Composite diaphragm and preparation method, lithium battery
By using a composite structure of a modified ceramic layer and a conductive layer in the lithium battery separator, the problems of low liquid absorption rate and easy loss of ceramic powder in the existing lithium battery separator are solved, and the electrochemical performance and safety of the lithium battery are improved. .
Patent Information
- Application Number
- CN202211319017.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-26
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-10-26
AI Technical Summary
Existing lithium battery separators have poor liquid absorption and low conductivity, and the ceramic powder on the surface of the ceramic separator is easy to agglomerate and fall off, resulting in reduced lithium battery performance and increased safety risks.
Using a composite separator, including a base film, a modified ceramic layer and a modified conductive layer, a dense network structure is formed through the esterification reaction of acrylate-polyethylene glycol-carboxylic acid with inorganic fillers and conductive agents to improve dispersion uniformity and Bonding strength, reducing surface free energy, enhancing liquid absorption and retention capabilities, and improving ionic conductivity.
It effectively improves the electrochemical performance and safety of lithium batteries, reduces the problems of lithium dendrite generation and separator powder loss, and improves the safety and performance stability of lithium batteries.
Smart Images

Figure CN115458868B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a composite diaphragm and a preparation method thereof, and a lithium battery. Background Art
[0002] In lithium batteries, the diaphragm is a crucial part, which needs to ensure the free passage of lithium ions to form a circuit, and prevent the positive and negative electrodes from contacting each other, that is, it plays an insulating role to avoid battery short circuit. Although the diaphragm does not participate in the electrochemical reaction of the battery, the physicochemical properties of the diaphragm, such as thickness, pore size and distribution, porosity, closed-cell temperature and puncture strength, greatly affect the internal resistance, capacity, cycle performance and safety performance of the lithium battery.
[0003] At present, most commercial liquid lithium battery separators use polyolefin separators and ceramic separators with polyolefin as the base film. The surface energy and strong hydrophobicity of such polyolefin separators easily lead to their difficulty in being fully wetted in the electrolyte, that is, the liquid absorption rate of the polyolefin separator is poor, which makes its conductivity low, affecting the performance of the lithium battery; while the ceramic separator has a certain degree of improvement in liquid absorption and retention capacity and thermal stability, but the ceramic powder on the surface of the ceramic separator has a large specific surface energy and is prone to agglomeration. Furthermore, if the uniformity of the ceramic powder coating is poor, there will be obvious "powder falling" phenomenon, which will lead to rolling breakage and self-discharge of the lithium battery, and more seriously will cause internal short circuit. Summary of the invention
[0004] The purpose of the present invention is to overcome the deficiencies in the prior art and to provide a composite diaphragm and a preparation method and a lithium battery that can improve the dispersion uniformity and stability while improving the liquid absorption and retention capacity and conductivity of the diaphragm.
[0005] The objective of the present invention is achieved through the following technical solutions:
[0006] A composite diaphragm, comprising:
[0007] Basement membrane;
[0008] At least one modified ceramic layer, wherein the at least one modified ceramic layer is disposed on one side of the base film;
[0009] At least one modified conductive layer, wherein the at least one modified conductive layer is disposed on a side of the modified ceramic layer away from the base film;
[0010] Wherein, the modified ceramic layer comprises monomer A, monomer B and inorganic filler, and the modified conductive layer comprises monomer A, monomer B and conductive agent;
[0011] The monomer A is acrylate-polyethylene glycol-carboxylic acid, and has a molecular weight of 1000 to 20000;
[0012] The structural formula of the monomer B is as follows:
[0013] (Monomer B).
[0014] In one embodiment, the inorganic filler is at least one of boehmite, alumina, halloysite nanotubes, magnesium oxide, silicon dioxide and titanium dioxide.
[0015] In one embodiment, the conductive agent is at least one of single-walled carbon nanotubes, multi-walled carbon nanotubes, conductive carbon fibers, conductive carbon black and conductive graphite.
[0016] In one embodiment, the modified ceramic layer comprises the following components in parts by weight:
[0017] Monomer A 10 to 50 parts;
[0018] Monomer B 40 to 90 parts;
[0019] 1 to 10 parts of inorganic filler.
[0020] In one embodiment, the modified conductive layer comprises the following components in parts by weight:
[0021] Monomer A 10 to 50 parts;
[0022] Monomer B 45-90 parts;
[0023] Conductive agent 5 to 8 parts.
[0024] In one embodiment, the base film is a polyethylene film, a polypropylene film, a polypropylene / polyethylene / polypropylene film, a polyvinylidene fluoride film or a polyvinylidene fluoride-hexafluoropropylene film.
[0025] In one embodiment, the base film has a thickness of 7 μm to 20 μm.
[0026] In one embodiment, the thickness of the modified ceramic layer is 1 μm to 5 μm.
[0027] In one embodiment, the thickness of the modified conductive layer is 1 μm to 5 μm.
[0028] In one embodiment, the peripheral width of the modified ceramic layer minus the peripheral width of the modified conductive layer is greater than or equal to 1 mm.
[0029] In one embodiment, the modified ceramic layer is centrally disposed on the base film.
[0030] In one embodiment, the modified conductive layer is centrally disposed on the modified ceramic layer.
[0031] A method for preparing a composite diaphragm, used to prepare the composite diaphragm described in any of the above embodiments, the method for preparing the composite diaphragm comprising the following steps:
[0032] Obtaining a base film, a monomer A, a monomer B, an inorganic filler and a conductive agent;
[0033] Adding the monomer A, the monomer B and the inorganic filler into a first solvent to perform a first mixing operation to obtain a modified ceramic layer slurry;
[0034] Adding the monomer A, the monomer B and the conductive agent into a second solvent for a second mixing operation to obtain a modified conductive layer slurry;
[0035] Using the modified ceramic layer slurry to perform a first forming treatment on the base film, so that a modified ceramic layer is formed on the side of the base film;
[0036] The modified conductive layer slurry is used to perform a second forming process on the base film after the coating process, so that a modified conductive layer is formed on a side of the modified ceramic layer away from the base film.
[0037] In one embodiment, the step of adding the monomer A, the monomer B and the inorganic filler into a first solvent for a first mixing operation specifically includes the following steps:
[0038] placing the inorganic filler in the first solvent and performing a stirring and dispersing treatment;
[0039] Adding the monomer A to the first solvent after the stirring and dispersion treatment and performing a heating and stirring treatment;
[0040] The monomer B and azobisisobutyronitrile initiator are added to the first solvent after the heating and stirring treatment to carry out a cooling reaction treatment.
[0041] A lithium battery comprises an aluminum-plastic film, a positive electrode sheet, a negative electrode sheet and the composite separator described in any of the above embodiments, wherein the positive electrode sheet, the separator and the negative electrode sheet are sequentially stacked or stacked and wound to form an inner core, the inner core is arranged in the aluminum-plastic film, the aluminum-plastic film is filled with an electrolyte, and the inner core is used to be immersed in the electrolyte when arranged in the aluminum-plastic film.
[0042] Compared with the prior art, the present invention has at least the following advantages:
[0043] The composite diaphragm of the present invention utilizes the fact that the inorganic filler and the conductive agent have a large number of hydroxyl active groups on their surfaces, and cooperates with acrylate-polyethylene glycol-carboxylic acid to produce an esterification reaction, thereby obtaining a modified inorganic filler and a modified conductive agent containing double bonds, and the acrylate-polyethylene glycol-carboxylic acid itself, the acrylate-polyethylene glycol-carboxylic acid and the generated modified inorganic filler and modified conductive agent, and the modified inorganic filler and the modified conductive agent themselves or the modified inorganic filler and the modified conductive agent can undergo free radical polymerization under the action of an initiator, and a dense network structure can be formed well, thereby realizing that the inorganic filler or the conductive agent can be stably filled and attached to the network structure, and the dispersibility of the inorganic filler and the conductive agent can be effectively improved, that is, the agglomeration of the ceramic is effectively reduced, and the base The molecular forces between the materials of the membrane, the modified ceramic layer and the modified conductive layer effectively improve the bonding strength of the base membrane, the modified ceramic layer and the modified conductive layer, thereby effectively alleviating the problem of powder falling of the diaphragm; in addition, the introduction of lithium benzenesulfonamide groups into monomer B effectively reduces the surface free energy of the diaphragm, thereby effectively enhancing the wetting ability of the diaphragm in the electrolyte, improving the liquid absorption and retention capacity of the diaphragm, and further cooperating with the use of conductive agents, effectively improving the ionic conductivity of the diaphragm, thereby improving the electrochemical performance of the lithium battery, especially under ultra-high current density, which can obviously prevent local lithium precipitation, thereby reducing the formation of lithium dendrites, thereby reducing the easy piercing of lithium dendrites through the diaphragm, and effectively improving the safety of lithium battery use. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0045] Figure 1 The present invention is a flow chart of a method for preparing a composite membrane according to an embodiment of the present invention. DETAILED DESCRIPTION
[0046] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.
[0047] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only and do not represent the only implementation method.
[0048] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0049] The present application also provides a composite diaphragm. The above-mentioned composite diaphragm includes a base membrane, at least one modified ceramic layer and at least one modified conductive layer. At least one modified ceramic layer is arranged on one side of the base membrane. At least one modified conductive layer, at least one modified conductive layer is arranged on the side of the modified ceramic layer away from the base membrane. Among them, the modified ceramic layer includes monomer A, monomer B and inorganic filler, and the modified conductive layer includes monomer A, monomer B and a conductive agent. Monomer A is acrylate-polyethylene glycol-carboxylic acid with a molecular weight of 1000 to 20000; the structural formula of monomer B is as follows:
[0050] (Monomer B).
[0051] The above-mentioned composite diaphragm utilizes the fact that the inorganic filler and the conductive agent have a large number of hydroxyl active groups on their surfaces, and cooperates with acrylate-polyethylene glycol-carboxylic acid to undergo an esterification reaction to obtain a modified inorganic filler and a modified conductive agent containing double bonds, and acrylate-polyethylene glycol-carboxylic acid itself, acrylate-polyethylene glycol-carboxylic acid and the generated modified inorganic filler and modified conductive agent, and the modified inorganic filler and the modified conductive agent themselves or the modified inorganic filler and the modified conductive agent can undergo free radical polymerization under the action of an initiator, and a dense network structure can be formed well, thereby achieving that the inorganic filler or the conductive agent can be stably filled and attached to the network structure, which can effectively improve the dispersibility of the inorganic filler and the conductive agent, that is, effectively reduce the agglomeration of the ceramic, and the base The molecular forces between the materials of the membrane, the modified ceramic layer and the modified conductive layer effectively improve the bonding strength of the base membrane, the modified ceramic layer and the modified conductive layer, thereby effectively alleviating the problem of powder falling of the diaphragm; in addition, the introduction of lithium benzenesulfonamide groups into monomer B effectively reduces the surface free energy of the diaphragm, thereby effectively enhancing the wetting ability of the diaphragm in the electrolyte, improving the liquid absorption and retention capacity of the diaphragm, and further cooperating with the use of conductive agents, effectively improving the ionic conductivity of the diaphragm, thereby improving the electrochemical performance of the lithium battery, especially under ultra-high current density, which can obviously prevent local lithium precipitation, thereby reducing the formation of lithium dendrites, thereby reducing the easy piercing of lithium dendrites through the diaphragm, and effectively improving the safety of lithium battery use.
[0052] In order to better understand the composite diaphragm of the present application, the composite diaphragm of the present application is further explained below:
[0053] A composite diaphragm of one embodiment includes a base film, at least one modified ceramic layer and at least one modified conductive layer. At least one modified ceramic layer is arranged on one side of the base film. At least one modified conductive layer, at least one modified conductive layer is arranged on the side of the modified ceramic layer away from the base film. Among them, the modified ceramic layer includes monomer A, monomer B and inorganic filler, and the modified conductive layer includes monomer A, monomer B and conductive agent. Monomer A is acrylate-polyethylene glycol-carboxylic acid with a molecular weight of 1000 to 20000; the structural formula of monomer B is as follows:
[0054] (Monomer B).
[0055] The above-mentioned composite diaphragm utilizes the fact that the inorganic filler and the conductive agent have a large number of hydroxyl active groups on their surfaces, and cooperates with acrylate-polyethylene glycol-carboxylic acid to undergo an esterification reaction to obtain a modified inorganic filler and a modified conductive agent containing double bonds, and acrylate-polyethylene glycol-carboxylic acid itself, acrylate-polyethylene glycol-carboxylic acid and the generated modified inorganic filler and modified conductive agent, and the modified inorganic filler and the modified conductive agent themselves or the modified inorganic filler and the modified conductive agent can undergo free radical polymerization under the action of an initiator, and a dense network structure can be formed well, thereby achieving that the inorganic filler or the conductive agent can be stably filled and attached to the network structure, which can effectively improve the dispersibility of the inorganic filler and the conductive agent, that is, effectively reduce the agglomeration of the ceramic, and the base The molecular forces between the materials of the membrane, the modified ceramic layer and the modified conductive layer effectively improve the bonding strength of the base membrane, the modified ceramic layer and the modified conductive layer, thereby effectively alleviating the problem of powder falling of the diaphragm; in addition, the introduction of lithium benzenesulfonamide groups into monomer B effectively reduces the surface free energy of the diaphragm, thereby effectively enhancing the wetting ability of the diaphragm in the electrolyte, improving the liquid absorption and retention capacity of the diaphragm, and further cooperating with the use of conductive agents, effectively improving the ionic conductivity of the diaphragm, thereby improving the electrochemical performance of the lithium battery, especially under ultra-high current density, which can obviously prevent local lithium precipitation, thereby reducing the formation of lithium dendrites, thereby reducing the easy piercing of lithium dendrites through the diaphragm, and effectively improving the safety of lithium battery use.
[0056] It should be noted that monomer A is an existing substance, and the synthesis method please refer to the general conventional method; the synthesis method of monomer B please refer to Chen Shaoshan; Li Yu; Wang Yong; Li Zeyu; Peng Cong; Feng Yiyu; et al. (2021): Cross-linked single-ion solid polymer electrolyte for lithium metal batteries, with alternatingly distributed lithium source and ion conductive segments.
[0057] In one embodiment, the inorganic filler is at least one of boehmite, alumina, halloysite nanotubes, magnesium oxide, silicon dioxide and titanium dioxide.
[0058] In one embodiment, the conductive agent is at least one of single-walled carbon nanotubes, multi-walled carbon nanotubes, conductive carbon fibers, conductive carbon black, and conductive graphite.
[0059] In one embodiment, the modified ceramic layer includes the following components in parts by weight:
[0060] Monomer A 10 to 50 parts;
[0061] Monomer B 40 to 90 parts;
[0062] 1 to 10 parts of inorganic filler.
[0063] In one embodiment, the modified conductive layer includes the following components in parts by weight:
[0064] Monomer A 10 to 50 parts;
[0065] Monomer B 45-90 parts;
[0066] Conductive agent 5 to 8 parts.
[0067] In one embodiment, the base film is a polyethylene film, a polypropylene film, a polypropylene / polyethylene / polypropylene film, a polyvinylidene fluoride film or a polyvinylidene fluoride-hexafluoropropylene film.
[0068] In one embodiment, the thickness of the base film is 7 μm to 20 μm.
[0069] In one embodiment, the thickness of the base film is 10 μm to 15 μm.
[0070] In one embodiment, the thickness of the base film is 12 μm.
[0071] In one embodiment, the thickness of the modified ceramic layer is 1 μm to 5 μm.
[0072] In one embodiment, the thickness of the modified ceramic layer is 3 μm.
[0073] In one embodiment, the thickness of the modified conductive layer is 1 μm to 5 μm.
[0074] In one embodiment, the thickness of the modified conductive layer is 2 μm.
[0075] In one of the embodiments, the peripheral width of the modified ceramic layer minus the peripheral width of the modified conductive layer is greater than or equal to 1 mm, which better ensures the insulation performance of the diaphragm.
[0076] In one embodiment, the modified ceramic layer is centrally disposed on the base film.
[0077] In one embodiment, the modified conductive layer is centrally disposed on the modified ceramic layer.
[0078] The present application also provides a method for preparing a composite diaphragm, which is used to prepare the composite diaphragm of any of the above embodiments. The above-mentioned method for preparing a composite diaphragm includes the following steps: obtaining a base film, a monomer A, a monomer B, an inorganic filler and a conductive agent; adding the monomer A, the monomer B and the inorganic filler to a first solvent for a first mixing operation to obtain a modified ceramic layer slurry; adding the monomer A, the monomer B and the conductive agent to a second solvent for a second mixing operation to obtain a modified conductive layer slurry; using the modified ceramic layer slurry to perform a first forming treatment on the base film so that a modified ceramic layer is formed on the side of the base film; using the modified conductive layer slurry to perform a second forming treatment on the coated base film so that a modified conductive layer is formed on the side of the modified ceramic layer away from the base film.
[0079] The above-mentioned preparation method of the composite diaphragm allows monomer A, monomer B and inorganic filler to be added to a first solvent for a first mixing operation, and allows monomer A, monomer B and conductive agent to be added to a second solvent for a second mixing operation, thereby respectively achieving better dispersion uniformity and stability of the inorganic filler and the conductive agent. Furthermore, the modified ceramic layer slurry is used to perform a first forming treatment on the base film, so that the modified conductive layer slurry is formed on the modified ceramic layer in the form of a slurry, which is beneficial to the mutual penetration of the modified ceramic layer and the modified conductive layer, and is beneficial to promoting the molecular force between the modified ceramic layer and the modified conductive layer. Furthermore, the modified conductive layer slurry is used to perform a second forming treatment on the coated base film, so that the modified conductive layer slurry is formed on the modified ceramic layer in the form of a slurry, which is beneficial to the mutual penetration of the modified ceramic layer and the modified conductive layer, and is beneficial to promoting the molecular force between the modified ceramic layer and the modified conductive layer, thereby better achieving the bonding strength of the diaphragm, thereby effectively alleviating the problem of diaphragm powder falling.
[0080] In order to better understand the composite membrane of the present application, the composite membrane of the present application is further explained below. A method for preparing the composite membrane of one embodiment includes the following steps:
[0081] S100, obtaining a base film, monomer A, monomer B, inorganic filler and conductive agent. It can be understood that the combination of monomer A and monomer B can better achieve the dispersion uniformity and dispersion stability of the inorganic filler and the conductive agent, and can better achieve the bonding strength between the base film, the modified ceramic layer and the modified conductive layer, thereby obtaining the base film, monomer A, monomer B, inorganic filler and conductive agent to prepare the diaphragm.
[0082] S200, adding monomer A, monomer B and inorganic filler into a first solvent for a first mixing operation to obtain a modified ceramic layer slurry. It can be understood that during the mixing process, monomer A will gradually react with the inorganic filler to generate a modified inorganic filler, and further, monomer A and monomer B further undergo a free radical reaction to form a denser network structure, which effectively improves the dispersion uniformity of the inorganic filler.
[0083] S300, adding monomer A, monomer B and a conductive agent to a second solvent for a second mixing operation to obtain a modified conductive layer slurry. It can be understood that during the mixing process, monomer A will gradually react with the conductive agent to generate a modified conductive agent, and further, monomer A and monomer B further undergo a free radical reaction to form a denser network structure, which effectively improves the dispersion uniformity of the conductive agent.
[0084] S400, using the modified ceramic layer slurry to perform a first forming treatment on the base film, so that a modified ceramic layer is formed on the side of the base film. It can be understood that the first forming treatment of the base film using the modified ceramic layer slurry allows the modified ceramic layer slurry to be formed on the base film in the form of slurry, which is conducive to promoting the molecular force between the modified ceramic layer and the base film, thereby better achieving the bonding strength of the modified ceramic layer on the base film, thereby effectively reducing the problem of powder falling of the diaphragm.
[0085] S500, using a modified conductive layer slurry to perform a second forming treatment on the coated base film, so that a modified conductive layer is formed on the side of the modified ceramic layer away from the base film. It can be understood that the second forming treatment of the coated base film using a modified conductive layer slurry allows the modified conductive layer slurry to be formed on the modified ceramic layer in the form of a slurry, which is beneficial to the mutual penetration of the modified ceramic layer and the modified conductive layer, and is beneficial to promoting the molecular force between the modified ceramic layer and the modified conductive layer, thereby better achieving the bonding strength of the modified conductive layer on the modified ceramic layer, thereby effectively reducing the problem of diaphragm powder falling.
[0086] The above-mentioned preparation method of the composite diaphragm allows monomer A, monomer B and inorganic filler to be added to a first solvent for a first mixing operation, and allows monomer A, monomer B and conductive agent to be added to a second solvent for a second mixing operation, thereby respectively achieving better dispersion uniformity and stability of the inorganic filler and the conductive agent. Furthermore, the modified ceramic layer slurry is used to perform a first forming treatment on the base film, so that the modified conductive layer slurry is formed on the modified ceramic layer in the form of a slurry, which is beneficial to the mutual penetration of the modified ceramic layer and the modified conductive layer, and is beneficial to promoting the molecular force between the modified ceramic layer and the modified conductive layer. Furthermore, the modified conductive layer slurry is used to perform a second forming treatment on the coated base film, so that the modified conductive layer slurry is formed on the modified ceramic layer in the form of a slurry, which is beneficial to the mutual penetration of the modified ceramic layer and the modified conductive layer, and is beneficial to promoting the molecular force between the modified ceramic layer and the modified conductive layer, thereby better achieving the bonding strength of the diaphragm, thereby effectively alleviating the problem of diaphragm powder falling.
[0087] In one embodiment, both the first solvent and the second solvent are organic solvents.
[0088] In one embodiment, the first solvent and the second solvent are independently selected from alcohol solvents and / or ether solvents.
[0089] In one embodiment, the first solvent and the second solvent are independently selected from at least one of ethanol, ether, styrene, perchloroethylene, trichloroethylene, ethylene glycol ether and triethanolamine.
[0090] In one embodiment, the solid content of the modified ceramic layer slurry is 35% to 40%.
[0091] In one embodiment, the solid content of the modified conductive layer slurry is 35% to 50%.
[0092] In one embodiment, monomer A, monomer B and an inorganic filler are added to a first solvent to perform a first mixing operation, which specifically includes the following steps:
[0093] placing the inorganic filler in a first solvent and performing a stirring and dispersing treatment;
[0094] Adding monomer A to the first solvent after the stirring and dispersion treatment and performing a heating and stirring treatment;
[0095] The monomer B and azobisisobutyronitrile initiator are added to the first solvent after the heating and stirring treatment to carry out the cooling reaction treatment.
[0096] In one embodiment, monomer A, monomer B and a conductive agent are added to a second solvent to perform a second mixing operation, which specifically includes the following steps:
[0097] placing the conductive agent in a second solvent and performing a stirring and dispersion treatment;
[0098] Adding monomer A to the second solvent after the stirring and dispersion treatment and performing a heating and stirring treatment;
[0099] The monomer B and azobisisobutyronitrile initiator are added to the second solvent after the heating and stirring treatment to carry out the cooling reaction treatment.
[0100] In one embodiment, the stirring speeds of the stirring dispersion process and the heating stirring process are both 300 r / min to 500 r / min.
[0101] In one embodiment, the temperature of the heating and stirring treatment is 90° C. to 150° C., and the stirring time is 2 h to 5 h.
[0102] In one embodiment, the temperature of the cooling reaction treatment is 40°C to 70°C, and the reaction time is 2h to 5h.
[0103] In one embodiment, the modified ceramic layer slurry is used to perform a first forming treatment on the base film, specifically, the base film is soaked in the modified ceramic layer slurry, and then dried until the moisture content is reduced by 50% to 60%.
[0104] In one embodiment, the base film is soaked in the modified ceramic layer slurry for 30 minutes to 120 minutes.
[0105] In one embodiment, the drying is performed until the moisture content is reduced by 50% to 60% at a drying temperature of 65° C. to 80° C.
[0106] The present application also provides a lithium battery. The above-mentioned lithium battery includes an aluminum-plastic film, a positive electrode sheet, a negative electrode sheet and a composite diaphragm of any of the above-mentioned embodiments. The positive electrode sheet, the diaphragm and the negative electrode sheet are stacked or stacked and wound in sequence to form an inner core. The inner core is arranged in the aluminum-plastic film, and the aluminum-plastic film is filled with an electrolyte. The inner core is used to be immersed in the electrolyte when it is arranged in the aluminum-plastic film. In this embodiment, the composite diaphragm includes a base film, at least one modified ceramic layer and at least one modified conductive layer. At least one modified ceramic layer is arranged on one side of the base film. At least one modified conductive layer, at least one modified conductive layer is arranged on the side of the modified ceramic layer away from the base film. Among them, the modified ceramic layer includes monomer A, monomer B and an inorganic filler, and the modified conductive layer includes monomer A, monomer B and a conductive agent. Monomer A is acrylate-polyethylene glycol-carboxylic acid with a molecular weight of 1000 to 20000; the structural formula of monomer B is as follows:
[0107] (Monomer B).
[0108] The above-mentioned lithium battery adopts a composite diaphragm. Since the composite diaphragm has good liquid separation and liquid retention capabilities, and since the composite diaphragm has good conductivity, the electrochemical performance of the lithium battery is better ensured; and the dispersibility and stability of the inorganic filler and the conductive agent in the composite diaphragm are good, thereby better ensuring the electrochemical performance and safety of the lithium battery.
[0109] In one embodiment, the active material of the positive electrode sheet is at least one of lithium nickel cobalt manganese oxide, lithium iron phosphate, lithium iron manganese phosphate and lithium manganese oxide.
[0110] In one embodiment, the active material of the negative electrode sheet is at least one of lithium metal, silicon-based negative electrode, graphite, hard carbon and soft carbon.
[0111] Compared with the prior art, the present invention has at least the following advantages:
[0112] The composite diaphragm of the present invention utilizes the fact that the inorganic filler and the conductive agent have a large number of hydroxyl active groups on their surfaces, and cooperates with acrylate-polyethylene glycol-carboxylic acid to produce an esterification reaction, thereby obtaining a modified inorganic filler and a modified conductive agent containing double bonds, and the acrylate-polyethylene glycol-carboxylic acid itself, the acrylate-polyethylene glycol-carboxylic acid and the generated modified inorganic filler and modified conductive agent, and the modified inorganic filler and the modified conductive agent themselves or the modified inorganic filler and the modified conductive agent can undergo free radical polymerization under the action of an initiator, and a dense network structure can be formed well, thereby realizing that the inorganic filler or the conductive agent can be stably filled and attached to the network structure, and the dispersibility of the inorganic filler and the conductive agent can be effectively improved, that is, the agglomeration of the ceramic is effectively reduced, and the base The molecular forces between the materials of the membrane, the modified ceramic layer and the modified conductive layer effectively improve the bonding strength of the base membrane, the modified ceramic layer and the modified conductive layer, thereby effectively alleviating the problem of powder falling of the diaphragm; in addition, the introduction of lithium benzenesulfonamide groups into monomer B effectively reduces the surface free energy of the diaphragm, thereby effectively enhancing the wetting ability of the diaphragm in the electrolyte, improving the liquid absorption and retention capacity of the diaphragm, and further cooperating with the use of conductive agents, effectively improving the ionic conductivity of the diaphragm, thereby improving the electrochemical performance of the lithium battery, especially under ultra-high current density, which can obviously prevent local lithium precipitation, thereby reducing the formation of lithium dendrites, thereby reducing the easy piercing of lithium dendrites through the diaphragm, and effectively improving the safety of lithium battery use.
[0113] Some specific examples are listed below, and if % is mentioned, it means percentage by weight. It should be noted that the following examples do not exhaust all possible situations, and the materials used in the following examples can be obtained from commercial sources unless otherwise specified.
[0114] Example 1
[0115] 1 kg of a mixture of boehmite and alumina (the mass ratio of boehmite to alumina is 2:5) was added to ethanol, stirred and dispersed evenly, the stirring speed was 300 r / min, 10 kg of monomer A (molecular weight was 1000) was added, the temperature was raised to 90° C., stirred for 5 h, the temperature was lowered to 40° C., and then 40 kg of monomer B and 1 kg of azobisisobutyronitrile initiator were added, and the reaction was carried out for 5 h to obtain a modified ceramic layer slurry with a solid content of 35%;
[0116] Add 5 kg of conductive agent to ethanol, stir and disperse evenly, add 10 kg of monomer A (molecular weight 1000), heat to 90 ° C, stir for 5 hours, the stirring speed is 300 r / min, the temperature is reduced to 40 ° C, then add 45 kg of monomer B and 1 kg of azobisisobutyronitrile initiator, react for 5 hours, and obtain a modified conductive layer slurry with a solid content of 35%;
[0117] A polypropylene film with a thickness of 7 μm was immersed in the modified ceramic layer slurry for 30 minutes, dried in a 65°C oven to a semi-dry state, and then the modified conductive layer slurry was coated on the semi-dry modified ceramic layer slurry and continued to be dried to obtain a composite diaphragm. The thickness of the modified ceramic layer was 1 μm and the thickness of the modified conductive layer was 1 μm.
[0118] Example 2
[0119] 3 kg of a mixture of halloysite nanotubes and magnesium oxide (the mass ratio of halloysite nanotubes to magnesium oxide is 3:5) was added to styrene, and the mixture was stirred and dispersed evenly at a stirring speed of 350 r / min. 20 kg of monomer A (molecular weight 8000) was added, and the mixture was heated to 100° C. and stirred for 3 h. The temperature was lowered to 50° C. and the stirring speed was 350 r / min. Then 60 kg of monomer B and 1 kg of azobisisobutyronitrile initiator were added, and the mixture was reacted for 3 h to obtain a modified ceramic layer slurry with a solid content of 38%;
[0120] Add 6 kg of conductive agent to styrene, stir and disperse evenly, add 20 kg of monomer A (molecular weight 8000), heat to 120 ° C, stir for 3 hours, the stirring speed is 350 r / min, the temperature is reduced to 50 ° C, and then add 60 kg of monomer B and 1 kg of azobisisobutyronitrile initiator, react for 3 hours to obtain a modified conductive layer slurry with a solid content of 40%;
[0121] A polypropylene film with a thickness of 10 μm was immersed in the modified ceramic layer slurry for 50 minutes, dried in an oven at 70°C to a moisture content of 55%±1, and then the modified conductive layer slurry was coated on the semi-dry modified ceramic layer slurry and continued to be dried to obtain a composite diaphragm. The thickness of the modified ceramic layer was 2 μm and the thickness of the modified conductive layer was 3 μm.
[0122] Example 3
[0123] 7 kg of a mixture of boehmite and silica (the mass ratio of boehmite to silica is 2:7) was added to ethylene glycol ether, and the mixture was stirred and dispersed uniformly at a stirring speed of 400 r / min. 40 kg of monomer A (molecular weight of 15,000) was added, and the mixture was heated to 130° C. and stirred for 3 h. The temperature was lowered to 60° C., and then 70 g of monomer B and 1 kg of azobisisobutyronitrile initiator were added and reacted for 3 h to obtain a modified ceramic layer slurry with a solid content of 38%;
[0124] 7 kg of conductive agent was added to ethylene glycol ether, stirred and dispersed evenly, 40 kg of monomer A (molecular weight 15000) was added, the temperature was raised to 130°C, stirred for 3 hours, the stirring speed was 400 r / min, the temperature was lowered to 60°C, and then 80 kg of monomer B and 1 kg of azobisisobutyronitrile initiator were added, reacted for 3 hours, and a modified conductive layer slurry was obtained with a solid content of 38%;
[0125] A polypropylene film with a thickness of 16 μm was immersed in the modified ceramic layer slurry for 100 minutes, dried in a 70°C oven to a semi-dry state, and then the modified conductive layer slurry was coated on the 58%±1 modified ceramic layer slurry and continued to be dried to obtain a composite diaphragm. The thickness of the modified ceramic layer was 3 μm and the thickness of the modified conductive layer was 2 μm.
[0126] Example 4
[0127] 10 kg of a mixture of halloysite nanotubes and titanium dioxide (the mass ratio of halloysite nanotubes to titanium dioxide is 5:4) is added to styrene, stirred and dispersed evenly, the stirring speed is 500 r / min, 50 kg of monomer A (molecular weight is 20000) is added, the temperature is raised to 150° C., stirred for 2 h, the temperature is lowered to 70° C., and then 90 kg of monomer B and 1 kg of azobisisobutyronitrile initiator are added, reacted for 2 h, and a modified ceramic layer slurry is obtained with a solid content of 40%;
[0128] 8 kg of conductive agent was added to styrene, stirred and dispersed evenly, 50 kg of monomer A (molecular weight 20,000) was added, the temperature was raised to 150°C, stirred for 2 hours, the stirring speed was 500 r / min, the temperature was lowered to 70°C, and then 90 kg of monomer B and 1 kg of azobisisobutyronitrile initiator were added, reacted for 5 hours, and a modified conductive layer slurry was obtained with a solid content of 50%;
[0129] A polypropylene film with a thickness of 20 μm was immersed in the modified ceramic layer slurry for 120 minutes, dried in an 80°C oven to a semi-dry state, and then the modified conductive layer slurry was coated on the semi-dry modified ceramic layer slurry and continued to be dried to obtain a composite diaphragm. The thickness of the modified ceramic layer was 5 μm and the thickness of the modified conductive layer was 5 μm.
[0130] The following tests were conducted on the composite membranes obtained in Examples 1-4.
[0131] 1. The ionic conductivity of the composite membranes of Examples 1 to 4 was measured by blocking the electrodes and measuring the AC impedance. Specifically, the ionic conductivity of Example 1 was 1.04×10 -3 , 1.01×10 -3 ,9.87×10 -2 and 9.97×10 -2 .
[0132] 2. The peeling strength of the adhesion layer on the surface of the base film of the composite diaphragm of Examples 1 to 4 was tested by a LLOYD material mechanical testing machine. The test results are shown in Table 1:
[0133] Example 1 Example 2 Example 3 Example 4 Peel strength (N / cm) 8.2 9.0 8.9 9.2
[0134] Table 1: Peeling strength of the adhesion layer on the surface of the base film of the composite diaphragm of Examples 1 to 4 3. The particle size distribution of the modified ceramic layer slurry of Examples 1 to 4 was detected. The test results are shown in Table 2:
[0135] Example 1 Example 2 Example 3 Example 4 Particle size less than 10 microns (%) 40 38 35 32 Particle size less than 30μm (%) 85 89 93 90 Particle size less than 50μm (%) 98.6 98.3 99.1 98.9
[0136] Table 2: Particle size distribution of modified ceramic layer slurry of Examples 1 to 4
[0137] 4. Taking lithium cobalt oxide batteries as an example, the composite diaphragm of each embodiment is used to prepare 200 lithium cobalt oxide batteries, and the short-circuit rate of the lithium cobalt oxide batteries of each embodiment is tested. Among them, the short-circuit rate of the battery cell of Example 1 is 0.1%, the short-circuit rate of the battery cell of Example 2 is 0.11%, the short-circuit rate of the battery cell of Example 3 is 0.08%, and the short-circuit rate of the battery cell of Example 3 is 0.08%.
[0138] 5. The composite diaphragms of Examples 1 to 4 were respectively applied to lithium cobalt oxide batteries to obtain corresponding lithium batteries, and the obtained lithium batteries were subjected to rate charge and discharge cycle tests. At a rate of 8c, the discharge retention rates of the lithium batteries corresponding to Examples 1 to 4 were all greater than 75%.
[0139] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A composite diaphragm, characterized in that: include: Basement membrane; At least one modified ceramic layer, wherein the at least one modified ceramic layer is disposed on one side of the base film; At least one modified conductive layer, wherein the at least one modified conductive layer is disposed on a side of the modified ceramic layer away from the base film; Wherein, the modified ceramic layer comprises monomer A, monomer B and inorganic filler, and the modified conductive layer comprises monomer A, monomer B and conductive agent; The monomer A is acrylate-polyethylene glycol-carboxylic acid, and has a molecular weight of 1000 to 20000; The structural formula of the monomer B is as follows: The preparation method of the composite diaphragm comprises the following steps: Obtaining a base film, a monomer A, a monomer B, an inorganic filler and a conductive agent; Adding the monomer A, the monomer B and the inorganic filler into a first solvent to perform a first mixing operation to obtain a modified ceramic layer slurry; Adding the monomer A, the monomer B and the conductive agent into a second solvent for a second mixing operation to obtain a modified conductive layer slurry; Using the modified ceramic layer slurry to perform a first forming treatment on the base film, so that a modified ceramic layer is formed on the side of the base film; The modified conductive layer slurry is used to perform a second forming process on the base film after the coating process, so that a modified conductive layer is formed on a side of the modified ceramic layer away from the base film.
2. The composite diaphragm according to claim 1, characterized in that: The inorganic filler is at least one of boehmite, alumina, halloysite nanotubes, magnesium oxide, silicon dioxide and titanium dioxide.
3. The composite diaphragm according to claim 1, characterized in that: The conductive agent is at least one of single-walled carbon nanotubes, multi-walled carbon nanotubes, conductive carbon fibers, conductive carbon black and conductive graphite.
4. The composite diaphragm according to claim 1, characterized in that: The modified ceramic layer comprises the following components in parts by mass: 10 to 50 parts of monomer A; Monomer B 40 to 90 parts; 1 to 10 parts of inorganic filler.
5. The composite diaphragm according to claim 1, characterized in that: The modified conductive layer comprises the following components in parts by mass: 10 to 50 parts of monomer A; Monomer B 45-90 parts; Conductive agent 5 to 8 parts.
6. The composite diaphragm according to claim 1, characterized in that: The base film is a polyethylene film, a polypropylene film, a polypropylene / polyethylene / polypropylene film, a polyvinylidene fluoride film or a polyvinylidene fluoride-hexafluoropropylene film.
7. The composite diaphragm according to claim 1, characterized in that: The thickness of the base film is 7 μm to 20 μm; and / or, The thickness of the modified ceramic layer is 1 μm to 5 μm; and / or, The thickness of the modified conductive layer is 1 μm to 5 μm; and / or, The peripheral width of the modified ceramic layer minus the peripheral width of the modified conductive layer is greater than or equal to 1 mm; and / or, The modified ceramic layer is centrally disposed on the base film; and / or, The modified conductive layers are all centrally arranged on the modified ceramic layer.
8. The composite diaphragm according to claim 1, characterized in that: The step of adding the monomer A, the monomer B and the inorganic filler into the first solvent for a first mixing operation specifically includes the following steps: placing the inorganic filler in the first solvent and performing a stirring and dispersing treatment; Adding the monomer A to the first solvent after the stirring and dispersion treatment and performing a heating and stirring treatment; The monomer B and azobisisobutyronitrile initiator are added to the first solvent after the heating and stirring treatment to carry out a cooling reaction treatment.
9. A lithium battery, characterized in that: The invention comprises an aluminum-plastic film, a positive electrode sheet, a negative electrode sheet and a composite separator according to any one of claims 1 to 8, wherein the positive electrode sheet, the separator and the negative electrode sheet are sequentially stacked or stacked and wound to form an inner core, the inner core is arranged in the aluminum-plastic film, the aluminum-plastic film is filled with an electrolyte, and the inner core is used to be immersed in the electrolyte when arranged in the aluminum-plastic film.