A multi-active component brazing material and a method for in-situ generation of high entropy ceramic phase joints

By designing the interfacial reaction between multi-active component solder and SiC ceramics, a high-entropy carbide ceramic phase is generated in situ, which solves the problems of poor oxidation resistance of existing solder at high temperatures and joint brittleness, and achieves high-temperature stability of the joint. and increased strength.

CN115464302BActive Publication Date: 2024-10-29AVIC BEIJING INST OF AERONAUTICAL MATERIALS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211264149.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-14
Publication Date
2024-10-29
Estimated Expiration
2042-10-14

AI Technical Summary

Technical Problem

Existing solder materials have poor oxidation resistance in high-temperature environments and are difficult to match the temperature resistance of SiC ceramic materials. Moreover, the joints are highly brittle and difficult to maintain stability at high temperatures.

Method used

Design a multi-active component brazing material, including active components such as Ti, Zr, Hf, Nb and V, which can generate quaternary or quintuple high-entropy carbide ceramic phases in situ through the interface reaction with SiC ceramics to improve the joint strength. High temperature resistance. The components of the solder are prepared into solder foil or powder by arc melting under the protection of argon gas, which is prepared by a rapid cooling method and subjected to high-temperature brazing in a vacuum furnace.

Benefits of technology

By generating high-entropy carbide ceramic phases in situ, the high-temperature resistance of the joint is significantly improved, ensuring improved stability and strength in high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115464302B_ABST
    Figure CN115464302B_ABST
Patent Text Reader

Abstract

The present invention relates to a multi-active component brazing material, wherein the multi-active component brazing material comprises any four or all active components selected from Ti, Zr, Hf, Nb and V, the mass percentage of each active component in the brazing material is 5% to 35%, and the total mass percentage of the active components in the brazing material is 70% to 90%, and the remainder is Ni and / or Co, and the melting point of the brazing material is regulated to be 1150 to 1280°C. The present invention also relates to a method for in-situ generation of a high-entropy ceramic phase joint using the multi-active component brazing material. The present invention generates a quaternary or quinary high-entropy carbide ceramic phase in-situ inside the joint through the interface reaction between the active elements and SiC ceramics, thereby improving the high temperature resistance of the joint.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of welding, and in particular relates to a multi-active component brazing filler metal and a method for in-situ generating a high-entropy ceramic phase brazing joint by using the multi-active component brazing filler metal. Background Art

[0002] High entropy ceramics (HEC) are a new type of ceramic material that has recently emerged. The concept comes from high entropy alloys (HEA), which are formed by the solid solution of multiple carbide ceramic phases to form a single-phase solid solution. The research on high entropy ceramics can be traced back to 2015, when North Carolina State University and Duke University in the United States reported a rock salt structure entropy-stabilized oxide ceramic, namely high entropy ceramics. Compared with traditional ceramics, high entropy ceramics have a thermodynamic high entropy effect and high configurational entropy, which can stabilize the high entropy solid solution phase and promote the compatibility between elements. Five or more carbide ceramics are the ultimate goal of high entropy ceramic preparation. This type of carbide can significantly improve mechanical properties and other properties due to its solid solution strengthening and high entropy effect, such as high toughness, good thermal stability and good electrical conductivity.

[0003] Transition metal carbide ceramics are carbide ceramic phases formed by transition metal elements of the IV subgroup (Ti, Zr, Hf) and the V subgroup (V, Nb, Ta). The crystal structure of these carbide ceramic phases is NaCl cubic crystal type (belonging to the Fm3m space group), with strong covalent bond characteristics and high melting points, excellent thermal strength and thermal shock resistance. It is precisely because the crystal structure of transition metal carbides is the same and the lattice constants are close that when transforming from single-component carbides to multi-component carbides, the crystal structure remains unchanged and is still NaCl crystal type.

[0004] Compared with single-component carbides, the comprehensive properties of multi-component carbides will be greatly improved. For example, HfC has a high melting point and high hardness, but poor plasticity. On the contrary, TaC has good plasticity. The two can form a solid solution phase in the entire composition range. Reasonable design of the two components (Ta x Hf 1-x )C, can obtain ideal comprehensive properties. Ternary carbide ceramics can also form single-phase solid solutions. Demirskyi prepared single-phase (Ta-Zr-Nb)C carbides by regulating the sintering process. Ye et al. prepared (Zr0.25Nb0.25Ti0.25V0.25)C four-component carbide ceramics, forming single-phase high-entropy carbide ceramics with uniform components from microscale to nanoscale.

[0005] Therefore, by designing a multi-active component brazing filler metal system and forming a multi-component carbide ceramic composite phase (high entropy ceramic phase) through in-situ reaction during the brazing process, it will be beneficial to improve the high-temperature performance of the joint.

[0006] At present, there are many methods for connecting SiC ceramic materials, such as diffusion connection, mechanical connection, brazing, etc. Brazing has the advantages of simple process, high operability, and suitability for mass production. The commonly used AgCuTi system brazing filler metal has good wettability to ceramic materials and high connection strength, which is suitable for brazing of ceramic materials. However, the high-temperature oxidation resistance of AgCuTi brazing filler metal is poor, and it is difficult to use it above 500°C in an aerobic environment, which is obviously not compatible with the temperature resistance of SiC ceramic materials. Xiong et al. designed CoFeNiCrTi brazing filler metal for brazing SiC ceramics (Huaping Xiong, Wetting behavior of Co based active brazing alloys on SiC and the interfacial reactions, Materials letters, 2003, 57: 3417-3421), but the joint contains a large amount of binary silicides such as Co-Si, which leads to joint brittleness. Patent CN202010646283.2 discloses a SiC ceramic brazing method and brazing material based on a multi-element high entropy alloy. A CoFeCrNiCu high entropy alloy brazing filler metal with an equimolar ratio is designed to braze SiC ceramics. The high entropy effect is used to form a solid solution in the joint to improve the joint strength. However, the Cu-based solid solution formed in the joint will limit the high temperature resistance of the joint. Summary of the invention

[0007] In view of the above-mentioned situation of the prior art, the purpose of the present invention is to provide a multi-active component brazing material, and a method for in-situ generating a high-entropy ceramic phase joint using the multi-active component brazing material, through the interfacial reaction between the active elements and SiC ceramics, a quaternary or quinary high-entropy carbide ceramic phase is in-situ generated inside the joint, thereby improving the high temperature resistance of the joint.

[0008] According to one aspect of the present invention, a multi-active component solder is provided, comprising any four or all active components selected from Ti, Zr, Hf, Nb and V, the mass percentage of each active component in the solder being 5% to 35%, and the total mass percentage of the active components in the solder being 70% to 90%, with the remainder being Ni and / or Co, and the melting point of the solder being regulated to be 1150 to 1280°C.

[0009] According to another aspect of the present invention, there is provided a method for in-situ generation of high entropy ceramic phase joints using the above-mentioned multi-active component solder, the method comprising: preparing raw materials according to the composition of the solder; then melting the raw materials into alloy ingots by arc melting under argon protection; preparing the alloy ingots into solder foil or solder powder; then placing the solder foil or solder powder between two ceramic materials to be welded, and after assembly, high-temperature brazing in a vacuum furnace. The preferred brazing specification is 1200-1300°C, and the insulation is 10-120 minutes. In addition, the heating rate is 10°C / min, and the vacuum degree in the furnace is not less than 10 during the insulation process. -3 Pa; After brazing is completed, the cooling rate from the brazing temperature to 500℃ is no more than 5℃ / min, and then it can be furnace cooled to room temperature.

[0010] Further, the alloy ingot is prepared into a solder foil by a rapid cooling method (i.e., using a rapid cooling foil device), and the thickness of the solder foil is 60 to 120 microns. Further, the alloy ingot is prepared into a solder powder by grinding the rapid cooling foil into powder, and then sieving to obtain a powdered solder, and the powder particle size is less than 50 mesh.

[0011] The multi-active component brazing filler metal can also be used for C f / SiC、SiC f / SiC、SiC f High temperature brazing of ceramic matrix composites such as / SiBCN.

[0012] The system of the multi-active component brazing material of the present invention is TiZrHfNbV (Ni, Co), the active components contain four or all of Ti, Zr, Hf, Nb, and V, the mass percentage is 5% to 35%, Ni and Co elements are the remainder, and the melting point of the brazing material is regulated to be 1150 to 1280° C. The brazing temperature of brazing SiC ceramics is controlled within the range of 1200 to 1300° C. Through the interface reaction between the active elements and the SiC ceramics, a quaternary or quinary high entropy carbide ceramic phase is in situ generated inside the joint, thereby improving the high temperature resistance of the joint. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 The SiC brazing process is carried out by using the TiZrHfNbNi brazing filler metal according to Example 1 of the present invention. f SEM photograph of the joint of / SiBCN ceramic composite material (brazing temperature 1260℃, time 60min). DETAILED DESCRIPTION

[0014] In order to more clearly understand the purpose, technical solutions and advantages of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0015] The present invention provides a multi-active component brazing material, and a method for generating a high-entropy ceramic phase brazing joint by in-situ reaction of the multi-active component brazing material. The multi-active component brazing material system is TiZrHfNbV (Ni, Co), the active components contain four or all of Ti, Zr, Hf, Nb, and V, the mass percentage is 5% to 35%, Ni and Co elements are the remainder, and the melting point of the brazing material is regulated to 1150 to 1280°C.

[0016] The preparation method of the multi-active component solder is as follows: raw materials are prepared according to the solder components, and the raw materials are melted into alloy ingots by arc melting method under argon protective atmosphere, and the solder is prepared by one of the following methods:

[0017] (1) A quenched foil strip brazing material is prepared by using a quenched foil material equipment under argon protection conditions. The thickness of the foil strip is 60 to 120 microns. For the single-roll method rapid solidification process, the single roller needs to rotate at a high speed of 5000 to 12000 r / min. After the brazing ingot melts to form a liquid, the cooling rate is between 10 3 ~10 6 Between K / s.

[0018] (2) After the quenched foil solder is prepared according to the above method, the foil is ground into powder by mechanical grinding, and then the powder is sieved by a 50-mesh manual sieve to obtain a powder solder with a particle size less than 50 mesh.

[0019] Place the brazing material between the two ceramic materials to be welded and place them in a vacuum furnace for brazing. The brazing specification is preferably 1200-1300℃ and kept warm for 10-120 minutes. During the insulation process, the vacuum degree in the furnace should not be less than 10 -3 Pa; in addition, the heating rate is preferably 10°C / min. After brazing, the cooling rate from the brazing temperature to 500°C is no more than 5°C / min, and then the furnace can be cooled to room temperature to obtain a ceramic brazed joint.

[0020] Example 1

[0021] The solder composition is Ti-30Zr-5Hf-15Nb-15Ni (wt.%), and high-purity Ti, Zr, Hf, Nb, and Ni with a purity of not less than 99.0% are selected and weighed according to the weight ratio to prepare the raw materials; the alloy is melted into an alloy ingot by an arc melting method under argon protection conditions, and a solder foil strip with a thickness of 80 microns is prepared by a rapid cooling foil material equipment; the foil strip solder is placed between two SiC f / SiBCN ceramic composite materials to form a sandwich structure, after assembly, put it into a vacuum brazing furnace. The brazing temperature is 1260℃ for 60min, and the vacuum degree is not less than 10 -3Pa; the heating rate was 10℃ / min, and the cooling process was first 5℃ / min to 500℃, and then cooled with the furnace to obtain SiC f / SiBCN ceramic self brazing joint, its structure is shown in Figure 1 .

[0022] Example 2

[0023] The solder composition is Ti-28Zr-5Hf-15Nb-5V-15Ni (wt%), and high-purity Ti, Zr, Hf, Nb, V, and Ni with a purity of not less than 99.0% are selected and weighed according to the weight ratio to prepare the raw materials; the alloy is melted into an alloy ingot by an arc melting method under argon protection conditions, and the solder foil strip is thrown out by a rapid cooling foil equipment, and then the foil strip is ground into powder by a mechanical grinding method, and the powder is sieved with a 50-mesh manual sieve to obtain a powder solder with a particle size of less than 50 mesh; the solder powder is placed between two pieces of SiC ceramic materials to form a sandwich structure, and after assembly, it is placed in a vacuum brazing furnace. The brazing temperature is 1280℃ for 100 minutes, and the vacuum degree during the brazing insulation process is not less than 10 -3 Pa; the heating rate was 10°C / min, and the temperature was first cooled to 500°C at 5°C / min, and then cooled with the furnace to obtain the SiC ceramic self-brazed joint.

[0024] Example 3

[0025] The solder composition is Ti-25Zr-5Hf-15Nb-5V-10Ni-10Co (wt%), and high-purity Ti, Zr, Hf, Nb, V, Ni, and Co with a purity of not less than 99.0% are selected and weighed according to weight ratio to prepare raw materials; the alloy is melted into an alloy ingot by an arc melting method under argon protection conditions, a solder foil strip is thrown out by a quenching foil material equipment, and then the foil strip is ground into powder by a mechanical grinding method, and the powder is sieved by a 50-mesh manual screen to obtain a powder solder with a particle size of less than 50 mesh; the solder powder is placed between two SiC f / SiC ceramic composite materials to form a sandwich structure, after assembly, put it into a vacuum brazing furnace. The brazing temperature is 1240℃ for 30min, and the vacuum degree is not less than 10 -3 Pa; the heating rate was 10℃ / min, and the cooling process was first 5℃ / min to 500℃, and then cooled with the furnace to obtain SiC f / SiC ceramic composite self-brazed joint.

[0026] Example 4

[0027] The solder composition is Ti-28Zr-5Hf-15Nb-10V-10Ni-5Co (wt%), and high-purity Ti, Zr, Hf, Nb, V, Ni, and Co with a purity of not less than 99.0% are selected and weighed according to the weight ratio to prepare the raw materials; the alloy is melted into an alloy ingot by an arc melting method under argon protection conditions, and a solder foil with a thickness of 100 microns is thrown out by a rapid cooling foil equipment; the solder foil is placed between two C f / SiC ceramic composite materials to form a sandwich structure, after assembly, put it into a vacuum brazing furnace. The brazing temperature is 1220℃ for 80min, and the vacuum degree is not less than 10 -3 Pa; the heating rate is 10℃ / min, the cooling process is first 5℃ / min to 500℃, and then cooled with the furnace to obtain C f / SiC ceramic composite self-brazed joint.

[0028] Example 5

[0029] The solder composition is Ti-28Zr-15Nb-10V-10Ni-10Co (wt%), and high-purity Ti, Zr, Nb, V, Ni, and Co with a purity of not less than 99.0% are selected and weighed according to the weight ratio to prepare the raw materials; the alloy is melted into an alloy ingot by an arc melting method under argon protection conditions, and a solder foil with a thickness of 60 microns is thrown out by a rapid cooling foil equipment; the solder foil is placed between two C f / SiC ceramic composite materials to form a sandwich structure, after assembly, put it into a vacuum brazing furnace. The brazing temperature is 1200℃ for 30 minutes, and the vacuum degree during the brazing insulation process is not less than 10 -3 Pa; the heating rate is 10℃ / min, the cooling process is first 5℃ / min to 500℃, and then cooled with the furnace to obtain C f / SiC ceramic composite self-brazed joint.

[0030] Example 6

[0031] The solder composition is Ti-28Zr-10Hf-10Nb-5V-10Ni-5Co (wt%), and high-purity Ti, Zr, Hf, Nb, V, Ni, and Co with a purity of not less than 99.0% are selected and weighed according to weight ratio to prepare raw materials; the alloy is melted into an alloy ingot by an arc melting method under argon protection conditions, a solder foil strip is thrown out by a quenching foil equipment, the foil strip is ground into powder by a mechanical grinding method, and the powder is sieved by a 50-mesh manual screen to obtain a powder solder with a particle size of less than 50 mesh; the solder powder is placed between two SiC f / SiC ceramic composite materials to form a sandwich structure, after assembly, put it into a vacuum brazing furnace. The brazing temperature is 1300℃ for 120min, and the vacuum degree is not less than 10 -3 Pa; the heating rate was 10℃ / min, and the cooling process was first 5℃ / min to 500℃, and then cooled with the furnace to obtain SiC f / SiC ceramic composite self-brazed joint.

[0032] Example 7

[0033] The solder composition is Ti-30Zr-5Hf-15Nb-20Ni (wt.%). High-purity Ti, Zr, Hf, Nb, and Ni with a purity of not less than 99.0% are selected and weighed according to the weight ratio to prepare the raw materials; the alloy is melted into an alloy ingot by arc melting under argon protection conditions, and a solder foil strip with a thickness of 80 microns is prepared by a rapid cooling foil equipment; the foil strip solder is placed between two SiC ceramics to form a sandwich structure, and after assembly, it is placed in a vacuum brazing furnace. The brazing temperature is 1260℃ for 60 minutes, and the vacuum degree during the brazing insulation process is not less than 10 -3 Pa; the heating rate was 10°C / min, and the temperature was first cooled to 500°C at 5°C / min, and then cooled with the furnace to obtain the SiC ceramic self-brazed joint.

[0034] Example 8

[0035] The solder composition is Ti-23Zr-10Hf-10Nb-5V-20Ni-5Co (wt%). High-purity Ti, Zr, Hf, Nb, V, Ni, and Co with a purity of not less than 99.0% are selected and weighed according to the weight ratio to prepare the raw materials. The alloy is melted into an alloy ingot by an arc melting method under argon protection conditions. The solder foil strip is thrown out by a rapid cooling foil equipment. The foil strip is ground into powder by a mechanical grinding method. The powder is sieved with a 50-mesh manual screen to obtain a powder solder with a particle size of less than 50 mesh. The solder powder is placed between two pieces of SiC ceramics to form a sandwich structure. After assembly, it is placed in a vacuum brazing furnace. The brazing temperature is 1300°C for 120 minutes, and the vacuum degree during the brazing insulation process is not less than 10 -3 Pa; the heating rate was 10°C / min, and the temperature was first cooled to 500°C at 5°C / min, and then cooled with the furnace to obtain the SiC ceramic self-brazed joint.

Claims

1. A multi-active component solder, comprising active components Ti, Zr, Hf, Nb and V, wherein the mass percentage of each active component in the solder is 5% to 35%, and the total mass percentage of the active components in the solder is 70% to 90%, with the remainder being Ni and Co, and the melting point of the solder is regulated to be 1150 to 1280°C.

2. A method for in-situ generation of a high entropy ceramic phase joint, comprising: The composition of the multi-active component solder according to claim 1; Then, the raw materials are melted into alloy ingots by arc melting under argon protection; the alloy ingots are prepared into brazing foil or brazing powder; the brazing foil or brazing powder is then placed between two ceramic materials to be welded, and after assembly, they are put into a vacuum furnace for high-temperature brazing.

3. The method according to claim 2, wherein the high temperature brazing temperature is 1200-1300°C and the heat preservation time is 10-120 minutes.

4. The method according to claim 3, wherein the heating rate is 10°C / min, and the vacuum degree in the vacuum furnace is not less than 10 -3 Pa.

5. The method according to claim 2, wherein the cooling rate from the brazing temperature to 500°C after brazing is completed is not greater than 5°C / min, and then the furnace is cooled to room temperature.

6. The method according to claim 2, wherein the preparation of the alloy ingot into a solder foil is carried out by a rapid cooling method, and the thickness of the solder foil is 60 to 120 microns.

7. The method according to claim 6, wherein when the single roller method is used for rapid solidification to prepare the quenched foil strip, the speed of the single roller is 5000-12000 r / min, and the cooling rate of the alloy ingot after melting to form a liquid state is between 10 3 ~10 6 Between K / s.

8. The method according to claim 2, wherein preparing the alloy ingot into solder powder comprises passing the alloy ingot through a quenched foil strip device to make a quenched foil strip, grinding the quenched foil strip into powder, and then sieving to obtain a powdered solder, wherein the powder particle size is less than 50 mesh.

Citation Information

Patent Citations

  • SiC ceramic brazing method based on multi-element high-entropy alloy and brazing filler metal

    CN111922468A

  • High-entropy brazing filler metal for TiAl alloy brazing and preparation method and application of high-entropy brazing filler metal

    CN114346519A