaptobenzimidazole and Cl- for 10 minutes, and then in a deposition solution containing JGB for 10 minutes. The cycle was repeated twice, and the total deposition was 40 minutes. The deposition solution process environment was: the deposition solution temperature was 30°C, and the deposition solution pH was 2.5. The electrodeposition process parameters were: the pulse width ratio was 4:1 (positive / negative), the pulse voltage was 2.5V / 0.6V, and the pulse current frequency was 500Hz. The deposition layer prepared under this condition and the process conditions had a uniform thickness of about 30μm, a small amount of protruding particles on the surface, general flatness, general density, and a surface roughness of 2.2±0.1μm. The process parameters of rolling annealing are: speed ratio 1.4, final deformation 30%, annealing temperature 200°C, annealing time 30min, the obtained composite coating has a tensile strength of 466MPa, a thermal conductivity of 720W / m·k, and a surface roughness of 0.9±0.1μm.
[0043] The preparation method of the graphene / copper composite deposition solution is the same as that of Example 1.
[0044] Example 3
[0045] Electrodeposition solution A: 140 g / L copper sulfate pentahydrate, 60 mg / L 2-mercaptobenzimidazole, 60 mg / L Cl- (provided by hydrochloric acid), 0.25 g / L graphene (Gr), and the balance is deionized water.
[0046] Electrodeposition solution B: 140 g / L of copper sulfate pentahydrate, 25 mg / L of Janus green (JGB), 0.25 g / L of graphene (Gr), and the balance is deionized water.
[0047] Use metallographic sandpaper to polish the anode (copper plate) and cathode (titanium plate) to remove oil stains and oxide film, and then activate the plates with 10% dilute hydrochloric acid solution for 10 minutes.
[0048] The pulse electrodeposition method was adopted. The deposition was first carried out in a deposition solution containing 2-mercaptobenzimidazole and Cl- for 10 minutes, and then in a deposition solution containing JGB for 10 minutes. The cycle was repeated twice, and the total deposition was 40 minutes. The deposition solution process environment was: the deposition solution temperature was 30°C, and the deposition solution pH was 2.0. The electrodeposition process parameters were: the pulse width ratio was 5:1 (positive / negative), the pulse voltage was 2.5V / 0.6V, and the pulse current frequency was 500Hz. The deposition layer prepared under this condition and the process conditions had a uniform thickness of about 50μm, a smooth surface, basically no protruding particles, good density, and a surface roughness of 0.8±0.1μm. The process parameters of rolling annealing are: speed ratio 1.6, final deformation 30%, annealing temperature 250°C, annealing time 45min, the tensile strength of the obtained composite coating is 509MPa, the thermal conductivity can reach 1180W / m·k, and the surface roughness is 0.3±0.1μm.
[0049] The preparation method of the graphene / copper composite deposition solution is the same as that of Example 1.
[0050] Example 4
[0051] Electrodeposition solution A: 180 g / L copper sulfate pentahydrate, 70 mg / L 2-mercaptobenzimidazole, 70 mg / L Cl- (provided by hydrochloric acid), 0.35 g / L graphene (Gr), and the balance is deionized water.
[0052] Electrodeposition solution B: 180 g / L of copper sulfate pentahydrate, 30 mg / L of Janus Green (JGB), 0.35 g / L of graphene (Gr), and the balance is deionized water.
[0053] Use metallographic sandpaper to polish the anode (copper plate) and cathode (titanium plate) to remove oil stains and oxide film, and then activate the plates with 10% dilute hydrochloric acid solution for 10 minutes.
[0054] The pulse electrodeposition method was adopted. The deposition was first carried out in a deposition solution containing 2-mercaptobenzimidazole and Cl- for 10 minutes, and then in a deposition solution containing JGB for 10 minutes. The cycle was repeated twice, and the total deposition was 40 minutes. The deposition solution process environment was: the deposition solution temperature was 35°C, and the deposition solution pH was 1.5. The electrodeposition process parameters were: pulse width ratio of 6:1 (positive / negative), pulse voltage of 2.5V / 0.6V, and pulse current frequency of 500Hz. The deposition layer prepared under this condition and the process conditions had a uniform thickness of about 60μm, with fewer protruding particles on the surface, general flatness, good density, and a surface roughness of 1.2±0.1μm. The process parameters of rolling annealing are: speed ratio 1.8, final deformation 30%, annealing temperature 300°C, annealing time 60min, the obtained composite coating has a tensile strength of 483MPa, a thermal conductivity of 850W / m·k, and a surface roughness of 0.5±0.1μm.
[0055] The preparation method of the graphene / copper composite deposition solution is the same as that of Example 1.
[0056] Example 5
[0057] Electrodeposition solution A: 220 g / L copper sulfate pentahydrate, 80 mg / L 2-mercaptobenzimidazole, 80 mg / L Cl- (provided by hydrochloric acid), 0.45 g / L graphene (Gr), and the balance is deionized water.
[0058] Electrodeposition solution B: 220 g / L of copper sulfate pentahydrate, 30 mg / L of Janus Green (JGB), 0.45 g / L of graphene (Gr), and the balance is deionized water.
[0059] Use metallographic sandpaper to polish the anode (copper plate) and cathode (titanium plate) to remove oil stains and oxide film, and then activate the plates with 10% dilute hydrochloric acid solution for 10 minutes.
[0060] The pulse electrodeposition method was adopted. The deposition was first carried out in a deposition solution containing 2-mercaptobenzimidazole and Cl- for 10 minutes, and then in a deposition solution containing JGB for 10 minutes. The cycle was repeated twice, and the total deposition was 40 minutes. The deposition solution process environment was: the deposition solution temperature was 35°C, and the deposition solution pH was 1.0. The electrodeposition process parameters were: the pulse width ratio was 6:1 (positive / negative), the pulse voltage was 2.5V / 0.6V, and the pulse current frequency was 500Hz. The deposition layer prepared under this condition and under this process condition had a uniform thickness of about 50μm, a good surface with few protruding particles, good flatness, good density, and a surface roughness of 1.0±0.1μm. The process parameters of rolling annealing are: speed ratio 2.0, final deformation 30%, annealing temperature 300°C, annealing time 90min, the tensile strength of the obtained composite coating is 524MPa, the thermal conductivity is 845W / m·k, and the surface roughness is 0.5±0.1μm.
[0061] The preparation method of the graphene / copper composite deposition solution is the same as that of Example 1.
[0062] Comparative Example 1
[0063] Electrodeposition solution A: 60 g / L copper sulfate pentahydrate, 40 mg / L 2-mercaptobenzimidazole, 40 mg / L Cl- (provided by hydrochloric acid), and the balance is deionized water.
[0064] Electrodeposition solution B: 60 g / L of copper sulfate pentahydrate, 10 mg / L of Janus Green (JGB), and the balance is deionized water.
[0065] Use metallographic sandpaper to polish the anode (copper plate) and cathode (titanium plate) to remove oil stains and oxide film, and then activate the plates with 10% dilute hydrochloric acid solution for 10 minutes.
[0066] The pulse electrodeposition method was adopted. The deposition was first carried out in a deposition solution containing 2-mercaptobenzimidazole and Cl- for 10 minutes, and then in a deposition solution containing JGB for 10 minutes. The cycle was repeated twice, and the total deposition was 40 minutes. The electrodeposition process environment was: the deposition solution temperature was 25°C, and the deposition solution pH was 3.0. The electrodeposition process parameters were: pulse width ratio of 3:1 (positive / negative), pulse voltage of 2.5V / 0.6V, and pulse current frequency of 500Hz. The thickness of the deposited layer prepared under this situation and process conditions was uniform, about 4020μm, the surface was relatively smooth, there were fewer protruding particles, the density was general, and the surface roughness was 1.9±0.1μm. The process parameters of rolling annealing are: speed ratio 1.2, final deformation 10%, annealing temperature 150°C, annealing time 15min, the obtained composite coating has a tensile strength of 298MPa, a thermal conductivity of 280W / m·k, and a surface roughness of 0.8±0.1μm.
[0067] Comparative Example 2
[0068] Electrodeposition solution A: 100 g / L copper sulfate pentahydrate, 50 mg / L 2-mercaptobenzimidazole, 50 mg / L Cl- (provided by hydrochloric acid), 0.15 g / L graphene (Gr), and the balance is deionized water.
[0069] Use metallographic sandpaper to polish the anode (copper plate) and cathode (titanium plate) to remove oil stains and oxide film, and then activate the plates with 10% dilute hydrochloric acid solution for 10 minutes.
[0070] The pulse electrodeposition method was used to deposit in CuSO4-graphene-2-mercaptobenzimidazole and Cl- deposition solution for 40 minutes. The deposition solution process environment was: deposition solution temperature 30℃, deposition solution pH 2.5. The electrodeposition process parameters were: pulse width ratio 4:1 (positive / negative), pulse voltage 2.5V / 0.6V, pulse current frequency 500Hz. Under this condition and under this process condition, the deposition layer prepared had a uniform thickness of about 30μm, a smooth surface, basically no protruding particles, good density, and a surface roughness of 1.4±0.1μm. The process parameters of rolling annealing were: speed ratio 1.4, final deformation 30%, annealing temperature 200℃, annealing time 30min, and the obtained composite coating had a tensile strength of 433MPa, a thermal conductivity of 734W / m·k, and a surface roughness of 0.7±0.1μm.
[0071] Comparative Example 3
[0072] Electrodeposition solution B: 140 g / L of copper sulfate pentahydrate, 25 mg / L of Janus green (JGB), 0.25 g / L of graphene (Gr), and the balance is deionized water.
[0073] Use metallographic sandpaper to polish the anode (copper plate) and cathode (titanium plate) to remove oil stains and oxide film, and then activate the plates with 10% dilute hydrochloric acid solution for 10 minutes.
[0074] The pulse electrodeposition method was used to deposit in CuSO4-graphene-JGB deposition solution for 40 minutes. The deposition solution process environment was: deposition solution temperature 30℃, deposition solution pH 2.0. The electrodeposition process parameters were: pulse width ratio 5:1 (positive / negative), pulse voltage 2.5V / 0.6V, pulse current frequency 500Hz. The deposition layer prepared under this condition and process conditions had a uniform thickness of about 50μm, a smooth surface, basically no protruding particles, good density, and a surface roughness of 1.1±0.1μm. The process parameters of rolling annealing were: speed ratio 1.6, final deformation 30%, annealing temperature 250℃, annealing time 120min, and the obtained composite coating had a tensile strength of 495MPa, a thermal conductivity of 697W / m·k, and a surface roughness of 0.5±0.1μm.
[0075] Comparative Example 4
[0076] Electrodeposition solution A: 180 g / L copper sulfate pentahydrate, 70 mg / L 2-mercaptobenzimidazole, 70 mg / L Cl- (provided by hydrochloric acid), 0.35 g / L graphene (Gr), and the balance is deionized water.
[0077] Electrodeposition solution B: 180 g / L of copper sulfate pentahydrate, 30 mg / L of Janus Green (JGB), 0.35 g / L of graphene (Gr), and the balance is deionized water.
[0078] Use metallographic sandpaper to polish the anode (copper plate) and cathode (titanium plate) to remove oil stains and oxide film, and then activate the plates with 10% dilute hydrochloric acid solution for 10 minutes.
[0079] The pulse electrodeposition method was adopted. The deposition was first carried out in a deposition solution containing 2-mercaptobenzimidazole and Cl- for 10 minutes, and then in a deposition solution containing JGB for 10 minutes. The cycle was repeated twice and the total deposition was 40 minutes. The deposition solution process environment was as follows: the deposition solution temperature was 35°C and the deposition solution pH was 1.5. The electrodeposition process parameters were as follows: the pulse width ratio was 6:1 (positive / negative), the pulse voltage was 2.5V / 0.6V, and the pulse current frequency was 500Hz. The deposition layer prepared under this condition and under this process condition had a uniform thickness of about 60μm, with fewer protruding particles on the surface, general flatness, and good density. The tensile strength of the obtained composite coating was 410MPa, the thermal conductivity was 750W / m·k, and the surface roughness was 1.2±0.1μm.
[0080] The preparation method of the graphene / copper composite deposition solution is the same as that of Example 1.
[0081] The above examples are all preferred embodiments of the present invention, but the present invention is not limited to the above embodiments. Any obvious improvements, substitutions or modifications that can be made by those skilled in the art without departing from the essential content of the present invention belong to the protection scope of the present invention.
Claims
1. A high-strength, high-thermal-conductivity, low-roughness graphene / copper composite material, characterized in that: The composite material has a tensile strength of 298 to 524 MPa, a thermal conductivity of 280 to 1180 W / m·k, and a roughness of 0.3±0.1 μm to 3±0.1 μm; The steps of preparing the composite material are as follows: (1) Prepare a graphene / copper composite deposition solution, wherein 2-mercaptobenzimidazole, Cl - and Janus Green (JGB) as additives; The composition of the electrodeposition solution according to mass concentration is as follows: Electrodeposition solution A: copper sulfate pentahydrate 60-240 g / L, 2-mercaptobenzimidazole 40-80 mg / L, Cl - 40~80mg / L, graphene (Gr) 0~0.45g / L, the balance is deionized water; Electrodeposition solution B: copper sulfate pentahydrate 60~240g / L, Janus green (JGB) 10~30mg / L, graphene (Gr) 0~0.45g / L, the balance is deionized water; (2) Use metallographic sandpaper to polish the anode copper plate and cathode titanium plate to remove oil stains and oxide film, and then activate the plates with 10% dilute hydrochloric acid solution for 5 to 20 minutes; (3) Pulse electrodeposition is used in the deposition solution for alternating electrodeposition, that is, firstly in a solution containing 2-mercaptobenzimidazole and Cl - The graphene / copper composite coating with high strength and high thermal conductivity was obtained by depositing in a deposition solution containing JGB for 10 minutes, and then depositing in a deposition solution containing JGB for 10 minutes, repeating the process twice, and co-depositing for 40 minutes. (4) Asynchronous rolling and recrystallization annealing treatment of the electrodeposited coating; The process conditions of asynchronous rolling and recrystallization annealing are: speed ratio 1.0-2.0, final deformation 10-30%, annealing temperature 150-300°C, and annealing time 15-120min.
2. The high-strength, high-thermal-conductivity, low-roughness graphene / copper composite material according to claim 1, characterized in that: The preparation method of the electrodeposition solution in step (1) is as follows: firstly, the graphene solution is dispersed by ultrasonication, and then dispersed by a high-speed homogenizer at a speed of 5000 r / min; 2-mercaptobenzimidazole, Cl - After mechanical stirring with JGB, it was mixed with copper sulfate pentahydrate solution, and then stirred with an electric stirrer and dispersed with a high-speed homogenizer to obtain graphene / copper-2-mercaptobenzimidazole / Cl - and graphene / copper-Jana Green composite electrodeposition solutions.
3. The high-strength, high-thermal-conductivity, low-roughness graphene / copper composite material according to claim 1, characterized in that: The process parameters in the electrodeposition process of step (3) are: pulse width ratio of 3:1 to 6:1 (forward / reverse), pulse voltage of 1 to 2.5 V / 0.5 to 1 V, and pulse current frequency of 500 Hz.
4. The high-strength, high-thermal-conductivity, low-roughness graphene / copper composite material according to claim 1, characterized in that: The process environment during the electrodeposition process in step (3) is as follows: the temperature of the deposition liquid is 25 to 45° C., and the pH of the deposition liquid is 1.0 to 3.
0.
5. The high-strength, high-thermal-conductivity, low-roughness graphene / copper composite material according to claim 1, characterized in that: The thickness of the deposited layer obtained in step (3) is 20 to 80 μm.
6. An application of the graphene / copper composite material according to claim 1, characterized in that: The graphene / copper composite material is used in the field of heat conduction.