Raw material for coating material for secondary battery separator, coating material for secondary battery separator, secondary battery separator, method for producing secondary battery separator, and secondary battery

By using a combination of core-shell particles and inorganic fillers in the secondary battery separator, the problems of insufficient heat resistance and air permeability of the separator in the existing technology are solved, and efficient separator performance improvement is achieved, ensuring the stability and stability of the battery. Power generation efficiency.

CN115443578BActive Publication Date: 2024-10-01MITSUI CHEMICALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180027379.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-04-17
Filing Date
2021-04-09
Publication Date
2024-10-01
Estimated Expiration
2041-04-09

AI Technical Summary

Technical Problem

The functional layer of existing secondary battery separators has problems such as insufficient heat resistance, reduced air permeability, and insufficient adhesion, resulting in possible short circuits and risks of fire.

Method used

A coating material containing core-shell particles is used. The core-shell particles are composed of a first polymer core layer having (meth)acrylic acid alkyl ester repeating units and (meth)acrylamide and carboxyl-containing vinyl monomer repeating units. The second polymer shell layer has a mass ratio of 4 to 250 with respect to the first polymer, and combines an inorganic filler and a dispersant to form a separator with excellent heat resistance and air permeability.

Benefits of technology

A secondary battery separator with excellent heat resistance, air permeability, adhesion and electrolyte resistance has been realized, improving battery durability and power generation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004934000650000271
    Figure GDA0004934000650000271
  • Figure GDA0004934000650000281
    Figure GDA0004934000650000281
Patent Text Reader

Abstract

In a raw material for a coating material for a secondary battery separator, comprising core-shell particles having a core layer containing a first polymer and a shell layer covering the first polymer and containing a second polymer, the first polymer has repeating units derived from an alkyl (meth)acrylate, the second polymer has 40 to 97% by weight of repeating units derived from (meth)acrylamide and 3 to 60% by weight of repeating units derived from a carboxyl group-containing vinyl monomer, and the ratio of the second polymer to the first polymer is 4 to 250.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a coating material raw material for a secondary battery separator, a coating material for a secondary battery separator, a secondary battery separator, a method for producing the secondary battery separator, and a secondary battery. Background Art

[0002] Conventionally, a secondary battery is provided with a separator for isolating a positive electrode from a negative electrode and allowing ions in an electrolyte solution to pass therethrough.

[0003] As such a separator, for example, a polyolefin porous membrane is known, and it is also known that various functional layers are provided on the surface of the separator.

[0004] As a functional layer formed on the diaphragm, for example, a coating layer obtained by coating a functional layer composition containing aluminum oxide and a resin on a polyethylene diaphragm substrate and drying it is known. As such a functional layer composition, a mixture of a water-soluble polymer, a particulate polymer, aluminum oxide, a dispersant, and a surfactant has been proposed, wherein the water-soluble polymer is obtained by polymerizing acrylamide, methacrylic acid, and dimethylacrylamide, and the particulate polymer is obtained by polymerizing n-butyl acrylate, methacrylic acid, acrylonitrile, N-hydroxymethyl acrylamide, and allyl glycidyl ether (for example, see Patent Document 1 (Example 1).).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. WO2017 / 026095 Summary of the invention

[0008] Problems to be solved by the invention

[0009] On the other hand, the separator is required to have heat resistance because a short circuit may occur between the positive electrode and the negative electrode when the separator changes shape due to thermal shrinkage. However, the functional layer described above has a disadvantage in that the heat resistance is insufficient.

[0010] Furthermore, the separator of the secondary battery needs to allow ions to pass through in order to generate electricity, and therefore requires air permeability. However, the above-mentioned functional layer has the disadvantage of reducing the air permeability of the separator.

[0011] In addition, the functional layer is required to have improved adhesion to the separator, and further, from the viewpoint of suppressing ignition of the secondary battery, excellent electrolyte solution resistance is required.

[0012] The present invention provides a raw material for coating a secondary battery separator that can produce a secondary battery separator having excellent heat resistance and air permeability as well as excellent adhesion and electrolyte resistance, a coating material for a secondary battery separator comprising the raw material for coating a secondary battery separator, a secondary battery separator having a coating film of the coating material for a secondary battery separator, a method for manufacturing the secondary battery separator, and a secondary battery having the secondary battery separator.

[0013] Means for solving problems

[0014] The present invention [1] includes a raw material for a coating material for a secondary battery separator, which includes core-shell particles, wherein the core-shell particles have a core layer containing a first polymer and a shell layer covering the first polymer and containing a second polymer, wherein the first polymer has repeating units derived from an alkyl (meth)acrylate, and the second polymer has repeating units derived from (meth)acrylamide and repeating units derived from a carboxyl group-containing vinyl monomer, and the content of the repeating units derived from the (meth)acrylamide is 40% by mass or more and 97% by mass or less relative to the total amount of the second polymer, and the content of the repeating units derived from the carboxyl group-containing vinyl monomer is 3% by mass or more and 60% by mass or less, and the ratio of the mass of the second polymer to the mass of the first polymer (second polymer / first polymer) is 4 or more and 250 or less.

[0015] The present invention [2] comprises the raw material for coating a secondary battery separator as described in [1] above, wherein the volume average particle size (D 50 ) is greater than 0.4 μm and less than 2.0 μm.

[0016] The present invention [3] includes a secondary battery separator coating material comprising the secondary battery separator coating material raw material described in [1] or [2] above.

[0017] The present invention [4] includes the secondary battery separator coating material described in [3] above, further comprising an inorganic filler and a dispersant.

[0018] The present invention [5] includes a secondary battery separator comprising: a porous membrane; and a coating film of the secondary battery separator coating material according to [3] or [4] above, which is disposed on at least one surface of the porous membrane.

[0019] The present invention [6] includes a method for producing a secondary battery separator, comprising the steps of: preparing a porous film; and coating the secondary battery separator coating material described in [3] or [4] on at least one side of the porous film.

[0020] The present invention [7] includes a secondary battery comprising a positive electrode, a negative electrode, and the secondary battery separator described in [5] disposed between the positive electrode and the negative electrode.

[0021] Effects of the Invention

[0022] The raw material of the coating material for the secondary battery separator of the present invention comprises core-shell particles, wherein the core-shell particles have a core layer containing a first polymer and a shell layer covering the first polymer and containing a second polymer, wherein the first polymer has a repeating unit from an alkyl (meth)acrylate. In addition, the second polymer has a repeating unit from (meth)acrylamide and a repeating unit from a carboxyl-containing vinyl monomer in a specified ratio. Moreover, the ratio of the mass of the second polymer to the mass of the first polymer (second polymer / first polymer) is adjusted to a specified range.

[0023] Therefore, according to the secondary battery separator coating material raw material of the present invention, a secondary battery separator excellent in heat resistance and air permeability, and also excellent in adhesion and electrolyte resistance can be obtained.

[0024] The secondary battery separator coating material of the present invention contains the above-mentioned secondary battery separator coating material raw material, and therefore can provide a secondary battery separator having excellent heat resistance and air permeability, and also excellent adhesion and electrolyte resistance.

[0025] The secondary battery separator of the present invention includes a coating film of the above-mentioned secondary battery separator coating material, and therefore has excellent heat resistance and air permeability, and further has excellent adhesion and electrolyte resistance.

[0026] According to the method for producing a secondary battery separator of the present invention, a secondary battery separator having excellent heat resistance and air permeability and also excellent adhesion and electrolyte resistance can be efficiently produced.

[0027] The secondary battery of the present invention has the above-mentioned secondary battery separator, and therefore has excellent heat resistance and air permeability, and also excellent adhesion and electrolyte resistance. As a result, the secondary battery of the present invention has excellent durability and power generation efficiency. DETAILED DESCRIPTION

[0028] The coating material raw material for secondary battery separator of the present invention comprises core-shell particles, wherein the core-shell particles have a core layer containing a first polymer, and a shell layer covering the first polymer and containing a second polymer. Preferably, the coating material raw material for secondary battery separator comprises the following core-shell particles, wherein the core-shell particles have a core layer formed by a first polymer, and a shell layer formed by a second polymer covering the first polymer.

[0029] The first polymer is a polymer formed by polymerizing a first polymer raw material (monomer composition).

[0030] The first polymer raw material contains an alkyl (meth)acrylate as an essential component. It should be noted that the term "(meth)acrylic-" includes "acrylic-" and "methacrylic-" (hereinafter the same).

[0031] Examples of the alkyl (meth)acrylate include alkyl (meth)acrylates having an alkyl portion having 1 to 4 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, and tert-butyl (meth)acrylate; alkyl (meth)acrylates having an alkyl portion having 5 to 12 carbon atoms, such as n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, and octadecyl (meth)acrylate; and alkyl (meth)acrylates having an alkyl portion having 1 to 12 carbon atoms. Preferably, alkyl (meth)acrylates having an alkyl portion having 1 to 4 carbon atoms are used, and more preferably, n-butyl acrylate is used.

[0032] Furthermore, the first polymer raw material may contain a copolymerizable monomer copolymerizable with the (meth)acrylic acid alkyl ester (hereinafter referred to as a first copolymerizable monomer) as an optional component.

[0033] Examples of the first copolymerizable monomer include functional group-containing vinyl monomers.

[0034] Examples of the functional group-containing vinyl monomer include carboxyl group-containing vinyl monomers, hydroxyl group-containing vinyl monomers, amino group-containing vinyl monomers, glycidyl group-containing vinyl monomers, cyano group-containing vinyl monomers, sulfonic acid group-containing vinyl monomers and salts thereof, acetoacetoxy group-containing vinyl monomers, and phosphoric acid group-containing compounds.

[0035] Examples of the carboxyl group-containing vinyl monomer include monocarboxylic acids such as (meth)acrylic acid, dicarboxylic acids such as itaconic acid, maleic acid, fumaric acid, itaconic anhydride, maleic anhydride, fumaric anhydride, and salts thereof.

[0036] As a hydroxyl group-containing vinyl monomer, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, etc. are mentioned, for example.

[0037] Examples of the amino group-containing vinyl monomer include 2-aminoethyl (meth)acrylate, 2-(N-methylamino)ethyl (meth)acrylate, and 2-(N,N-dimethylamino)ethyl (meth)acrylate.

[0038] Examples of the glycidyl group-containing vinyl monomer include glycidyl (meth)acrylate and the like.

[0039] Examples of the cyano group-containing vinyl monomer include (meth)acrylonitrile and the like.

[0040] Examples of the sulfonic acid group-containing vinyl monomers include allylsulfonic acid, methallylsulfonic acid, acrylamido-tert-butylsulfonic acid, etc. Examples of salts of the sulfonic acid group-containing vinyl monomers include alkali metal salts such as sodium salts and potassium salts, and ammonium salts. Specifically, examples include sodium allylsulfonate, sodium methallylsulfonate, and ammonium methallylsulfonate.

[0041] As an acetoacetoxy group-containing vinyl monomer, acetoacetoxyethyl (meth)acrylate etc. are mentioned, for example.

[0042] Examples of the phosphoric acid group-containing compound include 2-methacryloyloxyethyl acid phosphate and the like.

[0043] These functional group-containing vinyl monomers may be used alone or in combination of two or more.

[0044] As the functional group-containing vinyl monomer, preferably, a carboxyl group-containing vinyl monomer is used.

[0045] Examples of the first copolymerizable monomer include vinyl esters, aromatic vinyl monomers, unsaturated carboxylic acid amides, heterocyclic vinyl compounds, vinylidene halide compounds, α-olefins, dienes, and crosslinkable vinyl monomers.

[0046] Examples of the vinyl esters include vinyl acetate and vinyl propionate.

[0047] Examples of the aromatic vinyl monomer include styrene, α-methylstyrene, p-methylstyrene, vinyltoluene, and chlorostyrene.

[0048] As unsaturated carboxylic acid amide, (meth)acrylamide, N-methylol (meth)acrylamide, etc. are mentioned, for example.

[0049] Examples of the heterocyclic vinyl compound include vinyl pyrrolidone and the like.

[0050] Examples of the vinylidene halide compound include vinylidene chloride and vinylidene fluoride.

[0051] Examples of the α-olefins include ethylene and propylene.

[0052] Examples of the dienes include butadiene and the like.

[0053] Examples of the crosslinkable vinyl monomer include vinyl monomers containing two or more vinyl groups, such as methylenebis(meth)acrylamide, divinylbenzene, polyethylene glycol chain-containing di(meth)acrylate, trimethylolpropane tetraacrylate, pentaerythritol triacrylate, and pentaerythritol tetraacrylate.

[0054] These first copolymerizable monomers may be used alone or in combination of two or more.

[0055] The first copolymerizable monomer is preferably selected so that the glass transition temperature of the first polymer is adjusted to fall within the range described below.

[0056] As the first copolymerizable monomer, preferably, a functional group-containing vinyl monomer and an aromatic vinyl monomer are mentioned, and more preferably, a carboxyl group-containing vinyl monomer, an unsaturated carboxylic acid amide, and an aromatic vinyl monomer are mentioned.

[0057] In addition, it is preferred that the first polymer raw material does not substantially contain a cyano group-containing vinyl monomer (specifically, (meth)acrylonitrile).

[0058] The phrase “substantially containing no cyano group-containing vinyl monomer” means that the cyano group-containing vinyl monomer is contained in an amount of, for example, 2.0% by mass or less, or preferably 1.0% by mass or less, based on the first polymer raw material.

[0059] If a cyano group-containing vinyl monomer is added, the electrolyte resistance of a secondary battery separator coating material (described later) may be reduced. Therefore, the first polymer raw material preferably does not contain a cyano group-containing vinyl monomer.

[0060] In the first polymer raw material, from the viewpoint of obtaining a secondary battery separator having excellent adhesion and electrolyte resistance, the content ratio of the (meth)acrylate is, for example, 20 parts by mass or more, preferably 30 parts by mass or more, and is, for example, 100 parts by mass or less, preferably 90 parts by mass or less, more preferably 80 parts by mass or less, and further preferably 70 parts by mass or less, relative to 100 parts by mass of the first polymer raw material.

[0061] The content ratio (total amount) of the first copolymerizable monomer relative to 100 parts by mass of the first polymer raw material is, for example, 0 parts by mass or more, preferably 10 parts by mass or more, more preferably 20 parts by mass or more, further preferably 30 parts by mass or more, for example, 70 parts by mass or less.

[0062] That is, the first polymer raw material may be a composition consisting of an alkyl (meth)acrylate without containing the first copolymerizable monomer, or may be a composition consisting of an alkyl (meth)acrylate and the first copolymerizable monomer.

[0063] The first polymer raw material is preferably a composition composed of an alkyl (meth)acrylate and a first copolymerizable monomer, more preferably a composition composed of an alkyl (meth)acrylate, an aromatic vinyl monomer, and a vinyl monomer containing a functional group, further preferably a composition composed of an alkyl (meth)acrylate, an aromatic vinyl monomer, and a vinyl monomer containing a carboxyl group and / or an unsaturated carboxylic acid amide, and particularly preferably a composition composed of an alkyl (meth)acrylate, an aromatic vinyl monomer, a vinyl monomer containing a carboxyl group, and an unsaturated carboxylic acid amide.

[0064] In addition, when the first copolymerizable monomer includes a carboxyl group-containing vinyl monomer, from the viewpoint of obtaining a secondary battery separator having excellent air permeability and thus excellent adhesion, the content ratio of the carboxyl group-containing vinyl monomer relative to 100 parts by mass of the first polymer raw material is, for example, 0.01 parts by mass or more, preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, further preferably 0.3 parts by mass or more, for example, 10 parts by mass or less, preferably 5 parts by mass or less, more preferably 1.0 parts by mass or less.

[0065] In addition, when the first copolymerizable monomer contains unsaturated carboxylic acid amide, from the viewpoint of obtaining a secondary battery separator having excellent heat resistance and air permeability and further excellent electrolyte resistance, the content ratio of the unsaturated carboxylic acid amide relative to 100 parts by mass of the first polymer raw material is, for example, 0.1 parts by mass or more, preferably 1 part by mass or more, more preferably 2 parts by mass or more, for example, 10 parts by mass or less, preferably 8 parts by mass or less.

[0066] In addition, when the first copolymerizable monomer contains an aromatic vinyl monomer, from the viewpoint of obtaining a secondary battery separator having excellent adhesion and electrolyte resistance, the content ratio of the aromatic vinyl monomer relative to 100 parts by mass of the first polymer raw material is, for example, 0.01 parts by mass or more, preferably 10 parts by mass or more, more preferably 20 parts by mass or more, further preferably 30 parts by mass or more, for example, 60 parts by mass or less, preferably 50 parts by mass or less, and more preferably 45 parts by mass or less.

[0067] The first polymer is a polymer formed by polymerizing the first polymer raw material described above by a method described later.

[0068] The first polymer obtained in this way is relatively hydrophobic compared to the second polymer.

[0069] The content of the repeating unit derived from the alkyl (meth)acrylate in the first polymer is the same as the content of the alkyl (meth)acrylate in the first polymer raw material.

[0070] That is, relative to the total amount of the first polymer, from the viewpoint of obtaining a secondary battery separator having excellent adhesion and electrolyte resistance, the content of repeating units derived from the (meth)acrylate is, for example, 20% by mass or more, preferably 40% by mass or more, and, for example, 100% by mass or less, preferably 90% by mass or less, more preferably 80% by mass or less, and further preferably 70% by mass or less.

[0071] The content of the repeating unit derived from the first copolymerizable monomer in the first polymer is the same as the content of the first copolymerizable monomer in the first polymer raw material.

[0072] That is, the content of the repeating unit derived from the first copolymerizable monomer relative to the total amount of the first polymer is, for example, 0 mass % or more, preferably 10 mass % or more, more preferably 20 mass % or more, further preferably 30 mass % or more, for example, 70 mass % or less.

[0073] In addition, when the first copolymerizable monomer includes a carboxyl group-containing vinyl monomer, from the viewpoint of obtaining a secondary battery separator having excellent air permeability and thus excellent adhesion, the content of repeating units derived from the carboxyl group-containing vinyl monomer relative to the total amount of the first polymer is, for example, greater than 0.01 mass %, preferably greater than 0.1 mass %, more preferably greater than 0.2 mass %, further preferably greater than 0.3 mass %, for example less than 10 mass %, preferably less than 5 mass %, more preferably less than 1.0 mass %.

[0074] In addition, when the first copolymerizable monomer contains unsaturated carboxylic acid amide, from the viewpoint of obtaining a secondary battery separator having excellent heat resistance and air permeability and thus excellent electrolyte resistance, the content of repeating units derived from the unsaturated carboxylic acid amide relative to the total amount of the first polymer is, for example, greater than 0.1% by mass, preferably greater than 1% by mass, more preferably greater than 2% by mass, for example less than 10% by mass, preferably less than 8% by mass.

[0075] In addition, when the first copolymerizable monomer includes an aromatic vinyl monomer, from the viewpoint of obtaining a secondary battery separator having excellent adhesion and electrolyte resistance, the content of repeating units derived from the aromatic vinyl monomer relative to the total amount of the first polymer is, for example, greater than 0.01 mass %, preferably greater than 10 mass %, more preferably greater than 20 mass %, further preferably greater than 30 mass %, for example less than 60 mass %, preferably less than 50 mass %, more preferably less than 45 mass %.

[0076] In addition, from the perspective of obtaining a secondary battery separator having excellent air permeability and further excellent adhesion and electrolyte resistance, the glass transition temperature of the first polymer is, for example, above -30°C, preferably above -20°C, more preferably above -10°C, for example below 40°C, preferably below 20°C, more preferably below 15°C.

[0077] When the glass transition temperature of the first polymer is too low, the air permeability of the separator may be reduced, and the surface may become sticky, thereby reducing the operability. In addition, when the glass transition temperature of the first polymer is too high, the adhesion of the core-shell particles to the separator may be reduced.

[0078] It should be noted that the glass transition temperature can be calculated by the FOX equation (the same below).

[0079] The second polymer is a polymer formed by polymerizing the second polymer raw material (monomer composition).

[0080] The second polymer raw material contains (meth)acrylamide and a carboxyl group-containing vinyl monomer as essential components. Preferably, the second polymer raw material does not contain the above-mentioned alkyl (meth)acrylate but contains (meth)acrylamide and a carboxyl group-containing vinyl monomer.

[0081] Examples of the (meth)acrylamide include acrylamide and methacrylamide, and preferably methacrylamide is used.

[0082] The carboxyl group-containing vinyl monomer is a copolymerizable monomer which is copolymerizable with (meth)acrylamide and contains a carboxyl group.

[0083] Examples of the carboxyl group-containing vinyl monomer include the above-mentioned monocarboxylic acids, the above-mentioned dicarboxylic acids, and salts thereof.

[0084] These carboxyl group-containing vinyl monomers may be used alone or in combination of two or more.

[0085] When the second polymer raw material contains a carboxyl group-containing vinyl monomer, a secondary battery separator (described below) obtained using a secondary battery separator coating material (described below) containing the secondary battery separator coating material raw material has excellent heat resistance and adhesion.

[0086] As the carboxyl group-containing vinyl monomer, preferably, a monocarboxylic acid is used, more preferably, (meth)acrylic acid is used, and further preferably, methacrylic acid is used.

[0087] When the second polymer raw material contains these substances, a secondary battery separator (described later) obtained using a secondary battery separator coating material (described later) containing the secondary battery separator coating material raw material has more excellent heat resistance and adhesion.

[0088] The second polymer raw material may contain, as an optional component, a copolymerizable monomer copolymerizable with (meth)acrylamide and / or the carboxyl group-containing vinyl monomer (hereinafter referred to as a second copolymerizable monomer).

[0089] Examples of the second copolymerizable monomer include the above-mentioned (meth)acrylic acid alkyl esters, the above-mentioned functional group-containing vinyl monomers (excluding carboxyl group-containing vinyl monomers), the above-mentioned vinyl esters, the above-mentioned aromatic vinyl monomers, the above-mentioned unsaturated carboxylic acid amides (excluding (meth)acrylamide), the above-mentioned heterocyclic vinyl compounds, the above-mentioned vinylidene halide compounds, the above-mentioned α-olefins, the above-mentioned dienes, the above-mentioned cross-linking vinyl monomers, and the like.

[0090] These second copolymerizable monomers may be used alone or in combination of two or more.

[0091] As the second copolymerizable monomer, preferably, a copolymerizable monomer containing a hydrophilic group is used, more specifically, a hydroxyl group-containing vinyl monomer, a sulfonic acid group-containing vinyl monomer, and a phosphoric acid group-containing vinyl monomer is used, and more preferably, a hydroxyl group-containing vinyl monomer is used.

[0092] The content ratio of (meth)acrylamide in the second polymer raw material is, from the viewpoint of obtaining excellent heat resistance, for example, 40 parts by mass or more, preferably 50 parts by mass or more, more preferably 60 parts by mass or more, and further preferably 70 parts by mass or more, and from the viewpoint of obtaining excellent heat resistance, for example, 97 parts by mass or less, preferably 96 parts by mass or less, and more preferably 95 parts by mass or less, based on 100 parts by mass of the total amount of the second polymer raw material.

[0093] In addition, the content ratio of the carboxyl group-containing vinyl monomer in the second polymer raw material is, from the viewpoint of improving the adsorption to the inorganic filler described later and obtaining excellent heat resistance, for example, 3 parts by mass or more, preferably 4 parts by mass or more, and more preferably 5 parts by mass or more, relative to 100 parts by mass of the total amount of the second polymer raw material, and from the viewpoint of suppressing excessive adsorption to the inorganic filler described later and obtaining excellent heat resistance, for example, 60 parts by mass or less, preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and further preferably 30 parts by mass or less.

[0094] In addition, the content ratio of the second copolymerizable monomer in the second polymer raw material is, for example, within the range that core-shell particles can be formed using the method described later, and is, for example, 27 parts by mass or less, preferably 15 parts by mass or less, and is 0 parts by mass or more, particularly preferably 0 parts by mass, relative to 100 parts by mass of the total amount of the second polymer raw material.

[0095] That is, the second polymer raw material may be a composition containing no second copolymerizable monomer and composed of (meth)acrylamide and a carboxyl group-containing vinyl monomer, or may be a composition containing (meth)acrylamide, a carboxyl group-containing vinyl monomer and a second copolymerizable monomer.

[0096] The second polymer raw material is preferably a composition composed of (meth)acrylamide and a carboxyl group-containing vinyl monomer.

[0097] The second polymer is a polymer formed by polymerizing the above-mentioned second polymer raw material by a method described later.

[0098] The second polymer thus obtained is relatively hydrophilic compared to the first polymer.

[0099] The content of the repeating unit derived from (meth)acrylamide in the second polymer is the same as the content of (meth)acrylamide in the second polymer raw material.

[0100] That is, the content of the repeating unit derived from (meth)acrylamide is 40% by mass or more, preferably 50% by mass or more, more preferably 60% by mass or more, further preferably 70% by mass or more, and particularly preferably 80% by mass or more, relative to the total amount of the second polymer, from the viewpoint of improving the adsorption to the inorganic filler described below and obtaining excellent heat resistance, and is 97% by mass or less, preferably 96% by mass or less, and more preferably 95% by mass or less, from the viewpoint of improving the adsorption to the inorganic filler described below and obtaining excellent heat resistance.

[0101] The content of the repeating unit derived from the carboxyl group-containing vinyl monomer in the second polymer is the same as the content of the carboxyl group-containing vinyl monomer in the second polymer raw material.

[0102] That is, the content of the repeating unit derived from the carboxyl group-containing vinyl monomer relative to the total amount of the second polymer is, from the viewpoint of improving the adsorption to the inorganic filler described later and obtaining excellent heat resistance, 3 mass % or more, preferably 4 mass % or more, more preferably 5 mass % or more, and from the viewpoint of suppressing excessive adsorption to the inorganic filler described later and obtaining excellent heat resistance, it is, for example, 60 mass % or less, preferably 50 mass % or less, more preferably 40 mass % or less, and further preferably 30 mass % or less.

[0103] The content of the repeating unit derived from the second copolymerizable monomer in the second polymer is the same as the content of the second copolymerizable monomer in the second polymer raw material.

[0104] That is, the content of the repeating unit derived from the second copolymerizable monomer relative to the total amount of the second polymer is, for example, 27 mass % or less, preferably 15 mass % or less, and 0 mass % or more, particularly preferably 0 mass %.

[0105] In addition, from the viewpoint of obtaining excellent heat resistance, the glass transition temperature of the second polymer is, for example, 150°C or more, preferably 200°C or more, more preferably 210°C or more, further preferably 220°C or more, particularly preferably 230°C or more, and is usually 400°C or less, preferably 300°C or less, and more preferably 280°C or less.

[0106] When the glass transition temperature of the second polymer is excessively low, the heat resistance of the separator may decrease.

[0107] Next, a method for producing the raw material of the coating material for secondary battery separators will be described.

[0108] Specifically, as a method for manufacturing a coating material raw material for a secondary battery separator, there can be cited: for example, a method in which a first polymer raw material is polymerized to obtain a first polymer, and then a second polymer raw material is polymerized in the presence of the first polymer (first method); for example, a method in which a second polymer raw material is polymerized to obtain a second polymer, and then the first polymer raw material is polymerized in the presence of the second polymer (second method).

[0109] First, the first method will be described.

[0110] The first method comprises the steps of obtaining a first polymer by polymerizing a first polymer raw material (first step) and obtaining a second polymer by polymerizing a second polymer raw material in the presence of the first polymer (second step).

[0111] In the first step, first, a first polymer raw material is polymerized.

[0112] Specifically, the first polymer raw material and a polymerization initiator are mixed in water, and the first polymer raw material is polymerized in water.

[0113] The polymerization initiator is not particularly limited, and examples thereof include water-soluble initiators such as persulfates (ammonium persulfate, potassium persulfate, etc.), hydrogen peroxide, organic hydrogen peroxide, 4,4'-azobis(4-cyanovaleric acid) acid, oil-soluble initiators such as benzoyl peroxide and azobisisobutyronitrile, and redox initiators, etc. Preferably, a water-soluble initiator can be used, more preferably a persulfate can be used, and further preferably, ammonium persulfate can be used. These polymerization initiators can be used alone or in combination of two or more.

[0114] The mixing ratio of the polymerization initiator can be appropriately set depending on the purpose and application, and is, for example, 0.05 parts by mass or more, for example, 10 parts by mass or less, and preferably 5 parts by mass or less, based on 100 parts by mass of the first polymer raw material.

[0115] As polymerization conditions, the polymerization temperature is, for example, 30° C. or higher, preferably 50° C. or higher, for example, 95° C. or lower, preferably 85° C. or lower, under normal pressure. The polymerization time is, for example, 1 hour or higher, preferably 2 hours or higher, for example, 30 hours or lower, preferably 20 hours or lower.

[0116] In the polymerization of the first polymer, an emulsifier (surfactant) may be added as necessary from the viewpoint of improving production stability.

[0117] Examples of the emulsifier include anionic surfactants such as sulfuric acid esters of higher alcohols, alkylbenzene sulfonates (such as dodecylbenzene sulfonate), aliphatic sulfonates, alkyldiphenyl ether sulfonates, and ammonium lauryl sulfate, and nonionic surfactants such as alkyl esters of polyethylene glycol, alkylphenyl ethers, and alkyl ethers. Anionic surfactants are preferred, and alkyldiphenyl ether sulfonates are more preferred.

[0118] The mixing ratio of the emulsifier can be appropriately set depending on the purpose and application, and is, for example, 0.01 parts by mass or more, for example, 5 parts by mass or less, and preferably 3 parts by mass or less, based on 100 parts by mass of the first polymer raw material.

[0119] In addition, in the polymerization of the first polymer, from the viewpoint of achieving improved manufacturing stability, known additives such as pH adjusters, metal ion blocking agents such as ethylenediaminetetraacetic acid and its salts, and molecular weight regulators (chain transfer agents) such as thiols and low molecular weight halogen compounds can be added in appropriate proportions.

[0120] Furthermore, before or after the polymerization of the first polymer, a neutralizing agent such as ammonia may be added to adjust the pH to a range of 7 or more and 11 or less.

[0121] Thus, the first polymer raw material is polymerized to obtain the first polymer.

[0122] In addition, such a first polymer can be obtained in the form of a dispersion in which the first polymer is dispersed in water.

[0123] The solid content concentration of the first polymer in the dispersion can be appropriately set according to the purpose and application.

[0124] Next, in the second step, the second polymer raw material is polymerized in the presence of the first polymer.

[0125] Specifically, the second polymer raw material and the above-mentioned polymerization initiator are mixed into the aqueous dispersion containing the first polymer, and then the mixture is preferably aged.

[0126] The polymerization initiator is not particularly limited, and may be the same polymerization initiator as that used in the polymerization of the first polymer raw material, preferably a water-soluble initiator, more preferably a persulfate, and further preferably ammonium persulfate. These polymerization initiators may be used alone or in combination of two or more.

[0127] It should be noted that there is no particular restriction on the timing of adding the polymerization initiator. For example, the polymerization initiator may be added before adding the second polymer raw material, or when adding the second polymer raw material, or after adding the second polymer raw material. In addition, the polymerization initiator used in the polymerization of the second polymer raw material may be added in advance during the polymerization of the first polymer raw material.

[0128] The mixing ratio of the polymerization initiator can be appropriately set depending on the purpose and application, and is, for example, 0.05 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of the second polymer raw material.

[0129] As polymerization conditions, the polymerization temperature is, for example, 30° C. or higher, preferably 50° C. or higher, for example, 95° C. or lower, preferably 85° C. or lower, under normal pressure. The polymerization time is, for example, 0.5 hour or higher, preferably 1.5 hours or higher, for example, 20 hours or lower, preferably 10 hours or lower.

[0130] The aging time is, for example, 0.5 hours or more, preferably 1.5 hours or more, and, for example, 6 hours or less, preferably 3 hours or less.

[0131] Thus, the second polymer raw material is polymerized to obtain a second polymer.

[0132] As a result, a dispersion liquid (raw material for secondary battery separator coating) containing the first polymer and the second polymer can be obtained.

[0133] Furthermore, when the second polymer raw material is polymerized on the surface of the first polymer, the secondary battery separator coating material raw material can be obtained as core-shell particles in which the first polymer (core) is coated with the second polymer (shell).

[0134] The content of the secondary battery separator coating material raw material in the dispersion (solid content concentration of the dispersion) is, for example, 5 mass % or more, and for example, 50 mass % or less.

[0135] The pH of the dispersion liquid is, for example, 5 or more, and, for example, 11 or less.

[0136] When the pH value is within the above range, dispersion stability is improved, and mixing stability of the secondary battery separator coating material raw material and the inorganic filler (described later) can be ensured.

[0137] Next, the second method will be described.

[0138] The second method comprises the steps of: obtaining a second polymer raw material by polymerizing it (third step); and obtaining a first polymer by polymerizing the first polymer raw material in the presence of the second polymer (fourth step).

[0139] In the third step, first, the second polymer raw material is polymerized.

[0140] Specifically, the second polymer raw material and the above-mentioned polymerization initiator are mixed in water, and the second polymer raw material is polymerized in water.

[0141] As the polymerization initiator, preferably a water-soluble initiator is used, more preferably a persulfate is used, and further preferably ammonium persulfate is used.

[0142] These polymerization initiators can be used alone or in combination of two or more.

[0143] The mixing ratio of the polymerization initiator can be appropriately set depending on the purpose and application, and is, for example, 0.05 parts by mass or more, for example, 10 parts by mass or less, and preferably 5 parts by mass or less, based on 100 parts by mass of the second polymer raw material.

[0144] As polymerization conditions, the polymerization temperature is, for example, 30° C. or higher, preferably 50° C. or higher, for example, 95° C. or lower, preferably 85° C. or lower, under normal pressure. The polymerization time is, for example, 0.5 hour or higher, preferably 1.5 hours or higher, for example, 20 hours or lower, preferably 10 hours or lower.

[0145] In addition, in the polymerization of the second polymer, from the viewpoint of achieving improved manufacturing stability, known additives such as pH adjusters, metal ion blocking agents such as ethylenediaminetetraacetic acid and its salts, and molecular weight regulators (chain transfer agents) such as thiols and low molecular weight halogen compounds can be added in appropriate proportions.

[0146] Thus, the second polymer raw material is polymerized to obtain a second polymer.

[0147] In addition, such a second polymer can be obtained in the form of an aqueous solution.

[0148] In the aqueous solution containing the second polymer, the solid content concentration of the second polymer is, for example, 5 mass % or more, and for example, 50 mass % or less.

[0149] Next, in the fourth step, the first polymer raw material is polymerized in the presence of the second polymer.

[0150] Specifically, the first polymer raw material and the above-mentioned polymerization initiator are mixed into an aqueous solution containing the second polymer, and then the mixture is preferably aged.

[0151] As the polymerization initiator, preferably a water-soluble initiator is used, more preferably a persulfate is used, and further preferably ammonium persulfate is used.

[0152] These polymerization initiators can be used alone or in combination of two or more.

[0153] It should be noted that there is no particular restriction on the timing of adding the polymerization initiator. For example, the polymerization initiator may be added before adding the first polymer raw material, or when adding the first polymer raw material, or after adding the first polymer raw material. In addition, the polymerization initiator used in the polymerization of the first polymer raw material may be added in advance during the polymerization of the second polymer raw material.

[0154] The mixing ratio of the polymerization initiator can be appropriately set depending on the purpose and application, and is, for example, 0.05 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the first polymer raw material.

[0155] The polymerization conditions are as follows: the polymerization temperature is, for example, 30° C. or higher, preferably 50° C. or higher, for example, 95° C. or lower, preferably 85° C. or lower, under normal pressure. The polymerization time is, for example, 0.5 hour or higher, for example, 20 hours or lower, preferably 10 hours or lower.

[0156] The aging time is, for example, 0.5 hours or more, preferably 1.5 hours or more, and, for example, 6 hours or less.

[0157] In the polymerization of the first polymer, from the viewpoint of improving production stability, the above-mentioned emulsifier (surfactant) and additives may be blended at appropriate ratios as necessary.

[0158] As the emulsifier, preferably an anionic surfactant is used, and more preferably an alkyl diphenyl ether sulfonate is used. These emulsifiers may be used alone or in combination of two or more.

[0159] The mixing ratio of the emulsifier can be appropriately set depending on the purpose and application, and is, for example, 0.1 parts by mass or more, and for example, 5 parts by mass or less, based on 100 parts by mass of the first polymer raw material.

[0160] Furthermore, before or after the polymerization of the first polymer, a neutralizing agent such as ammonia may be added to adjust the pH to a range of 7 or more and 11 or less.

[0161] Thus, the first polymer raw material is polymerized to obtain the first polymer.

[0162] As a result, a dispersion liquid (raw material for secondary battery separator coating) containing the first polymer and the second polymer can be obtained.

[0163] Furthermore, by polymerizing a relatively hydrophobic first polymer in a second polymer previously formed in water, a secondary battery separator coating material raw material can be obtained as core-shell particles in which the first polymer (core) is coated with the second polymer (shell).

[0164] The content of the secondary battery separator coating material raw material in the dispersion (solid content concentration of the dispersion) is, for example, 5 mass % or more, and for example, 50 mass % or less.

[0165] The pH of the dispersion liquid is, for example, 5 or more, and, for example, 11 or less.

[0166] When the pH value is within the above range, dispersion stability is improved, and mixing stability of the secondary battery separator coating material raw material and the inorganic filler (described later) can be ensured.

[0167] In such a raw material for coating materials for secondary battery separators, from the viewpoint of obtaining a secondary battery separator having excellent heat resistance and air permeability, and further excellent adhesion and electrolyte resistance, the ratio of the mass of the second polymer to the mass of the first polymer (second polymer / first polymer) is greater than 4, preferably greater than 7, more preferably greater than 9, and less than 250, preferably less than 200, more preferably less than 50, further preferably less than 40, and particularly preferably less than 20.

[0168] It should be noted that the mass of the first polymer and the mass of the second polymer can be calculated from the input amounts of the first polymer raw material and the second polymer raw material. That is, the mass of the second polymer mentioned above refers to the mass of the second polymer raw material, and the mass of the first polymer mentioned above refers to the mass of the first polymer raw material.

[0169] In addition, from the viewpoint of suppressing the penetration of the core-shell particles into the pores of the porous membrane described later and obtaining excellent air permeability, the volume average particle size (D50 ) is, for example, not less than 0.2 μm, preferably not less than 0.4 μm, more preferably not less than 0.6 μm, and is, for example, not more than 5.0 μm, preferably not more than 2.0 μm.

[0170] The above-mentioned volume average particle size can be determined by measuring the particle size using a particle size measuring device (manufactured by Otsuka Electronics Co., Ltd., FPAR1000).

[0171] The above-mentioned secondary battery separator coating material raw material comprises core-shell particles, wherein the core-shell particles have a core layer containing a first polymer and a shell layer covering the first polymer and containing a second polymer, wherein the first polymer has a repeating unit from an alkyl (meth)acrylate. In addition, the second polymer has a repeating unit from (meth)acrylamide and a repeating unit from a carboxyl-containing vinyl monomer in a specified ratio. Moreover, the ratio of the mass of the second polymer to the mass of the first polymer (second polymer / first polymer) is adjusted to a specified range.

[0172] Therefore, according to the above-mentioned raw material for coating material for secondary battery separators, a secondary battery separator having excellent heat resistance and air permeability, and also excellent adhesion and electrolyte resistance can be obtained.

[0173] That is, in the secondary battery separator coating material (described later), the core-shell particles containing the first polymer and the second polymer are adsorbed to the inorganic filler (described later), thereby binding the inorganic filler (described later) and improving the heat resistance.

[0174] In this regard, when the number of repeating units derived from (meth)acrylamide in the second polymer is too small, the second polymer does not have sufficient adhesion to an inorganic filler (described later), and sufficient heat resistance cannot be obtained.

[0175] When the repeating unit derived from (meth)acrylamide in the second polymer is excessively large, the repeating unit derived from the carboxyl group-containing vinyl monomer in the second polymer becomes small.

[0176] Furthermore, for example, when the repeating unit derived from the carboxyl group-containing vinyl monomer in the second polymer is too small, the adsorption of the second polymer to an inorganic filler (described later) is insufficient, and sufficient heat resistance cannot be obtained.

[0177] If the repeating unit derived from the carboxyl group-containing vinyl monomer in the second polymer is too large, the number of core-shell particles adsorbed on one inorganic filler (described later) increases, and the inorganic filler (described later) cannot be uniformly bonded, so that sufficient heat resistance cannot be obtained.

[0178] For them, if in the core-shell particles, the content of repeating units derived from (methyl)acrylamide in the shell layer (second polymer) and the content of repeating units derived from a carboxyl-containing vinyl monomer are adjusted to a specified range, and then the ratio of the mass of the second polymer to the mass of the first polymer (second polymer / first polymer) is adjusted to a specified range, then heat resistance, air permeability, adhesion and electrolyte resistance can be obtained in a well-balanced manner.

[0179] The secondary battery separator coating material of the present invention comprises the above-mentioned secondary battery separator coating material raw material, and, if necessary, an inorganic filler and a dispersant.

[0180] Relative to 100 parts by mass (solid content) of the total amount of the coating material raw materials for secondary battery separators, inorganic fillers, and dispersants (hereinafter referred to as the coating material components for secondary battery separators), the mixing ratio of the coating material raw materials for secondary battery separators is, for example, more than 0.1 parts by mass (solid content), and, for example, less than 10 parts by mass (solid content).

[0181] Examples of the inorganic filler include oxides such as aluminum oxide, silicon dioxide, titanium oxide, zirconium oxide, magnesium oxide, cerium oxide, yttrium oxide, zinc oxide, and iron oxide; nitrides such as silicon nitride, titanium nitride, and boron nitride; carbides such as silicon carbide and calcium carbonate; sulfates such as magnesium sulfate and aluminum sulfate; hydroxides such as aluminum hydroxide and diaspore (aluminum hydroxide oxide); silicates such as talc, kaolinite, dickite, nacrite, halloysite, pyrophyllite, montmorillonite, sericite, mica, chlorite, bentonite, asbestos, zeolite, calcium silicate, magnesium silicate, diatomaceous earth, silica sand, and glass; and potassium titanate. Preferably, the oxides and hydroxides are used, and more preferably, aluminum oxide and diaspore are used.

[0182] The mixing ratio of the inorganic filler is, for example, 50 parts by mass or more (solid content) and, for example, 99.7 parts by mass or less (solid content) relative to 100 parts by mass (solid content) of the secondary battery separator coating material component.

[0183] Examples of the dispersant include ammonium polycarboxylate and sodium polycarboxylate.

[0184] When the dispersant is ammonium polycarboxylate, the above-mentioned raw material for the secondary battery separator coating material and the inorganic filler can be uniformly dispersed, and a coating film having a uniform thickness can be obtained (described later).

[0185] The blending ratio of the dispersant is, for example, 0.1 parts by mass or more (solid content) and, for example, 5 parts by mass or less (solid content) relative to 100 parts by mass (solid content) of the secondary battery separator coating material component.

[0186] In order to obtain the secondary battery separator coating material, first, an inorganic filler and a dispersant are mixed in water at the above ratio to prepare an inorganic filler dispersion.

[0187] Next, the secondary battery separator coating material raw material (or the dispersion containing the secondary battery separator coating material raw material) is mixed in the inorganic filler dispersion at the above ratio, and the mixture is stirred.

[0188] The stirring method is not particularly limited, and examples thereof include mechanical stirring using a ball mill, a bead mill, a planetary ball mill, a vibration ball mill, a sand mill, a colloid mill, an attritor, a roll crusher, a high-speed impeller dispersion, a disperser, a homogenizer, a high-speed impact mill, ultrasonic dispersion, and a stirring blade.

[0189] In this way, a coating material for a secondary battery separator can be obtained.

[0190] In addition, such a secondary battery separator coating material can be obtained in the form of a dispersion in which the coating material is dispersed in water.

[0191] Furthermore, additives such as a hydrophilic resin, a thickener, a wetting agent, a defoaming agent, and a pH adjuster may be blended in appropriate proportions in the secondary battery separator coating material as required.

[0192] These additives may be used alone or in combination of two or more.

[0193] Since the coating material for secondary battery separators described above includes the raw material for secondary battery separator coating, a secondary battery separator having excellent heat resistance and air permeability, and also excellent adhesion and electrolyte resistance can be obtained.

[0194] Furthermore, the coating material for a secondary battery separator can be suitably used as a coating material for a secondary battery separator.

[0195] The secondary battery separator of the present invention can be produced by a production method comprising the steps of: preparing a porous film; and applying the above-mentioned separator coating material on at least one surface of the porous film.

[0196] In the step of preparing a porous membrane, a porous membrane is prepared.

[0197] Regarding the porous film, polyolefin porous films such as polyethylene and polypropylene, for example, aromatic polyamide porous films, etc. can be cited, and preferably polyolefin porous films can be cited. The porous film can be surface treated as needed. As surface treatment, for example, corona treatment and plasma treatment can be cited.

[0198] The thickness of the porous film is, for example, 1 μm or more, preferably 5 μm or more, and, for example, 40 μm or less, preferably 20 μm or less.

[0199] Next, in the step of applying the separator coating material onto at least one side of the porous membrane, the dispersion of the separator coating material is applied onto at least one side of the porous membrane and then dried as necessary to obtain a coating film.

[0200] There are no particular restrictions on the coating method, and examples include gravure coating, small-diameter gravure coating, reverse roll coating, transfer roll coating, kiss coating, dip coating, micro gravure coating, knife coating, air knife coating, blade coating, rod coating, extrusion coating, cast coating, die coating, screen printing, spray coating, and the like.

[0201] As the drying conditions, the drying temperature is, for example, 40° C. or higher and, for example, 80° C. or lower.

[0202] The thickness of the coating film is, for example, 1 μm or more, preferably 3 μm or more, and, for example, 10 μm or less, preferably 8 μm or less.

[0203] In this way, a secondary battery separator including a porous membrane and a coating film of the secondary battery separator coating material disposed on at least one surface of the porous membrane can be produced.

[0204] In the above description, the coating film of the secondary battery separator coating material is disposed on at least one surface of the porous membrane, but the coating film may be disposed on both surfaces of the porous membrane.

[0205] Since the secondary battery separator described above includes a coating film of the secondary battery separator coating material described above, it is excellent in heat resistance and air permeability, and further, is also excellent in adhesion and electrolyte resistance.

[0206] Furthermore, according to the above-mentioned method for producing a secondary battery separator, a secondary battery separator having excellent heat resistance and air permeability, and also excellent adhesion and electrolyte resistance can be efficiently produced.

[0207] Furthermore, the secondary battery separator can be suitably used as a separator for a secondary battery.

[0208] The secondary battery of the present invention comprises a positive electrode, a negative electrode, the secondary battery separator disposed between the positive electrode and the negative electrode, and an electrolyte impregnated in the positive electrode, the negative electrode and the secondary battery separator.

[0209] As the positive electrode, for example, a known electrode including a positive electrode current collector and a positive electrode active material stacked on the positive electrode current collector can be used.

[0210] Examples of the positive electrode current collector include conductive materials such as aluminum, titanium, stainless steel, nickel, calcined carbon, conductive polymers, and conductive glass.

[0211] The positive electrode active material is not particularly limited, and examples thereof include known positive electrode active materials such as lithium-containing transition metal oxides, lithium-containing phosphates, and lithium-containing sulfates.

[0212] These positive electrode active materials may be used alone or in combination of two or more.

[0213] As the negative electrode, for example, a known electrode including a negative electrode current collector and a negative electrode active material stacked on the negative electrode current collector can be used.

[0214] Examples of the negative electrode current collector include conductive materials such as copper and nickel.

[0215] The negative electrode active material is not particularly limited, and examples thereof include carbon active materials such as graphite, soft carbon, and hard carbon.

[0216] These negative electrode active materials may be used alone or in combination of two or more.

[0217] When a lithium ion battery is used as the secondary battery, the electrolyte may be a solution in which a lithium salt is dissolved in a carbonate compound such as ethylene carbonate (EC), propylene carbonate (PC), or ethyl methyl carbonate (EMC).

[0218] To manufacture a secondary battery, for example, a separator of the secondary battery is sandwiched between a positive electrode and a negative electrode, these are housed in a battery case (battery cell), and an electrolyte is injected into the battery case.

[0219] In this way, a secondary battery can be obtained.

[0220] Since the secondary battery has the secondary battery separator, it has excellent heat resistance and air permeability, and also excellent adhesion and electrolyte resistance. As a result, the secondary battery has excellent durability and power generation efficiency.

[0221] Example

[0222] The specific numerical values ​​such as the mixing ratio (containing ratio), physical property values, and parameters used in the following descriptions can be replaced by the upper limit values ​​(values ​​defined in the form of "below" or "less than") or lower limit values ​​(values ​​defined in the form of "above" or "greater than") of the corresponding mixing ratios (containing ratios), physical property values, and parameters described in the above-mentioned "Specific Implementation Methods". In addition, in the following descriptions, "parts" and "%" are based on mass unless otherwise specified.

[0223] 1. Preparation of raw materials for coating materials for secondary battery separators

[0224] Manufacturing Example 1

[0225] 260.0 parts of distilled water were placed in a separable flask equipped with a stirrer and a reflux condenser, and the atmosphere was replaced with nitrogen and then heated to 80° C. Then, 0.5 parts of ammonium persulfate was added, and the emulsified first polymer raw material described below was continuously added over 20 minutes.

[0226] 5.0 parts of n-butyl acrylate

[0227] 4.5 parts of styrene

[0228] Acrylamide 0.47 parts

[0229] Methacrylic acid 0.03 parts

[0230] 0.1 part ammonium lauryl sulfate

[0231] 10.0 parts of distilled water

[0232] After keeping for 30 minutes, the mixture of the second polymer raw material and water was added continuously for 3 hours while stirring, and then aged for 3 hours at the same temperature to complete the polymerization. Thereafter, water was added in an appropriate amount to obtain a coating material raw material for a diaphragm. The solid content concentration of the dispersion was 10.0% by mass.

[0233] Methacrylamide 291.0 parts

[0234] Methacrylic acid 32.3 parts

[0235] 25% ammonia water 18.1 parts

[0236] 1017.5 parts of distilled water

[0237] In addition, the glass transition temperatures (Tg) of the first polymer and the second polymer were calculated from the following FOX equation.

[0238] 1 / Tg=W 1 / Tg 1 +W 2 / Tg 2 +···+W n / Tg n (1)

[0239] [Wherein, Tg represents the glass transition temperature of the copolymer (unit: K), Tg i (i=1, 2, ..., n) represents the glass transition temperature (unit: K) when monomer i forms a homopolymer, W i (i=1, 2, ... n) represents the mass fraction of monomer i in all monomers.]

[0240] In addition, the volume average particle size (D 50 ) for determination.

[0241] Manufacturing Examples 2 to 3, and Manufacturing Comparative Examples 1 to 4

[0242] The raw material of the coating material for a separator was produced in the same manner as in Example 1 except that the formula was changed as described in Table 1. In addition, the glass transition temperatures of the first polymer and the second polymer were calculated in the same manner as in Example 1, and the volume average particle size (D 50 ).

[0243] Manufacturing Comparative Example 5

[0244] According to Example 1 of International Publication No. WO2017 / 026095, a dispersion liquid as a raw material of a coating material for a separator was obtained.

[0245] That is, the following water-soluble polymer raw material components were put into a four-necked flask equipped with a stirrer, a thermometer, a reflux condenser and a nitrogen inlet tube, and the oxygen in the reaction system was removed by nitrogen. Then, 7 parts of a 5% ammonium persulfate aqueous solution and 3 parts of a 5% sodium bisulfite aqueous solution as polymerization initiators were put into the flask under stirring, and then the temperature was raised from room temperature to 80°C and kept for 3 hours to perform polymerization. Thereafter, 162 parts of ion exchange water were added to obtain an aqueous solution of a water-soluble polymer.

[0246] Acrylamide 90 parts

[0247] Methacrylic acid 9 parts

[0248] 1 part dimethyl acrylamide

[0249] 365 parts of ion exchange water

[0250] 5 parts of isopropyl alcohol

[0251] Separately, 70 parts of ion exchange water, 0.15 parts of sodium lauryl sulfate as an emulsifier, and 0.5 parts of ammonium persulfate as a polymerization initiator were supplied to a reactor equipped with a stirrer, the gas phase was replaced with nitrogen, and the temperature was raised to 60° C. Thereafter, the following particulate polymer was continuously added to the reactor, and polymerization was performed at 60° C. during the addition process. After the addition was completed, the reaction was terminated by stirring at 70° C. for 3 hours. Thus, a dispersion of the particulate polymer was obtained.

[0252] 50 parts of ion exchange water

[0253] 0.5 parts of sodium dodecylbenzene sulfonate

[0254] 94.8 parts of n-butyl acrylate

[0255] Methacrylic acid 1 part

[0256] 2 parts of acrylonitrile

[0257] 1.2 parts of N-hydroxymethyl acrylamide

[0258] Allyl glycidyl ether 1 part

[0259] Then, the obtained water-soluble polymer dispersion and the particulate polymer dispersion are mixed to obtain a mixed dispersion. The mixing ratio is set to a ratio of 2 parts by mass of the particulate polymer to 1 part by mass of the water-soluble polymer.

[0260] In addition, in the same manner as in Production Example 1, the glass transition temperatures of the water-soluble polymer and the particulate polymer were calculated.

[0261] In addition, the volume average particle size (D 50 ) for determination.

[0262] 2. Coating materials for secondary battery separators and manufacturing of secondary battery separators

[0263] Example 1

[0264] 100 parts by mass of diaspore (Boehmite Grade C06, particle size: 0.7 μm, manufactured by Da Ming Chemical Co., Ltd.) as a pigment and 3.0 parts by mass (in terms of solid content) of polycarboxylic acid ammonium aqueous solution (SAN NOPCO, Inc., SN Dispersant 5468) as a dispersant were uniformly dispersed in 110 parts by mass of water to obtain a pigment dispersion. Next, the dispersion prepared in Example 1 was added to the pigment dispersion in a manner in which the solid content was converted to 5 parts by mass, and water was further added to adjust the solid content to 40%, and stirred for 15 minutes to prepare a coating material for a secondary battery separator.

[0265] On the other hand, the surface of the polyolefin resin porous membrane was subjected to corona treatment. More specifically, as a polyolefin resin porous membrane, a product number SW509C+ (membrane thickness 9.6 μm, porosity 40.6%, air permeability 158 g / 100 ml, surface density 5.5 g / m 2, Changzhou Xingyuan New Energy Materials Co., Ltd.). Next, the surface of the polyolefin resin porous membrane was cut into A4 size, and then the surface of the polyolefin resin porous membrane was corona treated using a steering automatic driving corona surface treatment device (manufactured by WEDGE Co., Ltd.) under the conditions of output power 0.15 KW, conveying speed 3.0 m / s×2 times, and corona discharge distance 9 mm.

[0266] Next, the aforementioned secondary battery separator coating material was applied to the surface of the corona-treated polyolefin resin porous membrane using a wire bar and dried at 50° C. to form a 5 μm coating film on the surface of the polyolefin resin porous membrane.

[0267] Thus, a secondary battery separator was manufactured.

[0268] Examples 2 to 3 and Comparative Examples 1 to 5

[0269] Secondary battery separators were produced in the same manner as in Example 1 except that the dispersions produced in Production Examples 2 to 3 and Comparative Examples 1 to 5 were used instead of the dispersion produced in Production Example 1.

[0270] 3. Evaluation

[0271] (Heat resistance)

[0272] The secondary battery separator of each embodiment and each comparative example was cut into 5 cm × 5 cm pieces and used as test pieces. After the test pieces were placed in an oven at 150°C for 1 hour, the length of each side was measured and the thermal shrinkage was calculated. In addition, the heat resistance was evaluated according to the following criteria. The results are shown in Table 2.

[0273] A: The thermal shrinkage is less than 15%.

[0274] B: The heat shrinkage rate is 15% or more and less than 25%.

[0275] C: The heat shrinkage is 25% or more and less than 60%.

[0276] D: The heat shrinkage is 60% or more.

[0277] (Ion Permeability)

[0278] For the secondary battery separators of each embodiment and each comparative example, the air permeability measured in accordance with JIS-P-8117 was obtained using a Wangyan air permeability smoothness tester manufactured by Asahi Seiko Co., Ltd. The smaller the air permeability, the better the ion permeability is evaluated. In addition, the ion permeability is evaluated according to the following criteria. The results are shown in Table 2.

[0279] A: Air resistance is less than 180s / 100mL.

[0280] B: The air resistance is 180 s / 100 mL or more and less than 220 s / 100 mL.

[0281] C: The air resistance is 220 s / 100 mL or more and less than 300 s / 100 mL.

[0282] D: The air resistance is 300s / 100mL or more.

[0283] (Adhesion)

[0284] The secondary battery separator of each embodiment and each comparative example was cut into 5 cm × 10 cm and used as a test piece. A 180° peel test was performed according to the method of JIS Z1522. At this time, the tensile speed of the cellophane adhesive tape was set to 10 mm / min. The measurement was performed 3 times and the average value was calculated. In addition, the adhesion was evaluated according to the following criteria. The results are shown in Table 2.

[0285] A: The average value of the adhesive strength is 70 N / m or more.

[0286] B: The average value of the adhesive strength is 50 N / m or more and less than 70 N / m.

[0287] C: The average value of the adhesive strength is 30 N / m or more and less than 50 N / m.

[0288] D: The average value of the adhesive strength is less than 30 N / m.

[0289] (Electrolyte resistance)

[0290] The raw material of the coating material for the secondary battery separator of each embodiment and each comparative example was applied to a polypropylene tray, and then dried at room temperature for a day and night, and further dried under reduced pressure at room temperature for 8 hours, thereby obtaining a 500μm film. The obtained film was placed in a solution of ethylene carbonate (EC) / ethyl methyl carbonate (EMC) = 1 / 1 (w / w) at 90°C for 7 hours, and the weight of the swollen film was measured. The weight of the swollen film / the weight before swelling was calculated. In addition, the electrolyte resistance was evaluated according to the following criteria. The results are shown in Table 2

[0291] A: The swelling ratio is less than 150%.

[0292] B: The swelling ratio is 150% or more and less than 200%.

[0293] C: The swelling rate is 200% or more and less than 300%.

[0294] D: The swelling rate is 300% or more.

[0295] [Table 1]

[0296]

[0297] [Table 2]

[0298]

[0299] In addition, the details of the abbreviations in the table are described below.

[0300] Mam: methacrylamide

[0301] Mac: Methacrylic acid

[0302] HEMA: 2-Hydroxyethyl Methacrylate

[0303] AM: Acrylamide

[0304] DMAM: dimethylacrylamide

[0305] St:Styrene

[0306] BA: n-butyl acrylate

[0307] AN: Acrylonitrile

[0308] N-MAM: N-hydroxymethyl acrylamide

[0309] AGE: Allyl glycidyl ether

[0310] It should be noted that the above invention is provided as an exemplary embodiment of the present invention, which is merely an illustration and is not to be construed as limiting. Modifications of the present invention that are obvious to those skilled in the art are also included in the appended claims.

[0311] Industrial Applicability

[0312] The secondary battery separator coating material raw material, the secondary battery separator coating material, the secondary battery separator, the method for producing the secondary battery separator, and the secondary battery of the present invention can be suitably used in various industrial fields requiring secondary batteries.

Claims

1. A raw material for coating a secondary battery separator, characterized in that: The invention comprises core-shell particles, wherein the core-shell particles include a core layer containing a first polymer and a shell layer covering the first polymer and containing a second polymer. The first polymer has a repeating unit derived from an alkyl (meth)acrylate and does not have a repeating unit derived from a cyano group-containing vinyl monomer. The second polymer has a repeating unit derived from (meth)acrylamide and a repeating unit derived from a carboxyl group-containing vinyl monomer, With respect to the total amount of the second polymer, the content of the repeating unit derived from the (meth)acrylamide is 40% by mass or more and 97% by mass or less, and the content of the repeating unit derived from the carboxyl group-containing vinyl monomer is 3% by mass or more and 60% by mass or less, The ratio of the mass of the second polymer to the mass of the first polymer (second polymer / first polymer) is 4 or more and 20 or less.

2. The raw material for coating the secondary battery separator according to claim 1, characterized in that: The volume average particle size (D 50 ) is greater than 0.4 μm and less than 2.0 μm.

3. A coating material for a secondary battery separator, characterized in that: The invention comprises the coating material raw material for secondary battery separator according to claim 1.

4. The coating material for secondary battery separator according to claim 3, characterized in that: Also contains inorganic fillers and dispersants.

5. A secondary battery separator, characterized in that: have: a porous membrane; and The coating film of the coating material for secondary battery separator according to claim 3 is arranged on at least one side of the porous film.

6. A method for manufacturing a secondary battery separator, characterized in that: The following processes are available: A step of preparing a porous membrane; and A step of applying the secondary battery separator coating material according to claim 3 onto at least one side of the porous film.

7. A secondary battery, characterized in that A secondary battery comprising a positive electrode, a negative electrode, and the secondary battery separator according to claim 5 disposed between the positive electrode and the negative electrode.