A method for preparing an aperture and a film system integrated in a meta-lens

By integrating apertures and film systems on metalenses, the problems of high precision requirements and large space requirements are solved, and the advantages of thinness and lightness of metalenses and efficient imaging testing are realized.

CN115437212BActive Publication Date: 2024-10-22CHANGCHUN INST OF OPTICS FINE MECHANICS & PHYSICS CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211008115.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-22
Publication Date
2024-10-22
Estimated Expiration
2042-08-22

AI Technical Summary

Technical Problem

In the existing technology, the coordination between the metalens, the diaphragm and the film system requires extremely high precision, and requires a large space to set up the optical path, which affects the lightness and thinness of the metalens.

Method used

By preparing a metalens structure material film layer on the surface of the substrate, plating a functional film system on the back side, coating a photoresist layer on the front side, preparing a photoresist mask and an alignment mark mask, and converting it into metal Mask, prepare a metalens on the metalens structural material film layer, and prepare a metal aperture on its surface to realize the integration of the aperture, film system and metalens.

Benefits of technology

It reduces the difficulty of assembly and adjustment during the metalens imaging test process, greatly reduces the space requirements of the entire optical system, and improves the accuracy and integration of combined components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115437212B_ABST
    Figure CN115437212B_ABST
Patent Text Reader

Abstract

The present application provides a method for preparing an aperture and a film system integrated in a meta-lens, which comprises preparing a film layer of a meta-lens structural material on the surface of a substrate, coating a functional film system on the back side of the substrate, coating a photoresist layer on the front side of the substrate, preparing a photoresist mask and an alignment mark mask on the photoresist layer, converting the photoresist mask into a metal mask, preparing a meta-lens on the film layer of the meta-lens structural material, and preparing a metal aperture on the surface of the meta-lens. The method solves the problems in the prior art that the coordination between the aperture and the meta-lens, and between the film system and the meta-lens has extremely high precision requirements, and requires a large space to set the optical path. The aperture, the film system and the meta-lens are integrated into a combined component, thereby reducing the difficulty of assembly and adjustment during the imaging test of the meta-lens and greatly reducing the space of the entire optical system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of micro-nano optical technology, and in particular to a method for preparing an aperture and a film system integrated in a meta-lens. Background Art

[0002] As a cutting-edge micro-nano optical device, metalens controls light waves through sub-wavelength nanostructure arrays to achieve high-resolution imaging and sub-wavelength focusing. It has the significant advantages of thin volume, light weight, small size and high integration.

[0003] In the imaging performance test of meta-lens, due to the requirements of efficiency, field of view, elimination of stray light and functions, it is often necessary to add apertures and film systems to the optical system. In current research, meta-lenses are usually used as separate components to assemble and adjust the optical system with light sources, imaging targets, apertures, film systems and other functional devices. Since the size of the lens itself is small, usually at the millimeter to centimeter level, there are problems such as extremely high precision requirements for the coordination between the aperture and the meta-lens, the film system and the meta-lens, and the need for a larger space to set the light path, which to some extent affects the advantage of the meta-lens itself in being light and thin. Summary of the invention

[0004] In view of this, it is necessary to provide a method for preparing a highly integrated and thin diaphragm and film system integrated in a meta-lens in order to address the defects in the prior art.

[0005] To solve the above problems, this application adopts the following technical solutions:

[0006] The present application provides a method for preparing an aperture and a film system integrated in a meta-lens, comprising the following steps:

[0007] Preparing a film layer of a meta-lens structure material on a substrate surface;

[0008] Plating a functional film system on the back side of the substrate;

[0009] coating a photoresist layer on the front side of the substrate;

[0010] Preparing a photoresist mask and an alignment mark mask on the photoresist layer;

[0011] converting the photoresist mask into a metal mask;

[0012] Preparing a meta-lens on the meta-lens structure material film layer;

[0013] A metal aperture is prepared on the surface of the meta-lens.

[0014] In some of the embodiments, in the step of preparing a meta-lens structure material film layer on the surface of a substrate, specifically: a meta-lens structure material film layer is prepared on the surface of the substrate by a coating process, and the coating process includes vacuum evaporation or magnetron sputtering or ion beam plating or physical vapor deposition or chemical vapor deposition or atomic layer deposition.

[0015] In some of the embodiments, the meta-lens structure material film layer includes but is not limited to at least one of polymer, TiO2, HfO2, ZrO2, GaN, Si2N3, Si, SiO2, GaAs, ZnS, and AlN.

[0016] In some of the embodiments, in the step of coating the functional film system on the back side of the substrate, specifically: a functional film system is coated on the back side of the substrate using a coating process, and the coating process includes vacuum evaporation or magnetron sputtering or ion beam plating or physical vapor deposition or chemical vapor deposition or atomic layer deposition.

[0017] In some of the embodiments, in the step of coating a functional film system on the back side of the substrate, the functional film system includes anti-reflection, anti-reflection, beam splitting, light splitting, light filtering, or polarization.

[0018] In some embodiments, the coating method includes spray coating, spin coating, or blade coating.

[0019] In some of the embodiments, in the step of preparing a photoresist mask and an alignment mark mask on the photoresist layer, specifically: a metalens photoresist mask and an alignment mark mask are prepared by a photolithography process, and the photolithography process includes electron beam lithography, two-photon lithography, stepper lithography, or ultraviolet lithography.

[0020] In some of the embodiments, in the step of preparing a metalens on the metalens structure material film layer, specifically: an etching process is used to prepare a metalens structure on the metalens structure material film layer, and the etching process includes wet etching or reactive ion etching or inductively coupled plasma etching or ion beam etching or laser etching.

[0021] In some of the embodiments, the material of the meta-lens includes Cr or Al or Au or Ag.

[0022] In some of the embodiments, after the step of preparing a meta-lens on the meta-lens structure material film layer and before proceeding to the next step, the following step is also included: preparing an isolation layer with grooves using a two-photon lithography process or an electron beam lithography double-layer glue process.

[0023] In some of the embodiments, the electron beam lithography double-layer resist process uses PMMA / LOR or ZEP / LOR type double-layer photoresist.

[0024] In some embodiments, the thickness of the metal aperture is determined according to different metal materials and the wavelength range of the meta-lens, wherein the minimum metal aperture thickness, i.e., the skin depth of the metal, can be expressed by the following formula:

[0025]

[0026] Among them, δ is the skin depth of the metal, that is, the distance the electromagnetic wave propagates in the good conductor when the amplitude of the wave drops to 1 / e of the amplitude at the surface; α is the attenuation coefficient, which is positively correlated with the frequency of the electromagnetic wave and can be expressed as f is the frequency of the electromagnetic wave, μ is the magnetic permeability of the metal, and σ is the electrical conductivity of the metal.

[0027] This application adopts the above technical solution, and its beneficial effects are as follows:

[0028] The present application provides a method for preparing an aperture and a film system integrated in a meta-lens, which comprises preparing a film layer of a meta-lens structural material on the surface of a substrate, coating a functional film system on the back side of the substrate, coating a photoresist layer on the front side of the substrate, preparing a photoresist mask and an alignment mark mask on the photoresist layer, converting the photoresist mask into a metal mask, preparing a meta-lens on the film layer of the meta-lens structural material, and preparing a metal aperture on the surface of the meta-lens. The method solves the problems in the prior art that the coordination between the aperture and the meta-lens, and between the film system and the meta-lens has extremely high precision requirements, and requires a large space to set the optical path. The aperture, the film system and the meta-lens are integrated into a combined component, thereby reducing the difficulty of assembly and adjustment during the imaging test of the meta-lens and greatly reducing the space of the entire optical system. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0030] Figure 1 It is a flowchart of the steps of a method for preparing an aperture and a film system integrated in a meta-lens provided in the present application;

[0031] Figure 2 It is a process flow chart of a method for preparing an aperture and a film system integrated in a meta-lens provided in Example 1 of the present application;

[0032] Figure 3 is a process flow chart of another method for preparing an aperture and a film system integrated in a meta-lens provided in Example 1 of the present application;

[0033] Figure 4 This is a process flow chart for preparing an aperture and a film system integrated in a meta-lens provided in Example 2 of the present application.

[0034] Figure 5 This is a process flow chart for preparing an aperture and film system integrated into a meta-lens provided in Example 3 of the present application. DETAILED DESCRIPTION

[0035] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present application, and should not be construed as limiting the present application.

[0036] In the description of the present application, it should be understood that the terms "upper", "lower", "horizontal", "inside", "outside", etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0037] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0038] In order to make the objectives, technical solutions and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0039] See also Figure 1 The present embodiment provides a method for preparing an aperture and a film system integrated in a meta-lens, including the following steps S110 to S120. The implementation method of each step is described in detail below.

[0040] Step S110: preparing a meta-lens structure material film layer on the surface of the substrate.

[0041] In some of the embodiments, in the step of preparing a meta-lens structure material film layer on the surface of a substrate, specifically: a meta-lens structure material film layer is prepared on the surface of the substrate by a coating process, and the coating process includes vacuum evaporation or magnetron sputtering or ion beam plating or physical vapor deposition or chemical vapor deposition or atomic layer deposition.

[0042] In some of the embodiments, the meta-lens structure material film layer includes but is not limited to at least one of polymer, TiO2, HfO2, ZrO2, GaN, Si2N3, Si, SiO2, GaAs, ZnS, and AlN.

[0043] Step S120: coating a functional film system on the back side of the substrate.

[0044] In some of the embodiments, in the step of coating the functional film system on the back side of the substrate, specifically: a functional film system is coated on the back side of the substrate using a coating process, and the coating process includes vacuum evaporation or magnetron sputtering or ion beam plating or physical vapor deposition or chemical vapor deposition or atomic layer deposition.

[0045] In some embodiments, the functional film system includes anti-reflection, anti-reflection, beam splitting, light splitting, light filtering or polarization.

[0046] Step S130: coating a photoresist layer on the front surface of the substrate.

[0047] In some embodiments, the coating method includes spray coating, spin coating, or blade coating.

[0048] Step S140: preparing a photoresist mask and an alignment mark mask on the photoresist layer.

[0049] In some of the embodiments, in the step of preparing a photoresist mask and an alignment mark mask on the photoresist layer, specifically: a metalens photoresist mask and an alignment mark mask are prepared by a photolithography process, and the photolithography process includes electron beam lithography, two-photon lithography, stepper lithography, or ultraviolet lithography.

[0050] Step S150: converting the photoresist mask into a metal mask.

[0051] In some of the embodiments, a stripping process is used to convert the photoresist mask into a metal mask.

[0052] Step S160: preparing a metalens on the metalens structure material film layer.

[0053] In some of the embodiments, in the step of preparing a metalens on the metalens structure material film layer, specifically: an etching process is used to prepare a metalens structure on the metalens structure material film layer, and the etching process includes wet etching or reactive ion etching or inductively coupled plasma etching or ion beam etching or laser etching.

[0054] In some of the embodiments, the material of the meta-lens includes Cr or Al or Au or Ag.

[0055] In some of the embodiments, after the step of preparing a meta-lens on the meta-lens structure material film layer and before proceeding to the next step, the following step is also included: preparing an isolation layer with grooves using a two-photon lithography process or an electron beam lithography double-layer glue process.

[0056] It can be understood that the size of the aperture and the distance between the aperture and the lens can be controlled by providing an isolation layer with grooves.

[0057] It can be understood that the two-photon lithography process can perform three-dimensional micro-nano processing with almost no restrictions at the spatial level, and is suitable for situations where the distance between the aperture and the lens is large; the electron beam lithography double-layer resist process uses PMMA / LOR or ZEP / LOR type double-layer photoresist to achieve a large bottom cut profile, and is suitable for situations where the distance between the aperture and the lens is small.

[0058] Step S170: preparing a metal aperture on the surface of the meta-lens.

[0059] In some of the embodiments, an overlay process is used in conjunction with a lift-off process to prepare a metal aperture on the surface of the meta-lens.

[0060] It can be understood that the thickness of the metal aperture is determined according to different metal materials and the wavelength range of the meta-lens, wherein the minimum metal aperture thickness, i.e., the skin depth of the metal, can be expressed by the following formula:

[0061]

[0062] Among them, δ is the skin depth of the metal, that is, the distance the electromagnetic wave propagates in the good conductor when the amplitude of the wave drops to 1 / e of the amplitude at the surface; α is the attenuation coefficient, which is positively correlated with the frequency of the electromagnetic wave and can be expressed as f is the frequency of the electromagnetic wave, μ is the magnetic permeability of the metal, and σ is the electrical conductivity of the metal.

[0063] The present application provides a method for preparing an aperture and a film system integrated in a meta-lens, which comprises preparing a film layer of a meta-lens structural material on the surface of a substrate, coating a functional film system on the back side of the substrate, coating a photoresist layer on the front side of the substrate, preparing a photoresist mask and an alignment mark mask on the photoresist layer, converting the photoresist mask into a metal mask, preparing a meta-lens on the film layer of the meta-lens structural material, and preparing a metal aperture on the surface of the meta-lens. The method solves the problems in the prior art that the coordination between the aperture and the meta-lens, and between the film system and the meta-lens has extremely high precision requirements, and requires a large space to set the optical path. The aperture, the film system and the meta-lens are integrated into a combined component, thereby reducing the difficulty of assembly and adjustment during the imaging test of the meta-lens and greatly reducing the space of the entire optical system.

[0064] The above technical solution of the present application is described in detail below in conjunction with specific embodiments.

[0065] Embodiment 1:

[0066] like Figure 2 As shown, it is a process flow chart of a method for preparing an aperture and a film system integrated in a meta-lens provided in this embodiment 1, which specifically includes the following steps when the substrate material is consistent with the meta-lens structural material and the photoresist can meet the selection ratio:

[0067] S1: coating a functional film system 1-2 on the back of a substrate 1-1 by a coating process;

[0068] S2: coating a layer of photoresist 1-3 on the front side of the substrate 1-1;

[0069] S3: using a photolithography process to prepare a meta-lens photoresist mask 1-4 and an alignment mark mask 1-5 required for subsequent preparation of an aperture;

[0070] S4: preparing a meta-lens structure 1-6 and an alignment mark structure 1-7 on the substrate 1-1 by an etching process;

[0071] S5: Prepare a metal aperture 1-8 on the surface of the meta-lens structure 1-6 by using an overlay process combined with a peeling process.

[0072] It can be understood that, according to the size and position of the aperture, an additive manufacturing process such as two-photon lithography or an electron beam lithography double-layer glue process can be used before step S5 to make an isolation layer with grooves to control the size of the aperture and the distance between the aperture and the lens.

[0073] Specifically, the two-photon lithography process can perform three-dimensional micro-nano processing almost without restriction in the spatial level, and is suitable for the case where the distance between the aperture and the lens is large. The electron beam lithography double-layer resist process uses PMMA / LOR or ZEP / LOR type double-layer photoresist to achieve a large undercut profile, and is suitable for the case where the distance between the aperture and the lens is small.

[0074] like Figure 3 As shown, taking the two-photon lithography process as an example, the following steps are specifically included:

[0075] SS1: coating a layer of photosensitive polymer 2-5 on the surface of the substrate 2-1 with the film system 2-2, the lens structure 2-3 and the alignment mark structure 2-4;

[0076] SS2: using two-photon lithography to make an isolation layer 2-6 with a groove, wherein the size of the groove is determined by the size and position of the aperture 2-7;

[0077] SS3: The metal aperture 2-7 is prepared on the surface of the meta-lens structure 2-3 by using an overlay process combined with a peeling process.

[0078] Embodiment 2:

[0079] like Figure 4 As shown, it is a process flow chart of preparing an aperture and a film system integrated in a meta-lens provided in this embodiment 2. For the case where the substrate material is inconsistent with the meta-lens structure material and the use of photoresist cannot meet the selection ratio, the process specifically includes the following steps:

[0080] SSS1: using a coating process to prepare a meta-lens structure material film layer 3-2 on the surface of a substrate 3-1;

[0081] SSS2: a functional film system 3-3 is plated on the back of the substrate 3-1 by using a coating process;

[0082] SSS3: Coat a layer of photoresist 3-4 on the front side of the substrate;

[0083] SSS4: Use photolithography to prepare the meta-lens reverse structure photoresist mask 3-5 and the alignment mark mask 3-6 required for the subsequent preparation of the aperture;

[0084] SSS5: converting the photoresist mask 3-5 and the alignment mark mask 3-6 into a metal mask 3-7 by using a coating stripping process;

[0085] SSS6: preparing a meta-lens structure 3-8 on the meta-lens structure material film layer 3-2 by an etching process;

[0086] SSS7: A metal aperture 3-9 is prepared on the surface of the meta-lens structure 3-8 using an overlay process combined with a peeling process.

[0087] Furthermore, according to the size and position of the aperture, an additive manufacturing process such as two-photon lithography or an electron beam lithography double-layer glue process can be used before step SSS7 to make an isolation layer with a groove to control the size of the aperture and the distance between the aperture and the lens.

[0088] The two-photon lithography process can perform three-dimensional micro-nano processing almost without restriction in the spatial level, and is suitable for the case where the distance between the aperture and the lens is large. The electron beam lithography double-layer resist process uses PMMA / LOR or ZEP / LOR type double-layer photoresist to achieve a large undercut profile, and is suitable for the case where the distance between the aperture and the lens is small.

[0089] Embodiment 3:

[0090] like Figure 5As shown, it is a process flow chart of preparing an aperture and a film system integrated in a meta-lens provided in Example 3 of the present application, which specifically includes the following steps for a meta-lens prepared by a batch process such as nanoimprinting:

[0091] SSSS1: A meta-lens structure material film layer 4-2 is prepared on the surface of the substrate 4-1 by using a coating process;

[0092] SSSS2: coating a layer of nanoimprint glue 4-3 on the meta-lens structure material film layer 4-2;

[0093] SSSS3: Prepare a meta-lens imprint glue mask 4-4 and an alignment mark mask 4-5 on the meta-lens structure material film layer 4-2 using a nano-imprint process;

[0094] SSSS4: converting the photoresist mask 4-4 and the alignment mark mask 4-5 into a metal mask 4-6 by using a coating stripping process;

[0095] SSSS5: preparing a meta-lens structure 4-7 on the meta-lens structure material film layer 4-2 by using an etching process;

[0096] SSSS6: Coating a layer of protective glue 4-8 on the meta-lens structure 4-7;

[0097] SSSS7: a functional film system 4-9 is plated on the back of the substrate 4-1 by using a coating process;

[0098] SSSS8: A metal aperture 4-10 is prepared on the surface of the meta-lens structure 4-7 using an overlay process combined with a peeling process.

[0099] Optionally, depending on the size and position of the aperture, an additive manufacturing process such as two-photon lithography or an electron beam lithography double-layer glue process can be used before step SSSS8 to make an isolation layer with grooves to control the size of the aperture and the distance between the aperture and the lens.

[0100] The two-photon lithography process can perform three-dimensional micro-nano processing with almost no restrictions at the spatial level, and is suitable for situations where the distance between the aperture and the lens is large.

[0101] The electron beam photolithography double-layer resist process adopts PMMA / LOR or ZEP / LOR type double-layer photoresist to realize a large undercut profile, which is suitable for the case where the distance between the aperture and the lens is small.

[0102] It can be understood that the technical features of the above-described embodiments can be arbitrarily combined. In order to make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0103] The above are only preferred embodiments of the present application, and only specifically describe the technical principles of the present application. These descriptions are only for explaining the principles of the present application and cannot be interpreted as limiting the scope of protection of the present application in any way. Based on the explanation here, any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application, and other specific implementation methods of the present application that can be associated with the technicians in this field without creative work, should be included in the scope of protection of the present application.

Claims

1. A method for preparing an aperture and a film system integrated in a meta-lens, characterized in that: The steps include: Preparing a film layer of a meta-lens structure material on a substrate surface; Plating a functional film system on the back side of the substrate; coating a photoresist layer on the front side of the substrate; Preparing a photoresist mask and an alignment mark mask on the photoresist layer; converting the photoresist mask into a metal mask; Preparing a meta-lens on the meta-lens structure material film layer; A metal aperture is prepared on the surface of the meta-lens.

2. The method for preparing the aperture and film system integrated in the meta-lens according to claim 1, characterized in that: In the step of preparing a meta-lens structure material film layer on the substrate surface, specifically: a meta-lens structure material film layer is prepared on the substrate surface by a coating process, and the coating process includes vacuum evaporation or magnetron sputtering or ion beam plating or physical vapor deposition or chemical vapor deposition or atomic layer deposition.

3. The method for preparing the aperture and film system integrated in the meta-lens according to claim 2, characterized in that: The meta-lens structure material film layer includes but is not limited to at least one of polymer, TiO2, HfO2, ZrO2, GaN, Si2N3, Si, SiO2, GaAs, ZnS, and AlN.

4. The method for preparing the aperture and film system integrated in the meta-lens according to claim 1, characterized in that: In the step of coating the functional film system on the back side of the substrate, specifically: a functional film system is coated on the back side of the substrate using a coating process, and the coating process includes vacuum evaporation or magnetron sputtering or ion beam plating or physical vapor deposition or chemical vapor deposition or atomic layer deposition.

5. The method for preparing the aperture and film system integrated in the meta-lens according to claim 4, characterized in that: The functional film system includes anti-reflection, anti-reflection, beam splitting, light splitting, light filtering or polarization.

6. The method for preparing the aperture and film system integrated in the meta-lens according to claim 1, characterized in that: In the step of coating a photoresist layer on the front side of the substrate, the coating method includes spray coating, spin coating or scraping coating.

7. The method for preparing the aperture and film system integrated in the meta-lens according to claim 1, characterized in that: In the step of preparing a photoresist mask and an alignment mark mask on the photoresist layer, specifically: a metalens photoresist mask and an alignment mark mask are prepared by a photolithography process, and the photolithography process includes electron beam lithography, two-photon lithography, stepper lithography, or ultraviolet lithography.

8. The method for preparing the aperture and film system integrated in the meta-lens according to claim 1, characterized in that: In the step of preparing a metalens on the metalens structure material film layer, specifically: an etching process is used to prepare a metalens structure on the metalens structure material film layer, and the etching process includes wet etching or reactive ion etching or inductively coupled plasma etching or ion beam etching or laser etching.

9. The method for preparing the aperture and film system integrated in the meta-lens according to claim 8, characterized in that: The material of the meta-lens includes Cr, Al, Au or Ag.

10. The method for preparing the aperture and film system integrated in the meta-lens according to claim 1, characterized in that: After the step of preparing a meta-lens on the meta-lens structure material film layer and before proceeding to the next step, the method further includes the following steps: preparing an isolation layer with grooves by using a two-photon lithography process or an electron beam lithography double-layer glue process.

11. The method for preparing the aperture and film system integrated in the meta-lens according to claim 10, characterized in that: The electron beam photolithography double-layer resist process adopts PMMA / LOR or ZEP / LOR type double-layer photoresist.

12. The method for preparing the aperture and film system integrated in the meta-lens according to claim 10, characterized in that: The thickness of the metal aperture is determined according to different metal materials and the wavelength range of the meta-lens, wherein the minimum metal aperture thickness, i.e., the skin depth of the metal, can be expressed by the following formula: Among them, δ is the skin depth of the metal, that is, the distance the electromagnetic wave propagates in the good conductor when the amplitude of the wave drops to 1 / e of the amplitude at the surface; α is the attenuation coefficient, which is positively correlated with the frequency of the electromagnetic wave and can be expressed as f is the frequency of the electromagnetic wave, μ is the magnetic permeability of the metal, and σ is the electrical conductivity of the metal.