Coordinated control method of microstructure and properties of high alloy content heavy rail steel
By controlling the solidification process of the steel and using waste heat diffusion, combined with rolling and heat treatment technology, the problem of uneven structural performance of heavy rail steel with high alloy content is solved, and the hardness and service life of the rail are significantly improved.
Patent Information
- Application Number
- CN202211172003.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-26
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-09-26
AI Technical Summary
The prior art lacks overall collaborative control technology for structural properties of heavy rail steel with high alloy content, resulting in uneven hardness of rails, affecting its fatigue performance and service life.
By controlling the precipitation, diffusion and convection transmission of solute alloy elements during the liquid steel solidification process during continuous casting, the waste heat after solidification of the casting billet is used for high-temperature diffusion treatment, and combining rolling and gradient high-efficiency cooling heat transfer heat treatment, the rail structure performance is achieved collaborative control.
It significantly improves the cross-sectional hardness of the rail head of heavy rail with high alloy content and the uniformity of micro-phase change structure, extends the service life of the rail, and improves its comprehensive mechanical properties.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron and steel metallurgical production, and in particular to a method for coordinated control of microstructure and properties of heavy rail steel with high alloy content. Background Art
[0002] As the main component of railway transportation construction, rails play an important role. On the one hand, they guide the train forward, and on the other hand, they bear the huge load of the train. Therefore, the quality of rails has an important impact on driving safety. In addition, with the continuous development of railway transportation, the transportation of passenger, high-speed and heavy-load freight has put forward higher requirements on the quality and performance of rails. The service performance of rails greatly determines the service life of rails and their maintenance costs.
[0003] It is necessary to improve the quality and performance of existing products and develop new high-performance products. Many scholars at home and abroad have carried out a lot of research. For example, many researchers have conducted in-depth research on the fatigue damage of rails. Their research usually homogenizes the hardness inside the rails, but actual product testing finds that the hardness inside the rails is not uniform. In addition, some scholars have pointed out that hardness is a very important influencing factor on the fatigue damage of rails. The researchers measured the cross-sectional hardness of rail heads of different varieties of rails, and the results showed that the cross-sectional hardness of the rail head gradually decreases from the surface to the inside. In addition, ASITHAC.ATHUKORALA studied the non-uniform hardness distribution, metallurgy and ratcheting behavior of Australian AS60HH rail steel. The results show that the non-uniformity of the material will affect the ratcheting effect of the rail as the wear progresses, thereby affecting the service life of the rail.
[0004] Therefore, studying the distribution and control of rail hardness is of great significance to improving rail performance. Reducing the hardness gradient inside the rail head can reduce the difference in results produced by hardness homogenization research. Even for materials with small gradient hardness, the research within a smaller area can be simplified to hardness uniformity, thereby achieving the purpose of simplifying the research. For steel materials, the uniformity of organizational properties is a very important quality indicator. A large gradient of organizational properties will greatly weaken the comprehensive mechanical properties of the material, thereby reducing the reliability of the material performance.
[0005] In the process of developing new high-performance steel products, scientists mainly control the mechanical properties through microstructure, among which alloying combined with heat treatment process control is a relatively conventional technical means. With the continuous improvement of steel performance requirements, the alloy content of steel is increasing, but when the alloy element content in steel increases to a certain level, its CCT curve changes, and the tendency of abnormal organization in the heat treatment process increases. It is particularly important to control segregation and accurately implement the heat treatment process.
[0006] A large number of scholars have conducted research on the segregation of steel and the organizational properties of steel materials, such as the control of segregation during steel solidification, research on heat treatment processes, analysis of the causes of incompatibility between hardness and organization, and the impact of hardness on other application properties. However, the coordinated control technology of the organizational properties of a high-alloy heavy rail steel has not yet been addressed.
[0007] Based on this, the existing technology still needs to be improved. Summary of the invention
[0008] The main purpose of the present invention is to provide a method for coordinated control of the microstructure and properties of heavy rail steel with high alloy content, so as to achieve coordinated control of steel microstructure and properties from continuous casting, insulation, rolling and heat treatment, and solve the technical problem of lack of overall coordinated control technology for steel microstructure and properties in the prior art.
[0009] The embodiment of the present invention provides a method for coordinated control of microstructure and properties of high alloy content heavy rail steel, comprising:
[0010] Control the precipitation, diffusion and convection transport of solute alloy elements during the solidification of molten steel in the continuous casting process;
[0011] The residual heat after the ingot is completely solidified is used to carry out high-temperature diffusion treatment under heat preservation conditions to obtain a highly homogenized ingot;
[0012] Rolling the highly homogenized ingot to obtain a rail;
[0013] The formed rails are subjected to a matching heat treatment process.
[0014] In some embodiments, controlling the precipitation, diffusion and convection transport of solute alloy elements during the solidification of molten steel inside the ingot during the continuous casting process includes:
[0015] The high superheated steel liquid in the middle layer is used to form a large temperature gradient in the cross section of the ingot under forced cooling, which promotes the rapid advancement of the solidification front vertically inward from the ingot surface;
[0016] Through secondary cooling electromagnetic stirring, the timing of nucleation of the molten steel in the molten pool inside the ingot is accurately controlled, the regional solute concentration gradient caused by convection is reduced, the free nucleation growth time is reduced, and the improvement of macro and semi-macro homogeneity is promoted.
[0017] In some embodiments, the high superheated molten steel is used to maintain the superheated molten steel at 35-45°C during the casting process.
[0018] In some embodiments, the secondary cooling water volume of the forced cooling is 0.36-41 L / kg steel.
[0019] In some embodiments, the crystallizer electromagnetic stirring is not provided, and a single intensity secondary cooling electromagnetic stirring is adopted.
[0020] In some embodiments, the stirring mode of the secondary cooling electromagnetic stirring is unidirectional continuous stirring, and the magnetic field strength at the center of the stirring coil is 260×10 -4 ~300×10 -4 T.
[0021] In some embodiments, the ingot entering end of the secondary cooling electromagnetic stirring is 4000 mm away from the liquid level of the crystallizer.
[0022] In some embodiments, utilizing the residual heat after the ingot is completely solidified to perform high temperature diffusion treatment under heat preservation conditions includes:
[0023] The shell temperature of the ingot after leaving the flame cutting is 900-1000℃, and the center temperature of the ingot is 1200-1300℃. After cutting, it is immediately put into the pit for insulation. The insulation duration is 4h. The temperature in the pit is 1000-1050℃ during the insulation period. After 4h of insulation, the heat source supply is stopped, and the residual heat insulation is carried out for 20h before leaving the pit.
[0024] In some embodiments, the heat treatment process for the formed rail includes: the formed rail is controlled by a gradient high-efficiency cooling and heat transfer heat treatment method.
[0025] In some embodiments, the gradient efficient cooling heat transfer heat treatment method includes:
[0026] The surface temperature of the rail before cooling is 740-750℃. The cooling is carried out in three stages. The first stage is cooled with a wind pressure of 16kPa. The second stage relies on the ground surface temperature obtained in the first stage and the large-section temperature gradient heat transfer combined with 12kPa wind pressure cooling. The third stage implements the second highest wind pressure cooling of 14.5-15kPa to ensure that the surface temperature after cooling is ≤500℃.
[0027] By adopting the above technical solution, the present invention has at least the following beneficial effects:
[0028] The method for coordinated control of the microstructure and properties of heavy rail steel with high alloy content provided by the present invention is aimed at coordinated control of the microstructure and properties of heavy rail steel, especially coordinated control of the cross-sectional hardness and microscopic phase change structure of the rail head of heavy rail steel with high alloy content, by controlling the precipitation, diffusion and convection transmission of solute alloy elements during the solidification process of molten steel inside the ingot during the continuous casting process, further coordinating with the use of residual heat after the ingot is completely solidified to perform heat preservation and high-temperature diffusion treatment, further rolling the highly homogenized ingot to obtain the rail, and further performing a matching heat treatment process on the formed rail, thereby achieving coordinated control of the microstructure and properties of the rail head of heavy rail steel with high alloy content, and providing a process technology for high-performance rail and high-quality production control. DETAILED DESCRIPTION
[0029] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in conjunction with specific embodiments.
[0030] It should be noted that all expressions using "first" and "second" in the embodiments of the present invention are for distinguishing two non-identical entities with the same name or non-identical parameters. It can be seen that "first" and "second" are only for the convenience of expression and should not be understood as limitations on the embodiments of the present invention. The subsequent embodiments will not explain this one by one.
[0031] Some embodiments of the present invention disclose a method for coordinated control of microstructure and properties of high alloy content heavy rail steel, comprising:
[0032] Control the precipitation, diffusion and convection of solute alloy elements during the solidification of molten steel in the continuous casting process. This may include:
[0033] The high superheated steel liquid in the middle layer is used to form a large temperature gradient in the cross section of the ingot under forced cooling, which promotes the rapid advancement of the solidification front vertically inward from the ingot surface;
[0034] Through the secondary cooling electromagnetic stirring, the timing of nucleation of the molten steel in the molten pool inside the ingot is accurately controlled, the regional solute concentration gradient caused by convection is reduced, the free fusion growth time is reduced, and the macro and semi-macro homogeneity is improved. The high superheated steel liquid in the package is to maintain the superheat of the steel liquid at 35-45°C during the casting process. The secondary cooling water volume of the forced cooling is 0.36-41L / kg steel. During the continuous casting process, the crystallizer electromagnetic stirring is not set, and only the single-intensity secondary cooling electromagnetic stirring is used. The stirring mode of the secondary cooling electromagnetic stirring is unidirectional continuous stirring, and the magnetic field strength at the center of the stirring coil is 260×10 -4 ~ 300×10 -4 T. The inlet end of the secondary cooling electromagnetic stirring is 4000 mm away from the liquid level of the crystallizer.
[0035] The residual heat after the ingot is completely solidified is used for high-temperature diffusion treatment under heat preservation conditions to obtain highly homogenized ingots. This may include:
[0036] The shell temperature of the ingot after leaving the flame cutting is 900-1000℃, and the center temperature of the ingot is 1200-1300℃. After cutting, it is immediately put into the pit for insulation. The insulation duration is 4h. The temperature in the pit is 1000-1050℃ during the insulation period. After 4h of insulation, the heat source supply is stopped, and the residual heat insulation is carried out for 20h before leaving the pit.
[0037] The highly homogenized ingot is rolled to obtain a rail.
[0038] The formed rails are subjected to a matching heat treatment process. This may include: the formed rails are controlled by a gradient high-efficiency cooling and heat transfer heat treatment method. The surface temperature of the rails before cooling is 740 to 750°C, and the cooling is carried out in three stages. The first stage is cooled by a wind pressure of 16kPa, the second stage relies on the ground surface temperature obtained in the first stage and the large-section temperature gradient heat transfer combined with 12kPa wind pressure cooling, and the third stage implements 14.5 to 15kPa of the second highest wind pressure cooling to ensure that the surface temperature after cooling is ≤500°C.
[0039] The method for coordinated control of the microstructure and properties of heavy rail steel with high alloy content disclosed in the embodiment of the present invention adopts a high superheated molten steel in a clad under strong secondary cooling to form a large temperature gradient on the cross section of the ingot, promotes the solidification front to advance rapidly inward perpendicular to the surface of the ingot, thereby improving the uniformity of the solidification microstructure and the homogeneity of the solute elements; cooperates with appropriate electromagnetic stirring regulation to accurately control the nucleation timing of the molten steel in the molten pool inside the ingot, reduce the regional solute concentration gradient generated by convection, reduce the growth time of free crystal nuclei, and promote the improvement of macro and semi-macro homogeneity; utilizes the residual heat after solidification of the highly homogeneous solidified ingot to carry out high-temperature diffusion under insulation conditions, and promotes the homogenization of short-range solute diffusion; gradient high-efficiency cooling and heat transfer heat treatment technology promotes efficient heat transfer in the target area, refines the grain structure, and stabilizes the high-performance control of the rail.
[0040] Example 1
[0041] This embodiment is a steel mill using the high alloy content heavy rail steel structure and performance coordinated control method of the present invention to continuously cast and produce 280mm×380mm cross-section high alloy heavy rail steel blooms, whose alloy content reaches 3.0% to 3.2%. The specific implementation of the technology of the present invention is:
[0042] (1) The continuous casting process uses an electromagnetic induction heating system for the tundish to maintain the superheat of the molten steel at 36-45°C during the casting process;
[0043] (2) The secondary cooling water volume of forced cooling is controlled at 0.36~38L / kg 钢 ;
[0044] (3) No crystallizer electromagnetic stirring, using a single intensity secondary cooling electromagnetic stirring control, stirring mode is unidirectional continuous stirring, stirring coil center magnetic field strength of 260 × 10 -4 T, the distance between the inlet end of the secondary cooling electromagnetic stirring and the liquid level of the crystallizer is 4000 mm;
[0045] (4) The shell temperature of the ingot after leaving the flame cutting is 900-1000℃, and the center temperature of the ingot is 1200-1300℃. After cutting, it is immediately put into the pit for insulation. The insulation duration is 4 hours. The temperature in the pit is 1000-1050℃ during the insulation period. After 4 hours of insulation, the heat source supply is stopped, and the residual heat is kept for 20 hours before leaving the pit.
[0046] (5) The casting is heated and rolled into shape by conventional processes;
[0047] (6) The formed rails are controlled by gradient high-efficiency cooling and heat transfer technology. The surface temperature of the rails before cooling is 740-750°C. The cooling is carried out in three stages. The first stage is cooled by 16 kPa wind pressure. The second stage relies on the ground surface temperature obtained in the first stage and the large-section temperature gradient heat transfer combined with 12 kPa wind pressure cooling. The third stage further implements 14.5-15 kPa of the second highest wind pressure cooling to ensure that the surface temperature after cooling is ≤500°C.
[0048] After the implementation of this technology, the hardness of the produced rails was tested on the iron standard A line (A1 to A4 with a distance of 5mm, 10mm, 15mm, and 20mm from the tread), and the microstructure identification of the 5mm×5mm area at each hardness test point of the rails was further performed. The results show that the hardness of the rails obtained in this embodiment is 4 to 8HRC higher than that of the conventional process at the same position point, and the results of further microstructure identification of the 5mm×5mm area at each hardness test point of the rails show that no abnormal tissue appears in each area of the rails.
[0049] Comparative Example
[0050] A domestic factory produces high-alloy heavy rail steel blooms with a super-large cross-section of 320mm×410mm, with an alloy content of 3.0%. The key process technologies implemented include: using secondary cooling electromagnetic stirring with a stirring magnetic field strength of 300×10 -4 ~350×10 -4 T; the superheat of the tundish casting molten steel is controlled at 40-45°C; the water volume of the continuous casting secondary cooling is 0.33-0.34L / kg 钢; Further, the reduction at the end of solidification was implemented and the total reduction was 10-12mm. After the cast billet was rolled into a rail, the produced rail was pickled and corroded. The rail had good low-power quality and no obvious dispersed segregation on the rail head; the rail was further tested for the hardness of the iron standard A line (A1-A4 with a distance of 5mm, 10mm, 15mm, and 20mm from the tread), and the microstructure of the 5mm×5mm area of each hardness test point of the rail was identified. The results show that the hardness of the obtained rail meets the standard requirements. The results of further microstructure identification of the 5mm×5mm area of each hardness test point of the rail show that obvious martensitic structure appears in the two areas of 15mm and 20mm from the tread, that is, the microstructure does not meet the standard requirements. After reducing the cooling intensity of the heat treatment process of the produced rail, the microstructure of each area of the rail is normal, all of which are pearlite structures, but the hardness value of the point 20mm away from the tread is lower than the standard lower limit, averaging 5.4HRC. That is, under the process conditions, the rails rolled from the resulting ingots cannot achieve coordinated control of their microstructure and properties.
[0051] Example 2
[0052] This embodiment is a steel mill using the method of the invention to continuously cast and produce a large square billet of high-alloy heavy rail steel with a cross-section of 280mm×380mm, the alloy content of which reaches 3.3% to 3.6%. The specific implementation of the technology of the present invention is:
[0053] (1) The continuous casting process uses an electromagnetic induction heating system for the tundish to maintain the superheat of the molten steel at 35-42°C during the casting process;
[0054] (2) The secondary cooling water volume of forced cooling is controlled at 0.38~41L / kg 钢 ;
[0055] (3) No crystallizer electromagnetic stirring, using a single intensity secondary cooling electromagnetic stirring control, the stirring mode is unidirectional continuous stirring, the magnetic field strength of the stirring coil center is 300×10 -4 T, the distance between the inlet end of the secondary cooling electromagnetic stirring and the liquid level of the crystallizer is 4000 mm;
[0056] (4) The shell temperature of the ingot after leaving the flame cutting is 900-1000℃, and the center temperature of the ingot is 1200-1300℃. After cutting, it is immediately put into the pit for insulation. The insulation duration is 4 hours. The temperature in the pit is 1000-1050℃ during the insulation period. After 4 hours of insulation, the heat source supply is stopped, and the residual heat is kept for 20 hours before leaving the pit.
[0057] (5) The casting is heated and rolled into shape by conventional processes;
[0058] (6) The formed rails are controlled by gradient high-efficiency cooling and heat transfer technology. The surface temperature of the rails before cooling is 740-750°C. The cooling is carried out in three stages. The first stage is cooled by 16 kPa wind pressure. The second stage relies on the ground surface temperature obtained in the first stage and the large-section temperature gradient heat transfer combined with 12 kPa wind pressure cooling. The third stage further implements 14.5-15 kPa of the second highest wind pressure cooling to ensure that the surface temperature after cooling is ≤500°C.
[0059] After the implementation of this technology, the hardness of the produced rails was tested on the iron standard A line (A1 to A4 with a distance of 5mm, 10mm, 15mm, and 20mm from the tread), and the microstructure identification of the 5mm×5mm area at each hardness test point of the rails was further performed. The results show that the hardness of the rails obtained in this embodiment is 7 to 10HRC higher than that of the conventional process at the same position point, and the microstructure identification of the 5mm×5mm area at each hardness test point of the rails shows that no abnormal structure appears in each area of the rails.
[0060] Example 3
[0061] This embodiment is a steel mill using the method of the invention to continuously cast and produce a large square billet of high-alloy heavy rail steel with a cross-section of 280mm×380mm, the alloy content of which reaches 3.8% to 4.0%. The specific implementation of the technology of the present invention is:
[0062] (1) The continuous casting process uses an electromagnetic induction heating system for the tundish to maintain the superheat of the molten steel at 39-45°C during the casting process;
[0063] (2) The secondary cooling water volume of forced cooling is controlled at 0.39~41L / kg 钢 ;
[0064] (3) No crystallizer electromagnetic stirring, using a single intensity secondary cooling electromagnetic stirring control, stirring mode is unidirectional continuous stirring, stirring coil center magnetic field strength of 285 × 10 -4 T, the distance between the inlet end of the secondary cooling electromagnetic stirring and the liquid level of the crystallizer is 4000 mm;
[0065] (4) The shell temperature of the ingot after leaving the flame cutting is 900-1000℃, and the center temperature of the ingot is 1200-1300℃. After cutting, it is immediately put into the pit for insulation. The insulation duration is 4 hours. The temperature in the pit is 1000-1050℃ during the insulation period. After 4 hours of insulation, the heat source supply is stopped, and the residual heat is kept for 20 hours before leaving the pit.
[0066] (5) The casting is heated and rolled into shape by conventional processes;
[0067] (6) The formed rails are controlled by gradient high-efficiency cooling and heat transfer technology. The surface temperature of the rails before cooling is 740-750°C. The cooling is carried out in three stages. The first stage is cooled by 16 kPa wind pressure. The second stage relies on the ground surface temperature obtained in the first stage and the large-section temperature gradient heat transfer combined with 12 kPa wind pressure cooling. The third stage further implements 14.5-15 kPa of the second highest wind pressure cooling to ensure that the surface temperature after cooling is ≤500°C.
[0068] After the implementation of this technology, the hardness of the produced rails was tested on the iron standard A line (A1-A4 with a distance of 5mm, 10mm, 15mm, and 20mm from the tread), and the microstructure identification of the 5mm×5mm area at each hardness test point of the rails was further performed. The results show that the hardness of the rails obtained in this embodiment is 10-15HRC higher than that of the conventional process at the same position point, and the microstructure identification of the 5mm×5mm area at each hardness test point of the rails shows that no abnormal structure appears in each area of the rails.
[0069] The above implementation examples show that after adopting this technical invention, the cross-sectional hardness of the high-alloy rail head produced is significantly improved, and the microstructure of the hardness test points of the obtained rails is normal. This technology provides important technical support for the research and development of high-alloy heavy rail steel and provides technical support for the coordinated control of the organizational properties of high-performance rails.
[0070] It should be particularly pointed out that the various components or steps in the above-mentioned embodiments can be cross-linked, replaced, added, or deleted with each other. Therefore, the combinations formed by these reasonable arrangements and combinations should also fall within the scope of protection of the present invention, and the scope of protection of the present invention should not be limited to the embodiments.
[0071] The above are exemplary embodiments disclosed in the present invention. The order disclosed in the above embodiments of the present invention is only for description and does not represent the advantages and disadvantages of the embodiments. However, it should be noted that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope disclosed in the embodiments of the present invention (including claims) is limited to these examples. Various changes and modifications may be made without departing from the scope defined in the claims. The functions, steps and / or actions of the method claims according to the disclosed embodiments described herein do not need to be performed in any particular order. In addition, although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.
[0072] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the embodiments of the present invention as described above, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.
Claims
1. A method for coordinated control of microstructure and properties of high alloy content heavy rail steel, characterized in that: include: Control the precipitation, diffusion and convection transport of solute alloy elements during the solidification of molten steel in the continuous casting process; The residual heat after the ingot is completely solidified is used to carry out high-temperature diffusion treatment under heat preservation conditions to obtain a highly homogenized ingot; Rolling the highly homogenized ingot to obtain a rail; Carry out matching heat treatment process on the formed rails; Control of the precipitation, diffusion and convection transport of solute alloy elements during the solidification of molten steel in the continuous casting process includes: The high superheated steel liquid in the middle layer is used to form a large temperature gradient in the cross section of the ingot under forced cooling, which promotes the rapid advancement of the solidification front vertically inward from the ingot surface; Through secondary cooling electromagnetic stirring, the timing of nucleation of the molten steel in the molten pool inside the ingot is precisely controlled, the regional solute concentration gradient caused by convection is reduced, the free nucleation growth time is reduced, and the macro and semi-macro homogeneity is improved; The high superheated steel liquid is used to maintain the superheated steel liquid at 35-45°C during the casting process; The secondary cooling water volume of the forced cooling is 0.36~41L / kg steel; The crystallizer electromagnetic stirring is not set, and the secondary cooling electromagnetic stirring with a single intensity is adopted; The stirring mode of the secondary cooling electromagnetic stirring is unidirectional continuous stirring, and the magnetic field strength at the center of the stirring coil is 260×10 -4 ~300×10 -4 T; The high temperature diffusion treatment under insulation conditions using the residual heat after the ingot is completely solidified includes: The shell temperature of the ingot after leaving the flame cutting is 900-1000℃, and the center temperature of the ingot is 1200-1300℃. After cutting, it is immediately put into the pit for insulation. The insulation duration is 4h. The temperature in the pit is 1000-1050℃ during the insulation period. After 4h of insulation, the heat source supply is stopped. The residual heat insulation is carried out for 20h before leaving the pit. The heat treatment process for the formed rail includes: the formed rail is controlled by a gradient high-efficiency cooling and heat transfer heat treatment method; Gradient efficient cooling heat transfer heat treatment methods include: The surface temperature of the rail before cooling is 740-750℃. The cooling is carried out in three stages. The first stage is cooled with a wind pressure of 16kPa. The second stage relies on the ground surface temperature obtained in the first stage and the large-section temperature gradient heat transfer combined with 12kPa wind pressure cooling. The third stage implements the second highest wind pressure cooling of 14.5-15kPa to ensure that the surface temperature after cooling is ≤500℃.
2. The method for coordinated control of microstructure and properties of high alloy heavy rail steel according to claim 1, characterized in that: The ingot entry end of the secondary cooling electromagnetic stirring is 4000mm away from the liquid level of the crystallizer.
Citation Information
Patent Citations
Turnout rail manufacturing method
CN104561497A
Production process for continuous casting and rolling of sheet steel
CN105033238A
Postweld heat treatment method of 136RE+SS heat treatment steel rail welding joint
CN107502730A
Method for controlling dispersing segregation of bloom heavy-rail steel
CN110216253A
Control method for synergistic improvement of homogeneity and compactness of ultra-large section heavy rail steel
CN110280732A