Polishing pad and method for manufacturing semiconductor device using the same

By using ether-bonded tertiary amine polyol as a curing agent in the polishing pad, controlling its surface roughness and elastic recovery coefficient, the problems of surface defects and hardness of semiconductor substrates caused by the polishing pad are solved, and more efficient Improved polishing and mechanical properties.

CN115431168BActive Publication Date: 2024-11-08SK ENPULSE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210629779.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-06-02
Filing Date
2022-06-02
Publication Date
2024-11-08
Estimated Expiration
2042-06-02

AI Technical Summary

Technical Problem

In the CMP process, existing polishing pads cause surface defects such as residues, scratches and tremors on the surface of semiconductor substrates, and the increase in hardness leads to poor polishing performance.

Method used

Polyurethane-based prepolymer compositions using tertiary amine polyols containing ether bonds as curing agents are formed to improve polishing by controlling the reduction rate of surface roughness and elastic recovery coefficient of the polishing pad within a specific range, a low hardness polishing layer is formed to improve polishing. performance.

Benefits of technology

It effectively reduces the hardness and surface roughness of the polishing pad, reduces surface defects on the semiconductor substrate, and improves the polishing rate and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115431168B_ABST
    Figure CN115431168B_ABST
Patent Text Reader

Abstract

The present invention discloses a polishing pad and a method for preparing a semiconductor device using the polishing pad. Specifically, a polishing pad for a chemical mechanical planarization process of a semiconductor, a method for preparing the polishing pad, and a method for preparing a semiconductor device using the polishing pad are disclosed. A polishing pad according to an embodiment can achieve low hardness by including a polishing layer formed by a curing agent using a specific component. By controlling the surface roughness reduction rate and elastic recovery coefficient of the polishing pad within a specific range, the mechanical properties of the polishing pad can be improved, and surface defects appearing on the surface of a semiconductor substrate can be improved. The polishing rate can also be further increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polishing pad and a method for preparing a semiconductor device using the polishing pad. Background Art

[0002] Chemical mechanical planarization (CMP) or chemical mechanical polishing (CMP) processes can be used for various purposes in various technical fields. The CMP process is performed on one side of the object to be polished. The CMP process is performed for the purpose of planarizing the surface to be polished, removing aggregated materials, addressing damage to the crystal lattice, and removing scratches and contamination sources.

[0003] In this CMP process, the polishing pad is an indispensable component that plays an important role. Generally, the polishing pad is composed of a polyurethane-based resin and has grooves for a large flow of slurry and holes for supporting a thin flow on its surface. Among them, the pores of the polishing pad can be formed by using a solid-phase foaming agent, a gas-phase foaming agent, or a liquid-phase foaming agent having pores, or can be formed by generating gas through a chemical reaction.

[0004] Since the polishing layer directly interacts with the semiconductor substrate surface during the CMP process, it affects the processing quality of the semiconductor substrate surface. In particular, the thermal stability and polishing stability of the CMP process may be affected by the composition and physical properties of the polishing layer and the shape of the pores.

[0005] Various studies have been conducted to solve this problem. For example, a method of improving the polishing rate and polishing stability by using 4,4'-methylenebis(2-chloroaniline) (MOCA) as a curing agent has been studied.

[0006] However, if MOCA is used as a curing agent, the hardness of the polishing pad will increase, resulting in severe hardening, and the surface roughness reduction rate will increase, resulting in poor glazing and polishing performance of the polishing pad. In addition, there is also the problem of increasing surface defects such as residues, scratches, and chatter marks on the surface of the semiconductor substrate.

[0007] [Prior art documents]

[0008] [Patent document]

[0009] (Patent Document 1) Korean Patent Publication No. 2008-0037719. Summary of the invention

[0010] Technical issues

[0011] The present invention aims to solve the above-mentioned problems in the prior art.

[0012] One of the objects of the present invention is to provide a polishing pad and a method for preparing the polishing pad, wherein the polishing pad can achieve low hardness by including a polishing layer formed using a curing agent of specific components, and can improve surface defects such as residues, scratches, and chatter marks on the surface of a semiconductor substrate by controlling the surface roughness reduction rate and elastic recovery coefficient of the polishing pad within a specific range, and can further increase the polishing rate.

[0013] Another object of the present invention is to provide a method for preparing a useful semiconductor device on a thin film substrate (semiconductor substrate) to be polished using a polishing pad.

[0014] Solution to the problem

[0015] The present invention provides a polishing pad, comprising a polishing layer, wherein the polishing layer comprises a cured product of a composition comprising a polyurethane-based prepolymer, a curing agent and a foaming agent, the curing agent comprises a tertiary amine-based polyol containing an ether bond, and the polishing pad has a surface roughness reduction rate (RSk (%)) of less than 50%, and a coefficient of elastic recovery (RERI) of 40 or less, the surface roughness reduction rate (RSk (%)) is represented by the following equation 1, and the coefficient of elastic recovery (RERI) is represented by the following equation 2:

[0016] [Equation 1]

[0017]

[0018] In Equation 1, Sk1 is the core roughness depth of the polishing pad before polishing, and Sk2 is the core roughness depth of the polishing pad measured after polishing the silicon oxide layer of the semiconductor substrate for 60 seconds under the conditions of a carrier pressure of 4.0 psi, a carrier rotation speed of 87 rpm and a platen rotation speed of 93 rpm, spraying a calcined cerium oxide slurry at a rate of 250 ml / min.

[0019] Sk1 and Sk2 are values ​​calculated from data before and after polishing of the polishing pad measured by an optical surface roughness meter according to ISO 25178-2, respectively.

[0020] [Equation 2]

[0021]

[0022] In equation 2, RSk (%) is defined as in equation 1 above, H 25 is the Shore D hardness of the polishing pad measured at 25° C., and the elastic recovery coefficient (RERI) is the ratio between the values ​​excluding units.

[0023] In addition, the present invention provides a method for preparing a polishing pad, which includes mixing a polyurethane-based prepolymer, a curing agent and a foaming agent to prepare a composition for preparing a polishing layer; and injecting the composition for preparing the polishing layer into a mold and curing it to obtain a polishing pad including a polishing layer, wherein the curing agent includes a tertiary amine polyol containing an ether bond, and the polishing pad has a surface roughness reduction rate (RSk (%)) of less than 50%, and an elastic recovery coefficient (RERI) of 40 or less, the surface roughness reduction rate (RSk (%)) is expressed by the above equation 1, and the elastic recovery coefficient (RERI) is expressed by the above equation 2.

[0024] In addition, the present invention provides a method for preparing a semiconductor device, which includes providing a polishing pad including a polishing layer; and making a polishing surface of the polishing layer and a surface of an object to be polished contact each other while relatively rotating to polish the object to be polished, wherein the polishing pad includes a polishing layer, the polishing layer includes a cured product of a composition including a polyurethane-based prepolymer, a curing agent and a foaming agent, the curing agent includes a tertiary amine polyol containing an ether bond, and the polishing pad has a surface roughness reduction rate (RSk (%)) of less than 50%, and an elastic recovery coefficient (RERI) of 40 or less, the surface roughness reduction rate (RSk (%)) is expressed by the above equation 1, and the elastic recovery coefficient (RERI) is expressed by the above equation 2.

[0025] Beneficial Effects of the Invention

[0026] The polishing pad according to the embodiment of the present invention can achieve low hardness by including a polishing layer formed using a curing agent of a specific component. By controlling the surface roughness reduction rate and elastic recovery coefficient of the polishing pad within a specific range, the mechanical properties of the polishing pad can be improved, and surface defects appearing on the surface of the semiconductor substrate can be improved. The polishing rate can also be further increased. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Schematically illustrates a method for preparing a semiconductor device according to an embodiment;

[0028] Figure 2 A graph showing the surface roughness obtained from an area material ratio curve based on the ISO 25178-2 standard when a polishing pad is measured using an optical surface roughness meter;

[0029] Figure 3 A method for preparing a polishing pad according to an embodiment of the present invention is shown;

[0030] Figure 4 A method for preparing a semiconductor device according to an embodiment of the present invention is shown;

[0031] Figure 5are scanning electron microscope (SEM) photographs of cross sections of the polishing pads prepared in Examples 1-3 and Comparative Example 1; Figure 5 (a) and 5(b) are scanning electron microscope (SEM) photographs of cross sections of the polishing pads prepared in Examples 1-3 and Comparative Example 1 analyzed at magnifications of 100 and 300, respectively;

[0032] Figure 6 is a photograph showing the shape of residue on a wafer according to an embodiment;

[0033] Figure 7 is a photograph showing the shape of a scratch on a wafer according to an embodiment;

[0034] Figure 8 is a photograph showing the shape of chatter marks on a wafer according to an embodiment. DETAILED DESCRIPTION

[0035] Best Mode for Carrying Out the Invention

[0036] Hereinafter, the present invention will be described in detail.

[0037] The advantages and features of the present invention and methods for achieving the advantages and features will become apparent with reference to the following embodiments. However, the present invention is not limited to the embodiments disclosed below, but will be implemented in various forms. These embodiments make the disclosure of the present invention complete and enable those of ordinary skill in the art to which the present invention belongs to fully understand the scope of the present invention. The present invention is limited only by the scope of the claims.

[0038] In order to clearly show the various layers and regions in the drawings, the thickness is exaggerated. For ease of explanation, the thickness of some layers and regions is exaggerated in the drawings. Throughout the specification, the same reference numerals refer to the same elements.

[0039] [Polishing pad]

[0040] In one embodiment of the present invention, there is provided a polishing pad comprising a polishing layer, wherein the polishing layer comprises a cured product of a composition comprising a polyurethane-based prepolymer, a curing agent and a foaming agent, the curing agent comprises a tertiary amine polyol containing an ether bond, and the polishing pad has a surface roughness reduction rate (RSk (%)) of less than 50%, and a coefficient of elastic recovery (RERI) of 40 or less, the surface roughness reduction rate (RSk (%)) is represented by the following equation 1, and the coefficient of elastic recovery (RERI) is represented by the following equation 2:

[0041] [Equation 1]

[0042]

[0043] In Equation 1, Sk1 is the core roughness depth of the polishing pad before polishing, and Sk2 is the core roughness depth of the polishing pad measured after polishing the silicon oxide layer of the semiconductor substrate for 60 seconds under the conditions of a carrier pressure of 4.0 psi, a carrier rotation speed of 87 rpm and a platen rotation speed of 93 rpm, spraying a calcined cerium oxide slurry at a rate of 250 ml / min.

[0044] Sk1 and Sk2 are values ​​calculated from data before and after polishing of the polishing pad measured by an optical surface roughness meter according to ISO 25178-2, respectively.

[0045] [Equation 2]

[0046]

[0047] In equation 2, RSk (%) is defined as in equation 1 above, H 25 is the Shore D hardness of the polishing pad measured at 25° C., and the elastic recovery coefficient (RERI) is the ratio between the values ​​excluding units.

[0048] The polishing process in the semiconductor manufacturing method is carried out in a manner that the polishing pad, the polishing slurry and the film material to be polished are closely combined. Generally, this process is carried out by applying the polishing slurry to the contact interface between the polishing pad and the film material to be polished.

[0049] Since the polishing pad includes a polishing layer containing pores, and since the polishing layer directly interacts with the surface of the semiconductor substrate during the CMP process, it affects the processing quality of the surface of the semiconductor substrate. In particular, mechanical properties such as hardness, tensile strength and elongation vary depending on the composition of the polishing layer, specifically, the composition of the prepolymer and the curing agent as the main raw materials of the polishing layer. In particular, among these physical properties, hardness has a significant effect not only on the polishing rate, which is an important property of the polishing pad, but also on the surface defects of the film material to be polished. Further, hardness also has an effect on the uniformity of the polishing removal rate.

[0050] Therefore, it is very important to properly design the composition of the polishing layer and control its physical properties within the required range.

[0051] Specifically, during polishing, a polishing slurry is applied to the polishing pad between the polishing pad and the semiconductor substrate, and chemical components in the polishing slurry react with the surface of the semiconductor substrate to form a reaction layer. When the polishing head and the polishing pad rotate relative to each other around their respective drive axes, the reaction layer is physically removed; therefore, the polishing surface of the semiconductor substrate attached to the polishing head and the polishing pad rub against each other in close contact.

[0052] Here, reactants, slurry particles, foreign matter, etc. on the semiconductor substrate are vitrified under high pressure and high temperature, and then adhere to the surface of the polishing pad, causing the so-called glazing phenomenon. Therefore, due to the difference in relative movement distance between the polishing pad and the semiconductor substrate, uneven surface deformation may occur. In this case, the polishing rate and surface roughness may be degraded, resulting in the problem of increased defects such as residues, scratches, and chatter marks on the film material to be polished (semiconductor substrate).

[0053] In particular, if the glazing phenomenon occurs in large quantities, the area in contact with the polishing surface of the semiconductor substrate increases, and polishing particles of the slurry are sandwiched between the area where glazing occurs and the polishing surface of the semiconductor substrate and aggregate, thereby causing more defects.

[0054] Therefore, a technical feature of one embodiment of the present invention is that the surface roughness reduction rate (RSk (%)) and the elastic recovery coefficient (RERI) of the polishing pad are controlled within a specific range or below, thereby reducing the glazing phenomenon and reducing the incidence of surface deformation of the polishing pad after polishing, thereby minimizing surface defects and degradation of polishing performance.

[0055] In this specification, the surface roughness reduction rate (RSk (%)) is the ratio (%) of the difference between the surface roughness of the polishing pad before and after polishing to the surface roughness of the polishing pad before polishing. It is represented by the following Equation 1.

[0056] [Equation 1]

[0057]

[0058] In Equation 1, Sk1 is the core roughness depth of the polishing pad before polishing, and Sk2 is the core roughness depth of the polishing pad measured after polishing the silicon oxide layer of the semiconductor substrate for 60 seconds under the conditions of a carrier pressure of 4.0 psi, a carrier rotation speed of 87 rpm and a platen rotation speed of 93 rpm, spraying a calcined cerium oxide slurry at a rate of 250 ml / min.

[0059] Sk1 and Sk2 are values ​​calculated from data before and after polishing of the polishing pad measured by an optical surface roughness meter according to ISO 25178-2, respectively.

[0060] In this specification, surface roughness refers to the surface roughness of a polishing pad, wherein the surface of the polishing pad is formed by machining or polishing. The optical surface roughness meter used in the present invention is a Contour GT model manufactured by Bruker. For detailed conditions for measuring the surface roughness of the polishing pad, refer to the embodiments of this specification.

[0061] If the surface roughness of the polishing pad is kept constant before, during and after polishing, glazing can be reduced, thereby maintaining a constant polishing rate and reducing surface defects occurring on the surface of the semiconductor substrate.

[0062] As an example, refer to Figure 1 A polishing pad is used in a CMP process, wherein the surface shape of the polishing pad is deformed by pressure applied in a vertical direction to a semiconductor substrate (or wafer) (120) attached to a head (110) and by shear stress applied in a horizontal direction by rotation of a platen (130) during the process.

[0063] The polishing pad is provided with grooves for a large flow of slurry (140) and holes for supporting a small flow thereof on its surface. In the polishing pad, not only the shape of the grooves on the surface but also the shape of the holes (150) deformed by external stress may cause the surface roughness of the polishing pad to change.

[0064] In particular, changes in pore shape and pore aggregation degree, which cause changes in the surface roughness of the polishing pad during polishing, may have an impact on the polishing rate, planarization of the semiconductor substrate, and residues, scratches, and chatter marks on the semiconductor substrate surface, which are important performances in the CMP process. Therefore, their control is particularly important.

[0065] The surface roughness of the polishing pad adjusted by these characteristics after polishing varies depending on the type of polyurethane-based prepolymer, foaming agent, and curing agent. In addition, the surface roughness may vary depending on the rotation speed of the mixing head when mixing the components, the degree of grooving, pretreatment conditions, etc. In addition, the surface roughness can be controlled by various variables.

[0066] The surface roughness reduction rate (RSk (%)) of the polishing pad according to one embodiment of the present invention is the ratio of the difference (Sk1-Sk2) between the core roughness depths of the polishing pad before polishing (Sk1) and after polishing (Sk2) to the core roughness depth of the polishing pad before polishing, expressed as a percentage (%). The surface roughness reduction rate RSk (%) can be, for example, less than 50%, for example, 48% or less, for example, 47% or less, for example, 45% or less, for example, 43% or less, for example, 42% or less, for example, 41% or less, for example, 38% or less, or for example, 35% or less. Specifically, the surface roughness reduction rate RSk(%) can be, for example, 5% to less than 50%, for example, 10% to 48%, for example, 15% to 48%, for example, 20% to 48, for example, 25% to 48%, for example, 30% to 48%, for example, 32% to 48%, for example, 34% to 47%, for example, 34% to 45%, for example, 34% to 42%, for example, 34% to 40%, or for example, 34% to 38%.

[0067] Since the surface roughness reduction rate RSk (%) of the polishing pad according to one embodiment of the present invention is adjusted to less than 50%, the glazing phenomenon is reduced, thereby improving the polishing rate and the surface defect characteristics occurring on the surface of the semiconductor substrate. If the surface roughness reduction rate (RSk (%)) is 50% or higher, the irregular surface deformation of the polishing pad due to the glazing phenomenon increases. Therefore, the polishing rate, the non-uniformity within the wafer, the surface roughness, etc. may be degraded, and the defects on the film material to be polished may increase.

[0068] The surface roughness reduction rate (RSk (%)) represented by Equation 1 can be calculated by measuring the core roughness depths of the polishing pad before and after polishing, respectively, and substituting the values ​​into Equation 1.

[0069] The surface roughness of the polishing pad, such as the core roughness depth of the polishing pad, can be obtained from the area material ratio curve measured by an optical surface roughness meter. The area material ratio curve is called the bearing area curve (BAC) or the profile support length ratio (Abbott-Firestone) curve. It is a curve graph plotted with the cumulative data of the unit area height measured by the surface roughness measuring device.

[0070] refer to Figure 2 The parameters obtained from the area-material ratio curve of surface roughness are S parameters, that is, parameters converted into depth (height), specifically Spk, Svk and Sk.

[0071] Spk is the reduced peak height that provides the initial contact area when the polishing pad contacts the surface of the semiconductor substrate during the CMP process; therefore, it refers to a surface composed of high peaks that provide high contact stress areas (force / area). Spk can refer to the nominal height of material that can be removed during operation.

[0072] Sk is the core roughness depth, which refers to the core roughness of the surface that can distribute the load after surface wear.

[0073] Svk is the reduced valley depth, which is a value obtained by measuring the valley depth under the surface core roughness, and is related to the slurry carrying capacity or the capture ability of polishing pad debris.

[0074] At the same time, Figure 2 In , SMr1 is the peak material portion, which refers to the ratio of the material constituting the peak structure associated with Spk.

[0075] In addition, SMr2 is the valley material portion, which refers to the percentage of the measured area constituting the deeper valley structure associated with Svk (100% - SMr2).

[0076] In particular, the polishing pad according to an embodiment of the present invention is characterized in that the surface roughness reduction rate (RSk(%)) is controlled using the core roughness depth (Sk) of the polishing pad among the S parameters. That is, in the polishing pad, the reduction rate of the core roughness of the surface capable of distributing the load after the surface is worn after polishing is controlled to be less than 50% compared with that before polishing; therefore, the polishing performance can be improved and the surface defects of the semiconductor substrate can be minimized.

[0077] Sk1 is the core roughness depth (μm) before polishing by the polishing pad. It may be 10 to 40, 10 to 35, 10 to 30, 15 to 30, 18 to 30, or 20 to 30. If Sk1 satisfies the above range, the polishing performance may be more excellent.

[0078] Sk2 is the core roughness depth (μm) of the polishing pad after polishing. It can be 3 to 30, 5 to 25, 9 to 25, 9 to 20, 10 to 18 or 12 to 17. If Sk2 meets the above range, it is more advantageous to achieve excellent polishing performance and low surface defect characteristics by reducing the surface roughness reduction rate (RSk (%)) of the polishing pad. Here, the silicon oxide layer of the semiconductor substrate can be polished for 60 seconds under the conditions of a carrier pressure of 4.0psi, a carrier rotation speed of 87rpm and a platen rotation speed of 93rpm, spraying a calcined cerium oxide slurry at a rate of 250 ml / min. Sk2 is the core roughness depth of the polishing pad measured after polishing under the above conditions.

[0079] The difference (Sk1-Sk2) (μm) between Sk1 and Sk2 may be 15 or less, 13 or less, 12 or less, 11 or less, 10 or less, or 9 or less. Specifically, the difference (Sk1-Sk2) (μm) between Sk1 and Sk2 may be 5 to 15, 7 to 13, 7 to 12, or 8 to 12. If the difference (Sk1-Sk2) between Sk1 and Sk2 satisfies the above range, excellent polishing performance and low surface defect characteristics can be achieved by reducing the surface roughness reduction rate (RSk (%)) of the polishing pad.

[0080] Meanwhile, the elastic recovery coefficient (RERI) quantifies the degree to which the performance of returning to the original state after polishing is hindered by elasticity. It may vary depending on the surface roughness reduction rate (RSk (%)) and hardness of the polishing pad.

[0081] The elastic recovery coefficient (RERI) can be expressed by the following equation 2, and the elastic recovery coefficient (RERI) is 40 or less:

[0082] [Equation 2]

[0083]

[0084] In equation 2, RSk (%) is defined as in equation 1 above, H 25 is the Shore D hardness of the polishing pad measured at 25° C., and the elastic recovery coefficient (RERI) is the ratio between the values ​​without units.

[0085] Specifically, according to one embodiment of the present invention, in order to achieve a low surface roughness reduction rate (RSk(%)) and a low hardness, the elastic recovery coefficient (RERI) can be controlled to be 40 or less. That is, the lower the surface roughness reduction rate (RSk(%)) and the hardness of the polishing pad are, the smaller the elastic recovery coefficient (RERI). The higher the surface roughness reduction rate (RSk(%)) and the hardness of the polishing pad are, the larger its value is. For example, if the surface roughness reduction rate (RSk(%)) of the polishing pad is low, and the difference between the surface roughness of the polishing pad after polishing and the surface roughness of the polishing pad before polishing is small, the elastic recovery coefficient (RERI) may be reduced. In this case, even if the protrusions of the surface roughness are tilted due to the polishing process, these protrusions may return to their original upright state due to the elasticity caused by the low hardness of the polishing pad. Therefore, it can reduce surface defects such as residues, scratches and chatter marks that appear on the surface of the semiconductor substrate. Therefore, the smaller the elastic recovery coefficient (RERI), the fewer surface defects appear on the surface of the semiconductor substrate.

[0086] The coefficient of elastic recovery (RERI) may specifically be, for example, 38 or less, for example, 35 or less, for example, 32 or less, for example, 30 or less, for example, 25 or less, for example, 23 or less, or for example, 20 or less. Since the coefficient of elastic recovery (RERI) satisfies the above range, defects occurring on the surface of the semiconductor substrate may be reduced.

[0087] Meanwhile, the polishing pad according to an embodiment of the present invention may have a low hardness. Specifically, the surface hardness of the polishing pad at 25° C. may be 40 to 60 Shore D, 40 to 55 Shore D, 40 to 52 Shore D, 40 to 50 Shore D, or 42 to 48 Shore D. If the surface hardness of the polishing pad at 25° C. satisfies the above range, the elastic recovery coefficient (RERI) required by an embodiment of the present invention may be advantageously controlled to be 40 or less, thereby minimizing defects occurring on the surface of the semiconductor substrate.

[0088] The polishing pad according to one embodiment of the present invention may have a strength of 10 N / mm 2 Up to 100N / mm 2 , 15N / mm 2 Up to 70N / mm 2 , 15N / mm 2 Up to 50N / mm 2or 15N / mm 2 Up to 40N / mm 2 In addition, the polishing pad according to an embodiment of the present invention may have a low tensile strength. For example, the polishing pad may have a tensile strength of 10 N / mm 2 Up to 25N / mm 2 , 15N / mm 2 Up to 25N / mm 2 or 16N / mm 2 Up to 25N / mm 2 tensile strength.

[0089] The polishing pad according to an embodiment of the present invention may have an elongation of 30% to 320% or 50% to 320%. In addition, the polishing pad according to an embodiment of the present invention may have a high elongation. For example, the polishing pad may have an elongation of 80% to 320%, 90% to 320%, 100% to 320%, 150% to 320%, 200% to 320%, or 220% to 320%.

[0090] The polishing pad according to one embodiment of the present invention may have a thickness of 0.6 g / cm 3 Up to 0.9g / cm 3 More specifically, the polishing pad may have a specific gravity of 0.7 g / cm 3 Up to 0.85g / cm 3 proportion, but not limited to this.

[0091] The polishing pad according to one embodiment of the present invention may have a surface hardness of 40 to 60 Shore D at 25° C. and a tensile strength of 10 N / mm. 2 Up to 25N / mm 2 , and the elongation is 80% to 320%.

[0092] Meanwhile, the polishing pad includes a plurality of holes.

[0093] In a polishing pad according to one embodiment of the present invention, the average diameter of the plurality of holes may be 5 μm to 200 μm. In addition, the average diameter of the plurality of holes may be 7 μm to 100 μm, 10 μm to 60 μm, 10 μm to 50 μm, 10 μm to 32 μm, or 20 μm to 32 μm. The average diameter of the plurality of holes is calculated as the number average of the hole diameters. For example, the polishing pad is observed at a magnification of 200 times using a scanning electron microscope (SEM). The diameter of each hole is measured from an image obtained using image analysis software, from which the average diameter (Da) is calculated. The average diameter is defined as the sum of the diameters of the plurality of holes divided by 1 mm. 2 The number of holes in the polished surface is obtained as an average value.

[0094] The pores include closed pores located inside the polishing pad and open pores located on the polishing surface of the polishing pad.

[0095] Specifically, in an open hole, the entrance of the hole is exposed on the polishing surface.

[0096] Here, the diameter of the open hole entrance refers to the diameter of a circle having the same plane area as the open hole entrance. In addition, the average diameter of the open hole entrance can be calculated by averaging the diameters of the entrances of a plurality of open holes present on the polishing surface.

[0097] Polishing pad per unit area (mm 2 ) may be 700 or more. More specifically, the polishing pad may have a plurality of holes per unit area (mm 2 ) can be 750 or more. Even more specifically, the polishing pad has a plurality of holes per unit area (mm 2 ) may be 800 or more. Even more specifically, the polishing pad may have a plurality of holes per unit area (mm 2 The total number of holes of the polishing pad may be 900 or more. However, it is not limited thereto. In addition, the polishing pad may have a plurality of holes per unit area (mm 2 The total number of holes of the polishing pad may be 2,500 or less, specifically 2,200 or less, 1,500 or less, or 1,200 or less, but is not limited thereto. 2 ) can be a total of 700 to 2,500 holes, such as 750 to 2,200, 800 to 1,500, or 800 to 1,200, but is not limited thereto.

[0098] Specifically, the polishing pad may have a 60 kgf / cm 2 More specifically, the polishing pad may have an elastic modulus of 100 kgf / cm 2 The upper limit of the elastic modulus of the polishing pad may be 150 kgf / cm 2 , but not limited to this.

[0099] The polishing pad according to an embodiment of the present invention may have a thickness of 1 mm to 10 mm. Specifically, the polishing pad may have a thickness of 1 mm to 9 mm, 1 mm to 8.5 mm, 1.5 mm to 10 mm, 1.5 mm to 9 mm, 1.5 mm to 8.5 mm, 1.8 mm to 10 mm, 1.8 mm to 9 mm, or 1.8 mm to 8.5 mm.

[0100] In addition, the polishing pad may have a thickness of 1 mm to 5 mm. Specifically, the polishing pad may have a thickness of 1 mm to 3 mm, 1 mm to 2.5 mm, 1.5 mm to 5 mm, 1.5 mm to 3 mm, 1.5 mm to 2.5 mm, 1.8 mm to 5 mm, 1.8 mm to 3 mm, or 1.8 mm to 2.5 mm. If the thickness of the polishing pad is within the above range, the basic physical properties of the polishing pad can be fully exerted.

[0101] As described above, since the surface roughness reduction rate (RSk(%)) and the elastic recovery coefficient (RERI) are controlled within a specific range or lower in the polishing pad according to one embodiment, the polishing rate can be increased and surface defects occurring on the surface of the semiconductor substrate can be reduced.

[0102] Meanwhile, when a semiconductor substrate including a silicon oxide layer is polished using the calcined ceria slurry, the polishing pad may have to to to or to If the polishing rate of the oxide layer is within the above range, the pad glazing phenomenon can be advantageously suppressed, thereby maintaining an appropriate level of excellent polishing rate in the subsequent repeated polishing process.

[0103] In addition, after polishing the silicon oxide layer under the above conditions, the number of surface defects occurring on the surface of the semiconductor substrate (wafer) measured using a defect inspection device (AIT XP+, KLA Tencor) can be 20 or less. Here, the number of surface defects can refer to the sum of residues, scratches, and chatter marks occurring on the surface of the semiconductor substrate.

[0104] Residue refers to substantially amorphous foreign matter attached to the surface of a semiconductor substrate. For example, it refers to Figure 6 Defects in the shape shown.

[0105] Scratches are essentially continuous linear scratches. For example, they are Figure 7 Defects in the shape shown.

[0106] Meanwhile, chatter marks refer to substantially discontinuous linear scratches. For example, it refers to Figure 8 Defects in the shape shown.

[0107] The number of surface defects occurring on the surface of the semiconductor substrate may be 15 or less, 10 or less, 8 or less, 7 or less, 5 or less, or 3 or less.

[0108] Meanwhile, the polishing pad may have grooves on its surface for mechanical polishing. The grooves may have a depth, width, and pitch required for mechanical polishing, without particular limitation.

[0109] The polishing pad according to an embodiment may simultaneously have the physical properties of the polishing pad as described above.

[0110] Meanwhile, a polishing pad according to an embodiment of the present invention includes a polishing layer, and the polishing layer includes a cured product of a composition including a polyurethane-based prepolymer, a curing agent, and a foaming agent.

[0111] According to one embodiment of the present invention, the surface roughness reduction rate (RSk (%)) and the elastic recovery coefficient (RERI) of the polishing pad can be changed according to the composition used to form the cured product. Specifically, the surface roughness reduction rate (RSk (%)) and the elastic recovery coefficient (RERI) of the polishing pad can be changed according to the polyurethane-based prepolymer, the curing agent and the foaming agent. In addition, the surface roughness reduction rate (RSk (%)) and the elastic recovery coefficient (RERI) of the polishing pad may vary due to the cleanliness of the raw materials of each component, the rotation speed of the mixing head when mixing the components, the degree of grooving, pretreatment conditions, etc. In addition, the above characteristics can be controlled by various variables.

[0112] Each component contained in the composition will be described in detail below.

[0113] According to one embodiment of the present invention, the curing agent used in the composition for forming the polishing layer includes a tertiary amino polyol containing an ether bond.

[0114] Since a tertiary amine polyol containing an ether bond is used as a curing agent in one embodiment of the present invention, it can chemically react with the polyurethane-based prepolymer to form a final cured structure in the polishing layer, and can achieve the desired properties of the polishing pad of the present invention.

[0115] Specifically, by using a tertiary amino polyol of a specific component in the composition for forming the polishing layer, a polishing pad with low hardness can be obtained, and the surface roughness reduction rate (RSk (%)) and elastic recovery coefficient (RERI) of the polishing pad can be controlled within the range required by the present invention.

[0116] The curing agent may include, for example, a compound represented by the following formula.

[0117] [Mode]

[0118]

[0119] In the above formula, n is an integer from 1 to 10. n can be, for example, 1 to 9, for example, 1 to 8, for example, 1 to 7, or for example, 1 to 6.

[0120] The curing agent may include, for example, a 1,2-ethylenediamine polymer compound containing methyl ethylene oxide, such as the trade name LA-480.

[0121] The tertiary amine polyol may have a weight average molecular weight (Mw) of 400 g / mole to 3,000 g / mole. Specifically, the weight average molecular weight of the tertiary amine polyol may be, for example, 400 g / mole to 2,700 g / mole, for example, 400 g / mole to 2,500 g / mole, for example, 400 g / mole to 2,490 g / mole, for example, 400 g / mole to 2,450 g / mole, for example, 400 g / mole to 2,400 g / mole, for example, 400 g / mole to 2,000 g / mole, for example, 400 g / mole to 1,800 g / mole, for example, 400 g / mole to 1,500 g / mole, for example, 400 g / mole to 1,300 g / mole, or for example, 400 g / mole to 1,000 g / mole. If the weight average molecular weight of the tertiary amino polyol satisfies the above range, an appropriate gelation time can be ensured during curing, a polishing pad with low hardness can be obtained, and the surface roughness reduction rate (RSk (%)) and elastic recovery coefficient (RERI) can be more advantageously controlled within the specific range required by the present invention.

[0122] If the weight average molecular weight of the tertiary amino polyol is too small, the gelation time may be shortened. Here, the composition for forming the polishing layer needs a certain time to gel by curing, which is called the gelation time. The gelation time of the composition may be at least 50 seconds, at least 70 seconds, at least 80 seconds, or at least 100 seconds. In addition, the gelation time of the composition may be at least 50 seconds, at least 70 seconds, at least 80 seconds, or at least 100 seconds. For example, the gelation time of the composition may be 50 seconds to 200 seconds, 50 seconds to 150 seconds, 50 seconds to 100 seconds, 100 seconds to 200 seconds, or 150 seconds to 200 seconds. As a specific embodiment, the gelation time of the composition may be 80 seconds to 120 seconds. The gelation time may be, for example, a value measured at 70°C.

[0123] According to one embodiment of the present invention, the curing agent may further include an aromatic amine compound, that is, the curing agent may include a mixture of a tertiary amine polyol and an aromatic amine compound.

[0124] The aromatic amine compound may include diethyltoluenediamine; 3,5-dimethylthio-2,4-toluenediamine; 3,5-diethyltoluene-2,4-diamine; N,N'-bis-(sec-butylamino)-diphenylmethane; 4,4'-methylene-bis-(3-chloro-2,6-diethylaniline); polytetrahydrofuran-bis-p-aminobenzoate; N,N'-dialkyldiaminodiphenylmethane; p,p'-methylenedianiline; m-phenylenediamine; 4,4'-methylene-bis-(2,6-diethylaniline); 4,4'-methylene-bis-(2,3 -dichloroaniline); 4,4'-diamino-3,3'-diethyl-5,5'-dimethyldiphenylmethane; 2,2',3,3'-tetrachlorodiaminodiphenylmethane; trimethylene glycol di-p-aminobenzoate; 3,5-diamino-4-chlorobenzoic acid-2-methylpropyl ester; bis(4-amino-2-chloro-3,5-diethylphenyl)methane; propylene glycol di-p-aminobenzoate; diaminochlorobutylbenzoate; methylene bis-o-aminobenzoate; chlorodiethyltoluenediamine; methylene bis-o-ethylaniline; and at least one of the group consisting of isomers thereof.

[0125] Specifically, the aromatic amine compound may include at least one selected from the group consisting of N,N'-bis-(sec-butylamino)-diphenylmethane; 3,5-diamino-4-chlorobenzoic acid-2-methylpropyl ester; bis(4-amino-2-chloro-3,5-diethylphenyl)methane; propylene glycol di-p-aminobenzoate; diaminochlorobutyl benzoate; methylene bis-o-aminobenzoate; chlorodiethyltoluenediamine; methylene di-o-ethylaniline; and their isomers.

[0126] The aromatic amine compound may include a secondary amine compound.

[0127] The aromatic amine compound may have a weight average molecular weight (Mw) of 450 g / mole to 600 g / mole, for example, 450 g / mole to 580 g / mole or 450 g / mole to 550 g / mole.

[0128] If a tertiary amino polyol and an aromatic amine compound are used together, a polishing pad having a low hardness can be obtained, and the surface roughness reduction rate (RSk (%)) and the elastic recovery coefficient (RERI) are advantageously controlled to the specific ranges required by the present invention.

[0129] However, the mixing weight ratio of the tertiary amine-based polyol to the aromatic amine compound may be a very important factor for controlling the mechanical properties and polishing performance of the polishing pad and controlling the surface defect characteristics of the semiconductor substrate.

[0130] Specifically, the content of the tertiary amine-based polyol may be equal to or greater than the content of the aromatic amine compound by weight.

[0131] For example, the weight content of the tertiary amine polyol may be greater than the weight content of the aromatic amine compound. If the content of the tertiary amine polyol is the same as or greater than the content of the aromatic amine compound, the core roughness depth (Sk2) of the polishing pad measured after polishing can be prevented from decreasing, which is more conducive to achieving the effect. That is, as the content of the tertiary amine polyol increases, the shape of the polishing pad can be well maintained even after polishing, and the surface roughness reduction rate (RSk (%)) of the polishing pad can be easily controlled.

[0132] In addition, if a mixture of a tertiary amino polyol and an aromatic amine compound is used as a curing agent according to one embodiment of the present invention, the isocyanate (NCO) group at the end of the polyurethane-based prepolymer reacts with the hydroxyl (OH) group of the tertiary amino polyol to form a carbamate bond, and the isocyanate (NCO) group at the end of the polyurethane-based prepolymer can react with the amine group (NH) of the aromatic amine compound to form a urea bond. In this case, the reaction rate of the carbamate bond may be faster than the reaction rate of the urea bond. That is, since the tertiary amino polyol can act as a catalyst, the reaction speed can be faster. In particular, since the non-shared electron pair of the tertiary amine in the tertiary amino polyol strongly attracts electrons, it can accelerate the reaction.

[0133] In addition, as the content of the tertiary amino polyol increases, the formation of urethane bonds becomes more active, which can improve the polishing characteristics when used. If the content of the aromatic amine compound is further increased, in the process of preparing a polishing layer by curing the composition for preparing a polishing layer, curing does not proceed well, causing problems.

[0134] According to one embodiment of the present invention, the mixing weight ratio of the tertiary amine polyol to the aromatic amine compound can be, for example, 5:5 to 9:1, for example, 5:5 to 8:2, for example, 6:4 to 9:1, for example, 6:4 to 8:2, or for example, 7:3 to 8:2.

[0135] Meanwhile, based on 100 parts by weight of the polyurethane-based prepolymer, the content of the curing agent may be about 18 parts by weight to about 27 parts by weight, such as about 19 parts by weight to about 26 parts by weight, such as about 20 parts by weight to about 26 parts by weight. If the content of the curing agent satisfies the above range, the desired surface properties of the polishing pad, specifically, the surface roughness reduction rate (RSk (%)) and the elastic recovery coefficient (RERI) can be more advantageously achieved.

[0136] In one embodiment, the curing agent may not include 4,4'-methylenebis(2-chloroaniline) (MOCA). If the curing agent includes 4,4'-methylenebis(2-chloroaniline), the hardness increases, making it difficult to achieve the desired effect of the present invention.

[0137] According to one embodiment of the present invention, the composition for forming the polishing layer includes a polyurethane-based prepolymer.

[0138] Prepolymers generally refer to polymers with relatively low molecular weights, in which the degree of polymerization is adjusted to a moderate level in order to facilitate molding in the process of producing cured products. Prepolymers can be molded into final cured products alone or after reacting with another polymerizable compound.

[0139] In one embodiment, the polyurethane-based prepolymer may be prepared by reacting an isocyanate compound with a polyol.

[0140] The isocyanate compound used for preparing the polyurethane-based prepolymer may be one selected from the group consisting of aromatic diisocyanate, aliphatic diisocyanate, alicyclic diisocyanate, or a combination thereof.

[0141] For example, the isocyanate compound may include one selected from the group consisting of 2,4-toluene diisocyanate (2,4-TDI), 2,6-toluene diisocyanate (2,6-TDI), naphthalene-1,5-diisocyanate, p-phenylene diisocyanate, toluene diisocyanate, 4,4′-diphenylmethane diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, and combinations thereof.

[0142] The polyol is a compound containing at least two or more hydroxyl groups (—OH) per molecule. For example, it may include one selected from the group consisting of polyether polyol, polyester polyol, polycarbonate polyol, acryl polyol, and a combination thereof.

[0143] For example, the polyol may include one selected from the group consisting of polytetramethylene ether glycol, polypropylene ether glycol, ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 2-methyl-1,3-propylene glycol, 1,4-butylene glycol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol, tripropylene glycol, and combinations thereof.

[0144] The polyol may have a weight average molecular weight (Mw) of about 100 g / mole to about 3,000 g / mole. For example, the polyol may have a weight average molecular weight (Mw) of about 100 g / mole to about 3,000 g / mole, such as about 100 g / mole to about 2,000 g / mole, such as about 100 g / mole to about 1,800 g / mole.

[0145] In one embodiment, the polyol may include a low molecular weight polyol having a weight average molecular weight (Mw) of about 100 g / mole to less than about 300 g / mole and a high molecular weight polyol having a weight average molecular weight (Mw) of about 300 g / mole to about 1,800 g / mole.

[0146] The polyurethane-based prepolymer may have a weight average molecular weight (Mw) of about 500 g / mole to about 3,000 g / mole. The polyurethane-based prepolymer may have, for example, a weight average molecular weight (Mw) of about 1,000 g / mole to about 2,000 g / mole, such as about 1,000 g / mole to about 1,500 g / mole.

[0147] In one embodiment, the isocyanate compound used to prepare the polyurethane-based prepolymer may include an aromatic diisocyanate compound, and the aromatic diisocyanate compound, for example, may include 2,4-toluene diisocyanate (2,4-TDI) and 2,6-toluene diisocyanate (2,6-TDI). The polyol compound used to prepare the polyurethane-based prepolymer may include polytetramethylene ether glycol (PTMEG) and diethylene glycol (DEG).

[0148] In another embodiment, the isocyanate compound for preparing the polyurethane-based prepolymer may include an aromatic diisocyanate compound and an alicyclic diisocyanate compound. For example, the aromatic diisocyanate compound may include 2,4-toluene diisocyanate (2,4-TDI) and 2,6-toluene diisocyanate (2,6-TDI), and the alicyclic diisocyanate compound may include dicyclohexylmethane diisocyanate (H12MDI). The polyol compound for preparing the polyurethane-based prepolymer may include polytetramethylene ether glycol (PTMEG) and diethylene glycol (DEG).

[0149] The polyurethane-based prepolymer may have an isocyanate end group content (NCO %) of about 9 wt % to about 12 wt %, such as about 9 wt % to about 11 wt %, such as about 9 wt % to about 10 wt %, such as about 10 wt % to about 12 wt %, or such as about 10 wt % to about 11 wt %.

[0150] The isocyanate end group content (NCO%) of the polyurethane-based prepolymer can be designed by comprehensively adjusting the types and contents of the isocyanate compounds and polyol compounds used to prepare the polyurethane-based prepolymer, the process conditions such as temperature, pressure and time in the process of preparing the polyurethane-based prepolymer, and the types and contents of the additives used to prepare the polyurethane-based prepolymer.

[0151] If the isocyanate terminal group content (NCO%) of the polyurethane-based prepolymer satisfies the above range, the reaction rate, reaction time and final cured structure in the subsequent reaction of the polyurethane-based prepolymer with the curing agent can be adjusted in a manner favorable to the polishing performance from the perspective of the use and purpose of the final polishing pad.

[0152] According to one embodiment of the present invention, the composition for forming the polishing layer includes a foaming agent.

[0153] The foaming agent is a component for forming a pore structure in the polishing layer, and it may include a solid-phase foaming agent.

[0154] According to one embodiment of the present invention, the shape of micropores and the pore coalescence phenomenon can be controlled according to the type, shape or physical properties of the solid-phase foaming agent. Therefore, the surface roughness of the polishing pad before and after polishing can be adjusted.

[0155] The solid phase foaming agent may include expandable particles. Expandable particles are particles having the property of being expandable by heat or pressure. The size of the final polishing layer may be determined by the heat or pressure applied during the preparation of the polishing layer. The expandable particles may include heat-expandable particles, unexpanded particles, or a combination thereof.

[0156] Thermally expandable particles are particles that have been thermally expanded in advance. They are particles whose size changes little or not at all by applying heat or pressure during the process of preparing the polishing layer.

[0157] Unexpanded particles are particles that have not been thermally expanded in advance. They refer to particles whose final size is determined when they are expanded by heating or pressurization during the process of preparing the polishing layer. According to one embodiment of the present invention, from the perspective of achieving a more uniform pore size distribution of the polishing pad, the solid-phase foaming agent may preferably include unexpanded particles.

[0158] The solid phase foaming agent comprising unexpanded particles may be microspheres encapsulating a hydrocarbon gas with a polymer shell.

[0159] The expandable particles may include a resin shell; and an expansion inducing component encapsulated within the shell.

[0160] For example, the shell may include a thermoplastic resin. The thermoplastic resin may be at least one selected from the group consisting of a vinylidene chloride-based copolymer, an acrylonitrile-based copolymer, a methacrylonitrile-based copolymer, and an acrylic acid-based copolymer.

[0161] The expansion inducing component may include one selected from the group consisting of hydrocarbon compounds, chlorofluoro compounds, tetraalkylsilane compounds, and combinations thereof.

[0162] Specifically, the hydrocarbon may include one selected from the group consisting of ethane, ethylene, propane, propylene, n-butane, isobutane, n-butene, isobutene, n-pentane, isopentane, neopentane, n-hexane, heptane, petroleum ether, and combinations thereof.

[0163] The chlorofluorine compound may include one selected from the group consisting of trichlorofluoromethane (CCl3F), dichlorodifluoromethane (CCl2F2), chlorotrifluoromethane (CClF3), tetrafluoroethylene (CClF2-CClF2), and combinations thereof.

[0164] The tetraalkylsilane compound may include one selected from the group consisting of tetramethylsilane, trimethylethylsilane, trimethylisopropylsilane, trimethyl-n-propylsilane, and combinations thereof.

[0165] The solid phase foaming agent may optionally include particles treated with an inorganic component. For example, the solid phase foaming agent may include expandable particles treated with an inorganic component. In one embodiment, the solid phase foaming agent may include expandable particles treated with silicon dioxide (SiO2) particles. Treating the solid phase foaming agent with an inorganic component can prevent aggregation between multiple particles. The solid phase foaming agent treated with an inorganic component may be different from a solid phase foaming agent that has not been treated with an inorganic component in terms of chemical, electrical and / or physical properties on the foaming agent surface.

[0166] The solid phase foaming agent may be included in an amount of about 0.5 to about 10.0 parts by weight, such as about 1.0 to about 6.0 parts by weight, such as about 1.5 to about 5.5 parts by weight, such as about 2.0 to about 5.0 parts by weight, based on 100 parts by weight of the polyurethane-based prepolymer.

[0167] According to an embodiment of the present invention, since a solid-phase foaming agent is used, excellent polishing characteristics and mechanical properties can be achieved without using a liquid-phase foaming agent, a gas-phase foaming agent, or both.

[0168] The type and content of the solid-phase foaming agent can be designed according to the desired pore structure and physical properties of the polishing layer.

[0169] The composition for preparing the polishing layer may further include other additives such as surfactants and reaction rate controllers. Names such as "surfactant" and "reaction rate controller" are arbitrarily named according to the main function of the substance. Each substance does not necessarily perform functions limited to the functions defined by the name.

[0170] The surfactant is not particularly limited as long as it plays a role in preventing pores from agglomerating and overlapping with each other. For example, the surfactant may include a siloxane-based surfactant.

[0171] Based on the polyurethane-based prepolymer of 100 weight parts, the surfactant can be used with an amount of about 0.2 weight part to about 2 weight parts. Specifically, based on the polyurethane-based prepolymer of 100 weight parts, the surfactant can be used with an amount of about 0.2 weight part to about 1.9 weight parts, such as about 0.2 weight part to about 1.8 weight parts, such as about 0.2 weight part to about 1.7 weight parts, such as about 0.2 weight part to about 1.6 weight parts, such as about 0.2 weight part to about 1.5 weight parts, such as 0.5 weight part to 1.5 amount use. If the amount of the surfactant is within the above range, then a hole can be stably formed and maintained in a mold.

[0172] The reaction rate controller is used to promote or delay the reaction. Depending on the purpose, a reaction promoter, a reaction retarder or both can be used. The reaction rate controller can include a reaction promoter. For example, the reaction rate controller can be at least one reaction promoter selected from the group consisting of a tertiary amine compound and an organometallic compound.

[0173] Specifically, the reaction rate control agent may include a compound selected from triethylenediamine, dimethylethanolamine, tetramethylbutylenediamine, 2-methyl-triethylenediamine, dimethylcyclohexylamine, triethylamine, triisopropanolamine, 1,4-diazabicyclo (2,2,2) octane, bis (2-methylaminoethyl) ether, trimethylaminoethylethanolamine, N,N,N,N,N "-pentamethyldiethylenetriamine, dimethylaminoethylamine, dimethylaminopropylamine, benzyldimethylamine, N-ethyl At least one of the group consisting of morpholine, N,N-dimethylaminoethylmorpholine, N,N-dimethylcyclohexylamine, 2-methyl-2-azanorbornane, dibutyltin dilaurate, stannous octoate, dibutyltin diacetate, dioctyltin diacetate, dibutyltin maleate, di-2-ethylhexanoate dibutyltin and dibutyltin dithiol. Specifically, the reaction rate control agent may include at least one selected from the group consisting of benzyldimethylamine, N,N-dimethylcyclohexylamine and triethylamine.

[0174] Based on 100 parts by weight of the polyurethane-based prepolymer, the amount of the reaction rate controller can be from about 0.05 parts by weight to about 2 parts by weight. Specifically, based on 100 parts by weight of the polyurethane-based prepolymer, the reaction rate controller can be from about 0.05 parts by weight to about 1.8 parts by weight, for example, from about 0.05 parts by weight to about 1.7 parts by weight, for example, from about 0.05 parts by weight to about 1.7 parts by weight, for example, from about 0.05 parts by weight to about 1.6 parts by weight, for example, from about 0.1 parts by weight to about 1.5 parts by weight, for example, from about 0.1 parts by weight to about 0.3 parts by weight, for example, from about 0.2 parts by weight to about 1.8 parts by weight, for example, from about 0.2 parts by weight to about 1.7 parts by weight, for example, from about 0.2 parts by weight to about 1.6 parts by weight, for example, from about 0.2 parts by weight to about 1.5 parts by weight, for example, 0.5 parts by weight to about 1 part by weight. If the reaction rate controller is used within the above content range, the curing reaction rate of the prepolymer composition can be appropriately controlled to form a polishing layer having pores of a desired size and hardness.

[0175] In one embodiment, the content of inorganic substances in the polishing layer may be from about 5 ppm to about 500 ppm.

[0176] For example, the inorganic substance may include at least one element selected from the group consisting of silicon (Si) element, phosphorus (P) element, and calcium (Ca) element.

[0177] The inorganic substance can come from various sources. For example, the inorganic substance can come from various additives, such as a foaming agent for preparing the polishing layer. Here, the additive as a source of the inorganic substance can include, for example, one selected from the group consisting of a foaming agent, a surfactant, a reaction rate control agent, and a combination thereof.

[0178] The content of the inorganic substance in the polishing layer can be designed within an appropriate range by using only one of the foaming agent and the additional additive and adjusting the kind and content thereof, or by using both the foaming agent and the additional additive and adjusting their kinds and contents.

[0179] The content of inorganic substances in the polishing layer may be about 5 ppm to about 500 ppm, for example, about 5 ppm to about 400 ppm, for example, about 8 ppm to about 300 ppm, for example, about 220 ppm to about 400 ppm, for example, about 5 ppm to about 180 ppm. In this case, the content of inorganic substances in the polishing layer may be measured by inductively coupled plasma atomic emission spectrometer (ICP) analysis.

[0180] Hereinafter, a method for preparing a polishing pad will be described in detail.

[0181] [Method for preparing polishing pad]

[0182] In another embodiment of the present invention, a method for preparing a polishing pad can be provided, the method comprising mixing a polyurethane-based prepolymer, a curing agent and a foaming agent to prepare a composition for preparing a polishing layer; injecting the composition for preparing the polishing layer into a mold and curing it to obtain a polishing pad including a polishing layer, wherein the curing agent comprises a tertiary amine polyol containing an ether bond, and the polishing pad has a surface roughness reduction rate (RSk (%)) of less than 50%, and an elastic recovery coefficient (RERI) of 40 or less, the surface roughness reduction rate (RSk (%)) is expressed by the above equation 1, and the elastic recovery coefficient (RERI) is expressed by the above equation 2.

[0183] refer to Figure 3 , a method ( S100 ) for preparing a polishing pad including a polishing layer includes a step ( S110 ) of preparing a composition for preparing a polishing layer.

[0184] The composition for preparing the polishing layer may be obtained by mixing a polyurethane-based prepolymer, a curing agent, and a foaming agent.

[0185] The polyurethane-based prepolymer can be prepared by reacting a diisocyanate compound with a polyol compound. The details of the diisocyanate compound and the polyol compound are as described above with respect to the polishing pad.

[0186] The prepolymer composition can have an isocyanate group (NCO group) content of about 9 wt % to about 12 wt %, such as about 9 wt % to about 11 wt %, such as about 9 wt % to about 11 wt %, such as about 10 wt % to about 12 wt % or such as about 10 wt % to about 11 wt %.

[0187] The content of the isocyanate group in the polyurethane-based prepolymer composition may be derived from the terminal isocyanate group of the polyurethane-based prepolymer, the unreacted isocyanate group in the diisocyanate compound, and the like.

[0188] The polyurethane-based prepolymer composition may have a viscosity of about 100 cps to about 1,000 cps, such as about 200 cps to about 800 cps, such as about 200 cps to about 600 cps, such as about 200 cps to about 550 cps, such as about 300 cps to about 500 cps at about 80°C.

[0189] The detailed compositions of the blowing agent and curing agent are as described above.

[0190] The polyurethane-based prepolymer and the curing agent react with each other when they are mixed to form a solid polyurethane, which is then formed into a sheet or the like. Specifically, the isocyanate (NCO) terminal group in the polyurethane-based prepolymer can react with an amine group, an alcohol group, etc. in the curing agent. Specifically, the isocyanate (NCO) group at the end of the polyurethane-based prepolymer reacts with a hydroxyl (OH) group of a tertiary amino polyol to form a urethane bond. In addition, the isocyanate (NCO) group at the end of the polyurethane-based prepolymer reacts with an amine (NH) group of an aromatic amine compound to form a urea bond.

[0191] If a mixture of a tertiary amino polyol and an aromatic amine compound is used as a curing agent, the reaction rate of the isocyanate (NCO) group at the end of the polyurethane-based prepolymer and the hydroxyl (OH) group of the tertiary amino polyol to form a urethane bond is faster than the reaction rate of the isocyanate (NCO) group at the end of the polyurethane-based prepolymer and the amine (NH) group of the aromatic amine compound to form a urea bond. That is, since the tertiary amino polyol can act as a catalyst, the reaction speed can be faster. In particular, since the non-shared electron pair of the tertiary amine in the tertiary amino polyol strongly attracts electrons, it can accelerate the reaction.

[0192] In this case, a foaming agent such as a solid-phase foaming agent is uniformly dispersed in the raw material to form pores without participating in the reaction between the polyurethane-based prepolymer and the curing agent.

[0193] According to one embodiment of the present invention, the polyurethane-based prepolymer, curing agent and blowing agent can be mixed at the same time. In addition, if a surfactant, an inert gas, etc. are further added, they can also be mixed at the same time.

[0194] As another example, the polyurethane-based prepolymer, the blowing agent, and the surfactant may be premixed, and then the curing agent may be introduced.

[0195] During the mixing process, the polyurethane-based prepolymer and the curing agent initiate a reaction by mixing, and the blowing agent is uniformly dispersed in the raw material. In this case, the reaction rate controller can intervene in the reaction between the polyurethane-based prepolymer and the curing agent mixture from the beginning of the reaction, thereby controlling the reaction rate. Specifically, the mixing can be performed at a rate of 1,000rpm to 10,000rpm or 4,000rpm to 7,000rpm. Within the above speed range, the blowing agent can be more advantageously uniformly dispersed in the raw material.

[0196] The method of preparing a polishing pad ( S100 ) includes injecting a composition for preparing a polishing layer into a mold and curing ( S120 ) to obtain a polishing pad including a polishing layer.

[0197] In one embodiment, the step of obtaining a polishing pad including a polishing layer includes preparing a mold preheated to a first temperature; and injecting a composition for preparing a polishing layer as a raw material mixture into the preheated mold and curing the mixture.

[0198] In one embodiment, when the composition for preparing the polishing layer is injected into the preheated mold, an inert gas may not be injected, specifically, an inert gas, specifically nitrogen (N2) may not be injected. Generally, when the composition for preparing the polishing layer is injected, for example, nitrogen (N2) may be injected. In the present invention, if an inert gas is injected, the density may become unstable due to the use of a tertiary amino polyol of a specific component. In particular, if a tertiary amino polyol is used as a curing agent, the curing speed is fast, so it may be difficult to inject an inert gas.

[0199] In one embodiment, the first temperature may be from about 60°C to about 120°C, such as from about 65°C to about 110°C, such as from about 70°C to about 110°C.

[0200] The step of curing the composition for preparing a polishing layer at the first temperature can be performed for about 5 minutes to about 60 minutes, such as about 5 minutes to about 40 minutes, such as about 5 minutes to about 30 minutes, such as about 5 minutes to about 25 minutes.

[0201] The reaction between the polyurethane-based prepolymer and the curing agent is completed in the mold, thereby producing a molded body in the form of a cured block that conforms to the shape of the mold.

[0202] Afterwards, the molded body thus obtained can be appropriately sliced ​​or cut into sheets for the production of polishing pads. For example, a molded body is prepared in a mold having a height of 5 to 50 times the thickness of the polishing pad finally produced, and then sliced ​​with the same thickness to produce multiple sheets for polishing pads at one time. In this case, a reaction retarder can be used as a reaction rate controller to ensure sufficient curing time. Therefore, the height of the mold can be about 5 times to about 50 times the thickness of the polishing pad finally produced to prepare sheets therefor. However, the sliced ​​sheets can have holes of different diameters depending on the molding position in the mold. That is, the sheet molded in the lower part of the mold can have holes of fine diameter, while the sheet molded in the upper part of the mold can have holes of larger diameter than the sheet formed in the lower part.

[0203] Therefore, it is preferred to use a mold that can produce one sheet by one-time molding so that each sheet has a hole of uniform diameter. For this reason, the height of the mold may not be significantly different from the thickness of the polishing pad finally produced. For example, a mold having a height of 1 to 3 times the thickness of the polishing pad finally produced can be used for molding. More specifically, the height of the mold can be 1.1 to 4.0 times, or 1.2 to 3.0 times the thickness of the polishing pad finally produced. In this case, a reaction promoter can be used as a reaction rate controller to form holes with a more uniform diameter. The polishing pad prepared from a single sheet can have a thickness of 1 mm to 10 mm. Specifically, the polishing pad can have a thickness of 1 mm to 9 mm, 1 mm to 8.5 mm, 1.5 mm to 10 mm, 1.5 mm to 9 mm, 1.5 mm to 8.5 mm, 1.8 mm to 10 mm, 1.8 mm to 9 mm, or 1.8 mm to 8.5 mm.

[0204] Thereafter, the top and bottom ends of the molded body obtained from the mold may be cut, respectively. For example, each of the top and bottom ends of the molded body may be cut off by 1 / 3 or less, 1 / 22 to 3 / 10, or 1 / 12 to 1 / 4 of the total thickness of the molded body.

[0205] As a specific embodiment, molding is performed using a mold having a height of 1.2 to 2 times the thickness of the final polishing pad, and then a step can be further performed to cut out the top and bottom ends of the molded body obtained from the mold at the time of molding, which are 1 / 12 to 1 / 4 of the total thickness of the molded body.

[0206] After the above-mentioned cutting step, the above-mentioned preparation process may further include the steps of machining grooves on the surface of the molded body, bonding with a lower part, testing, packaging, etc. These steps may be carried out in a conventional manner for preparing a polishing pad.

[0207] Furthermore, the polishing pad produced by the above-described production method can have all the characteristics of the polishing pad according to the above-described embodiment.

[0208] Meanwhile, according to an embodiment, the process may further include machining the polishing layer.

[0209] The step of machining at least one side of the polishing layer may include: (1) forming grooves on at least one side of the polishing layer; (2) wire turning at least one side of the polishing layer; and (3) roughening at least one side of the polishing layer.

[0210] In step (1), the grooves may include at least one concentric circular groove spaced a certain distance from the center of the polishing layer; and radial grooves continuously connected from the center of the polishing layer to the edge of the polishing layer.

[0211] In step (2), wire turning may be performed by cutting the polishing layer into a certain thickness using a cutting tool.

[0212] In step (3), the roughening may be performed by mechanically processing the surface of the polishing layer with a grinding wheel.

[0213] The method of preparing the polishing pad may further include laminating a buffer layer on a side of the polishing layer opposite to the polishing surface.

[0214] The polishing layer and the buffer layer may be laminated using a heat seal adhesive.

[0215] Heat seal adhesive is applied to the side of the polishing layer opposite to the polishing surface, heat seal adhesive is applied to the side of the buffer layer in contact with the polishing layer, the polishing layer and the buffer layer are laminated so that the sides to which the heat seal adhesive has been applied are in contact, and a pressure wheel can be used to fuse the two layers.

[0216] The buffer layer is used to support the polishing layer and absorb and disperse the impact applied to the polishing layer. Therefore, damage and defects to the object to be polished during the polishing process using the polishing pad can be minimized.

[0217] The cushioning layer may include non-woven fabric or suede, but is not limited thereto.

[0218] In one embodiment, the buffer layer may be a resin-impregnated nonwoven fabric. The nonwoven fabric may be a nonwoven fabric including a fiber selected from the group consisting of polyester fiber, polyamide fiber, polypropylene fiber, polyethylene fiber and a combination thereof.

[0219] The resin impregnated in the non-woven fabric may include polyurethane resin, polybutadiene resin, styrene-butadiene copolymer resin, styrene-butadiene-styrene copolymer resin, acrylonitrile-butadiene copolymer resin, styrene-ethylene-butadiene-styrene copolymer resin, silicone rubber resin, polyester-based elastomer resin, polyamide-based elastomer resin and combinations thereof.

[0220] [Method for manufacturing semiconductor device]

[0221] According to another embodiment of the present invention, a method for preparing a semiconductor device is provided, which includes providing a polishing pad including a polishing layer; and making a polishing surface of the polishing layer and a surface of an object to be polished contact each other while relatively rotating to polish the object to be polished, wherein the polishing pad includes a polishing layer, the polishing layer includes a cured product of a composition including a polyurethane-based prepolymer, a curing agent and a foaming agent, the curing agent includes a tertiary amine polyol containing an ether bond, and the polishing pad has a surface roughness reduction rate (RSk (%)) of less than 50%, and an elastic recovery coefficient (RERI) of 40 or less, the surface roughness reduction rate (RSk (%)) is expressed by the above equation 1, and the elastic recovery coefficient (RERI) is expressed by the above equation 2.

[0222] refer to Figure 4 , a method of manufacturing a semiconductor device ( S200 ) includes providing a polishing pad including a polishing layer ( S210 ).

[0223] The step ( S210 ) of providing a polishing pad including a polishing layer is as described above.

[0224] The method of manufacturing a semiconductor device (S200) includes polishing an object to be polished (S220).

[0225] Specifically, once the polishing pad according to an embodiment is mounted on the platen, the semiconductor substrate is placed on the polishing pad. In this case, the semiconductor substrate may be a semiconductor substrate, and the surface of the semiconductor substrate is in direct contact with the polishing surface of the polishing pad. The polishing slurry may be sprayed onto the polishing pad through a nozzle for polishing. The flow rate of the polishing slurry supplied through the nozzle may be about 10 cm / s depending on the purpose. 3 / min to about 1,000cm 3 / minute. For example, it can be about 50cm 3 / min to about 500cm 3 / minute, but not limited to this.

[0226] Afterwards, the surface of the semiconductor substrate is polished by relatively rotating the semiconductor substrate and the polishing pad. In this case, the rotation direction of the semiconductor substrate and the rotation direction of the polishing pad may be the same direction or opposite directions. The rotation speed of the semiconductor substrate and the polishing pad may be selected in the range of about 10 rpm to about 500 rpm according to the purpose. For example, it may be about 30 rpm to about 200 rpm, but is not limited thereto.

[0227] The semiconductor substrate mounted on the polishing head is pressed against the polishing surface of the polishing pad with a predetermined load to contact it, and then its surface can be polished. The load applied by the polishing head to bring the surface of the semiconductor substrate into contact with the polishing surface of the polishing pad can be about 1 gf / cm2 according to the purpose. 2 To about 1,000gf / cm 2 For example, it can be about 10gf / cm 2 To about 800gf / cm 2 , but not limited to this.

[0228] According to one embodiment of the present invention, the polishing pad can achieve low hardness by including a polishing layer formed by a curing agent using a specific component. By controlling the surface roughness reduction rate and elastic recovery coefficient of the polishing pad within a specific range, the mechanical properties of the polishing pad can be improved, and the surface defects occurring on the surface of the semiconductor substrate can be improved. The polishing rate can also be further increased. Therefore, semiconductor devices with excellent quality can be effectively manufactured using the polishing pad.

[0229] Embodiments of the present invention

[0230] Hereinafter, the present invention is described in detail by the following examples. However, these examples are for illustrating the present invention, and the scope of the present invention is not limited thereto.

[0231] Example

[0232] Example 1: Preparation of polishing pad

[0233] (1) Preparation of polyurethane-based prepolymers

[0234] Toluene diisocyanate (TDI; BASF), dicyclohexylmethane diisocyanate (H12MDI), polytetramethylene ether glycol (PTG, Korea) and diethylene glycol were added to a four-necked flask and then reacted at 80° C. for 3 hours to prepare a polyurethane-based prepolymer. Here, NCO% was adjusted to 10%.

[0235] (2) Preparation of polishing pad

[0236] A casting machine equipped with tanks and feed lines for raw materials such as a polyurethane-based prepolymer, a curing agent, and a blowing agent was provided. Using the polyurethane-based prepolymer prepared as described above, a mixed curing agent was prepared as a curing agent, wherein a 1,2-ethylenediamine polymer (LA-480, CAS No. 25214-63-5) containing methyl oxirane as a tertiary amine polyol was mixed with N,N'-bis(sec-butylamino)diphenylmethane as an aromatic amine compound in a weight ratio of 50:50. A solid-phase blowing agent (551DU40, Akzonobel) containing unexpanded particles was prepared. In addition, a silicone-based surfactant (Evonik) was prepared.

[0237] In a casting machine equipped with a feed line for a polyurethane-based prepolymer, a mixed curing agent, a solid-phase foaming agent, and a surfactant, the prepared polyurethane-based prepolymer having an NCO% of 10% was charged into a prepolymer tank, and the mixed curing agent was charged into a curing agent tank. While adding the solid-phase foaming agent, they were stirred at a mixing head speed of 5,000 rpm. Here, the content of each component is as shown in Table 1, and the equivalent ratio of the polyurethane-based prepolymer to the mixed curing agent was adjusted to 1:1. The mixture was discharged at a rate of 10 kg / min, injected into a mold preheated to 100°C, having an opening shape of 1000 mm in length and width, and 3 mm in height, and a molded body was obtained by a thermal curing reaction.

[0238] After that, the solidified material of the molded body is sliced ​​and processed into a sheet. The processed sheet is slotted to obtain a sheet (or polishing layer) with a thickness of 2 mm. The completed sheet is laminated with a sub-pad using an adhesive to finally obtain a polishing pad.

[0239] Example 2-3

[0240] The same procedures as in Example 1 were performed except that the weight ratio of the tertiary amine polyol and the aromatic amine compound was changed as shown in Table 1 below to obtain a polishing pad.

[0241] Example 4

[0242] The same procedures as in Example 1 were performed to obtain a polishing pad, except that 1,2-ethylenediamine polymer containing methylethylene oxide (LA-480, CAS No. 25214-63-5) was used alone as a tertiary amino polyol as a curing agent as shown in Table 1 below.

[0243] Comparative Example 1

[0244] The same procedures as in Example 1 were performed to obtain a polishing pad, except that 4,4′-methylenebis(2-chloroaniline) (MOCA) was used alone as a curing agent as shown in Table 1 below.

[0245] Comparative Example 2

[0246] The same procedures as in Example 1 were performed to obtain a polishing pad, except that a 1,2-ethylenediamine polymer containing methylethylene oxide (LA-480, CAS No. 25214-63-5) was used as a mixed curing agent of a tertiary amino polyol and 4,4′-methylenebis(2-chloroaniline) (MOCA) as shown in Table 1 below.

[0247] The following Table 1 summarizes the detailed conditions of the CMP process.

[0248] Table 1

[0249]

[0250]

[0251] Test Case

[0252] Test Example 1: Physical Properties

[0253] The polishing pads obtained in the examples and comparative examples were tested for the following items. The results are shown in Table 3.

[0254] (1) Hardness

[0255] The Shore D hardness of the polishing pads prepared in the examples and comparative examples was measured. The polishing pads prepared in the examples and comparative examples were cut into a size of 2 cm×2 cm (thickness: 2 mm), respectively, and then left at a temperature of 25° C. for 16 hours. Thereafter, the hardness of the polishing pad was measured using a hardness tester (D-type hardness tester).

[0256] (2) Specific gravity

[0257] The polishing pads prepared in the examples and comparative examples were cut into rectangles of 4 cm×8.5 cm (thickness: 2 mm) and then placed in an environment of 23±2° C. and 50±5% humidity for 16 hours. The specific gravity of the polishing pads was measured using a gravimeter.

[0258] (3) Tensile strength

[0259] The polishing pads prepared in Examples and Comparative Examples were cut into 4 cm×1 cm (thickness: 2 mm), respectively. When the polishing pad was tested at a rate of 50 mm / min using a universal testing machine (UTM), the ultimate strength before fracture was measured.

[0260] (4) Elongation

[0261] The polishing pads prepared in the examples and comparative examples were cut into 4 cm×1 cm (thickness: 2 mm). When the polishing pads were tested at a rate of 50 mm / min using a universal testing machine (UTM), the maximum deformation before fracture was measured. The ratio of the maximum deformation to the initial length was expressed as a percentage (%).

[0262] Test Example 2: Surface Roughness

[0263] The polishing pads prepared according to the examples and comparative examples were measured for Sk values ​​before and after polishing using a roughness measuring device (manufacturer: Bruker, model: contour-gt) under the conditions of Table 2. The surface roughness reduction rate (RSk (%)) was calculated according to the following equation 1.

[0264] [Equation 1]

[0265]

[0266] In Equation 1, Sk1 is the core roughness depth of the polishing pad before polishing, and Sk2 is the core roughness depth of the polishing pad measured after polishing the silicon oxide layer of the semiconductor substrate for 60 seconds under the conditions of a carrier pressure of 4.0 psi, a carrier rotation speed of 87 rpm and a platen rotation speed of 93 rpm, spraying a calcined cerium oxide slurry at a rate of 250 ml / min.

[0267] Sk1 and Sk2 are values ​​calculated from data before and after polishing of the polishing pad measured by an optical surface roughness meter according to ISO 25178-2, respectively.

[0268] Table 2

[0269]

[0270] Test Example 3: Scanning Electron Microscope (SEM)

[0271] The cross sections of the polishing pads prepared in the examples and comparative examples were observed by scanning electron microscopy (SEM), and it was shown that Figure 5 middle. Figure 5 (a) shows an SEM image of a cross section of the polishing pads prepared in Examples 1 to 3 and Comparative Example 1 observed at a magnification of 100 times. Figure 5 (b) shows an SEM image of the cross section of the polishing pads prepared in Examples 1 to 3 and Comparative Example 1 observed at a magnification of 300 times.

[0272] like Figure 5 As shown, compared with Comparative Example 1, the pores of the polishing pads in Examples 1 to 3 are finely and evenly distributed over a large area.

[0273] Test Example 4: Polishing Rate (Removal Rate)

[0274] After the polishing pad is prepared, the initial polishing rate is measured immediately.

[0275] A silicon wafer with a diameter of 300 mm was deposited with silicon oxide by a chemical vapor deposition (CVD) process. The polishing pad was mounted on a CMP machine, and the silicon oxide layer of the silicon wafer was set toward the polishing surface of the polishing pad. Afterwards, under a polishing load of 4.0 psi, the pressing plate was rotated at a speed of 100 rpm for 60 seconds, and a calcined silicon dioxide slurry was applied to the polishing pad at a rate of 250 ml / min to polish the silicon oxide layer. After polishing was completed, the silicon wafer was removed from the carrier, mounted in a spin dryer, washed with deionized water (DIW), and then dried with nitrogen (N2) for 15 seconds. The film thickness of the dried silicon wafer before and after polishing was measured using a spectral reflection thickness gauge (manufacturer: Keyence, model: SI-F80R). The polishing rate was calculated using the following equation 3.

[0276] [Equation 3]

[0277]

[0278] Test Example 5: Measurement of surface defects

[0279] After polishing using the polishing pads of the examples and comparative examples, the residues, scratches and chatter marks on the wafer surface during polishing were measured using a wafer inspection device (AIT XP+, KLA Tencor) (threshold value: 150, mold filter threshold value: 280).

[0280] Specifically, after polishing, the silicon wafer was transferred to a cleaning machine and washed with 1% HF, pure water (DIW), 1% H2NO3, and pure water (DIW) for 10 seconds, respectively. After that, it was transferred to a spin dryer, washed with pure water (DIW), and then dried with nitrogen for 15 seconds. The defect changes of the dried silicon wafer before and after polishing were measured using a wafer detection device.

[0281] Residue refers to substantially amorphous foreign matter attached to the surface of the wafer. For example, it refers to Figure 6 The shape defect shown.

[0282] Scratches are essentially continuous linear scratches. For example, they are Figure 7 The shape defect shown.

[0283] Meanwhile, chatter marks refer to substantially discontinuous linear scratches. For example, it refers to Figure 8 The shape defect shown.

[0284] The total number of defects for residue, scratches and chatter marks is shown in Table 4 below.

[0285] Table 3

[0286]

[0287]

[0288] Table 4

[0289]

[0290] As can be seen from Table 3, the surface roughness reduction rate (RSk (%)) and elastic recovery coefficient (RERI) of the polishing pads of Examples 1-4 using tertiary amino polyols containing ether bonds as curing agents are adjusted to a specific range, and they generally perform well in mechanical properties such as hardness, tensile strength and elongation.

[0291] Specifically, the hardness of the polishing pads of Examples 1 to 4 was 45.6 Shore D to 47.3 Shore D, thereby achieving low hardness. In contrast, the hardness of the polishing pad of Comparative Example 1 was 65.7 Shore D, and the hardness of the polishing pad of Comparative Example 2 was 52.1 Shore D. Since they have higher hardness than the polishing pads of Examples 1 to 4, they are relatively harder.

[0292] In addition, the tensile strength of the polishing pad of Examples 1-4 is 16.5 N / mm 2 Up to 19.2N / mm 2 , and the elongation is 232% to 302%. In contrast, the polishing pads of Comparative Examples 1 and 2 have 25.3 N / mm 2 and 20.2N / mm 2 Very high tensile strength of 72% and very low elongation of 130%.

[0293] In particular, in the polishing pads of Examples 1 to 4, as the content of the tertiary amino polyol containing an ether bond increases, the hardness and tensile strength decrease, and the elongation increases, thereby achieving the desired mechanical properties of the present invention.

[0294] Such mechanical properties can improve the polishing performance of the polishing pad and reduce the effect of surface defects occurring on the surface of the semiconductor substrate.

[0295] Specifically, it can be seen from Table 4 that the polishing pads of Examples 1 to 4 have excellent polishing rates. Compared with the polishing pads of Comparative Examples 1 and 2, the number of surface defects such as residues, surface scratches, and chatter marks on the wafer surface is significantly reduced.

[0296] Specifically, the to The polishing speed of the polishing pads of Comparative Examples 1 and 2 is excellent overall. The initial polishing rate is too fast because the ratio of the friction area to the pores capable of carrying the slurry becomes larger. Therefore, the polishing pads of Comparative Examples 1 and 2 may further increase the polishing rate due to the pad glazing phenomenon.

[0297] In addition, regarding the surface defects occurring on the wafer surface, in the case of using the polishing pads of Examples 1 to 4, the number of surface defects was 3 to 8, while in the case of using the polishing pads of Comparative Examples 1 and 2, the number of surface defects exceeded 20, which was significantly increased by 3 to 8 times or more compared to the case of using the polishing pads of Examples 1 to 4. It can be seen that due to the pad glazing phenomenon of the polishing pad of Comparative Example 1, the number of surface defects occurring on the wafer surface increased.

[0298] Meanwhile, when comparing Example 1 and Comparative Example 2 using the same content of the mixed curing agent, the polishing pad of Example 1 using the mixed curing agent of LA-480 as the tertiary amino polyol and N,N'-bis(sec-butylamino)diphenylmethane as the aromatic amine compound satisfies the surface roughness reduction rate (RSk(%)) and elastic recovery coefficient (RERI) within the specific ranges expected by the present invention, compared with the polishing pad of Comparative Example 2. The results confirm that the polishing pad of Example 1 is significantly improved in mechanical properties and polishing rate, and the surface defects occurring on the wafer surface are improved, compared with the polishing pad of Comparative Example 2.

[0299] Therefore, by using a curing agent of a specific composition and by adjusting the surface roughness reduction rate (RSk (%)) and the elastic recovery coefficient (RERI) to a specific range, mechanical properties such as low hardness, low tensile strength and high elongation can be improved. In particular, since the polishing pad has a low surface roughness reduction rate (RSk (%)), the pad glazing phenomenon can be minimized. Therefore, it has the advantages of being able to reduce the polishing rate and reduce surface defects on the wafer surface.

[0300] Reference numerals:

[0301] 110: Head 120: Semiconductor substrate (or wafer)

[0302] 130: Pressing plate 140: Slurry

[0303] 150: Hole

Claims

1. A polishing pad comprising a polishing layer, wherein the polishing layer comprises a cured product of a composition comprising a polyurethane-based prepolymer, a curing agent and a foaming agent, the curing agent comprising a tertiary amine-based polyol containing an ether bond, and the polishing pad has a surface hardness of 40 to 60 Shore D at 25° C., a surface roughness reduction rate (RSk (%)) of less than 50%, and an elastic recovery coefficient (RERI) of 30 or less, the surface roughness reduction rate (RSk (%)) is represented by the following equation 1, and the elastic recovery coefficient (RERI) is represented by the following equation 2: [Equation 1] In Equation 1, Sk1 is the core roughness depth of the polishing pad before polishing, and Sk2 is the core roughness depth of the polishing pad measured after polishing the silicon oxide layer of the semiconductor substrate for 60 seconds under the conditions of a carrier pressure of 4.0 psi, a carrier rotation speed of 87 rpm, and a platen rotation speed of 93 rpm, spraying a calcined cerium oxide slurry at a rate of 250 ml / min; and Sk1 and Sk2 are values ​​calculated from data of the polishing pad before and after polishing measured by an optical surface roughness meter according to ISO 25178-2 standard, respectively; [Equation 2] In equation 2, RSk (%) is defined as in equation 1 above, H 25 is the Shore D hardness of the polishing pad measured at 25°C, and the elastic recovery coefficient (RERI) is the ratio between the values ​​excluding units; The tertiary amino polyol is represented by the following formula: [Mode] In the above formula, n is an integer of 1 to 10; and the weight average molecular weight of the tertiary amine polyol is 400 g / mol to 3,000 g / mol.

2. The polishing pad according to claim 1, having an elastic recovery coefficient (RERI) of 23 or less, or having a surface roughness reduction rate (RSk (%)) of less than 47%.

3. The polishing pad according to claim 1, wherein A difference between the Sk1 and the Sk2 (Sk1-Sk2) is 15 μm or less.

4. The polishing pad according to claim 1, wherein: The curing agent further includes an aromatic amine compound, and the content of the tertiary amine polyol is equal to or greater than the content of the aromatic amine compound by weight. 5 . The polishing pad according to claim 4 , wherein the aromatic amine compound has a weight average molecular weight of 450 g / mol to 600 g / mol.

6. The polishing pad according to claim 4, wherein: The aromatic amine compound includes diethyltoluenediamine; 3,5-dimethylthio-2,4-toluenediamine; 3,5-diethyltoluene-2,4-diamine; N,N'-bis-(sec-butylamino)-diphenylmethane; 4,4'-methylene-bis-(3-chloro-2,6-diethylaniline); polytetrahydrofuran-bis-p-aminobenzoate; N,N'-dialkyldiaminodiphenylmethane; p,p'-methylenedianiline; m-phenylenediamine; 4,4'-methylene-bis-(2,6-diethylaniline); 4,4'-methylene-bis-(2,3 -dichloroaniline); 4,4'-diamino-3,3'-diethyl-5,5'-dimethyldiphenylmethane; 2,2',3,3'-tetrachlorodiaminodiphenylmethane; trimethylene glycol di-p-aminobenzoate; 3,5-diamino-4-chlorobenzoic acid-2-methylpropyl ester; bis(4-amino-2-chloro-3,5-diethylphenyl)methane; propylene glycol di-p-aminobenzoate; diaminochlorobutylbenzoate; methylene bis-o-aminobenzoate; chlorodiethyltoluenediamine; methylene bis-o-ethylaniline; and at least one of the group consisting of isomers thereof.

7. The polishing pad according to claim 1, which satisfies at least one of the following properties: a tensile strength of 10 N / mm 2 Up to 25N / mm 2 ; elongation of 80% to 320%; and polishing rate of the oxide layer of to 8. A method for preparing a polishing pad, comprising: mixing a polyurethane-based prepolymer, a curing agent, and a foaming agent to prepare a composition for preparing a polishing layer; and injecting the composition for preparing a polishing layer into a mold and curing the mold to obtain a polishing pad including a polishing layer, The curing agent includes a tertiary amino polyol containing an ether bond, and the polishing pad has a surface hardness of 40 to 60 Shore D at 25° C., a surface roughness reduction rate (RSk (%)) of less than 50%, and an elastic recovery coefficient (RERI) of 30 or less, the surface roughness reduction rate (RSk (%)) is expressed by the following equation 1, and the elastic recovery coefficient (RERI) is expressed by the following equation 2: [Equation 1] In Equation 1, Sk1 is the core roughness depth of the polishing pad before polishing, and Sk2 is the core roughness depth of the polishing pad measured after polishing the silicon oxide layer of the semiconductor substrate for 60 seconds under the conditions of a carrier pressure of 4.0 psi, a carrier rotation speed of 87 rpm, and a platen rotation speed of 93 rpm, spraying a calcined cerium oxide slurry at a rate of 250 ml / min; and Sk1 and Sk2 are values ​​calculated from data of the polishing pad before and after polishing measured by an optical surface roughness meter according to ISO 25178-2 standard, respectively; [Equation 2] In equation 2, RSk (%) is defined as in equation 1 above, H 25 is the Shore D hardness of the polishing pad measured at 25°C, and the elastic recovery coefficient (RERI) is the ratio between the values ​​excluding units; The tertiary amino polyol is represented by the following formula: [Mode] In the above formula, n is an integer of 1 to 10; and the weight average molecular weight of the tertiary amino polyol is 400 g / mol to 3,000 g / mol.

9. The method for preparing a polishing pad according to claim 8, wherein the polishing pad has an elastic recovery coefficient (RERI) of 23 or less, or the polishing pad has a surface roughness reduction rate (RSk (%)) of less than 47%.

10. A method for preparing a semiconductor device, comprising: providing a polishing pad including a polishing layer; and The polishing surface of the polishing layer and the surface of the object to be polished are brought into contact with each other and rotated relative to each other to polish the object to be polished, The polishing pad includes a polishing layer, the polishing layer includes a tertiary amino polyol containing an ether bond, and the polishing pad has a surface hardness of 40 to 60 Shore D at 25° C., a surface roughness reduction rate (RSk (%)) of less than 50%, and an elastic recovery coefficient (RERI) of 30 or less, the surface roughness reduction rate (RSk (%)) is expressed by the following equation 1, and the elastic recovery coefficient (RERI) is expressed by the following equation 2: [Equation 1] In Equation 1, Sk1 is the core roughness depth of the polishing pad before polishing, and Sk2 is the core roughness depth of the polishing pad measured after polishing the silicon oxide layer of the semiconductor substrate for 60 seconds under the conditions of a carrier pressure of 4.0 psi, a carrier rotation speed of 87 rpm, and a platen rotation speed of 93 rpm, spraying a calcined cerium oxide slurry at a rate of 250 ml / min; and Sk1 and Sk2 are values ​​calculated from data of the polishing pad before and after polishing measured by an optical surface roughness meter according to ISO 25178-2 standard, respectively; [Equation 2] In equation 2, RSk (%) is defined as in equation 1 above, H 25 is the Shore D hardness of the polishing pad measured at 25°C, and the elastic recovery coefficient (RERI) is the ratio between the values ​​excluding units; The tertiary amino polyol is represented by the following formula: [Mode] In the above formula, n is an integer of 1 to 10; and the weight average molecular weight of the tertiary amine polyol is 400 g / mol to 3,000 g / mol.

11. The method for manufacturing a semiconductor device according to claim 10, wherein the polishing pad has an elastic recovery coefficient (RERI) of 23 or less, or the polishing pad has a surface roughness reduction rate (RSk (%)) of less than 47%.