Ferromagnetic powder and its preparation method and application

By reacting sulfonated polysulfone with the surface of the ferromagnetic powder to form a polymer complex, and combining epoxy resin, the shortcomings of ferromagnetic powder in terms of insulation, rust and corrosion protection are solved, and the stability of the inductance is improved and Weather resistance avoids the fragility of the phosphoric acid passivation layer.

CN115424801BActive Publication Date: 2024-11-08SUZHOU ZHIWEI SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211163955.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-23
Publication Date
2024-11-08
Estimated Expiration
2042-09-23

AI Technical Summary

Technical Problem

The existing ferromagnetic powder has high insulation requirements after thermal aging or reflow soldering and insufficient anti-rust and corrosion resistance. The phosphoric acid passivation process will damage ferromagnetic when improving insulation, and the generated passivation layer is thermally impacted and physical. It is easy to break under pressure and loses its protective effect.

Method used

The sulfonated polysulfone reacts with iron atoms on the surface of the ferromagnetic powder to form a polymer complex, forming a flexible and heat-resistant protective layer, and passivation treatment is combined with epoxy resin to form a ferromagnetic powder.

Benefits of technology

The insulation and chemical corrosion resistance of ferromagnetic powder are improved, the reliability, stability and weather resistance of the inductor are enhanced, and the fragility problem of the phosphoric acid passivation layer is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115424801B_ABST
    Figure CN115424801B_ABST
Patent Text Reader

Abstract

The present application relates to the field of inductance technology, and provides a ferromagnetic powder, a preparation method and an application thereof. The ferromagnetic powder comprises a passivated ferromagnetic powder, wherein the passivated ferromagnetic powder comprises a ferromagnetic powder and a polymer protective layer attached to the surface of the ferromagnetic powder, wherein the polymer protective layer is a complex formed by the reaction of sulfonated polysulfone and iron on the surface of the ferromagnetic powder. The technical solution of the embodiment of the present application can improve the anti-corrosion, insulation and pressure resistance of the ferromagnetic powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of inductance technology, and in particular to a ferromagnetic powder material and a preparation method and application thereof. Background Art

[0002] Ferromagnetic powders with iron or iron alloys as the main body have very important applications in microelectronics, biology, medicine and other fields, especially in the field of electronics. The ferromagnetic materials here include pure iron, carbonyl iron, iron alloys, etc.

[0003] In current molded inductors, ferromagnetic powder accounts for more than 90% of the entire inductor. As the requirements for the magnetic permeability and inductance of inductors become higher and higher, in many scenarios, ferromagnetic powder is required to exhibit sufficient ferromagnetism as we need, while also having sufficient insulation. Especially after thermal aging or reflow soldering, the insulation requirements for inductors are getting higher and higher. This requires that ferromagnetic powders be well protected and passivated for insulation. In addition, in many scenarios, the requirements for the anti-corrosion and anti-rust properties of inductors are also getting higher and higher, which also poses a challenge to the anti-rust and anti-corrosion effects of inductor ferromagnetic powders.

[0004] At present, the mainstream process for protecting and passivating ferromagnetic powder is to use phosphoric acid for passivation, generate a thin layer of iron phosphate on the surface of magnetic powder particles, and coat the surface of ferromagnetic powder particles. This passivation layer has a certain protective effect on the ferromagnetic powder particles facing the influence of the external environment and insulation, but the coating and passivation effect is still not ideal. If the amount of phosphoric acid added is small or the passivation reaction time is short, the protection and passivation effect will not be obvious. If the amount of phosphoric acid added is increased, or the passivation time is extended, the protection and passivation effect will be improved, but more iron elements on the surface of ferromagnetic particles will be sacrificed (turned into non-magnetic iron phosphate and other substances), resulting in a sharp decline in ferromagnetism. In addition, the passivation layer generated by phosphoric acid passivation is an inorganic salt of phosphoric acid. The protective layer is hard and brittle. Under conditions such as thermal shock and physical pressure, it will break, resulting in the loss of the protective effect of the insulating protective layer and the degradation of device performance.

[0005] A Chinese patent with publication number CN109754977A discloses a preparation method for passivating and protecting ferromagnetic materials by using a five-layer coating material method, which can effectively improve the anti-corrosion and pressure resistance of magnetic powder particles. However, it is certain that the process is very complicated, the innermost layer of the five-layer coating is also passivated with phosphoric acid, and the five-layer coating has a great influence on the magnetic properties of the ferromagnetic powder. Summary of the invention

[0006] The main purpose of the embodiments of the present application is to provide a ferromagnetic powder and a preparation method and application thereof, which can solve one or more technical problems in the prior art.

[0007] In a first aspect, an embodiment of the present application provides a ferromagnetic powder, including passivated ferromagnetic powder, the passivated ferromagnetic powder including ferromagnetic powder and a polymer protective layer attached to the surface of the ferromagnetic powder, the polymer protective layer being a complex formed by the reaction of sulfonated polysulfone and iron on the surface of the ferromagnetic powder.

[0008] In some embodiments, the ferromagnetic powder includes one or more combinations of pure iron, iron alloys, or carbonyl iron.

[0009] In some embodiments, the amount of sulfonated polysulfone is within 0.01 wt % to 1 wt % of the ferromagnetic powder.

[0010] In some embodiments, the sulfonated polysulfone has a sulfonation degree within a range of 10% to 45%, and a weight average molecular weight within a range of 10,000 to 200,000 Daltons.

[0011] In some embodiments, epoxy resin is further included, and the amount of epoxy resin is within a range of 2 wt % to 25 wt % of the passivated ferromagnetic powder.

[0012] In a second aspect, an embodiment of the present application provides a method for preparing ferromagnetic powder, comprising: taking sulfonated polysulfone and a solvent, dissolving the sulfonated polysulfone in the solvent to obtain a solution; taking ferromagnetic powder, mixing the ferromagnetic powder with the solution, so that the sulfonated polysulfone reacts with the iron on the surface of the ferromagnetic powder to form a complex and adheres to the surface of the ferromagnetic powder; after the reaction is completed, removing the solvent and drying to obtain ferromagnetic powder.

[0013] In some embodiments, mixing the ferromagnetic powder with the solution includes: adding the ferromagnetic powder to the solution and stirring the solution at a temperature within a range of 20 to 150° C. for a period of 30 to 150 minutes.

[0014] In some embodiments, after the reaction is completed, the solvent is removed and dried to obtain ferromagnetic powder, including: after the reaction is completed, the mixture is allowed to stand for more than 3 minutes, and the lower layer of the mixture is taken out to volatilize the solvent and dry in a temperature environment within room temperature to 120°C to obtain ferromagnetic powder.

[0015] In some embodiments, the ferromagnetic powder includes one or more combinations of pure iron, iron alloys, or carbonyl iron.

[0016] In some embodiments, the amount of sulfonated polysulfone is within 0.01 wt% to 1 wt% of the ferromagnetic powder; the degree of sulfonation of the sulfonated polysulfone is within 10% to 45%, and the weight average molecular weight is within 10,000 to 200,000 Daltons.

[0017] In some embodiments, the solvent includes dichloromethane, chloroform, N,N-dimethylformamide, dimethylacetamide, or N-methylpyrrolidone.

[0018] In a third aspect, embodiments of the present application further provide an application of the ferromagnetic powder described in any embodiment of the first aspect in an inductor.

[0019] The embodiment of the present application is a technical solution provided to solve the problems of rust prevention, insulation and pressure resistance of ferromagnetic powder. Through the technical solution of the present application, a polymer protective layer can be formed on the surface of ferromagnetic powder. Specifically, the acidic functional groups of sulfonated polysulfone will complex with the iron atoms on the surface of the ferromagnetic powder and deposit on the surface of the ferromagnetic powder. The polymer protective layer has very good flexibility, strength and heat resistance, which can effectively isolate the external chemical corrosion and provide excellent insulation protection for the ferromagnetic powder. The preparation method of the embodiment of the present application is efficient and controllable. The obtained passivated ferromagnetic powder is applied to molded inductors, which will greatly improve the reliability, stability and weather resistance of the molded inductors. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0021] Figure 1 A schematic diagram of the structure of a passivated ferromagnetic powder provided in an embodiment of the present application;

[0022] Figure 2 A schematic flow chart of a method for preparing ferromagnetic powder provided in an embodiment of the present application. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0024] The flowcharts shown in the accompanying drawings are only examples and do not necessarily include all the contents and operations / steps, nor must they be executed in the order described. For example, some operations / steps may also be decomposed, combined or partially merged, so the actual execution order may change according to actual conditions.

[0025] It should be understood that the terms used in this application specification are only for the purpose of describing specific embodiments and are not intended to limit the application. As used in this application specification and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.

[0026] The embodiment of the present application provides a ferromagnetic powder material and a preparation method and application thereof. The ferromagnetic powder material can be applied to inductors, such as molded inductors. Inductors using the ferromagnetic powder material as an inductor blank have good reliability, stability and weather resistance.

[0027] Some embodiments of the present application are described in detail below in conjunction with the accompanying drawings. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0028] The present application provides a ferromagnetic powder material, including passivated ferromagnetic powder. Figure 1 The schematic diagram of the structure of the passivated ferromagnetic powder is shown, and the passivated ferromagnetic powder includes ferromagnetic powder 11 and a polymer protective layer 12 attached to the surface of the ferromagnetic powder 11. The polymer protective layer 12 is a complex formed by the reaction of sulfonated polysulfone and iron on the surface of the ferromagnetic powder.

[0029] In some embodiments, the ferromagnetic powder includes a combination of one or more of pure iron, iron alloy or carbonyl iron. The ferromagnetic powder can be crystalline or amorphous; spherical or non-spherical. In some embodiments, the iron alloy is an alloy of iron with one or more of nickel, cobalt, chromium, silicon, manganese, and carbon, for example, an alloy of iron with one or more of nickel, cobalt, chromium, silicon, manganese, and carbon accounting for 70 to 100 weight percent.

[0030] In some embodiments, the size of the ferromagnetic powder is 100 nanometers to 100 micrometers.

[0031] In some embodiments, the sulfonated polysulfone includes polysulfone plastics (PSU), polyarylsulfone, polyethersulfone, or polyphenylsulfone.

[0032] In some embodiments, the amount of sulfonated polysulfone is within 0.01 wt% to 1 wt% of the ferromagnetic powder. In some preferred embodiments, the amount of sulfonated polysulfone is within 0.05% to 0.5% of the ferromagnetic powder.

[0033] In some embodiments, the sulfonation degree of the sulfonated polysulfone is within a range of 10% to 45%; and the weight average molecular weight is within a range of 10,000 to 200,000 Daltons. In some preferred embodiments, the sulfonation degree of the sulfonated polysulfone is within a range of 20% to 40%.

[0034] In some embodiments, the ferromagnetic powder further comprises epoxy resin, and the amount of the epoxy resin is within 2 wt% to 25 wt% of the passivated ferromagnetic powder. The epoxy resin may comprise at least one of a liquid epoxy resin and a solid epoxy resin.

[0035] The present application also provides a method for preparing ferromagnetic powder. Figure 2 , Figure 2 The following is a schematic diagram of a method for preparing a ferromagnetic powder provided in an embodiment of the present application. Figure 2 As shown, a method for preparing ferromagnetic powder includes steps S210 to S230. It should be understood that Figure 2 Please refer to the above for the detailed description of the ferromagnetic powder in the illustrated embodiment, which will not be repeated here.

[0036] S210, taking sulfonated polysulfone and a solvent, and dissolving the sulfonated polysulfone in the solvent to obtain a solution.

[0037] In step S210, required weights of sulfonated polysulfone and solvent are weighed, and the polymer compound sulfonated polysulfone is added into the solvent to completely dissolve to obtain a solution.

[0038] In some embodiments, the solvent can be dichloromethane, chloroform, N,N-dimethylformamide (DMF), dimethylacetamide (DMAC), or N-methylpyrrolidone (NMP).

[0039] S220, taking ferromagnetic powder, and mixing the ferromagnetic powder with a solution, so that the sulfonated polysulfone reacts with iron on the surface of the ferromagnetic powder to form a complex and adheres to the surface of the ferromagnetic powder.

[0040] In step S220, ferromagnetic powder is added to the solution, and the solution is stirred and heated so that the sulfonated polysulfone reacts with iron on the surface of the ferromagnetic powder to form a complex and adheres to the surface of the ferromagnetic powder. Through this reaction, a polymer protective layer is formed on the surface of the ferromagnetic powder.

[0041] In some embodiments, ferromagnetic powder is added to the solution and stirred at a temperature of 20 to 150° C. for 30 to 150 minutes, so that the sulfonated polysulfone reacts with iron on the surface of the ferromagnetic powder to form a complex and adheres to the surface of the ferromagnetic powder.

[0042] S230, after the reaction is completed, the solvent is removed and the mixture is dried to obtain ferromagnetic powder.

[0043] In step S230, after the reaction is completed, the solvent is removed by heating or heating under reduced pressure and then dried to obtain ferromagnetic powder.

[0044] In some embodiments, after the reaction is completed, the solvent is removed and dried to obtain a passivated ferromagnetic powder, and then the passivated ferromagnetic powder is mixed with an epoxy resin to obtain a ferromagnetic powder.

[0045] In some embodiments, the epoxy resin may be a liquid epoxy resin, a solid epoxy resin, or a combination of a liquid epoxy resin and a solid epoxy resin.

[0046] As a liquid epoxy resin, it is preferably a liquid epoxy resin having more than two epoxy groups in the molecule, and more preferably an aromatic liquid epoxy resin having more than two epoxy groups in the molecule. Aromatic epoxy resin refers to an epoxy resin having an aromatic ring in its molecule. As a liquid epoxy resin, it is preferably a bisphenol A type epoxy resin, a bisphenol F type epoxy resin, a bisphenol AF type epoxy resin, a naphthalene type epoxy resin, a glycidyl ester type epoxy resin, a glycidyl amine type epoxy resin, an alicyclic epoxy resin with an ester skeleton, a cyclohexane type epoxy resin, a cyclohexanedimethanol type epoxy resin, a glycidyl amine type epoxy resin, and an epoxy resin with a butadiene structure, etc., more preferably a bisphenol A type epoxy resin, etc. They can be used alone or in combination of two or more.

[0047] As the solid epoxy resin, preferably a solid epoxy resin having three or more epoxy groups in the molecule. As the solid epoxy resin, preferably a bixylenol type epoxy resin, a naphthalene type epoxy resin, a naphthalene type tetrafunctional epoxy resin, a dicyclopentadiene type epoxy resin, a trisphenol type epoxy resin, a naphthol type epoxy resin, a biphenyl type epoxy resin, a naphthyl ether type epoxy resin, anthracene type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, tetraphenylethane type epoxy resin, etc., more preferably a naphthol type epoxy resin, a bisphenol AF type epoxy resin, a naphthalene type epoxy resin, and a biphenyl type epoxy resin, etc. These can be used alone or in combination of two or more.

[0048] In some embodiments, the epoxy equivalent of the epoxy resin is 50 g / eq to 5000 g / eq, preferably 50 g / eq to 3000 g / eq, more preferably 70 g / eq to 2000 g / eq, and further preferably 70 g / eq to 1000 g / eq. By reaching this range, a cured product with sufficient crosslinking density, excellent strength and heat resistance can be obtained.

[0049] In some embodiments, after the reaction is completed, the mixture is allowed to stand for more than 3 minutes, and the lower layer of the mixture is taken out to evaporate the solvent and dry in a temperature environment within a range from room temperature to 120° C. to obtain a ferromagnetic powder.

[0050] In order to better illustrate the technical solutions of the embodiments of the present application, several embodiments are further explained below.

[0051] Example 1

[0052] At room temperature, 0.3 g of sulfonated polysulfone with a sulfonation degree of 25% and a weight-average molecular weight of 85,000 Daltons was dissolved in 80 g of chloroform. After complete dissolution, 61 g of carbonyl iron powder and 39 g of iron-based amorphous powder were added to the chloroform solution. Stirring was started to fully disperse the ferromagnetic powder in the solution, and stirring was continued for 45 minutes. After the reaction was completed, it was allowed to stand for 10 minutes, and the supernatant was taken for testing. The lower layer mixture was directly heated to remove the chloroform, and further dried to obtain the passivated ferromagnetic powder. The passivated ferromagnetic powder was mixed with an epoxy resin accounting for 2.6% of the weight of the passivated ferromagnetic powder, granulated, and molded to make a sample of the ferromagnetic powder. After testing, the solid matter content in the supernatant was less than 0.013%, that is, the amount of sulfonated polysulfone remaining in the solution was less than 3.5%, and it can be seen that most of the sulfonated polysulfone was attached to the surface of the ferromagnetic powder.

[0053] In order to verify the performance of the ferromagnetic powder sample obtained in Example 1 of the present application, Comparative Example 1 is also provided. In Comparative Example 1, the sulfonated polysulfone in Example 1 is replaced with 0.07 grams of phosphoric acid, and other conditions are the same. Among them, the resins used in both Comparative Example 1 and Example 1 are 27 grams of bisphenol A type cyanate and 6 grams of bisphenol A type epoxy resin. The salt spray test standard uses a 5% sodium chloride saline solution, and the pH value of the solution is adjusted to a neutral range (6 to 7) as a spray solution. The performance comparison of the ferromagnetic powder samples obtained in Comparative Example 1 and Example 1 is shown in Table 1 below.

[0054] Table 1

[0055]

[0056] Example 2

[0057] At room temperature, 3.5 grams of sulfonated polysulfone with a sulfonation degree of 35% and a weight average molecular weight of 85,000 Daltons is dissolved in 600 grams of DMAC. After complete dissolution, 500 grams of carbonyl iron powder, 310 grams of iron-based amorphous powder, and 190 grams of alloy powder are added to the DMAC solvent. Stirring is started and heated to 90 degrees so that the ferromagnetic powder is fully dispersed in the solvent, and heating and stirring are continued for 30 minutes. After the reaction is completed, the powder in the mixture is precipitated and the supernatant is retained for testing. The precipitated powder is washed and dried to obtain a passivated ferromagnetic powder coated with sulfonated polysulfone. The passivated ferromagnetic powder is mixed with an epoxy resin accounting for 2.6% of the weight of the passivated ferromagnetic powder, granulated, and molded to make a sample of the ferromagnetic powder. According to the test, the solid matter content in the supernatant is less than 0.01%, that is, the amount of sulfonated polysulfone remaining in the solution is less than 1.8%, which shows that most of the sulfonated polysulfone is attached to the surface of the ferromagnetic powder.

[0058] In order to verify the performance of the ferromagnetic powder sample provided in Example 2 of the present application, Comparative Example 2 is also provided. In Comparative Example 2, the sulfonated polysulfone in Example 2 is replaced by 1 gram of phosphoric acid, and other conditions are the same. Among them, the resins used in both Comparative Example 2 and Example 2 are 27g of bisphenol A type cyanate and 6g of bisphenol A type epoxy resin. The salt spray test standard uses a 5% sodium chloride saline solution, and the pH value of the solution is adjusted to a neutral range (6 to 7) as a spray solution. The performance comparison of the ferromagnetic powder samples obtained in Comparative Example 2 and Example 2 is shown in Table 2 below.

[0059] Table 2

[0060]

[0061] The test results show that the complex obtained by reacting sulfonated polysulfone with the iron on the surface of ferromagnetic powder as a coating polymer protective layer has very good insulation and corrosion resistance for the ferromagnetic powder, thereby greatly improving the performance of the inductor.

[0062] It should be understood that the term "and / or" used in the present specification and the appended claims refers to any combination of one or more of the associated listed items and all possible combinations, including these combinations. It should be noted that, in this article, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or system including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or system. In the absence of further restrictions, an element defined by the sentence "including a..." does not exclude the presence of other identical elements in the process, method, article or system including the element.

[0063] The serial numbers of the embodiments of the present application are only for description and do not represent the advantages and disadvantages of the embodiments. The above are only specific embodiments of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed in the present application, and these modifications or replacements should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.

Claims

1. A ferromagnetic powder, characterized in that: The invention comprises a passivated ferromagnetic powder, which comprises ferromagnetic powder and a polymer protective layer attached to the surface of the ferromagnetic powder. The polymer protective layer is a complex formed by the reaction of sulfonated polysulfone and iron on the surface of the ferromagnetic powder.

2. The ferromagnetic powder according to claim 1, characterized in that: The ferromagnetic powder includes one or more combinations of pure iron, iron alloy or carbonyl iron.

3. The ferromagnetic powder according to claim 1 or 2, characterized in that: The amount of the sulfonated polysulfone is within 0.01wt% to 1wt% of the ferromagnetic powder.

4. The ferromagnetic powder according to claim 1 or 2, characterized in that: The sulfonation degree of the sulfonated polysulfone is within a range of 10% to 45%, and the weight average molecular weight is within a range of 10,000 to 200,000 Daltons.

5. The ferromagnetic powder according to claim 1 or 2, characterized in that: It also includes epoxy resin, and the amount of the epoxy resin is within 2wt% to 25wt% of the passivated ferromagnetic powder.

6. A method for preparing ferromagnetic powder, characterized in that: Taking sulfonated polysulfone and a solvent, dissolving the sulfonated polysulfone in the solvent to obtain a solution; Taking ferromagnetic powder, mixing the ferromagnetic powder with the solution, so that the sulfonated polysulfone reacts with iron on the surface of the ferromagnetic powder to form a complex and adheres to the surface of the ferromagnetic powder; After the reaction is completed, the solvent is removed and the mixture is dried to obtain ferromagnetic powder.

7. The preparation method according to claim 6, characterized in that: The mixing of the ferromagnetic powder and the solution comprises: adding the ferromagnetic powder to the solution and stirring the solution in a temperature environment within a range of 20 to 150° C. for a period of 30 to 150 minutes; The method comprises: after the reaction is completed, the solvent is removed and dried to obtain ferromagnetic powder, comprising: after the reaction is completed, the mixture is allowed to stand for more than 3 minutes, and the lower layer of the mixture is taken out to volatilize the solvent and dry in a temperature environment within a range of room temperature to 120° C. to obtain the ferromagnetic powder.

8. The preparation method according to claim 6 or 7, characterized in that: The ferromagnetic powder includes one or more combinations of pure iron, iron alloy or carbonyl iron.

9. The preparation method according to claim 6 or 7, characterized in that: The amount of the sulfonated polysulfone is within 0.01wt% to 1wt% of the ferromagnetic powder; the sulfonation degree of the sulfonated polysulfone is within 10% to 45%, and the weight average molecular weight is within 10,000 to 200,000 Daltons.

10. The preparation method according to claim 6 or 7, characterized in that: The solvent includes dichloromethane, chloroform, N,N-dimethylformamide, dimethylacetamide, or N-methylpyrrolidone.

11. Use of the ferromagnetic powder according to any one of claims 1 to 5 in inductance.