A method for preparing silver / copper oxide composite honeycomb nanoparticles modified carbon paste electrode by electrospinning and its application
The preparation of silver/copper oxide composite honeycomb nanoparticles modified carbon paste electrodes through electrospinning has solved the problem of high cost and insufficient catalytic activity of H2O2 detection materials in the prior art, and achieved the detection effect of high sensitivity and wide linear range. Suitable for biological sample analysis.
Patent Information
- Application Number
- CN202211156016.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-22
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, hydrogen peroxide (H2O2) detection methods have problems such as high material cost, low catalytic activity, low sensitivity and small detection range. Especially when using pure nano copper oxide materials, agglomeration leads to poor catalytic performance. Affects the linear range and detection limit of the sensor.
The carbon paste electrode with silver/copper oxide composite honeycomb nanoparticles is prepared by electrospinning. The electrode material with high specific surface area and microporous structure is formed through electrospinning synthesis of Ag@CuO composite nanomaterials and high-temperature calcination treatment, which improves the Electrocatalytic activity.
It significantly improves the detection sensitivity and linear range of H2O2, increases the current response, achieves a lower detection limit, is low cost, has good reproducibility and stability, and is suitable for actual biological sample detection.
Smart Images

Figure CN115479980B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrochemical analysis and detection, in particular to a method for preparing a silver / copper oxide composite honeycomb nanoparticle modified carbon paste electrode by electrostatic spinning and application thereof. Background Art
[0002] Hydrogen peroxide (H2O2) is an inorganic compound that is widely used in medicine, chemical reactions, environmental analysis, electronics and other fields. Therefore, it is very important and necessary to quickly and accurately determine the content of hydrogen peroxide. At present, researchers have developed a variety of hydrogen peroxide detection methods, including fluorescence, surface enhanced Raman, colorimetry, etc., but these methods generally have problems such as complex experimental processes, high solvent toxicity, and low sensitivity. The electrochemical method has the advantages of simple equipment, easy portability, low cost, fast response speed, high sensitivity, good selectivity, and environmental protection, which has attracted widespread attention, making the research on electrochemical H2O2 sensors arouse widespread attention.
[0003] In addition, H2O2 is also one of the most important reactive oxygen species (ROS) and is involved in various physiological and pathological processes such as cell proliferation, differentiation and migration. H2O2 acts as a precursor in the formation of highly reactive and potentially harmful hydroxyl radicals (.OH), which are considered to be one of the most important signals of oxidative stress. Therefore, accurate and highly sensitive detection of H2O2, monitoring its concentration in the body, and understanding the related biological effects are also of great significance in analysis and diagnosis.
[0004] Previous studies mainly used precious metals such as gold (Au), platinum (Pt), lead (Pb), palladium (Pd) and metal oxide materials such as nickel oxide (NiO), copper oxide (CuO), manganese oxide (MnO2) and cobalt oxide (Co3O4) to construct hydrogen peroxide sensors. In practical applications, it is necessary to consider the cost of selecting modified materials and whether the catalytic activity is obvious. Based on the above properties of copper oxide materials, a considerable amount of research is currently focused on copper oxide materials. However, it is very easy to agglomerate in the process of preparing copper oxide materials. In electrochemical experiments, it is found that pure nano copper oxide materials often cannot show high catalytic performance, which seriously affects their catalytic properties. The linear range and detection limit effect shown in the construction of electrochemical sensors are not obvious. After the nanoparticles agglomerate, surface effects will occur, and the diffusion channel of the analyte will be blocked. With regard to this obstacle, it is possible to improve the electrocatalytic kinetics by regulating the micromorphology, thereby obtaining higher electrocatalytic activity, such as constructing porous structure materials. Moreover, the doping of precious metals on the surface of the composite material will form a Schottky barrier to inhibit its hole recombination. Therefore, doping with precious metals is an important means to enhance the catalytic activity, adsorption activity and other chemical activities of composite materials. However, there has been no public report on how to prepare electrocatalytically active, low-cost electrode materials that have a wider linear range, lower detection limit, higher sensitivity and selectivity for H2O2. Summary of the invention
[0005] In view of the above situation, in order to overcome the defects of the prior art, the purpose of the present invention is to provide a method and application of preparing silver / copper oxide composite honeycomb nanoparticles modified carbon paste electrode by electrospinning, which can effectively solve the problems of high material cost, unclear catalytic activity, low sensitivity and small detection range for the existing H2O2 determination.
[0006] To achieve the above object, the technical solution provided by the present invention is a method for preparing a silver / copper oxide composite honeycomb nanoparticle modified carbon paste electrode by electrospinning, comprising the following steps:
[0007] a. Electrospinning synthesis and high temperature calcination of Ag@CuO composite nanomaterials: PVP was slowly added to anhydrous ethanol, stirred at room temperature for 30 minutes, and then ultrasonicated for 40 minutes at a temperature not exceeding 40°C to obtain a PVP anhydrous ethanol mixed solution, wherein the weight percentage of PVP in anhydrous ethanol was 10wt%, and 8.7667g of PVP anhydrous ethanol mixed solution was taken to obtain colloidal solution A; then Cu(Ac)2 was added to anhydrous ethanol and stirred at room temperature for 30 minutes to obtain a Cu(Ac)2 anhydrous ethanol mixed solution, wherein the weight percentage of Cu(Ac)2 in anhydrous ethanol was 3.9wt%, and 10.5823g Cu(Ac)2 anhydrous ethanol mixed solution was obtained to obtain solution B; then AgNO3 was added to anhydrous ethanol at a molar ratio of Cu:Ag = 9:1 (the molar ratio of Cu in solution B), and stirred to dissolve to obtain an anhydrous ethanol solution of AgNO3, wherein the weight percentage of AgNO3 in anhydrous ethanol was 3.1wt%, and 0.8144g AgNO3 anhydrous ethanol solution to obtain solution C; pour solution B and solution C into colloidal solution A respectively, stir overnight for 8-12 hours to obtain a viscous precursor solution, load the precursor solution into a syringe, and connect it to a high-voltage power supply for electrospinning. The spinning voltage is 18 kV, the distance from the needle to the receiver is 15 cm, and the flow rate is 1.2 ml / h. After the spinning is completed, Cu(Ac)2 / AgNO3 / PVP nanofibers are obtained. The prepared Cu(Ac)2 / AgNO3 / PVP nanofibers are stabilized in a drying oven at 80°C for 12 hours, and then the dried Cu(Ac)2 / AgNO3 / PVP nanofibers are placed in a high-temperature furnace and heated at 5°C.min -1 The heating rate was raised to 500°C and kept at room temperature for 5 h to obtain Ag@CuO composite honeycomb nanoparticles;
[0008] b. Preparation of Ag@CuO composite honeycomb nanoparticle modified carbon paste electrode: carbon powder and paraffin oil were mixed at a mass ratio of 3.5, fully ground into a paste, and then loaded into a glass tube, and a copper wire was inserted to establish electrical contact to prepare a carbon paste electrode. The prepared carbon paste electrode was polished on suede with 0.05µm Al2O3 polishing powder until its surface was smooth and flat, and then ultrasonically cleaned with ethanol and deionized water for 3 minutes each, and then dried for use. 4 mg of Ag@CuO composite honeycomb nanoparticles were placed in a beaker, and 30 μL of 5% mass concentration naphthol solution, 0.75 ml of deionized water and 0.25 ml of anhydrous ethanol were added respectively, and ultrasonic dispersion was performed for 60 minutes, with the ultrasonic temperature not exceeding 20°C to obtain a silver / copper oxide dispersion modifier. 10 μL of the silver / copper oxide dispersion modifier was taken and dropped onto the surface of the ground bare carbon paste electrode, and dried at room temperature to obtain Ag@CuO-CPE (silver / copper oxide composite honeycomb nanoparticle modified carbon paste electrode).
[0009] The Ag@CuO-CPE has a diameter of 3 mm.
[0010] The invention discloses an application of the silver / copper oxide composite honeycomb nanoparticle modified carbon paste electrode prepared by the method in electrochemical determination of H2O2.
[0011] The application of the silver / copper oxide composite honeycomb nanoparticle modified carbon paste electrode in the electrochemical determination of H2O2 is to use the silver / copper oxide composite honeycomb nanoparticle modified carbon paste electrode as a working electrode, an Ag / AgCl electrode as a reference electrode, and a platinum wire electrode as an auxiliary electrode to form a three-electrode system; when determining H2O2, the three-electrode system is placed in 30 mL of 0.1M NaOH solution, and cyclic voltammetry is performed to scan 20 segments in the potential range from -1 V to 1 V to activate the electrode; the current-time curve is recorded, and when the background current reaches a steady state, a standard solution of H2O2 is added to the solution using a microinjector; under different concentrations of H2O2 solution, the current response value of the sensor is measured, and in the concentration range of 0.05 μM to 2000 μM, a linear relationship curve between the current and the H2O2 solution of different concentrations is obtained, and its linear correlation coefficient R = 0.9952, and the recovery rate of H2O2 detection results was 98.0%-101.5%.
[0012] The preparation method of the present invention is simple, low-cost, simple, fast and easy to operate. The electrode material of the electrochemical sensor with a honeycomb structure having a high surface area to volume ratio is constructed, which not only increases the specific surface area, but also improves the AC contact performance between electrons, improves the electrocatalytic kinetics by regulating the microscopic morphology, and improves the electrocatalytic activity of the new electrode material. Compared with the bare electrode, the current response of hydrogen peroxide on the electrode modified by the composite material is significantly increased, which greatly improves the sensitivity and detection range of the analysis and detection, and has significant social and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is a flow chart of the synthesis of Ag@CuO nano honeycomb particles of the present invention.
[0014] Figure 2 It is the XRD spectrum of the Ag@CuO particles of the present invention.
[0015] Figure 3These are SEM image characterization diagrams of Cu(Ac)2 / AgNO3 / PVP nanofibers and Ag@CuO nanoparticles in the present invention, wherein (a) - SEM image of electrospun Cu(Ac)2 / AgNO3 / PVP nanofibers, (b and d) - low-magnification SEM images of Ag@CuO nanoparticles, (c) - local enlarged image of Ag@CuO nanoparticles, and (e) - high-magnification SEM image of Ag@CuO nanoparticles.
[0016] Figure 4 It is a time-current curve diagram of the bare CPE, CuO-CPE and Ag@CuO-CPE modified electrodes of the present invention in 0.1M NaOH solution.
[0017] Figure 5 This is the time-current response diagram of the Ag@CuO modified electrode of the present invention to the H2O2 concentration.
[0018] Figure 6 It is the concentration-current standard working curve diagram of H2O2 of the present invention.
[0019] Figure 7 This is a table for determining H2O2 in coconut fruit in the present invention (n=4). DETAILED DESCRIPTION
[0020] The specific implementation of the present invention is described in detail below with reference to the accompanying drawings and examples. Example
[0021] A method for preparing a silver / copper oxide composite honeycomb nanoparticle modified carbon paste electrode by electrospinning, comprising the following steps:
[0022] a. Electrospinning synthesis and high temperature calcination treatment of Ag@CuO composite nanomaterials: PVP was slowly added to anhydrous ethanol, stirred at room temperature for 30 minutes, and then ultrasonicated for 40 minutes at a temperature not exceeding 40°C to obtain a PVP anhydrous ethanol mixed solution, wherein the weight percentage of PVP in anhydrous ethanol was 10wt%, and 8.7667g of PVP anhydrous ethanol mixed solution was taken to obtain a colloidal solution A; Cu(Ac)2 was then added to anhydrous ethanol, stirred at room temperature for 30 minutes to obtain a Cu(Ac)2 anhydrous ethanol mixed solution, wherein the weight percentage of Cu(Ac)2 in anhydrous ethanol was 3.9wt%, and 10.5823g of Cu(Ac)2 anhydrous ethanol mixed solution was taken to obtain a solution B; AgNO3 was then added to anhydrous ethanol at a molar ratio of Cu:Ag=9:1, stirred and dissolved to obtain an AgNO3 anhydrous ethanol solution, wherein the weight percentage of AgNO3 in anhydrous ethanol was 3.1wt%, and 0.8144g AgNO3 anhydrous ethanol solution to obtain solution C; pour solution B and solution C into colloidal solution A respectively, stir overnight for 8-12 hours to obtain a viscous precursor solution, load the precursor solution into a syringe, and connect it to a high-voltage power supply for electrospinning. The spinning voltage is 18kV, the distance from the needle to the receiver is 15cm, and the flow rate is 1.2ml / h. After the spinning is completed, Cu(Ac)2 / AgNO3 / PVP (copper acetate / silver nitrate / polyvinyl pyrrolidone) nanofibers are obtained. The prepared Cu(Ac)2 / AgNO3 / PVP nanofibers are stabilized in a drying oven at 80°C for 12 hours, and then the dried Cu(Ac)2 / AgNO3 / PVP nanofibers are placed in a high-temperature furnace and heated at 5°C.min -1 The heating rate was raised to 500°C and kept at room temperature for 5 h to obtain Ag@CuO composite honeycomb nanoparticles;
[0023] b. Preparation of Ag@CuO composite honeycomb nanoparticle modified carbon paste electrode: carbon powder and paraffin oil were mixed at a mass ratio of 3.5, and fully ground into a paste with fine particles and uniform wetness. Then, the mixture was placed in a glass tube, and a copper wire was inserted to establish electrical contact to prepare a carbon paste electrode. The prepared carbon paste electrode was polished on suede with 0.05µm Al2O3 polishing powder until its surface was smooth and flat. Then, the mixture was ultrasonically cleaned with ethanol and deionized water for 3 minutes each, and then dried for use. 4 mg of Ag@CuO composite honeycomb nanoparticles were placed in a small beaker, and 30 μL of 5% naphthol solution, 0.75 ml of deionized water, and 0.25 ml of anhydrous ethanol were added respectively. The mixture was ultrasonically dispersed for 60 minutes, and the ultrasonic temperature did not exceed 20°C to obtain a silver / copper oxide dispersion modifier. 10 μL of the silver / copper oxide dispersion modifier was dripped onto the surface of the ground bare carbon paste electrode, and dried at room temperature to obtain Ag@CuO-CPE.
[0024] The silver / copper oxide composite honeycomb nanoparticle modified electrode (Ag@CuO-CPE) prepared by the method of the present invention has good reproducibility and stability. Taking the embodiment as an example, the specific experimental data are as follows:
[0025] 1. Structural and morphological characterization of modified electrode materials
[0026] The crystal structure of the final product of the Ag@CuO sample was characterized by X-ray diffractometer. Figure 2 The XRD spectrum of Ag@CuO particles is shown in Figure 2. The CuO diffraction peak is consistent with the peak of monoclinic CuO. The morphology of Cu(Ac)2 / AgNO3 / PVP fibers and Ag@CuO nanoparticles was characterized by SEM. The results are shown in Figure 2. Figure 3 Attached Figure 3 (a) shows the SEM image of electrospun Cu(Ac)2 / AgNO3 / PVP nanofibers. The fibers have a smooth surface, no obvious difference in overall morphology, uniform surface morphology, and a diameter of about 100-150nm. Figure 3 (b) shows the surface morphology of Ag@CuO nanoparticles after high temperature calcination under low magnification scanning electron microscopy. Figure 3 (d) and 3(c), it can be seen that Ag@CuO particles form a unique network ring structure at the close contact position, which is orderly arranged and has good AC contact performance. Figure 3 (d), (e) It can be observed that the Ag particles are tightly attached to the porous CuO particles and have a larger specific surface area than the porous CuO.
[0027] 2. Characterization of the catalytic effect of the modified electrode as an electrochemical sensor
[0028] For comparison, the glassy carbon electrode was polished with Al2O3 polishing powder and suede to a mirror surface, and then cleaned with distilled water, anhydrous ethanol and double distilled water for ultrasonic time, to obtain a bare electrode (CPE) for standby use; CuO nanoparticles were prepared using the same process route and parameters as step a in the embodiment, and CuO modified electrodes (CuO-CPE) were prepared using the same process route and parameters as step b in the embodiment. Before each experiment, the modified electrode was in 0.1M NaOH buffer solution at 100mV.s -1 The activation was carried out at a scan rate of , and the scanning potential was -1~1V.
[0029] In a 0.1 M NaOH solution containing H2O2, the time current curves of the bare electrode, the CuO modified electrode and the Ag@CuO modified electrode prepared in the embodiment of the present invention are shown in the attached figure. Figure 4As shown in the figure, it can be seen that the bare electrode (CPE) cannot detect and analyze H2O2. Although the CuO modified electrode (CuO-CPE) has a peak current in the NaOH solution with H2O2 added, it is not very obvious. However, after adding H2O2, the peak current of the Ag@CuO modified electrode (Ag@CuO-CPE) is significantly enhanced, indicating that the Ag@CuO modified electrode has a more obvious catalytic oxidation effect on the detected substance.
[0030] 3. Electrochemical Detection of Hydrogen Peroxide
[0031] Under the optimal test conditions, the time-current response of the Ag@CuO modified electrode to H2O2 concentration is shown in the attached figure. Figure 5 As shown in the figure, as the concentration of H2O2 increases, the response current also gradually increases, and the response current of the Ag@CuO modified electrode in detecting low concentrations is more obvious than that of the pure CuO modified electrode. Figure 6 It can be seen that in the concentration range of 0.05μM to 2000μM, a linear relationship curve between current and H2O2 concentration is obtained, and the linear equation is I (μA) = 0.10457c( M) + 1.55363, its linear correlation coefficient R =0.9952, sensitivity S=1493.86μA.mM -1 .cm -2 The recovery rate of H2O2 detection results was 98.0%-101.5%.
[0032] The standard of residue analysis method in my country stipulates that the recovery rate range is between 80% and 120%. Within the controllable range of the experiment, the detection recovery rate should achieve the best result as much as possible. Therefore, the highest recovery rate in this experiment is 101.5%, which meets the requirements. In actual experiments, instrument fluctuations, system errors, sample matrix effects, etc. will affect the recovery rate.
[0033] 4. Reproducibility and stability test
[0034] Reproducibility, stability and anti-interference are important indicators to measure the quality of a sensor. In this experiment, the same Ag@CuO-CPE was used to test 25μM H2O2 10 times, and the relative standard deviation was 2.08%, which confirmed that the modified electrode was stable for the measurement of H2O2. This shows that the silver / copper oxide composite honeycomb nanoparticle modified electrode prepared by the method of the present invention has good reproducibility and stability.
[0035] Long-term stability was explored by intermittently measuring H2O2 solutions of the same concentration, and the stability was evaluated by measuring the current response of Ag@CuO-CPE to 25μM H2O2 over 15 days. The modified electrode was exposed to air and its current response was tested every day. The sensor based on Ag@CuO-CPE has good stability, and the current response loss after 15 days is only about 5%, reflecting that the H2O2 sensor has good long-term stability.
[0036] 5. Anti-interference performance
[0037] The effects of some common oxidizable substances on the detection of 25μM H2O2 were studied by time current method, that is, the anti-interference performance of the sensor was investigated. The concentration of these oxidizable substances was controlled within a certain range, and the relative error generated in the determination of H2O2 was about ±5%. The tolerance ratio of oxidizable substances to H2O2 was 50 times acetic acid, 20 times citric acid and 10 times ethanol, respectively, which did not affect the determination of hydrogen peroxide. Ascorbic acid and glucose had an impact on the determination results. Taking all factors into consideration, the Ag@CuO modified electrode has a high selectivity for the determination of H2O2. The minimum detection limit of H2O2 is 0.01μM.
[0038] 6. Testing of actual samples
[0039] In order to further verify the reliability of the developed electrochemical biosensor, the content and recovery rate of H2O2 in coconut cans were verified. First, the coconut was taken out and crushed into small particles with a mortar. Then it was put into a centrifuge tube, and the centrifuge tube was placed in a centrifuge for liquid extraction to obtain the liquid component of the coconut. Before measurement, the liquid component was diluted 20 times with 0.1M NaOH solution. By using Ag@CuO modified electrodes, amperometric studies were performed before and after H2O2 was added to these diluted samples. The results are shown in Figure 2. Figure 7 As shown in Supplementary Table 1, the analytical recoveries indicate that the sensor can be used for the determination of H2O2 in biological samples.
[0040] In summary, the preparation method of the present invention is simple, low in cost, simple, fast and easy to operate. It constructs an electrode material of an electrochemical sensor with a honeycomb structure having a high surface area to volume ratio, which not only increases the specific surface area, but also improves the AC contact performance between electrons, improves the electrocatalytic kinetics by regulating the microscopic morphology, and improves the electrocatalytic activity of the new electrode material. Compared with the bare electrode, the current response of the electrode modified with the composite material and hydrogen peroxide on the modified electrode is significantly increased, which greatly improves the sensitivity and detection range of the analysis and detection, and has good reproducibility and stability. The modified electrode in the present invention is a new type of electrochemical sensor used for actual sample determination, and has the characteristics of rapidity, sensitivity, accuracy, stability, and environmental protection. The test method of the present invention has good reproducibility and stability. It has significant social and economic benefits.
Claims
1. A method for preparing a silver / copper oxide composite honeycomb nanoparticle modified carbon paste electrode by electrospinning, characterized in that: The following steps are involved: a. Electrospinning synthesis and high temperature calcination treatment of Ag@CuO composite nanomaterials: PVP was slowly added to anhydrous ethanol, stirred at room temperature for 30 minutes, and then ultrasonicated for 40 minutes at a temperature not exceeding 40°C to obtain a PVP anhydrous ethanol mixed solution, wherein the weight percentage of PVP in anhydrous ethanol was 10wt%, and 8.7667g of PVP anhydrous ethanol mixed solution was taken to obtain colloidal solution A; then Cu(Ac)2 was added to anhydrous ethanol, stirred at room temperature for 30 minutes to obtain a Cu(Ac)2 anhydrous ethanol mixed solution, wherein the weight percentage of Cu(Ac)2 in anhydrous ethanol was 3.9wt%, and 10.5823g of Cu(Ac)2 anhydrous ethanol mixed solution was taken to obtain solution B; then AgNO3 was added to anhydrous ethanol at a molar ratio of Cu:Ag=9:1, stirred and dissolved to obtain an AgNO3 anhydrous ethanol solution, wherein the weight percentage of AgNO3 in anhydrous ethanol was 3.1wt%, and 0.8144g AgNO3 anhydrous ethanol solution to obtain solution C; pour solution B and solution C into colloidal solution A respectively, stir overnight for 8-12 hours to obtain a viscous precursor solution, load the precursor solution into a syringe, and connect it to a high-voltage power supply for electrostatic spinning. The spinning voltage is 18 kV, the distance from the needle to the receiver is 15 cm, and the flow rate is 1.2 ml / h. After the spinning is completed, Cu(Ac)2 / AgNO3 / PVP nanofibers are obtained. The prepared Cu(Ac)2 / AgNO3 / PVP nanofibers are stabilized in a drying oven at 80°C for 12 hours, and then the dried Cu(Ac)2 / AgNO3 / PVP nanofibers are placed in a high-temperature furnace and heated at 5°C·min -1 The heating rate was raised to 500°C and kept at room temperature for 5 h to obtain Ag@CuO composite honeycomb nanoparticles; b. Preparation of Ag@CuO composite honeycomb nanoparticles modified carbon paste electrode: carbon powder and paraffin oil were mixed at a mass ratio of 3.5, fully ground into a paste, and then loaded into a glass tube, and a copper wire was inserted to establish electrical contact to prepare a carbon paste electrode. The prepared carbon paste electrode was polished on suede with 0.05µm Al2O3 polishing powder until its surface was smooth and flat, and then ultrasonically cleaned with ethanol and deionized water for 3 minutes each, and then dried for use. 4 mg of Ag@CuO composite honeycomb nanoparticles were placed in a beaker, and 30 μL of 5% mass concentration naphthol solution, 0.75 ml of deionized water and 0.25 ml of anhydrous ethanol were added respectively, and ultrasonic dispersion was performed for 60 minutes. The ultrasonic temperature did not exceed 20°C to obtain a silver / copper oxide dispersion modifier. 10 μL of the silver / copper oxide dispersion modifier was taken and dropped onto the surface of the ground bare carbon paste electrode, and dried at room temperature to obtain an Ag@CuO-CPE with a diameter of 3 mm.
2. Application of the silver / copper oxide composite honeycomb nanoparticle modified carbon paste electrode prepared by the method of claim 1 in electrochemical determination of H2O2, characterized in that: The silver / copper oxide composite honeycomb nanoparticle modified carbon paste electrode was used as a working electrode, the Ag / AgCl electrode was used as a reference electrode, and the platinum wire electrode was used as an auxiliary electrode to form a three-electrode system; when determining H2O2, the three-electrode system was placed in 30 mL of 0.1M NaOH solution, and cyclic voltammetry was performed in the potential range from -1 V to 1 V for 20 segments to activate the electrode; the current-time curve was recorded, and when the background current reached a steady state, a standard solution of H2O2 was added to the solution using a microinjector; under different concentrations of H2O2 solution, the current response value of the sensor was measured, and a linear relationship curve between the current and different concentrations of H2O2 solution was obtained in the concentration range of 0.05 μM to 2000 μM, and its linear correlation coefficient R =0.9952, and the recovery rate of H2O2 detection results was 98.0%-101.5%.