A processing method for biodegradable polymer nanocomposite material

Through the surface polymerization modification of nanoparticles and the multi-element dry extrusion process of polyester polymer materials, high-performance biodegradable polymer nanocomposites are prepared, which solves the problem of insufficient mechanical properties of existing materials and achieves The effect of high bio-based content, excellent tensile properties and high degradation rate.

CN115466496BActive Publication Date: 2024-10-01JIANGNAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211144743.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-20
Publication Date
2024-10-01
Estimated Expiration
2042-09-20

AI Technical Summary

Technical Problem

The mechanical properties of existing biodegradable materials are insufficient, especially the poor tensile properties, which makes it difficult to meet the needs in many application scenarios. In addition, the poor compatibility between the toughened nanoparticles and the mixed base material during nanocomposite leads to the tensile properties of the composite materials. Deterioration.

Method used

Modified nanoparticles are prepared by polymerizing the surface of the nanoparticles, and are mixed with polyester polymer materials and processing aids in a specific ratio. A single-screw extruder is used for three-stage temperature dry processing to adjust the moisture content. content and screw speed to prepare biodegradable polymer nanocomposites that are highly compatible with each component.

Benefits of technology

It has realized a biodegradable polymer nanocomposite with high bio-based content, tensile strength of not less than 24MPa, and elongation at break of not less than 600%. The 90-day compost degradation rate is not less than 96% and is suitable for many fields. disposable plastic products and film-coated packaging materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115466496B_ABST
    Figure CN115466496B_ABST
Patent Text Reader

Abstract

The present invention relates to a processing method of a biodegradable polymer nanocomposite material, and belongs to the field of green environmentally friendly packaging materials. The present invention prepares a biodegradable polymer nanocomposite material by polymer modification of nanoparticle surface and multi-element dry extrusion reaction technology. The method of the present invention has a simple production process and a precise and controllable operation process. The components of the prepared biodegradable polymer nanocomposite material are highly compatible, and the comprehensive performance is excellent: high bio-based content (not less than 95%), mechanical properties, especially excellent tensile properties (tensile strength not less than 24MPa, elongation at break not less than 600%), 90-day composting degradation rate not less than 96%, can be used to produce disposable plastic products and / or film-coated packaging materials in many fields such as food, textiles, daily chemicals, and medicine, and has broad market prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a processing method of a biodegradable polymer nanocomposite material, and belongs to the field of green environmentally friendly packaging materials. Background Art

[0002] In 2020, the global biodegradable plastic production capacity is about 1.2 million tons, with an annual growth rate of 20%-30%. From the perspective of regional demand distribution, Western Europe accounts for 55% (the most stringent legislation on disposable plastics), Asia-Pacific accounts for 25% (of which China accounts for 12%), and North America accounts for 19%; from the perspective of application areas, food packaging, disposable tableware and plastic bags are the largest users, accounting for 49%. In Asia, disposable tableware and pre-prepared food packaging are also major end markets; China, with its rapidly growing potential demand, is the main market for biodegradable materials in the future. Most of the biodegradable materials on the market, such as PBAT, PCL, PLA, PBS, etc., are difficult to meet the needs of many application scenarios due to defects such as insufficient mechanical properties and unbalanced rigidity and toughness. At present, the modification methods used to improve the mechanical properties of biodegradable materials include polymer blending and nanocomposite toughening. However, during nanocomposite, the components are often unevenly dispersed in the matrix due to the poor compatibility of toughened nanoparticles with the mixed base material, the interfacial tension increases, the flow of polyester chains is hindered, and the tensile properties of the composite material deteriorate. Based on the above reasons, in order to broaden the application areas of biodegradable materials and improve their comprehensive performance, it is urgent to develop a processing method for biodegradable polymer nanocomposites. Summary of the invention

[0003] Technical issues:

[0004] Provided is a preparation process for a biodegradable polymer nanocomposite material. The components of the prepared biodegradable polymer nanocomposite material are highly compatible and have excellent comprehensive performance: high biobased content (not less than 95%), excellent mechanical properties, especially tensile properties (tensile strength not less than 24MPa, elongation at break not less than 600%), and a 90-day composting degradation rate not less than 96%.

[0005] Technical solution:

[0006] The first object of the present invention is to provide a process for preparing a biodegradable polymer nanocomposite material, comprising the following steps:

[0007] (1) performing surface polymer modification on nanoparticles to obtain modified nanoparticles;

[0008] (2) adding each substance in parts by weight, mixing 50-90 parts of polyester polymer material, 20-40 parts of modified nanoparticles and 1-3 parts of processing aid to obtain a mixed base material, and adjusting the water content to 8-15%;

[0009] (3) Using a single screw extruder as a reactor, setting three processing temperatures at 70-100, 105-120, and 120-125° C., an aspect ratio of (5-20):1, and a screw speed of 130-190 r / min, dry-extruding the mixed base material after adjusting the moisture content to obtain a biodegradable polymer nanocomposite material.

[0010] Preferably, in step (1), the surface polymer modification of the nanoparticles comprises at least one of: nanoparticle-polymer binary copolymerization, nanoparticle surface growth grafting modification, nanoparticle coupling modification, and nanoparticle surface heterogeneous precipitation coating.

[0011] Preferably, in step (3), the three processing temperatures are set to 70-85, 105-110, and 120-125° C., respectively, the aspect ratio is (6-20):1, the screw speed is 130-145 r / min, and the mixed base material after adjusting the moisture content is dry-extruded to obtain a biodegradable polymer nanocomposite material.

[0012] As an embodiment of the present invention, step (1) specifically comprises: mixing the dehydrated nanoparticles with an interface modifier, and heating the mixture to react to perform surface polymer modification to obtain modified nanoparticles.

[0013] In one embodiment of the present invention, the nanoparticles are derived from natural minerals or artificially synthesized minerals.

[0014] In one embodiment of the present invention, the preparation method of the nanoparticles is: using natural minerals or artificially synthesized minerals as raw materials, preparing them through preliminary crushing by mechanical hammer pressure, air flow crushing, double spraying process (spray carbonization and spray drying), nano-ultrafine crushing and screening and grading.

[0015] As an embodiment of the present invention, in step (1), the nanoparticles are at least one of sulfate, silicate, hydrous silicic acid and carbonate, and have a relative density of 2.0 to 2.8 g / cm 3 , particle size is 10-100nm, and Mohs hardness is 1-7.

[0016] Preferably, the nanoparticles are one of calcium sulfate nanoparticles, hydrated magnesium silicate nanoparticles and calcium carbonate nanoparticles, and have a relative density of 2.6 to 2.8 g / cm 3 , particle size 50-90 nm, Mohs hardness 1-7. Preferably, the nanoparticles include at least one of mineral salts such as barium sulfate, calcium sulfate, calcium sulfite, potassium aluminosilicate, potassium magnesium aluminosilicate, hydrous silicic acid, hydrated magnesium silicate and calcium carbonate.

[0017] As an embodiment of the present invention, in step (1), the interface modifier is one or more of epoxy silane, chelated phthalate, monoalkoxy phosphate titanate, aminosilane, sulfonyl azide silane, monoalkoxy phthalate, aluminate and monoalkoxy pyrophosphate titanate.

[0018] As an embodiment of the present invention, in step (1), the mass ratio of the interface modifier to the nanoparticles is (0.1-1): 100. Preferably, the mass ratio of the interface modifier to the nanoparticles is (0.5-1):100.

[0019] As an embodiment of the present invention, in step (1), the heating reaction is carried out at a temperature of 80 to 90° C. and a time of 0.5 to 1 h.

[0020] As an embodiment of the present invention, in step (1), dehydration: the temperature is 90-100°C.

[0021] As an embodiment of the present invention, in step (2), the polyester polymer material includes at least one of aromatic polyester, aliphatic polyester and polylactide, and has an average molecular weight of 50,000 to 200,000 Da. Preferably, the polyester polymer material includes at least one of polyhydroxyalkanoate, polycaprolactone, polylactide, polydioxanone, polybutylene succinate and polybutylene terephthalate adipate.

[0022] As an embodiment of the present invention, in step (2), the processing aid includes at least one of acrylic acid, glycidyl acrylate, glycidyl methacrylate, tetrabutyl titanate, tri-n-butyl citrate, tri-n-butyl acetyl citrate, isocyanate, zinc stearate, calcium stearate, barium stearate, n-butyl stearate, stearamide, methyl silicone oil, and maleic anhydride. Preferably, the processing aid includes at least one of tetrabutyl titanate, tri-n-butyl citrate, zinc stearate, calcium stearate, glycidyl acrylate, n-butyl stearate, stearamide, isocyanate, and maleic anhydride.

[0023] Preferably, the step (2) is: according to the weight proportion of each substance, 55-65 parts of polyester polymer material, 20-40 parts of modified nanoparticles and 1.5 parts of processing aid are mixed to obtain a mixed base material and the moisture content is adjusted to 8-15%.

[0024] Preferably, the step (2) comprises: weighing 20 parts of polyhydroxyalkanoate, 10 parts of polycaprolactone, 25 parts of polylactide, 30 parts of modified nanoparticles, 0.6 parts of tri-n-butyl citrate, 0.4 parts of zinc stearate and 0.5 parts of glycidyl acrylate according to the weight proportions of each substance, mixing them evenly to obtain a mixed base material, and adjusting the moisture content to 15%.

[0025] Preferably, the step (2) is as follows: according to the weight proportions of each substance, 20 parts of polybutylene terephthalate adipate, 25 parts of polycaprolactone, 15 parts of polylactide, 35 parts of modified nanoparticles, 0.5 parts of n-butyl stearate, 0.5 parts of stearamide and 0.5 parts of isocyanate are weighed and mixed to obtain a mixed base material, and the moisture content is adjusted to 8%.

[0026] Preferably, the step (2) is as follows: according to the weight proportions of each substance, 25 parts of polylactide, 15 parts of polyhydroxyalkanoate, 25 parts of polycaprolactone, 30 parts of modified nanoparticles, 0.5 parts of tetrabutyl titanate, 0.4 parts of calcium stearate and 0.6 parts of maleic anhydride are weighed and mixed to obtain a mixed base material, and the moisture content is adjusted to 10%.

[0027] The second object of the present invention is to provide a biodegradable polymer nanocomposite material prepared by the aforementioned process.

[0028] The third object of the present invention is to provide the use of the aforementioned biodegradable polymer nanocomposite material in the preparation of film materials, sheets or pellets.

[0029] Beneficial effects:

[0030] (1) The present invention provides a process for preparing a biodegradable polymer nanocomposite material, wherein the surface of nanoparticles is modified to obtain modified nanoparticles, and then a polyester polymer material, modified nanoparticles and processing aids are used as raw materials through a multi-component dry extrusion process with specific process parameters to successfully prepare a biodegradable polymer nanocomposite material with highly compatible components. The biodegradable polymer nanocomposite material has a high biobased content (not less than 95%), excellent mechanical properties, especially tensile properties (tensile strength not less than 24 MPa, elongation at break not less than 600%), and a 90-day composting degradation rate not less than 96%. It can be used in the production of disposable plastic products and / or film-coated packaging materials in many fields such as food, textiles, daily chemicals, and medicine, and has broad market prospects.

[0031] (2) The process steps of the present invention are simple, easy to operate, the reaction conditions are precisely controllable, the cost is relatively low, the entire process is clean and green, and there is almost no pollution to the environment.

[0032] (3) The present invention utilizes abundant natural mineral resources to develop environmentally friendly, recyclable biodegradable materials, which is in line with the national strategic industrial development plan and has development significance for alleviating the oil crisis and white pollution and responding to the national "plastic restriction" policy. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is an electron microscope photograph of the biodegradable polymer nanocomposite material obtained in Example 1. DETAILED DESCRIPTION

[0034] Performance testing method:

[0035] Biobased Content Test Methods : Quantitative analysis was performed with reference to the national standard GB / T29649-2013 Determination of bio-based content in bio-based materials using liquid scintillation counter method.

[0036] Tensile strength test method :The analysis was carried out with reference to the national standard GB / T 1040.2-2006 Determination of tensile properties of plastics Part 2: Test conditions for molded and extruded plastics.

[0037] Elongation at break test method :The analysis was carried out with reference to the national standard GB / T 1040.3-2006 Determination of tensile properties of plastics Part 3: Plastics-Test conditions for tensile properties test.

[0038] 90-day composting degradation rate test method : Referring to the national standard GB / T19277.1-2011 material biodegradability test under controlled composting conditions, the material is treated as an organic compound under controlled composting conditions, and the final aerobic biodegradability and its degree of disintegration are determined by measuring the amount of carbon dioxide emitted.

[0039] Example 1

[0040] A preparation process of a biodegradable polymer nanocomposite material comprises the following steps:

[0041] (1) Calcium sulfate nanoparticles (relative density: 2.76 g / cm 3 , particle size: 75nm, Mohs hardness: 3.59) was dehydrated and dried at 90°C, and then a chelated phthalate was added thereto and mixed thoroughly in a high-speed mixer, wherein the amount of the chelated phthalate added was 0.5% of the mass fraction of the calcium sulfate nanoparticles; the obtained mixture was placed at 90°C for reaction for 1 hour to obtain modified nanoparticles;

[0042] (2) According to the weight proportion of each substance, 20 parts of polyhydroxyalkanoate, 10 parts of polycaprolactone, 25 parts of polylactide, 30 parts of modified nanoparticles, 0.6 parts of tri-n-butyl citrate, 0.4 parts of zinc stearate and 0.5 parts of glycidyl acrylate were weighed and mixed to obtain a mixed base material, and the moisture content was adjusted to 15%. A single-screw extruder was used as a reactor, and three-stage processing temperatures were set to 85, 110, and 120° C., respectively, with an aspect ratio of 10 and a screw speed of 130 r / min, and dry extrusion was performed to obtain a biodegradable polymer nanocomposite material.

[0043] After testing, the target product obtained in Example 1, the biodegradable polymer nanocomposite material, has a biobased content of 98%, a tensile strength of 28.3 MPa, an elongation at break of 620%, and a 90-day composting degradation rate of 97%.

[0044] Example 2

[0045] A preparation process of a biodegradable polymer nanocomposite material comprises the following steps:

[0046] (1) Hydrated magnesium silicate nanoparticles (relative density: 2.62 g / cm 3 , particle size: 85nm, Mohs hardness: 1.18) was dehydrated and dried at 95°C, and then monoalkoxy phosphate type titanate was added thereto and mixed thoroughly in a high-speed mixer, wherein the amount of monoalkoxy phosphate type titanate added was 0.7% of the mass fraction of the hydrated magnesium silicate nanoparticles; the obtained mixture was placed at 85°C for reaction for 1 hour to obtain modified nanoparticles;

[0047] (2) According to the weight proportion of each substance, 20 parts of polybutylene terephthalate adipate, 25 parts of polycaprolactone, 15 parts of polylactide, 35 parts of modified nanoparticles, 0.5 parts of n-butyl stearate, 0.5 parts of stearamide and 0.5 parts of isocyanate were weighed and mixed to obtain a mixed base material, and the moisture content was adjusted to 8%. A single-screw extruder was used as a reactor, and three-stage processing temperatures were set to 80, 105, and 125° C., respectively, with an aspect ratio of 20 and a screw speed of 135 r / min. The biodegradable polymer nanocomposite material was obtained by dry extrusion.

[0048] After testing, the target product obtained in Example 2, the biodegradable polymer nanocomposite material, has a biobased content of 98%, a tensile strength of 27.4 MPa, an elongation at break of 615%, and a 90-day composting degradation rate of 98%.

[0049] Example 3

[0050] A preparation process of a biodegradable polymer nanocomposite material comprises the following steps:

[0051] (1) Calcium carbonate nanoparticles (relative density: 2.73 g / cm 3 , particle size: 56nm, Mohs hardness: 5.03) was dehydrated and dried at 100°C, and then epoxysilane was added thereto and mixed thoroughly in a high-speed mixer, wherein the amount of epoxysilane added was 1% of the mass fraction of the calcium carbonate nanoparticles; the obtained mixture was placed at 90°C for reaction for 0.5h to obtain modified nanoparticles;

[0052] (2) According to the weight proportion of each substance, 25 parts of polylactide, 15 parts of polyhydroxyalkanoate, 25 parts of polycaprolactone, 30 parts of modified nanoparticles, 0.5 parts of tetrabutyl titanate, 0.4 parts of calcium stearate and 0.6 parts of maleic anhydride were weighed and mixed to obtain a mixed base material, and the moisture content was adjusted to 10%. A single-screw extruder was used as a reactor, and three-stage processing temperatures were set to 70, 110, and 120°C, respectively, with an aspect ratio of 6 and a screw speed of 145 r / min. Dry extrusion was performed to obtain a biodegradable polymer nanocomposite material.

[0053] After testing, the target product obtained in Example 3, the biodegradable polymer nanocomposite material, has a biobased content of 95%, a tensile strength of 28.5 MPa, an elongation at break of 650%, and a 90-day composting degradation rate of 97%.

[0054] Comparative Example 1

[0055] A preparation process of a biodegradable polymer nanocomposite material is as described in Example 1, except that the interface modification of calcium sulfate nanoparticles in step (1) is omitted. Specifically:

[0056] According to the weight proportion of each substance, 20 parts of polyhydroxyalkanoate, 10 parts of polycaprolactone, 25 parts of polylactide, 30 parts of unmodified calcium sulfite nanoparticles, 0.6 parts of tri-n-butyl citrate, 0.4 parts of zinc stearate and 0.5 parts of glycidyl acrylate were weighed and mixed to obtain a mixed base material, and the moisture content was adjusted to 15%. A single-screw extruder was used as a reactor, three-stage processing temperatures were set to 85, 110 and 120° C., an aspect ratio of 10, a screw speed of 130 r / min, and dry extrusion was performed to obtain a biodegradable polymer nanocomposite material.

[0057] After testing, the biodegradable polymer nanocomposite material prepared in Comparative Example 1 had a biobased content of 95%, a tensile strength of only 15.0 MPa, an elongation at break of only 350%, and a 90-day composting degradation rate of 95%.

[0058] Table 1 Performance results of the products obtained in Examples 1 to 3 and Comparative Example 1

[0059] example Bio-based content / % Tensile strength / MPa Elongation at break / % 90-day composting degradation rate / % Example 1 98 28.3 620 97 Example 2 98 27.4 615 98 Example 3 95 28.5 650 97 Comparative Example 1 95 15.0 350 95

[0060] Comparative Example 2

[0061] The preparation process of a biodegradable polymer nanocomposite material is referred to Example 1, except that the weight proportions of the modified nanoparticles are adjusted to 0, 10, 20, 30 and 40 parts, respectively, to prepare the corresponding biodegradable polymer nanocomposite materials. The performance results of the obtained products are shown in Table 2.

[0062] Table 2 Performance results of products obtained with different amounts of modified nanoparticles added

[0063]

Claims

1. A process for preparing a biodegradable polymer nanocomposite material, characterized in that: The steps include: (1) Dehydrate and dry the calcium carbonate nanoparticles, then add epoxysilane to the nanoparticles and mix them thoroughly in a high-speed mixer, wherein the epoxysilane addition amount is 1% of the mass fraction of the calcium carbonate nanoparticles; place the resulting mixture at 90° C. for reaction for 0.5 h to obtain modified nanoparticles; wherein the parameters of the calcium carbonate nanoparticles are: relative density: 2.73 g / cm 3 , particle size: 56nm, Mohs hardness: 5.03; (2) According to the weight proportion of each substance, 25 parts of polylactide, 15 parts of polyhydroxyalkanoate, 25 parts of polycaprolactone, 30 parts of modified nanoparticles, 0.5 parts of tetrabutyl titanate, 0.4 parts of calcium stearate and 0.6 parts of maleic anhydride were weighed and mixed to obtain a mixed base material, the moisture content was adjusted to 10%, and a single screw extruder was used as a reactor. The three-stage processing temperatures were set to 70, 110 and 120° C., respectively, the aspect ratio was 6, the screw speed was 145 r / min, and a biodegradable polymer nanocomposite material was obtained by dry extrusion; wherein the biodegradable polymer nanocomposite material had a biobased content of 95%, a tensile strength of 28.5 MPa, an elongation at break of 650%, and a 90-day composting degradation rate of 97%.

2. A process for preparing a biodegradable polymer nanocomposite material, characterized in that: The steps include: (1) Dehydrate and dry calcium sulfate nanoparticles, then add chelated phthalate to the nanoparticles and mix them thoroughly in a high-speed mixer, wherein the amount of chelated phthalate added is 0.5% of the mass fraction of the calcium sulfate nanoparticles; place the resulting mixture at 90° C. for 1 hour to obtain modified nanoparticles; wherein the parameters of the calcium sulfate nanoparticles are: relative density: 2.76 g / cm 3 , particle size: 75nm, Mohs hardness: 3.59; (2) According to the weight proportion of each substance, 20 parts of polyhydroxyalkanoate, 10 parts of polycaprolactone, 25 parts of polylactide, 30 parts of modified nanoparticles, 0.6 parts of tri-n-butyl citrate, 0.4 parts of zinc stearate and 0.5 parts of glycidyl acrylate were weighed and mixed to obtain a mixed base material, the moisture content was adjusted to 15%, and a single screw extruder was used as a reactor. The three-stage processing temperatures were set to 85, 110 and 120° C., respectively, the aspect ratio was 10, the screw speed was 130 r / min, and a biodegradable polymer nanocomposite material was obtained by dry extrusion; wherein the biodegradable polymer nanocomposite material had a biobased content of 98%, a tensile strength of 28.3 MPa, an elongation at break of 620%, and a 90-day composting degradation rate of 97%.

3. A process for preparing a biodegradable polymer nanocomposite material, characterized in that: The steps include: (1) Dehydrated and dried magnesium silicate hydrate nanoparticles, and then added with monoalkoxy phosphate type titanate to the hydrated magnesium silicate nanoparticles and mixed thoroughly in a high-speed mixer, wherein the amount of monoalkoxy phosphate type titanate added is 0.7% of the mass fraction of magnesium silicate hydrate nanoparticles; the obtained mixture is placed at 85° C. for 1 hour to obtain modified nanoparticles; wherein the parameters of magnesium silicate hydrate nanoparticles are: relative density: 2.62 g / cm 3 , particle size: 85nm, Mohs hardness: 1.18; (2) According to the weight proportion of each substance, 20 parts of polybutylene terephthalate adipate, 25 parts of polycaprolactone, 15 parts of polylactide, 35 parts of modified nanoparticles, 0.5 parts of n-butyl stearate, 0.5 parts of stearamide and 0.5 parts of isocyanate are weighed and mixed to obtain a mixed base material, the moisture content is adjusted to 8%, and a single screw extruder is used as a reactor. The three-stage processing temperatures are set to 80, 105 and 125° C., respectively, the aspect ratio is 20, the screw speed is 135 r / min, and a biodegradable polymer nanocomposite material is obtained by dry extrusion; wherein the biodegradable polymer nanocomposite material has a biobased content of 98%, a tensile strength of 27.4 MPa, an elongation at break of 615%, and a 90-day composting degradation rate of 98%.

4. A biodegradable polymer nanocomposite material, characterized in that: The invention is prepared by the process described in any one of claims 1 to 3.

5. Use of the biodegradable polymer nanocomposite material according to claim 4 in the preparation of film materials, sheets or pellets.