Resin composition and method for producing the same
By rationally formulating aluminum hydroxide, magnesium hydroxide, phosphorus compounds and NOR-type hindered amine compounds in polyolefin resin, combined with fibrous fillers with an aspect ratio of more than 10, the mold wear and tear of polyolefin resin in injection molding are solved. Flame retardancy issues, achieving a resin composition with stable mechanical strength, flame retardancy and excellent appearance.
Patent Information
- Application Number
- CN202210624263.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-02
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-06-02
AI Technical Summary
In the injection molding of existing polyolefin resins, fillers such as high-hardness glass fibers cause increased wear of metal molds and reduced yields. In addition, phosphorus compound flame retardants produce acidic gases that corrode molds, resulting in increased production costs.
A resin composition containing aluminum hydroxide, magnesium hydroxide, a phosphorus compound and a NOR-type hindered amine compound is used, and a fibrous filler with an aspect ratio of 10 or more is added, and the resin composition is made by melting and kneading to reduce the melt viscosity. And inhibit metal mold wear.
It is possible to reduce metal mold wear, improve yield, reduce production costs, and optimize the appearance of injection molded products while maintaining mechanical strength and flame retardancy.
Smart Images

Figure BDA0003676116010000111 
Figure BDA0003676116010000131 
Figure BDA0003676116010000141
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition and a method for producing the same. More specifically, the present invention relates to a resin composition for injection molding capable of economically producing an injection-molded article having excellent mechanical strength, flame retardancy and appearance with stable quality, and a method for producing the same. Background Art
[0002] Polyolefin resins represented by polypropylene are lightweight and have excellent chemical resistance, high ductility and low price, and are therefore used in a variety of applications. Since polyolefin resins are flammable, when flame retardancy is required for molded products, a resin composition for molding in which a large amount of flame retardants are added to the resin is used. However, there are also cases where the advantages of polyolefin resins are impaired due to the addition of flame retardants. As flame retardants, various flame retardants such as halogen compounds, phosphorus compounds, and metal hydrates are known in the past. In addition, in order to increase the strength of molded products, it is also known to add fillers such as glass fibers to polyolefin resins.
[0003] As a technology for improving flame retardancy and strength at the same time, Patent Document 1 records: a flame retardant containing ammonium polyphosphate and a nitrogen compound and long glass fibers are added to a polyolefin resin, and a resin composition containing long glass fibers has excellent balanced characteristics of rigidity and impact resistance, good flame retardancy, elongation characteristics, and dimensional stability, and can obtain an effect of preventing dripping during combustion.
[0004] In addition, Patent Document 2 describes a method in which pellets obtained by impregnating long fiber glass with a length of 2 to 50 mm with a polyolefin resin are dry-mixed with pellets of a composition containing a polyolefin resin and a specific phosphate, and the mixture is directly molded as a flame-retardant resin composition containing long glass fibers to obtain a molded product. Patent Document 2 describes that when long fiber glass pellets impregnated with a polyolefin resin with a length of 2 to 50 mm are used, the average length of the glass fibers in the molded product becomes 1 to 6 mm, and describes that the glass fibers of this length increase the oxygen index.
[0005] However, among these technologies, polyolefin resin compositions contain fillers such as glass fibers with relatively high hardness, which causes the problem of metal mold wear during injection molding. This problem is more significant in particular at the gate of a metal mold where the resin composition flows at a high shear rate and high pressure. In addition, flame retardants that produce acidic gases, such as flame retardants using phosphorus compounds, promote the wear of metal molds as they corrode. When flame retardants such as metal hydroxides are used, the amount of fillers with high hardness increases, causing the problem of metal mold wear being promoted. As a result, the wear of metal molds is a problem that will cause the yield rate of molded products to decrease and the production cost to increase due to the replacement of metal molds.
[0006] In addition, although hindered amine light stabilizers are used in various fields as light stabilizers to prevent light degradation, it is also known that NOR-type hindered amine compounds (hereinafter also referred to as "NOR-type HALS") have a function as a flame retardant and can effectively improve flame retardancy (for example, see Patent Documents 3 and 4). In these patent documents, although it is described that the flame retardancy or weather resistance of films, sheets or fibers is improved, there is no mention of other effects, such as the effect of suppressing the wear and corrosion of metal molds in injection molding.
[0007] Prior art literature
[0008] Patent Literature
[0009] [Patent Document 1] Japanese Patent Application Laid-Open No. 10-338774
[0010] [Patent Document 2] Japanese Patent Application Publication No. 2011-88970
[0011] [Patent Document 3] Japanese Patent Publication No. 2002-507238
[0012] [Patent Document 4] Japanese Patent Application Publication No. 2015-189785 Summary of the invention
[0013] Technical Problems to be Solved by the Invention
[0014] The present invention has been made in view of the above problems and circumstances, and aims to provide a resin composition for injection molding and a method for producing the same, which can economically produce injection-molded products excellent in mechanical strength, flame retardancy and appearance with stable quality.
[0015] Technical means of solving problems
[0016] In the process of studying the causes of the above-mentioned technical problems in order to solve them, the inventors discovered that by making a resin composition for injection molding containing a polyolefin resin contain, in specific proportions: at least one selected from aluminum hydroxide, magnesium hydroxide and a phosphorus compound; a NOR-type hindered amine compound; and a fibrous filler having an aspect ratio of 10 or more, and at the same time making the phosphorus content in the resin composition below a specific amount, a resin composition for injection molding that can economically produce injection-molded products with excellent mechanical strength, flame retardancy and appearance with stable quality can be provided, thereby completing the present invention.
[0017] That is, the above-mentioned problems according to the present invention can be solved by the following means. 1.
[0019] A resin composition, which is a resin composition for injection molding containing a polyolefin resin, wherein:
[0020] Relative to the total amount of the resin composition, the resin composition comprises:
[0021] 10-60% by mass of at least one selected from aluminum hydroxide, magnesium hydroxide and a phosphorus compound,
[0022] 0.05 to 5% by mass of a NOR type hindered amine compound, and
[0023] 1-20% by mass of fibrous filler having an aspect ratio of 10 or more,
[0024] Furthermore, the phosphorus content is 5% by mass or less based on the total amount of the resin composition. 2.
[0026] The resin composition according to item 1, wherein
[0027] The polyolefin resin is a polypropylene resin. 3.
[0029] The resin composition according to item 1 or 2, wherein
[0030] The phosphorus compound includes a phosphate compound. 4.
[0032] The resin composition according to any one of items 1 to 3, wherein
[0033] The mass ratio of the total content of the aluminum hydroxide and the magnesium hydroxide to the content of the phosphorus compound is in the range of 100:0 to 75:25. 5.
[0035] The resin composition according to any one of items 1 to 4, wherein
[0036] The aspect ratio of the fibrous filler is 50 or more. 6.
[0038] The resin composition according to any one of items 1 to 5, wherein
[0039] The fibrous filler comprises halloysite. 7.
[0041] A method for producing a resin composition, which is a method for producing the resin composition according to any one of items 1 to 6, wherein:
[0042] The manufacturing method has the following features:
[0043] A first step of melt-kneading the polyolefin resin, the at least one selected from aluminum hydroxide, magnesium hydroxide and a phosphorus compound, and the NOR-type hindered amine compound to obtain a resin mixture; and
[0044] The second step is to melt-knead the resin mixture and the raw material components of the fibrous filler having an aspect ratio of 10 or more.
[0045] Effects of the Invention
[0046] According to the means of the present invention, it is possible to provide a resin composition for injection molding capable of economically producing an injection-molded article excellent in mechanical strength, flame retardancy and appearance with stable quality, and a method for producing the same.
[0047] The expression mechanism or action mechanism of the effect of the present invention can be inferred as follows.
[0048] The inventors of the present invention have found that in order to obtain mechanical strength of injection molded products, a specific amount of a fibrous filler having an aspect ratio of 10 or more must be contained in a resin composition containing a polyolefin resin. However, in injection molding, if a fibrous filler having an aspect ratio of 10 or more passes through a gate of a metal mold at high speed and high pressure, the metal mold will be worn. In the present invention, a specific amount of NOR-type HALS is added to reduce the melt viscosity of the resin composition at this time, thereby suppressing the wear of the metal mold.
[0049] It is generally known that NOR-type HALS has a radical scavenging effect (for example, Patent Document 3). In addition, it is described in Japanese Patent Application Laid-Open No. 2004-263033 that NOR-type HALS has a dripping promoting effect. The dripping promoting effect of NOR-type HALS is presumed to be an effect reflecting the phenomenon that the melt viscosity decreases sharply when the temperature rises sharply due to combustion.
[0050] Since shear heat is also generated at the gate where the resin composition flows at high pressure and high speed when the resin composition containing the fibrous filler is injection molded, it is expected that NOR-type HALS has the effect of reducing the melt viscosity at this time. Thus, it can be inferred that by adding a specific amount of NOR-type HALS to the resin composition containing the fibrous filler, the wear of the metal mold can be suppressed.
[0051] The resin composition of the present invention further contains at least one selected from aluminum hydroxide, magnesium hydroxide and a phosphorus compound as a flame retardant in a specific amount, wherein the phosphorus content is 5% by mass or less, thereby being able to impart flame retardancy while maintaining the effect of suppressing the wear of the metal mold. Here, although NOR type HALS also functions as a flame retardant, in the present invention, the flame retardancy in the molded product becomes sufficient by combining it with at least one selected from aluminum hydroxide, magnesium hydroxide and a phosphorus compound.
[0052] It should be noted that aluminum hydroxide, magnesium hydroxide and phosphorus compounds also have the risk of promoting the wear of the metal mold as described above, but their content can be suppressed by combining with NOR type HALS. In addition, when the resin composition of the present invention is used for injection molding, the load on the device in the injection molding such as the wear of the metal mold can be reduced, thereby improving the yield of the molded product and suppressing the production cost spent on the replacement of the metal mold, etc.
[0053] Thus, the resin composition of the present invention, by having the above-mentioned configuration, can economically produce an injection-molded article having excellent mechanical strength, flame retardancy, and appearance with stable quality.
[0054] Specific embodiments of the present invention
[0055] The resin composition of the present invention is a resin composition for injection molding containing a polyolefin resin, characterized in that: relative to the total amount of the resin composition, the resin composition contains: 10 to 60% by mass of at least one selected from aluminum hydroxide, magnesium hydroxide and a phosphorus compound, 0.05 to 5% by mass of a NOR type hindered amine compound, and 1 to 20% by mass of a fibrous filler with an aspect ratio of 10 or more, and the phosphorus content is 5% by mass or less relative to the total amount of the resin composition. This feature is a common technical feature in the following embodiments.
[0056] As an embodiment of the resin composition of the present invention, when the polyolefin resin is a polypropylene-based resin, the effect of the present invention is more significantly exerted, which is preferred.
[0057] As an embodiment of the resin composition of the present invention, from the viewpoint of exhibiting the effects of the present invention, it is preferred that the phosphorus compound includes a phosphate ester compound.
[0058] As an embodiment of the resin composition of the present invention, from the viewpoint of achieving the effects of the present invention, the mass ratio of the total content of the aluminum hydroxide and the magnesium hydroxide to the content of the phosphorus compound is preferably within a range of 100:0 to 75:25.
[0059] As an embodiment of the resin composition of the present invention, from the viewpoint of exhibiting the effects of the present invention, the aspect ratio of the fibrous filler is preferably 50 or more.
[0060] As an embodiment of the resin composition of the present invention, from the viewpoint of exhibiting the effects of the present invention, it is preferred that the fibrous filler contains halloysite.
[0061] The method for producing a resin composition of the present invention is a method for producing a resin composition of the present invention, characterized in that the method comprises: a first step of melt-kneading the polyolefin resin, at least one selected from aluminum hydroxide, magnesium hydroxide and a phosphorus compound, and the NOR-type hindered amine compound to obtain a resin mixture; and a second step of melt-kneading the resin mixture and the raw material components of the fibrous filler having an aspect ratio of 10 or more.
[0062] Even when a material whose aspect ratio is easily changed by cutting or the like during melt kneading is used as a raw material component of a fibrous filler having an aspect ratio of 10 or more, the aspect ratio of the obtained resin composition can be made 10 or more by the production method.
[0063] Hereinafter, the present invention and its constituent elements, as well as forms and modes for implementing the present invention will be described in detail. It should be noted that in the present application, "to" is used to mean that the numerical values described before and after it are included as lower limits and upper limits.
[0064] [Resin composition]
[0065] The resin composition of the present invention is a resin composition for injection molding containing a polyolefin resin, characterized in that, relative to the total amount of the resin composition, it contains: 10 to 60 mass % of at least one selected from aluminum hydroxide, magnesium hydroxide and a phosphorus compound (hereinafter also referred to as component (A)), 0.05 to 5 mass % of a NOR-type hindered amine compound (hereinafter also referred to as component (B)), and 1 to 20 mass % of a fibrous filler with an aspect ratio of 10 or more (hereinafter also referred to as component (C)), and the phosphorus content is less than 5 mass % relative to the total amount of the resin composition.
[0066] The resin composition of the present invention may optionally contain other resins other than the polyolefin resin and various additives generally contained in resin compositions in addition to the above-mentioned components within the range not impairing the effects of the present invention.
[0067] (Polyolefin resin)
[0068] The polyolefin resin is a homopolymer or copolymer obtained by polymerizing olefin as the main monomer component. It should be noted that in the present specification, "olefin" refers to an aliphatic chain unsaturated hydrocarbon having one double bond.
[0069] Here, the main component constituting the resin (polymer) refers to a component that is 50% by mass or more in all monomer components constituting the polymer. The polyolefin resin is preferably a homopolymer or copolymer containing olefins in 60 to 100% by mass, more preferably 70 to 100% by mass, and further preferably 80 to 100% by mass in all monomer components.
[0070] Olefin copolymers include copolymers of olefins and other olefins, or copolymers of olefins and other monomers copolymerizable with olefins. The content of the other monomers in the polyolefin resin is preferably 30% by mass or less, more preferably 0 to 20% by mass, based on all monomer components.
[0071] As the olefin, an α-olefin having 2 to 12 carbon atoms is preferred. Examples of the olefin include ethylene, propylene, 1-butene, isobutylene, 1-pentene, 3-methyl-1-butene, 1-hexene, 1-octene, and 1-decene. In the polymerization of the polyolefin resin, the olefin may be used alone or in combination of two or more.
[0072] As other monomers that can be copolymerized with olefins, for example, cyclic olefins such as cyclopentene and norbornene, and dienes such as 1,4-hexadiene and 5-ethylidene-2-norbornene, etc. can be cited. In addition, monomers such as vinyl acetate, styrene, (meth) acrylic acid and its derivatives, vinyl ether, maleic anhydride, carbon monoxide, N-vinyl carbazole, etc. can also be used. As for the other monomers, when polymerizing polyolefin resins, one kind can be used alone, or two or more kinds can be used in combination. It should be noted that "(meth) acrylic acid" refers to at least one of acrylic acid and methacrylic acid.
[0073] Specific examples of polyolefin resins include polyethylene resins with ethylene as the main component, such as high-density polyethylene (HDPE), low-density polyethylene (LDPE), and linear low-density polyethylene (LLDPE); polypropylene resins with propylene as the main component, such as polypropylene (propylene homopolymer), ethylene-propylene copolymer, propylene-butene copolymer, ethylene-propylene-butene copolymer, and ethylene-propylene-diene copolymer; polybutene; and polypentene, etc.
[0074] Specific examples of polyolefin resins include ethylene-vinyl acetate copolymers (EVA), ethylene-ethyl acrylate copolymers, polyketones, and copolymers produced using metallocene catalysts. In addition, these polymers are also modified by chemical reactions, specifically, ionomer resins, saponified products of EVA, and olefin elastomers produced using dynamic vulcanization in an extruder.
[0075] As the polyolefin resin, polyethylene resin and polypropylene resin are preferred, and polypropylene resin is more preferred. The stereoregularity of the structure of propylene derived from the polypropylene resin may be any of isotactic, syndiotactic and atactic. As the polypropylene resin, polypropylene is further preferred.
[0076] The polyolefin resin contained in the resin composition of the present invention may be one kind or two or more kinds. Commercially available products may be used as the polyolefin resin.
[0077] The content of the polyolefin resin in the resin composition of the present invention is the amount obtained by removing the contents of the component (A), component (B), component (C), and other components optionally contained from the resin composition. The content of the polyolefin resin can be set to, for example, a range of 20 to 90% by mass, more preferably a range of 30 to 80% by mass, relative to the total amount of the resin composition.
[0078] (Other resins)
[0079] The resin composition of the present invention may also contain other resins other than polyolefin resins. Other resins are, for example, thermoplastic resins, specifically, polyester resins such as polystyrene resins, acrylonitrile-butadiene-styrene copolymers (ABS resins), polycarbonate resins, and polyethylene terephthalate. These may be used alone or in combination of two or more. Other resins may use commercially available products.
[0080] In addition, as other resins, resins that function as toughening agents can also be used. Toughening agents are used for the purpose of improving the flexibility, processability, impact resistance, etc. of resin combinations, such as resins with rubber elasticity. As mentioned above, if toughening agents are added, it can be predicted that rigidity can be reduced as its side effect. Therefore, when using, it is necessary to pay attention to adjusting the content so that it does not damage the effect of the present invention.
[0081] The resin used as a toughening agent is preferably a thermoplastic elastomer comprising: a soft segment composed of a polymer containing a monomer containing butadiene, and a hard segment composed of a polymer containing a monomer having an aromatic group such as styrene, examples of which include: methyl methacrylate-butadiene-styrene copolymer (MBS), acrylonitrile-butadiene-styrene copolymer (ABS), styrene-butadiene-styrene copolymer (SBS), and butyl acrylate-methyl methacrylate copolymer. Among them, from the viewpoint of compatibility and flame retardancy of the resin composition and dispersibility of the thermoplastic elastomer in the resin composition, the toughening agent is preferably one or more selected from MBS and ABS. The toughening agent can be used alone or in combination of two or more.
[0082] The content of other resins in the resin composition of the present invention may be, for example, 0 to 20 parts by mass, more preferably 0 to 10 parts by mass, based on 100 parts by mass of the polyolefin resin. It is particularly preferred that no other resins be contained.
[0083] (ingredient (A))
[0084] Component (A) is at least one selected from aluminum hydroxide, magnesium hydroxide and a phosphorus compound. Hereinafter, aluminum hydroxide and magnesium hydroxide are sometimes referred to as component (A1), and the phosphorus compound is referred to as component (A2). In the resin composition of the present invention, component (A) mainly functions as a flame retardant.
[0085] Relative to the total amount of the resin composition of the present invention, the content of component (A) is 10 to 60% by mass. If the content of component (A) is less than 10% by mass, the flame retardancy of the injection molded product is insufficient, and if it exceeds 60% by mass, the mechanical strength of the injection molded product, especially the impact strength is insufficient. The content of component (A) relative to the total amount of the resin composition is preferably in the range of 10 to 45% by mass, more preferably in the range of 10 to 25% by mass.
[0086] It should be noted that the phosphorus content relative to the total amount of the resin combination of the present invention is 5% by mass or less. In the resin combination of the present invention, the content of component (A) is set to within the range, and it is a necessary element that the phosphorus content is set to 5% by mass or less relative to the total amount of the composition. The phosphorus content relative to the total amount of the resin combination is preferably 2% by mass or less, more preferably 1% by mass or less, and further preferably 0% by mass.
[0087] The phosphorus content (mass %) relative to the total amount of the resin composition can be measured using, for example, an energy dispersive fluorescent X-ray analyzer (for example, JSX-1000S (manufactured by JEOL Ltd.)).
[0088] The phosphorus compound as component (A2) lacks compatibility with the polyolefin resin and is therefore easily separated during melting, and the separated compound bleeds out and remains on the surface of the molded product, which easily leads to a reduction in appearance. If the phosphorus content relative to the total amount of the resin composition is set to 5% by mass or less, the reduction in appearance caused by the bleed of component (A2) can be suppressed.
[0089] In component (A), the mass ratio of the content of component (A1) to component (A2) is preferably in the range of 100:0 to 30:70, more preferably in the range of 100:0 to 50:50, and even more preferably in the range of 100:0 to 75:25, as the content of component (A1):the content of (A2). By making the mass ratio of the content of component (A1) to component (A2) within the above range, the generation of burrs etc. in continuous production during injection molding can be suppressed, and the quality of the molded product can be easily maintained at a good level.
[0090] Resin composition of the present invention is a resin composition for injection molding. In injection molding, in the process of filling the molten resin composition into the metal mold cavity, the decomposition gas of the organic components in the resin composition produced when the air originally present in the cavity, the decomposition gas of the organic components in the resin composition produced when being retained in the tube, or the decomposition gas produced due to shear heat generation, etc., are compressed adiabatically in the final filling part, and significant heating and subsequent decomposition are generated. In order to prevent this situation, for example, a vent is provided in the final filling part of the metal mold so that the gas is discharged. In particular, since the decomposition product of the phosphorus compound shows acidity, when the resin composition contains the phosphorus compound, the vent portion that becomes high temperature is easily corroded. If the corrosion of the vent portion progresses, the thickness of the vent portion can slowly expand, causing the molded product to produce burrs.
[0091] By setting the mass ratio of the content of component (A1) to component (A2) within the above range, the content of the phosphorus compound in the resin composition can be relatively reduced, and as a result, the effects of suppressing corrosion of the vent portion and suppressing the occurrence of burrs in injection molded products can be particularly significantly obtained.
[0092] <Ingredients (A1)>
[0093] Component (A1) is aluminum hydroxide or magnesium hydroxide. As component (A1), aluminum hydroxide or magnesium hydroxide can be used alone, or both can be used simultaneously. As described above, the ratio of component (A1) in component (A) is preferably 30 to 100% by mass, more preferably 50 to 100% by mass, and further preferably 75 to 100% by mass.
[0094] The form of component (A1) is preferably particles. The shape of the particles is not particularly limited, and may be spherical, spindle-shaped, plate-shaped, scaly, needle-shaped, fibrous, etc. When component (A1) is particles, the aspect ratio measured in the same manner as component (C) is less than 10.
[0095] The average particle size of the component (A1) in the resin composition is preferably in the range of 0.01 to 100 μm, more preferably 0.1 to 10 μm, and further preferably 0.2 to 2 μm. The average particle size of the component (A1) can be the same as the primary particle size of the particles of aluminum hydroxide or magnesium hydroxide used in the manufacture of the resin composition (hereinafter also referred to as "raw particles"). The primary particle size of the raw particles measured by the laser refraction and scattering method can be measured in the form of a volume-based median diameter (D50).
[0096] The raw material particles of component (A1) can also be surface-modified by surface modifier as required. As the surface modifier used in surface modification, alkylsilazane compounds such as hexamethyldisilazane (HMDS), dimethyldimethoxysilane, dimethyldiethoxysilane, trimethylmethoxysilane, methyltrimethoxysilane, alkylalkoxysilane compounds such as butyltrimethoxysilane, dimethyldichlorosilane, chlorosilane compounds such as trimethylchlorosilane, silicone oil, polysiloxane varnish (silicone varnish), various fatty acids, etc. can be used. These surface modifiers can be used alone or in combination with two or more.
[0097] <Ingredient (A2)>
[0098] Component (A2) is a phosphorus compound. As far as component (A2) is concerned, as long as it is a compound containing phosphorus, it can be used without particular limitation. It should be noted that, when using component (A2) as component (A) as described above, it is used in a manner that the phosphorus content relative to the total amount of the resin composition is 5% by mass or less. As described above, the phosphorus content relative to the total amount of the resin composition is preferably 2% by mass or less, more preferably 1% by mass or less, and further preferably 0% by mass. From such a viewpoint, the ratio of component (A2) in component (A) is preferably 0 to 70% by mass, more preferably 0 to 50% by mass, and further preferably 0 to 25% by mass.
[0099] Phosphorus compounds include, for example, salts of phosphinic acid, phosphonic acid, phosphoric acid, etc. with metals, ammonium, etc.; ester compounds of phosphinic acid, phosphonic acid, phosphoric acid, etc. As component (A2), phosphate ester compounds (described in detail later) are preferred from the viewpoint of flame retardancy effect.
[0100] Specific examples of the salt include metal phosphinates, particularly aluminum phosphinate and zinc phosphinate, metal phosphonates, particularly aluminum phosphinate, calcium phosphinate and zinc phosphinate, and hydrates of corresponding metal phosphonates, ammonium phosphate, ammonium polyphosphate and the like.
[0101] Examples of the phosphinate compound include dimethylphosphinic acid, methylethylphosphinic acid, methylpropylphosphinic acid, diethylphosphinic acid, dioctylphosphinic acid, phenylphosphinic acid, diethylphenylphosphinic acid, diphenylphosphinic acid, and bis(4-methoxyphenyl)phosphinic acid.
[0102] Examples of the phosphonate compound include methylphosphonic acid, dimethyl methylphosphonate, diethyl methylphosphonate, ethylphosphonic acid, propylphosphonic acid, butylphosphonic acid, 2-methyl-propylphosphonic acid, tert-butylphosphonic acid, 2,3-dimethylbutylphosphonic acid, octylphosphonic acid, phenylphosphonic acid, and dioctyl phenylphosphonate.
[0103] In addition, as phosphorus compounds other than those mentioned above, derivatives of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), polyphosphonates (for example, Nofia (trademark) HM1100 (FRX Polymers (Chelmsford, USA)), zinc bis(diethyl phosphinate), aluminum tris(diethyl phosphinate), melamine phosphate, melamine pyrophosphate, melamine polyphosphate, melamine poly(aluminum phosphate), melamine poly(zinc phosphate), methylphosphonic acid melamine salt, guanyl urea phosphate, guanidine phosphate, ethylenediamine phosphate and phosphazene compounds, such as phenoxyphosphazene oligomers, can be used as component (A2).
[0104] The phosphorus compounds may be used alone or in combination of two or more as the component (A2).
[0105] 〔Phosphate compounds〕
[0106] The phosphate compound may be an aliphatic phosphate compound or an aromatic phosphate compound, preferably an aromatic phosphate compound. If an aromatic phosphate compound is used as component (A), it is believed that the NOR type HALS generates free radicals more stably and is more likely to exhibit flame retardancy.
[0107] Examples of the phosphate ester compound include monomeric phosphate ester compounds obtained by reacting phosphoric acid with an aliphatic or aromatic alcohol, and aromatic condensed phosphate ester compounds that are reaction products of phosphorus oxychloride, a divalent phenolic compound, and phenol (or alkylphenol).
[0108] Specific examples of the phosphate ester compound include trimethyl phosphate (TMP), triethyl phosphate (TEP), tributyl phosphate, triphenyl phosphate (TPP), tricresyl phosphate (TCP), trixylene phosphate (TXP), cresyl diphenyl phosphate (CDP), tris(2,4-di-tert-butylphenyl) phosphate, distearyl pentaerythritol diphosphate, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphate, bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphate, resorcinol bis-dixylenyl phosphate, resorcinol bis-diphenyl phosphate, bisphenol A bis-diphenyl phosphate (BADP), bisphenol A bis-di-cresyl phosphate, biphenol A bis-diphenyl phosphate, and bisphenol A bis-dixylenyl phosphate.
[0109] Furthermore, the phosphoric acid ester compound is preferably a condensed phosphoric acid ester compound of a condensed type from the viewpoint of heat resistance, etc. Examples of the condensed phosphoric acid ester compound include aromatic condensed phosphoric acid ester compounds represented by the following chemical formula (A2).
[0110] [Chemical formula 1]
[0111] Formula (A2)
[0112]
[0113] In the formula (A2), R 1 ~R 5are independently a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, or a halogen atom, R 1 ~R 5 Can be the same or different. There are multiple (5) R 1 They may be the same or different from each other. 2 , R 3 , R 4 and R 5 The same applies. n is an integer of 1-30, and preferably an integer of 1-10.
[0114] Examples of the alkyl group include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, tert-pentyl, hexyl, 2-ethylhexyl, n-octyl, nonyl, and decyl.
[0115] Examples of the cycloalkyl group include a cyclohexyl group, and examples of the aryl group include a phenyl group, a tolyl group, a xylyl group, a 2,6-xylyl group, a 2,4,6-trimethylphenyl group, a butylphenyl group, and a nonylphenyl group.
[0116] Examples of the alkoxy group include a methoxy group, an ethoxy group, a propoxy group, a butoxy group, etc. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, etc.
[0117] The aromatic condensed phosphate compound is a reaction product of phosphorus oxychloride, a divalent phenolic compound and phenol (or alkylphenol) as described above, and the aromatic condensed phosphate compound having a structure represented by formula (A2) is a compound in the case where the divalent phenolic compound is resorcinol (hereinafter, also referred to as "resorcinol compound") which may have a substituent. The aromatic condensed phosphate compound may be a compound obtained by using 4,4′-biphenol or bisphenol A (each of which may have a substituent) instead of the resorcinol compound. Specifically, in the present invention, an aromatic condensed phosphate compound having a 4,4′-biphenol residue or a bisphenol A residue which may have a substituent instead of the resorcinol compound residue in formula (A2) may be used.
[0118] Commercially available phosphate compounds may be used. Examples of commercially available phosphate compounds include PX-200 (resorcinol bis-di-xylene phosphate) and CR-733S (resorcinol bis-diphenyl phosphate), both manufactured by Daihachi Chemical Industry Co., Ltd.
[0119] (Component (B))
[0120] Component (B) is a NOR type HALS. Relative to the total amount of the resin composition of the present invention, the content of component (B) is 0.05 to 5% by mass. As described above, component (B) has the effect of reducing the melt viscosity of the resin composition during injection molding, and thus, the resin composition of the present invention has the effect of suppressing the wear of the metal mold. If the content of component (B) is less than 0.05% by mass, the effect of suppressing the wear of the metal mold cannot be fully obtained when used for injection molding. If the content of component (B) exceeds 5% by mass, the mechanical strength, especially the bending strength, of the injection molded product is insufficient. The content of component (B) relative to the total amount of the resin composition is preferably in the range of 0.1 to 2% by mass, more preferably in the range of 0.2 to 1% by mass.
[0121] Component (B) has the function of imparting flame retardancy to injection molded articles in addition to the above-mentioned functions. In addition, NOR-type HALS is also widely known as a light stabilizer, and light resistance can also be imparted by adding NOR-type HALS.
[0122] NOR type HALS is a HALS having an alkoxyimino group (>N-OR). The alkoxyimino group refers to a group having an N-alkoxy structure in which H is substituted by an alkoxy group, as distinguished from the NH type in which the H of the NH part of the imino group (>NH) remains H, the NR type in which H is substituted by an alkyl group (R (same meaning as R of alkoxy)), typically by a methyl group, and the typical N-methyl type. The N-alkoxy group captures an alkyl peroxy radical (RO2·) and easily becomes a free radical, exerting a flame retardant effect. In addition, in the resin composition of the present invention, it functions in a manner that suppresses the wear of the metal mold.
[0123] On the other hand, in the case of NR-type hindered amine compounds, typically in the case of N-methyl-type hindered amine compounds or NH-type hindered amine compounds, the function of suppressing mold wear is lost and the flame retardant effect is also low.
[0124] The R in the alkoxy group (-OR) represents a substituted or unsubstituted saturated or unsaturated hydrocarbon group. Examples of R include alkyl, aralkyl, and aryl groups. The alkyl group may be linear, branched, or cyclic, or may be a combination of these.
[0125] The NOR type HALS used in the present invention is not particularly limited as long as it has an alkoxyimino (>N-OR) structure. As specific examples, for example, the NOR type HALS described in Japanese Unexamined Patent Application Publication No. 2002-507238, International Publication No. 2005 / 082852, International Publication No. 2008 / 003605, etc. can be cited as preferred examples.
[0126] Examples of NOR-type HALS include compounds having a structure represented by the following formula (B).
[0127] [Chemical formula 2]
[0128] Formula (B)
[0129]
[0130] [In formula (B), G 1 and G 2 Each of them independently represents an alkyl group having 1 to 4 carbon atoms, or together represents a pentamethylene group.
[0131] Z 1 and Z 2 Each represents a methyl group, or Z 1 With Z 2 Together, they form a cross-linking portion. The cross-linking portion may be further bonded to an organic group via an ester group, an ether group, an amide group, an amino group, a carbonyl group or a carbamate group.
[0132] E represents an alkoxy group having 1 to 18 carbon atoms, a cycloalkoxy group having 5 to 12 carbon atoms, an aralkoxy group having 7 to 25 carbon atoms, or an aryloxy group having 6 to 12 carbon atoms.]
[0133] As the NOR type HALS represented by formula (B), a high molecular weight substance is preferred. High molecular weight substances are generally oligomeric or polymeric compounds. If they are high molecular weight substances, they have excellent flame retardancy and heat resistance. As for the oligomeric or polymeric compounds of the high molecular weight substances, the number of repeating units is preferably 2 to 100, and more preferably 5 to 80.
[0134] As the NOR-type HALS represented by the formula (B), for example, a compound represented by the following formula (1) can be used.
[0135] [Chemical formula 3]
[0136]
[0137] In the formula (1), R 1 ~R 4 Each of them represents a hydrogen atom or an organic group of the following formula (2). 1 ~R 4 At least one of them is an organic group represented by the following formula (2).
[0138] [Chemical formula 4]
[0139]
[0140] In the formula, R 5represents an alkyl group having 1 to 17 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, a phenyl group, or a phenylalkyl group having 7 to 15 carbon atoms, and R 6 , R 7 , R 8 and R 9 Each of them represents an alkyl group having 1 to 4 carbon atoms. 10 It represents a hydrogen atom or a linear or branched alkyl group having 1 to 12 carbon atoms.
[0141] As R 5 Among the alkyl groups having 1 to 17 carbon atoms, methyl, propyl or octyl is preferred. Among the cycloalkyl groups having 5 to 10 carbon atoms, cyclohexyl is preferred. Among the phenyl groups or phenylalkyl groups having 7 to 15 carbon atoms, phenyl is preferred.
[0142] As R 6 ~R 9 Among the alkyl groups having 1 to 4 carbon atoms, a methyl group is preferred.
[0143] As R 10 Among the linear or branched alkyl groups having 1 to 12 carbon atoms, n-butyl group is preferred.
[0144] In formula (1), preferably R 1 , R 2 and R 3 is an organic group of formula (2), or R 1 , R 2 and R 4 It is an organic group of formula (2).
[0145] Specific examples of NOR-type HALS include the following compounds.
[0146] 1-Cyclohexyloxy-2,2,6,6-tetramethyl-4-octadecylaminopiperidine; bis(1-octyloxy-2,2,6,6-tetramethylpiperidin-4-yl) sebacate; 2,4-bis[(1-cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl)butylamino]-6-(2-hydroxyethylamino)-s-triazine; bis(1-cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl) adipate; as 4,4′-hexamethylenebis(amino-2,2,6 An oligomeric compound of a condensation product of 4,4′-hexamethylenebis(amino-2,2,6,6-tetramethylpiperidine) and 2,4-dichloro-6-[(1-octyloxy-2,2,6,6-tetramethylpiperidin-4-yl)butylamino]-s-triazine end-capped with 2-chloro-4,6-bis(dibutylamino)-s-triazine; -[(1-cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl)butylamino]-s-triazine condensation product oligomeric compound; 2,4-bis[(1-cyclohexyloxy-2,2,6,6-piperidin-4-yl)-6-chloro-s-triazine; reaction of peroxidized 4-butylamino-2,2,6,6-tetramethylpiperidine with 2,4,6-trichloro-s-triazine with cyclohexane and N,N′-ethane-1,2-diylbis(1,3-propanediamine) Product (N,N′,N″′-tri{2,4-bis[(1-cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl)n-butylamino]-s-triazine-6-yl}-3,3′-ethylenediiminobispropylamine); bis(1-undecyloxy-2,2,6,6-tetramethylpiperidin-4-yl) carbonate; 1-undecyloxy-2,2,6,6-tetramethylpiperidin-4-one; bis(1-stearyloxy-2,2,6,6-tetramethylpiperidin-4-yl) carbonate.
[0147] NOR type HALS can use commercial products. As commercial products of NOR type HALS, Flamestab NOR116FF, TINUVIN NOR371, TINUVIN XT850FF, TINUVIN XT855FF, TINUVIN PA123 manufactured by BASF, LA-81, FP-T80 manufactured by ADEKA, etc. can be cited. NOR type HALS can be used alone or in combination of two or more.
[0148] (ingredient (C))
[0149] Component (C) is a fibrous filler having an aspect ratio of 10 or more. The aspect ratio in component (C) is an average aspect ratio obtained by the following method. It should be noted that, hereinafter, a fibrous filler having an aspect ratio of 10 or more is also referred to as a fibrous filler (C).
[0150] <Measurement Method of Aspect Ratio>
[0151] The aspect ratio of the fibrous filler is expressed as a value obtained by dividing the fiber length (the length of the fiber) in the fibrous filler by the fiber diameter (the smallest diameter among the diameters of the cross section perpendicular to the length direction of the fiber, that is, the minimum value of the thickness of the fiber). In the present invention, for the fibrous filler in the resin composition, the fiber length and fiber diameter of 100 fiber fillers are measured respectively, the aspect ratio of each fiber filler is obtained, and the average value (average aspect ratio) of the 100 fibers is calculated as the aspect ratio.
[0152] The shape of the fibrous filler used as a raw material when manufacturing a resin composition may change due to the manufacturing process of the resin composition such as mixing, crushing, and molding. For example, the raw material fibrous filler is often broken during the manufacturing process, causing the fiber length to change. Therefore, in the present invention, the fiber length and fiber diameter of the fibrous filler present in the resin composition are measured to calculate the aspect ratio of the fibrous filler.
[0153] Specifically, by heating the resin composition with an electric furnace or the like, the resin containing the polyolefin resin, the organic component in the component (A), the organic component in the component (B) and the like are burned and removed, and the fibrous filler is taken out from the inorganic component that has become the residue. The heating temperature is a temperature at which the organic component can be burned, for example, it is set to be above 500°C. The inorganic component of the residue includes the inorganic component in the component (A) and the fibrous filler. The shape of the inorganic component in the component (A) is not fibrous, so it can be distinguished from the fibrous filler. 100 fibrous fillers are randomly selected from the inorganic component. It should be noted that the constituent material of the fibrous filler (C) as the component (C) is an inorganic material.
[0154] The fiber length and fiber diameter are measured by observing the given number of fibrous fillers in the resin composition obtained in this way with a scanning electron microscope, a transmission electron microscope, an atomic force microscope or the like.
[0155] The aspect ratio of the fibrous filler (C) is 10 or more. The aspect ratio is preferably 20 or more, more preferably 50 or more. When a fibrous filler having an aspect ratio of less than 10 is used, sufficient mechanical strength, in particular bending strength, cannot be obtained in the injection molded product of the resin composition. From the viewpoint of the fluidity of the resin during injection molding, the aspect ratio of the fibrous filler (C) is, for example, preferably 500 or less, more preferably 100 or less.
[0156] The average fiber length of the fibrous filler (C) obtained by the method is, for example, preferably 0.01 to 1 mm, and more preferably 0.02 to 0.5 mm. In addition, the average fiber diameter of the fibrous filler (C) is, for example, preferably 0.001 to 0.05 mm, and more preferably 0.005 to 0.02 mm. In addition, the average fiber length and average fiber diameter of the fibrous filler (C) may be nanometer sizes as described in the halloysite described later.
[0157] Relative to the total amount of the resin composition of the present invention, the content of component (C) is 1 to 20% by mass. If the content of component (C) is less than 1%, the mechanical strength of the injection molded product, especially the bending strength is insufficient, and if it exceeds 20% by mass, the effect of suppressing the wear of the metal mold cannot be fully obtained when used for injection molding. The content of component (C) relative to the total amount of the resin composition is preferably in the range of 2 to 15% by mass, and more preferably in the range of 5 to 10% by mass.
[0158] Examples of the fibrous filler (C) include glass fiber, carbon fiber, carbon nanotube, metal fiber, mineral fiber, ceramic fiber, rock wool, wollastonite, potassium titanate, barium titanate, sepiolite, halloysite, imogolite, and the like, which have an aspect ratio of 10 or more. These fibrous fillers (C) may be used alone or in combination of two or more.
[0159] As the fibrous filler (C), from the viewpoint of suppressing the wear of the metal mold, halloysite having an aspect ratio of 10 or more is preferred. Halloysite is represented by the composition formula Al2Si2O5(OH)4, and is typically available in the form of a tubular nanofiller having a fiber diameter of tens of nanometers and a fiber length of hundreds to thousands of nanometers. Halloysite is known to be nano-sized and has a highly active Al(OH) structure inside, so it has unique characteristics such as a large gas adsorption effect.
[0160] When halloysite is used as the fibrous filler (C), the effects of suppressing corrosion of the vents of the injection molding mold described above and suppressing the occurrence of burrs in the injection molded product can be particularly remarkable.
[0161] In consideration of the breakage of the fibrous filler used in manufacturing the resin composition (hereinafter, also referred to as "raw fiber filler" to distinguish it from the fibrous filler (C) in the resin composition) during the manufacturing process, for example, a material having a larger aspect ratio than the fibrous filler (C) is used depending on the constituent material of the fibrous filler. For example, in the case of including constituent materials that take into account the occurrence of breakage during the manufacturing process, the aspect ratio of the raw fiber filler is preferably 20 or more, and more preferably 100 or more, depending on the type.
[0162] In order to obtain better mechanical strength, the raw material fibrous filler is preferably pretreated with a coupling agent such as an isocyanate compound, an organic silane compound, an organic titanate compound, an organic borane compound, or an epoxy compound before use.
[0163] (Other additives)
[0164] The resin composition of the present invention may contain known components as additives in addition to the resin, component (A), component (B) and component (C) comprising the polyolefin resin, within the scope of not impairing the effect of the present invention. Other additives include flame retardants, dripping preventers, antioxidants, lubricants, etc. other than component (A) and component (B).
[0165] <Other flame retardants>
[0166] Other flame retardants may be organic flame retardants or inorganic flame retardants. Examples of organic flame retardants include bromine compounds, etc. Examples of inorganic flame retardants include antimony compounds and metal hydroxides other than component (A1).
[0167] <Drip prevention agent>
[0168] The dripping preventer is added for the purpose of preventing the resin material from dripping (drip) during combustion and improving the flame retardancy. Examples of the dripping preventer include fluorine-based dripping preventers, silicone rubbers, layered silicates, etc. The dripping preventer can be used alone or in combination of two or more.
[0169] <Antioxidants>
[0170] Examples of the antioxidant include hindered phenols and the like.
[0171] <Lubricant>
[0172] Examples of the lubricant include one or more selected from fatty acid salts, fatty acid amides, silane polymers, solid paraffin, liquid paraffin, calcium stearate, zinc stearate, stearic acid amide, polysiloxane powder, methylene bis stearic acid amide and N,N′-ethylene bis stearic acid amide.
[0173] The content of other additives in the resin composition of the present invention is within the range that does not impair the effect of the present invention, for example, within the range of about 0.1 to 30% by mass, preferably within the range of 0.1 to 20% by mass, relative to the total amount of the resin composition. In addition, it is preferably less than 30% by mass in total.
[0174] [Method for producing resin composition]
[0175] The resin composition of the present invention can be obtained by melt-kneading the raw material components including the resin of the polyolefin resin, component (A), component (B), component (C), and other additives that may be contained as needed into the resin composition of the present invention. In particular, with regard to component (C), there is a case where the aspect ratio of the raw material fiber filler changes (decreases) when it becomes a fibrous filler (C) during the manufacturing process.
[0176] With regard to the resin composition of the present invention, for example, it is preferred to take into account the change in the aspect ratio and to apply a manufacturing method having the following steps depending on the constituent materials of the raw material fibrous filler: a first step of melt-kneading the polyolefin resin, component (A), and component (B) to obtain a resin mixture; and a second step of melt-kneading the resin mixture and a raw material fibrous filler of a fibrous filler having an aspect ratio of 10 or more.
[0177] When the resin composition of the present invention contains other resins or other additives, the other resins or other additives may be melt-kneaded in the first step or in the second step.
[0178] In addition, pellets obtained by melt-kneading a raw material fibrous filler and a resin such as a polyolefin resin are sometimes used in the above. As long as at least a portion of the polyolefin resin contained in the resin composition is melt-kneaded in the first step, the remaining portion can be added and melt-kneaded in the second step as needed. The same is true for component (A) and component (B).
[0179] In the manufacture method of the present invention, the melt mixing in the first process and the second process is carried out using a mixing device such as a Banbury mixer, a roller, a plastograph, an extruder (single-axis extruder, a multi-axis extruder (e.g., a two-axis extruder), etc.), and a kneader. Among them, from the viewpoint of high production efficiency, it is preferred to use an extruder for melt mixing. And, from the viewpoint of being able to impart high shearing properties, it is preferred to use a multi-axis extruder for melt mixing, and more preferably a two-axis extruder. Here, the term extruder is used to include the scope of an extrusion mixer.
[0180] In the production method of the present invention, different kneading devices may be used in the first step and the second step, but it is preferred that an extruder, particularly a twin-screw extruder, be used in both steps.
[0181] The temperature during melt kneading (melt kneading temperature) is set to be above the melting temperature of the polyolefin resin in both the first step and the second step. The melt kneading temperature is, for example, preferably 150 to 280° C., and can be appropriately selected according to the polyolefin resin used. When a polypropylene resin is used as the polyolefin resin, the melt kneading temperature is preferably 180 to 270° C., more preferably 180 to 230° C. As long as it is within the temperature range, the melt kneading temperatures in the first step and the second step may be the same or different. When an extruder is used for melt kneading, the kneading melt temperature is equivalent to the barrel temperature.
[0182] When an extruder is used for melt kneading, the screw rotation speed of the first step and the second step is preferably in the range of 50 to 300 rpm. In addition, the screw rotation speeds in the first step and the second step may be the same or different. The ejection amount of the resin mixture or resin composition of the extruder in the first step and the second step is preferably in the range of 1 to 50 kg / hr, respectively.
[0183] In the present invention, the same extruder can be used to continuously carry out the first process and the second process, which is preferred from the viewpoint of productivity. For example, by using a two-axis extruder, the raw material components other than the raw material fibrous filler are supplied from the hopper at the rear end of the barrel of the two-axis extruder, and the raw material fibrous filler is supplied from the front of the barrel, for example, the side feeder arranged at the central part, and the first process and the second process can be continuously carried out. It should be noted that the end of the frontmost part of the barrel is the ejection portion of the resin combination, and the rearmost part is equivalent to the vicinity of the barrel end on the opposite side of the ejection portion.
[0184] Before the melt-kneading in the first step, the components may be mixed in advance (dry blended) using various mixers such as a tumble mixer or a high-speed mixer widely known as a Henschel mixer.
[0185] In the production method of the present invention, after the kneaded product is extruded into a stranded shape in the second step, the kneaded product extruded into a stranded shape may be processed into a form such as pellets or flakes.
[0186] It should be noted that the resin composition of the present invention can be made into various forms such as powder, granule, tablet (tablet), pellet, flake, fiber and liquid.
[0187] If the resin composition of the present invention is used, for example, the wear of the gate portion of the metal mold and the corrosion of the vent portion can be suppressed in long-term continuous production, and injection molded products can be economically produced with stable quality. In addition, the injection molded products obtained using the resin composition of the present invention have excellent appearance, mechanical strength (rigidity and toughness) and flame retardancy.
[0188] For example, the bending strength of the injection molded product formed by the resin composition of the present invention in the bending test implemented in accordance with JIS-K7171 is preferably 25 MPa or more, more preferably 35 MPa or more, and further preferably 50 MPa or more. If the bending strength is 25 MPa or more, it can be evaluated that the rigidity of the molded product has no problem in practical use.
[0189] For example, the Charpy impact strength of an injection-molded article formed from the resin composition of the present invention measured in a Charpy impact test (with notch) in accordance with JIS-K7110 is preferably 8 kJ / m 2 More preferably 15 kJ / m 2 More preferably, 20 kJ / m 2 If the Charpy impact strength is 8kJ / m 2 From the above, it can be evaluated that the toughness of the molded product has no practical problem.
[0190] Here, flame retardancy is a type of flame resistance, which means that the burning speed is slow, but the burning continues to a certain extent. There are JIS, ASTM, etc. for evaluating flame resistance, and generally speaking, the UL standard is particularly important. The UL standard is a standard established by the "Underwriters Laboratories" in the United States and evaluated by the company.
[0191] Injection molded articles formed from the resin composition of the present invention are preferably judged as V-2 or higher, more preferably V-1 or higher, and even more preferably V-0 in a combustion test according to UL-94 when evaluated in the form of a test piece of a given size in accordance with the UL standard.
[0192] (Molding products)
[0193] The resin composition of the present invention can be used to produce an injection-molded article. By using the injection-molded article, as described above, a product having excellent appearance, mechanical strength (rigidity and toughness) and flame retardancy can be obtained.
[0194] When manufacturing injection molded products, a conventionally known injection molding machine can be used. Injection molded products, for example, can be manufactured by melting a resin composition in a barrel, injecting the molten resin composition into a metal mold, and then cooling the metal mold. The injection speed and pressure can be adjusted appropriately. The injection molding conditions are preferably, for example: a barrel temperature (melting temperature) of 180 to 230°C, an injection speed of 30 to 200 mm / sec, and a pressure of 500 to 1000 kgf / cm 2 , the metal mold temperature is 40~80℃.
[0195] Here, the fiber length, fiber diameter and aspect ratio of the fibrous filler in the injection molded product can be measured or calculated by the same method as that of the fibrous filler in the resin composition. As for the fiber length, fiber diameter and aspect ratio of the fibrous filler in the injection molded product obtained using the resin composition of the present invention, it is preferably within a range that can fully exert the effect of the present invention. Specifically, the average aspect ratio of the fibrous filler is preferably in the range of 10 to 100. In addition, the average fiber length of the fibrous filler is preferably in the range of 0.01 to 1 mm, and the average fiber diameter is preferably in the range of 0.001 to 0.05 mm. The average fiber length and average fiber diameter of the fibrous filler can be the nanometer size described in the halloysite.
[0196] The injection-molded article obtained by injection molding the resin composition of the present invention is not particularly limited, and examples thereof include electrical and electronic components, electrical components, exterior components, and interior components in the fields of home appliances and vehicles, various packaging materials, household goods, office supplies, piping, and agricultural materials. Example
[0197] Hereinafter, the present invention will be specifically described with reference to the examples, but the present invention is not limited to these examples. It should be noted that the "parts" or "%" used in the examples refer to "parts by mass" or "mass %" unless otherwise specified.
[0198] [Resin composition; Examples 1 to 18, Comparative Examples 1 to 8]
[0199] As raw material components contained in the resin composition of each Example and Comparative Example, the following commercially available products were prepared.
[0200] <Resin>
[0201] Polypropylene resin: Prime Polypro J715M (product name, manufactured by Prime Polymer Co., Ltd.)
[0202] Polyethylene resin: HJ560 (product name, made by Japan Polyethylene Co., Ltd.)
[0203] <Ingredients (A1)>
[0204] Aluminum hydroxide: KH-101 (product name, manufactured by KC Corporation, particles having an average primary particle size of 1.0 μm)
[0205] Magnesium hydroxide: MAGSEEDS N-6 (product name, manufactured by Shinjima Chemical Industry Co., Ltd., average primary particle size 1.2 μm, particles surface-modified with higher fatty acids)
[0206] <Ingredient (A2)>
[0207] Phosphate compound: PX-200 (product name, manufactured by Daihachi Chemical Industry Co., Ltd., resorcinol bis-di-xylene phosphate)
[0208] Ammonium polyphosphate: Taien K (product name, manufactured by Taihei Chemical Industry Co., Ltd.)
[0209] Phosphonic acid metal salt: calcium phosphonate (manufactured by Kanto Chemical Co., Ltd.)
[0210] <Component (B)>
[0211] NOR type HALS: Flamestab NOR116FF: (product name, manufactured by BASF, N,N′,N″′-tris{2,4-bis[(1-cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl)n-butylamino]-s-triazine-6-yl}-3,3′-ethylenediiminobispropylamine)
[0212] <HALS other than component (B)>
[0213] NH type HALS: Tinuvin 770DF (manufactured by BASF, bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacic acid ester)
[0214] NR (methyl) type HALS: Tinuvin 765 (produced by BASF, a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacic acid ester and methyl-1,2,2,6,6-pentamethyl-4-piperidinyl-sebacic acid ester)
[0215] <Raw material fibrous filler of component (C)>
[0216] Glass fiber: ECS03T-430 (manufactured by Nippon Electric Glass Co., Ltd.; average fiber diameter 13 μm, average fiber length 3 mm)
[0217] Glass long fibers: FUNCSTER LR-24A (manufactured by Japan Polypropylene Co., Ltd.; polypropylene masterbatch pellets containing 40% by mass of glass long fibers; pellet length 10 mm) was used. In Tables I and II, the glass long fiber portion of the pellets (FUNCSTER LR-24A) blended in the resin composition is recorded in the component (C) column, and the polypropylene portion is recorded in the resin component column in the form of the amount combined with the J715M.
[0218] Halloysite: Dragonite APA:M (manufactured by Fimatec; average aspect ratio 18)
[0219] ·Wollastonite: WFC10 (manufactured by Japan Talc Co., Ltd.; average aspect ratio 14)
[0220] Potassium titanate: Tismo D (manufactured by Otsuka Chemical Co., Ltd.; average aspect ratio 30)
[0221] Carbon fiber: Chopped carbon fiber HT C413 (made by Teijin, average fiber diameter 7 μm, average fiber length 6 mm)
[0222] (Manufacture of resin composition)
[0223] In each of the Examples and Comparative Examples, each component was used in the content (mass %) shown in Table I and Table II. In addition, in the column of the content (mass %) of each component, a blank indicates that the component is not contained.
[0224] Using a two-axis extruder ("TEX30α" made by Nippon Steel Works), melt mixing was performed at a barrel temperature of 200°C and a screw rotation speed of 150rpm. Except for Comparative Example 1, the raw material components other than the fibrous filler were pre-dry mixed, and then supplied from a hopper at the rear of the barrel of the two-axis extruder, and the fibrous filler was supplied from a side feeder at the central portion of the barrel. For Comparative Example 1, all raw material components including the fibrous filler were pre-dry mixed, and then supplied from a hopper at the rear of the barrel of the two-axis extruder. In the resin composition manufacturing method column of Table I and Table II, Comparative Example 1 is recorded as "together", and other than Comparative Example 1 is recorded as "split".
[0225] The strands ejected from the extruder were cut with a pelletizer and processed into pellets of 2 mm in diameter x 3 mm in length to prepare a resin composition.
[0226] [Analysis of components in resin composition]
[0227] (1) Determination of aspect ratio of fibrous filler
[0228] The pellets of each resin composition obtained were heated at 600° C. for 4 hours in an electric furnace, and the organic matter was incinerated to obtain a residue. From the residue components, 100 fibrous fillers were randomly selected and observed with a scanning electron microscope (SEM), and the fiber length and fiber diameter were measured respectively, and the aspect ratio of each fibrous filler was obtained, and the average value thereof was calculated, thereby obtaining the average aspect ratio.
[0229] (2) Phosphorus concentration (mass %) determination
[0230] The phosphorus content of the pellets of each resin composition obtained above was measured. The phosphorus content (mass %) was measured using an energy dispersive fluorescent X-ray analyzer (JSX-1000S manufactured by JEOL Ltd.).
[0231] <Evaluation>
[0232] The resin compositions of Examples 1 to 18 and Comparative Examples 1 to 8 obtained above were evaluated for mechanical strength (flexural strength and impact strength), flame retardancy, continuous moldability, and molded product appearance. The results are shown in Tables I and II.
[0233] (Test piece manufacturing conditions)
[0234] The pellets of the resin composition of each example and comparative example were dried at 80°C for 4 hours and then formed into a molded product for evaluation by an injection molding machine (J140AD-110H, manufactured by Nippon Steel Works, Ltd.). The cylinder temperature during molding was set to 200°C, and the injection pressure was 1000 kgf / cm 2 , 2nd pressure 500kgf / cm 2 , injection speed 50 mm / sec, and metal mold temperature set to 50°C.
[0235] (1) Determination of flexural strength
[0236] Under the above forming conditions, a strip test piece of 80 mm × 10 mm × 4 mm was formed, and a bending test was performed in accordance with JIS-K7171 to measure the bending strength [MPa] and evaluate it according to the following criteria. It should be noted that if the bending strength is 25 MPa or more, it is judged that the strength of the molded product is not a problem in practical use.
[0237] (Evaluation Criteria)
[0238] ◎:More than 50MPa
[0239] ○: 35MPa or more, less than 50MPa
[0240] △: 25MPa or more, less than 35MPa
[0241] ×: less than 25MPa
[0242] (2) Determination of impact strength
[0243] Under the above molding conditions, a strip test piece (with notch) of 80 mm × 10 mm × 4 mm was prepared in accordance with JIS-K7110, and a Charpy impact test (with notch) was performed. The Charpy impact strength [kJ / m 2 ], and the following criteria were used for evaluation. It should be noted that if the Charpy impact strength is 8 kJ / m 2 As above, it is judged that the toughness of the molded product has no problem in practical use.
[0244] (Evaluation Criteria)
[0245] ◎:20kJ / m 2 above
[0246] ○:15kJ / m 2 Above, less than 20kJ / m 2
[0247] △: 8kJ / m 2 Above, less than 15kJ / m 2
[0248] ×: less than 8 kJ / m 2
[0249] (3) Combustion test (flame retardancy evaluation)
[0250] Under the above molding conditions, a 125 mm × 12.5 mm × 1.6 mm strip test piece was produced, and a combustion test was performed according to UL-94, and the evaluation was performed using the following criteria. It should be noted that if the judgment of the combustion test is V-2 or above, it is judged that there is no problem in practical use.
[0251] (Evaluation Criteria)
[0252] ○: Judged as any of V-0, V-1, and V-2.
[0253] ×: Judged as not satisfying V-2.
[0254] (4) Continuous formability
[0255] (Continuous forming test)
[0256] In the metal mold for making the bending test piece used for the evaluation of the bending strength, a nest-type gate portion is provided at the end in the length direction. The material of the nest is carbon steel S50C for mechanical structure. The gate size is set to 4mm in width × 1.5mm in thickness, and the length of the pad is set to 4mm. In addition, a nest-type vent portion is provided at the end on the opposite side of the gate portion. The material of the nest is carbon steel S50C for mechanical structure. The size of the vent is set to 4mm in width × 0.02mm in thickness, and the length of the pad is set to 1mm. An air guide groove with a thickness of 2mm is provided from the end of the pad toward the outer periphery of the metal mold.
[0257] Under the above molding conditions, a continuous molding test of 5,000 continuous molding bending test pieces was conducted for the resin compositions of each embodiment and comparative example. It should be noted that, for the resin compositions of each embodiment and comparative example, at the beginning of molding, the inserts of the gate and the vent were replaced with new ones, and the same test was conducted again. If the cross-sectional area of the gate increases due to wear, there is a problem that the quality cannot be kept constant due to the change in the filling amount of the molded product, and burrs are easily generated.
[0258] (4-1) Changes in gate cross-sectional area after continuous molding test
[0259] After the continuous molding test, the insert of the gate was removed, and the width and thickness of the gate were measured using an optical microscope. The cross-sectional area ratio of the gate before molding and after molding 5000 pieces (continuous molding test) was obtained.
[0260] Gate cross-sectional area = gate width × gate thickness
[0261] Gate cross-sectional area ratio (AR) = Gate cross-sectional area after 5000 pieces are formed / Gate cross-sectional area before forming begins
[0262] (Evaluation Criteria)
[0263] ○: Gate cross-sectional area ratio (AR) <1.002; (practically preferred level)
[0264] △: 1.002 ≤ Gate cross-sectional area ratio (AR) < 1.01; (not preferred but not a problem in practical use)
[0265] ×: 1.01 ≤ gate cross-sectional area ratio (AR); (level that causes practical problems)
[0266] (4-2) Burr evaluation of vent opening after continuous forming test
[0267] After the continuous molding test, the inserts of the vent portion were removed, and the appearance was observed with the naked eye, and the state of the burrs of the 5000th molded product was observed with an optical microscope.
[0268] (Evaluation Criteria)
[0269] ⊚: No discoloration was observed in the vent portion of the metal mold, and no burr was observed in the vent processed portion of the molded product (a very preferred level in practical use).
[0270] ○: Slight discoloration was observed in the vent portion of the metal mold, and generation of burrs was not observed in the vent processed portion of the molded product (a practically preferred level).
[0271] △: Discoloration was observed at the vent portion of the metal mold, and slight burrs were observed at the vent processed portion of the molded product (not desirable, but a level that does not cause a problem in practical use).
[0272] (5) Appearance of molded product
[0273] In the above-mentioned bending test piece molding, the appearance of the molded product was confirmed by visual observation and evaluated according to the following evaluation criteria.
[0274] (Evaluation Criteria)
[0275] ○: No liquid deposits were observed on the surface of the molded article (a practically preferred level).
[0276] ×: Liquid deposits were observed on the surface of the molded product (a level that is problematic in practical use).
[0277]
[0278]
[0279] As can be seen from Table I and Table II, when the resin composition of the present invention is used, an injection-molded article having excellent mechanical strength, flame retardancy and appearance can be economically produced with stable quality.
Claims
1. A resin composition, which is a resin composition for injection molding containing a polyolefin resin, wherein: Relative to the total amount of the resin composition, the resin composition comprises: 10-60% by mass of at least one selected from aluminum hydroxide, magnesium hydroxide and a phosphorus compound, 0.05 to 5% by mass of a NOR type hindered amine compound, and 1-20% by mass of fibrous filler having an aspect ratio of 10 or more, Furthermore, the phosphorus content is 5% by mass or less based on the total amount of the resin composition.
2. The resin composition according to claim 1, wherein The polyolefin resin is a polypropylene resin.
3. The resin composition according to claim 1 or claim 2, wherein The phosphorus compound includes a phosphate compound.
4. The resin composition according to claim 1 or 2, wherein The mass ratio of the total content of the aluminum hydroxide and the magnesium hydroxide to the content of the phosphorus compound is in the range of 100:0 to 75:
25.
5. The resin composition according to claim 1 or 2, wherein The aspect ratio of the fibrous filler is 50 or more.
6. The resin composition according to claim 1 or 2, wherein The fibrous filler comprises halloysite.
7. A method for producing a resin composition, the method comprising producing the resin composition according to any one of claims 1 to 6, wherein: The manufacturing method has the following features: A first step of melt-kneading the polyolefin resin, the at least one selected from aluminum hydroxide, magnesium hydroxide and a phosphorus compound, and the NOR-type hindered amine compound to obtain a resin mixture; and The second step is to melt-knead the resin mixture and the raw material components of the fibrous filler having an aspect ratio of 10 or more.
Citation Information
Patent Citations
Polyolefin-based flame retardant resin composition and its production
JP1998338774A
flame retardant composition
JP2002507238A
In-mold foam molding of polyolefin-based resin
JP2004263033A
Glass filament-containing flame-retardant resin composition and molded article
JP2011088970A
Flame-retardant soft resin composition
JP2015189785A