Method for cutting laminated glazing using a laser source
The method of cutting laminated assembly glass with a laser source solves the problems of hole misalignment and low manufacturing efficiency in laminated assembly glass, achieves high-precision, low-loss cutting, and improves production efficiency and stability.
Patent Information
- Application Number
- CN202280003366.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-03-28
AI Technical Summary
The existing method of forming holes in laminated glass has problems such as hole misalignment, low manufacturing efficiency, difficulty in obtaining good degassing, and safety risks and high costs in laser cutting.
The laser source is used to cut laminated glass. By detecting the inner contour, calculating the cutting path and using the laser source to cut, accurate holes are formed to avoid creep of the polymer material and release of harmful gases, and improve production efficiency and cutting quality.
High-precision, seamless cutting is achieved, reducing the risk of fragmentation and material loss, improving production efficiency and cutting quality, avoiding hole misalignment and polymer material creep, and significantly improving the manufacturing stability of laminated assembled glass.
Smart Images

Figure CN115500079B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for cutting laminated glazing, in particular for motor vehicles. Background Art
[0002] In particular in the field of motor vehicle glazing, there is a continuing need to be able to form one or more holes through the glazing, typically by drilling the glass, however the manner in which this need is achieved differs depending on whether it involves monolithic glazing or laminated glazing.
[0003] As a recap, monolithic glazing comprises a single glass sheet which is heated, for example, to a temperature of about 650° C. and then suddenly cooled with air in order to quench it, ie to thermally strengthen it, and at the same time, generally to give it the desired shape.
[0004] In contrast to such monolithic glazings, laminated glazings comprise an outer glass sheet and an inner glass sheet assembled together by an interlayer comprising at least one sheet of polymeric material, such as at least one sheet of polyvinyl butyral (PVB).
[0005] While drilling a hole(s) in monolithic glazing does not present any particular technical problems, this is not the case with laminated glazing, the use of which is increasing.
[0006] Indeed, motor vehicle manufacturers desire, in particular for certain classes of their vehicles, glazing that offers the best existing properties, such as, inter alia, sound attenuation qualities, resistance to vandalism theft, thermal insulation properties, in particular with respect to solar radiation (UV), and the like.
[0007] This is one of the reasons why laminated glazing is increasingly being sought in motor vehicles, particularly but not exclusively for side windows.
[0008] Although used more specifically as an application example in the following text, the case of side windows is by no means limited with respect to other types of glazing, such as windshields, rear windows or roof windows.
[0009] Laminated glazing also enables improved acoustic comfort compared to monolithic glazing by means of the absorption properties of the interlayer comprising at least one sheet of polymeric material, such as polyvinyl butyral (PVB), and also offers better resistance to vandalism theft and new properties, such as blocking UV radiation from the sun.
[0010] However, there are significant technical differences between monolithic glazing and laminated glazing which mean that the use of such laminated glazing is not without problems and which, for certain uses, have implications for the technical solutions that can be implemented to form holes in the glazing.
[0011] One of the differences is especially the mechanical properties such as strength, where laminated glazing does not have the same characteristics as monolithic glazing. In fact, the glass sheets that make up laminated glazing do not reach the stress levels of monolithic glazing, especially because the reduced thickness of these glass sheets does not allow them to generate sufficient thermal gradients when cooling that could generate the stresses required to obtain equivalent mechanical strength, especially bending strength.
[0012] Therefore, such laminated glazing is often also referred to by the term "hardened" or "semi-tempered" rather than the term "tempered" which is usually used for monolithic glazing.
[0013] For example, the use of laminated glazing as side windows does not in itself pose a safety problem, as long as the polymer sheet in the interlayer ensures cohesion of the assembly in the event of an accident, thereby avoiding the projection of glass fragments that could cause injury. Thus, in contrast to monolithic glazing, there is no need to achieve so-called "safe" shattering.
[0014] In contrast, in addition to their mechanical properties, laminated glazing also differs from monolithic glazing with regard to drilling possibilities.
[0015] In the case of side windows, this involves one or more holes, which are intended to be penetrated by fixing elements in order to ensure the connection between the glazing and a drive device accommodated in the vehicle door.
[0016] A side window comprising such a fixing hole enables the use of the same fixing elements as for the single-pane glazing, which is particularly advantageous for standardization of the fixing elements and, in particular, for interchangeability between two types of glazing on the same vehicle.
[0017] In the absence of fixing holes, it is known to connect side windows of laminated type to the drive device by means of fixings (also called "retainers"), which are fixed to the mounting glass by gluing according to a first type of connection, or by clamping (or clamping) according to a second type of connection, usually by means of two parts provided on both sides of the mounting glass and mounted to tighten the clamping.
[0018] Besides their own inherent disadvantages, both types of connection do not allow, in particular, interchangeability between monolithic glazing and laminated glazing.
[0019] In the case of other types of glazing, the rear window should, for example, have a hole for the passage of the windshield wiper shaft, and similarly the roof window will have at least one hole for mounting an antenna or a roof bar. The need to make holes in glass is thus by no means limited to fixed side windows, but rather relates more generally to all types of laminated glazing that can be mounted on a motor vehicle.
[0020] Compared to monolithic glazing, there are basically two possibilities for forming holes in laminated glazing, in particular in order to obtain through-holes.
[0021] A first possibility consists in first drilling the holes in each glass sheet and then assembling the glazing, while a second possibility consists in first assembling the glazing and then drilling the holes, ie drilling the holes when the two glass sheets are joined to one another by an intermediate layer.
[0022] Although it is common practice to drill holes in each glass sheet before assembling the glazing in order to obtain through-holes, for example in the case of side windows, for fixing, this first possibility is not without various problems.
[0023] When the holes are through-holes, the first problem is misalignment (or offset) between the holes of the two glass sheets, in particular due to different radii of curvature between the inner and outer surfaces of the glass sheets. Misalignment (also called "mismatch") results in the holes formed in each glass sheet of the glazing not being properly aligned with each other after the glazing is assembled.
[0024] Furthermore, this misalignment prevents the forces from being properly absorbed by each of the two glass sheets, thereby generating greater stresses therein and thus increasing the risk of breakage, especially in the event of contact between a mechanical part passing through the hole and the edge of the hole.
[0025] Furthermore, this misalignment is unsightly and is problematic especially when the edge of the hole is visible, but it can also sometimes make it difficult to incorporate the hole into mechanical parts whose adjustment tolerance is less than the offset between the two glass sheets.
[0026] However, these disadvantages are not limited to the effect on the laminated glazing obtained, since the manufacture of the glazing is also affected. In fact, the centering of the two glass sheets should be carried out more carefully in order to minimize the misalignment between the holes of the glass sheets, which then leads to a reduction in manufacturing efficiency.
[0027] Generally speaking, when the holes are formed in the interlayer before assembly, the manipulation of the interlayer to place it between the two glass sheets becomes more complicated, and special attention needs to be paid to align all the holes as much as possible, or if the holes are formed in the interlayer after assembly, special attention needs to be paid to not damage the holes provided in the glass sheets when the cutting tool passes through the glass sheets, and not to leave residual polymeric material.
[0028] In the absence of such holes in the interlayer prior to assembly, another problem is encountered due to the polymeric material of the interlayer creeping in the holes during autoclaving, necessitating time-consuming finishing operations to eliminate the creep.
[0029] Finally, it is difficult to obtain good degassing (or outgassing) when assembling the laminated glazing in the presence of holes in the glass sheets. For this reason, these holes are usually temporarily blocked, for example by attaching adhesive aluminum sheets, to avoid any air infiltration through the edges of the holes during degassing.
[0030] This therefore adds two additional operations, namely setting the adhesive and then removing it after the glazing is assembled, i.e. after applying a vacuum by peripheral sealing or by vacuum bagging followed by high temperatures (between 80 and 120°C), or after an autoclave operation.
[0031] Therefore, in any case, the first possibility consisting in drilling the holes first and then assembling the glazing may require at least one additional drilling operation (one for each glass sheet) than the second possibility consisting in assembling the laminated glazing first and then forming the holes.
[0032] In addition to the many disadvantages mentioned above, there is an additional problem when trying to drill holes in each glass sheet of a laminated glazing before assembly, because the drilling is usually done before it is formed and before the glass is strengthened. In fact, the thickness of the glass sheets of a laminated glazing is less than that of a single piece of glazing, making drilling holes in unstrengthened flat glass (i.e. 2D glass) technically difficult and leads to productivity losses.
[0033] Therefore, it is usually difficult to drill a hole having a diameter greater than 40 mm in a glass sheet having a thickness of 2.1 mm or a hole having a diameter greater than 16 mm in a glass sheet having a thickness of 1.6 mm.
[0034] The second possibility, which consists in first assembling the laminated glazing and then drilling the holes, also has various disadvantages.
[0035] In contrast to pre-assembly drilling, drilling of laminated glazing involves drilling holes into sheets of glass that have typically already been strengthened (usually chemically or thermally tempered).
[0036] Furthermore, when drilling is performed prior to assembly, the drilling is then performed on the laminated glazing in its final shape, which is typically a curved glass (in three dimensions or "3D") rather than a flat ("2D") glass sheet.
[0037] Drilling of the laminated glazing after assembly therefore proves to be more complicated to implement, in particular in order to ensure the geometry of the holes, in particular when the glazing is curved, for example having a ring shape.
[0038] In addition, conventional mechanical drilling of glass also has various disadvantages. One of the disadvantages is that the cutting quality depends on the tool, such as a diamond drill bit. In fact, these drill bits produce microscopic defects on the cut surface of the hole, resulting in points from which cracks can propagate under certain stresses.
[0039] The risk of crack propagation is particularly significant in cases where the side window glass includes fixing holes, as the glass assembly is subjected to repeated impacts, especially when the door is slammed hard. These stresses can then cause cracks to propagate from cutting defects such as micro-cracks or flaking fragments.
[0040] Additionally, drilling tools such as drill bits experience wear, which also results in a gradual decline in performance during the drilling process, necessitating the drill bit to be reground or replaced to maintain the cutting quality at the desired level.
[0041] In the case of laminated glazing, drilling can be done without breaking, but the mechanical strength of the glass will be weakened. The reason for this is the presence of tensile stresses in the glass, which exist in the mid-plane of each glass sheet of the glazing and originate from the cooling of the glass from both surfaces of each sheet.
[0042] When the hole is formed, these extension stresses change and decrease, but a residual extension persists at the edge of the hole, which then becomes an extreme brittle point of the glass, with a value, for example, half of what it had before drilling.
[0043] To remedy this problem, it has been proposed to carry out local contact cooling before drilling to produce compressive stresses in the area to be cut by means of a local cooling tool (for example an annular tool), the interior of which is air-cooled to prevent its temperature from rising during repeated contact with the hot glass.
[0044] For example, reference may be made to documents WO-2013 / 054059 or WO-2014 / 057200 for more details on implementation examples of this solution.
[0045] However, such localized cooling of the glass requires that the glass be stopped in order to locally apply a cooling tool in contact with the glass surface for a few seconds, thereby changing the temperature gradient across the thickness of the glass.
[0046] This solution cannot therefore be implemented when the manufacturing method is a continuous process that never stops the glass sheet, which is usually the case with the so-called “BT” (“Bombage Transvere”, transverse bending) manufacturing method, which is used in particular for the manufacture of side windows.
[0047] For more information on the “BT” manufacturing method and installation, reference is made, for example, to the following documents FR2204992; FR2642419, FR2549465 and FR2862056, which describe this manufacturing method and more particularly a glass sheet bending tool, especially a roller forming such a tool.
[0048] If it is envisaged that the holes in the laminated glazing are formed solely by mechanical drilling, advantageously after local cooling of the glass in the area to be drilled, a further solution is proposed which combines such mechanical drilling with the use of a laser source.
[0049] Document CN 104326649 A discloses a method for cutting a hole in a laminated glazing comprising an interlayer having a low hardness, an upper glass sheet and a lower glass sheet.
[0050] The glass sheets are quenched and have a higher hardness relative to the hardness of the interlayer. It is proposed to make a first guided cut by a laser beam on the surface of the upper glass sheet and then on the surface of the lower glass sheet to form a first groove and a second groove respectively. After the grooves are formed, a milling operation is performed to obtain a hole through the laminated glazing.
[0051] As previously reviewed, laminated glazing comprises an interlayer of polymeric material between a first sheet of glass and a second sheet of glass, the interlayer typically comprising polyvinyl butyral, better known by its acronym PVB.
[0052] However, polyvinyl butyral produces a gaseous release of a chemical agent called "CMR" during heating which causes it to burn, "CMR" being an acronym meaning "carcinogenic, mutagenic, toxic for reproduction".
[0053] It is therefore not possible to cut polyvinyl butyral with a laser source, as this would necessarily lead to combustion of the polymeric material, thereby releasing hazardous gases. Therefore, for obvious safety reasons and to preserve the health of the operators, technicians know that laser sources cannot be used to drill holes in laminated glazing.
[0054] According to this state of the art, the method therefore uses a laser source in a first step only for guided cutting of the glass with the laser source and in a second step, the glass and polyvinyl butyral are removed by mechanical drilling, thus eliminating any risk of releasing hazardous gases.
[0055] This method is therefore particularly expensive to implement since it requires additional production devices, namely a laser source on the one hand and a mechanical drilling device on the other hand.
[0056] The implementation of this method also requires more time, which is incompatible with the desired industrial production efficiency.
[0057] Furthermore, the above-mentioned disadvantages associated with the mechanical drilling performed in this second step still exist, in particular the sensitivity to wear and the resulting cut quality and the resulting risk of cracks.
[0058] Furthermore, the hole geometry is still limited by the tool used to drill the hole, namely to a circular shape.
[0059] It is therefore clear from the above that no prior art solution is currently satisfactory, whether for drilling glass before or after assembling the laminated glazing.
[0060] The object of the present invention is therefore in particular to overcome the disadvantages of the prior art by proposing a method for cutting laminated glazing by means of a laser source which is more reliable and quicker to perform than the methods proposed in the prior art. Summary of the invention
[0061] To this end, the invention proposes a method for cutting laminated glazing, in particular for motor vehicles, comprising at least a first glass sheet and a second glass sheet assembled together by an interlayer comprising at least one sheet of polymeric material, the glazing also comprising an insert having a hole delimited by an inner contour, the insert being housed in a hollow provided in the interlayer, the method comprising the following steps:
[0062] - a detection step of detecting the inner contour by means of a visual device;
[0063] - a calculation step of calculating the cutting path to be followed according to the detection of said inner contour;
[0064] - A cutting step of cutting the first glass sheet according to the calculated cutting path by means of a laser source having a beam.
[0065] Advantageously, the method according to the invention provides for making at least one cut in the laminated glazing, i.e. in the laminated glazing obtained after assembling the first and second glass sheets by means of the interlayer, such laminated glazing then forming a single assembly of glass sheets joined together.
[0066] Preferably, the laminated glazing is a motor vehicle glazing, such as a side window intended to be slidably mounted in a motor vehicle door. The cut made in the laminated glazing is then, for example, at least one hole, such as a fixing hole in the case of a side window.
[0067] However, such side window glass is only one non-limiting example of a motor vehicle glazing for which cuts, particularly but not exclusively holes, are sought. Although this may vary depending on the vehicle, the side window glass typically includes two fixing holes, and since vehicles typically have four side windows, this makes it a particularly advantageous application example for the cutting method according to the invention.
[0068] According to another application example, the laminated glazing may also be a rear window of a vehicle, wherein the hole is intended to enable the installation of a windshield wiper, usually through which a shaft for the windshield wiper connected to a drive device passes.
[0069] According to another application example, the laminated glazing may be a ceiling (or a roof) in which one or more cutouts are intended for mounting antennas or roof poles.
[0070] Advantageously, the glass of the laminated glazing is cut after assembly and not before assembly, ie in the nearly finished product state, especially in the case of motor vehicle glazing.
[0071] Therefore, the testing step of the method is preceded by an assembly of the laminated glazing, for example a step of clamping the glazing by means of holding devices, such as clamps, or a rolling step and a typical autoclave step.
[0072] Advantageously, the cutting method according to the invention makes it possible to make one or more cuts in the laminated glazing with complete freedom as to the shape of the cut, which may also be circular, typically a hole, but which may of course also be non-circular.
[0073] Advantageously, the cutting method according to the invention makes it possible to make at least one cut in the laminated glazing with extremely high precision. The method according to the invention makes it possible in particular to obtain excellent coaxiality with the aid of inserts drilled with holes, for example, and the precision of the laser, and this is independent of the cut made in the laminated glazing, in particular whether it is a blind hole or a through hole.
[0074] Cutting accuracy, like for example the coaxiality of one or more fixing holes for a side window pane, is particularly critical for the quality of the laminated glazing, since it helps to significantly reduce the risk of chipping in the glazing area comprising the cut, in particular micro-cracks present in the glass due to said cut.
[0075] Furthermore, compared to the prior art, the coaxiality defects encountered until now are remedied, in particular in the case of side windows, either in the case of drilling the glass sheets and then assembling the laminated glazing, where misalignment (or "mismatch") problems arise during assembly, or in the case of assembling and then drilling each glass sheet, since misalignment problems between the axes of the holes formed in each sheet always exist and accumulate with the uncertainties in the precision of the mechanical drilling.
[0076] According to a particularly advantageous feature, the insert in the laminated glazing is not visible, whatever the vehicle glazing. In the case of the side windows, the part including the fixing holes is located inside the door (i.e. below the visibility limit of the glazing) and is therefore never visible. However, in the case of the roof or rear window, the insert may also be not visible because, for example, it is covered by an added component (such as an antenna) or part of the wiper, or is concealed by the glazing glazing.
[0077] According to an important feature, the insert is housed in a hollow (or cutout) provided in the intermediate layer, by means of which there is no polymeric material around the hole of the insert, i.e. at least in the portion of the glazing where the cutting is carried out, thus completely eliminating the risk of gas release of the CRM chemical agent.
[0078] The present invention therefore runs counter to the technical prejudice of a person skilled in the art, for whom the presence of an intermediate layer of polymeric material precludes the use of a laser source, in particular for the formation of holes through laminated glazing.
[0079] Advantageously, cutting according to the invention with the aid of a laser source ensures a stable cutting quality during the production of laminated glazings, in particular in comparison with mechanical drilling, the cutting quality with a laser is not affected by wear over time like the tool.
[0080] Furthermore, the laser cutting method enables clean cut edges to be obtained with little to no debris and also eliminates the need for a subsequent polishing step, which is usually required after mechanical drilling.
[0081] Compared to mechanical drilling, laser cutting is carried out at a distance and "contactlessly", since only the beam from the laser source comes into contact with the glass sheet.
[0082] Advantageously, the laser cutting method according to the invention enables minimal material loss compared to mechanical drilling (eg with a diamond drill bit with a cutting width approaching 1 mm).
[0083] Advantageously, the laser source used in the cutting step of the method according to the invention can also be used to perform other operations, such as beveling or ablation of a coating (or paint) on a laminated glazing.
[0084] Thus, by using the laser source for a variety of operations other than just cutting, production costs are further improved.
[0085] Advantageously, the power of the laser source can be adjusted depending on the operation, for example low power for ablation and then higher power for cutting.
[0086] Preferably, in the calculation step, a shrinkage of between 0.1 mm and 1 mm, or between 0.5 mm and 1 mm, relative to the inner contour is calculated so that the beam does not touch the insert in the cutting step.
[0087] Advantageously, in the cutting step, the second glass sheet is also cut according to the calculated cutting path by means of the laser source.
[0088] Preferably, the cutting method further comprises a step of beveling by means of said laser source, comprising making at least one beveling on the edge of the hole of said first glass sheet resulting from the cutting step.
[0089] Preferably, the cutting method further comprises a step of performing a bevel cut by means of the laser source, performing at least one bevel cut on an edge of the first glass sheet and / or on an edge of the second glass sheet of the through hole produced by the cutting step.
[0090] Advantageously, the beveling step and the cutting step are performed with one and the same laser source, thereby reducing costs and production time, in particular with respect to the prior art, in which each of these steps is performed with a different tool.
[0091] Advantageously, the method according to the invention beveling the edges of a cut, such as a hole, made in at least one glass sheet makes it possible to reduce the risk of chipping.
[0092] Preferably, the method further comprises an additional cutting step of additionally cutting the second glass sheet according to the calculated cutting path by means of an additional laser source having a beam.
[0093] Preferably, the cutting step and the additional cutting step are performed simultaneously.
[0094] Preferably, the cutting step and the additional cutting step are performed successively, for example here the cutting step is performed first and then the additional cutting step.
[0095] Advantageously, the glazing cutting is carried out without one or more of the glass sheets being subjected to local cooling in the zone to be cut, as a variant, local cooling being carried out on at least one or both of the glass sheets of the glazing.
[0096] The invention also relates to a laminated glazing comprising at least one cut obtained by the method according to the invention, whereby the glazing comprises at least one hole in a first glass sheet or at least one through-hole through the first and second glass sheets, which through-hole is coaxial with the hole of the insert.
[0097] Advantageously, the roughness of the cut is less than 3 μm, preferably less than 2 μm, more preferably less than 1 μm.
[0098] In contrast, the roughness obtained by mechanical drilling is typically around 1.5 to 2 μm, so cutting with the aid of a laser source makes it possible to significantly reduce microscopic defects such as "flaking chips" that increase the risk of glass breakage, especially cracks in the glazing area that includes the cut.
[0099] Advantageously, at least one of the glass sheets is heat strengthened, preferably the first glass sheet and the second glass sheet are heat strengthened, preferably the heat strengthening is of the semi-quenching or hardening type, or annealing.
[0100] In practice, thermal strengthening of at least one glass sheet of the glazing, or advantageously of both glass sheets, is an operation performed prior to the assembly of the laminated glazing, so that, during the implementation of the laser cutting method according to the invention, each glass sheet has a hardness determined by the thermal strengthening applied, so as to compress the outer layers of glass and thus increase their mechanical strength.
[0101] Preferably, the first glass sheet and the second glass sheet have the same composition, in particular a composition of the soda-lime, aluminosilicate, borosilicate type. As a variant, the first glass sheet and the second glass sheet have different compositions.
[0102] According to one example, the first glass sheet and the second glass sheet have the same thickness so as to form a symmetrical laminated glazing, and the thickness of the glass sheets is between 0.7 mm and 3 mm, preferably between 1.1 mm and 2.6 mm.
[0103] According to another example, the first glass sheet and the second glass sheet have different thicknesses to form an asymmetric laminated glazing, the first glass sheet having a thickness between 1.5 mm and 3.5 mm and the second glass sheet having a thickness between 0.4 mm and 2.6 mm, preferably between 0.7 mm and 1.6 mm.
[0104] Preferably, the first glass sheet and the second glass sheet have the same hue, in particular clear glass, green glass or dark (or grey) glass. As a variant, the first glass sheet and the second glass sheet have different hues.
[0105] According to other characteristics, the subject of the invention is also a data processing system comprising a processor configured to implement the steps of the method according to the invention.
[0106] The invention also relates to a computer program-type product comprising at least one sequence of instructions stored and readable by a processor which, after being read by the processor, causes the execution of the steps of the method according to the invention.
[0107] The subject of the invention is also a computer-readable medium comprising said computer program product. BRIEF DESCRIPTION OF THE DRAWINGS
[0108] Several embodiments of the present invention will now be described by way of non-limiting examples with reference to the accompanying drawings, in which:
[0109] Figure 1 schematically shows a cross-sectional view of a laminated glazing according to a first configuration before carrying out the cutting method according to the invention;
[0110] Figure 2 schematically shows a cross-sectional view of a laminated glazing according to a second configuration before the cutting method according to the invention is carried out;
[0111] Figure 3 Schematically shows the inspection step of the method according to the invention, using a vision system such as a camera to inspect the inner contour of a hole of an insert incorporated in a laminated glazing according to a first configuration;
[0112] Figure 4 schematically illustrates a cutting step of a method according to the invention, using a device comprising a laser source to cut a glass sheet of a laminated glazing according to a first configuration;
[0113] Figure 5 schematically shows a cross-sectional view of a laminated glazing according to said first configuration, comprising a cavity obtained by the cutting method according to the invention;
[0114] Figure 6 schematically illustrates a cutting step of a laminated glazing according to a first configuration, using two devices, each device comprising a laser source;
[0115] Figure 7 schematically shows a laminated glazing according to a first configuration, comprising a through hole obtained by the cutting method according to the invention;
[0116] Figure 8 Schematically shows a side view of a side laminated glazing comprising two fixing holes obtained using the method according to the invention;
[0117] Fig. 9 The steps of the laminated glazing cutting method according to the present invention are schematically shown, namely, at least a detection step, a calculation step and a cutting step, or an additional cutting step (dashed line). DETAILED DESCRIPTION
[0118] refer to Figure 1 , which schematically shows a laminated glazing 10 according to a first configuration in a side view, comprising a first glass sheet 20 , a second glass sheet 30 and an interlayer 40 .
[0119] The laminated glazing 10 according to the invention will be described, as a non-limiting example, in the context of use as a side window glazing. As a variant, the laminated glazing 10 is a windshield, a rear window or a roof.
[0120] The first glass sheet 20 includes an outer surface 22 and an inner surface 24 , and the second glass sheet 30 includes an outer surface 32 and an inner surface 34 .
[0121] Preferably, the intermediate layer 40 comprises a single sheet of polymeric material. Preferably, the intermediate layer 40 is a sheet of polyvinyl butyral (PVB). As a variant, the intermediate layer 40 is a multilayer structure, ie consists of more than one sheet.
[0122] The intermediate layer 40 comprises, for example, two sheets of polymeric material, for example a first sheet and a second sheet of polyvinyl butyral (PVB), one of which advantageously has sound attenuating properties. Such a multilayer structure forming the intermediate layer 40 is also referred to by the term "double layer".
[0123] As a variant, the intermediate layer 40 may comprise an arrangement of two sheets and, for example, be composed of three sheets of polymeric material or a “trilayer”, comprising a sheet of polyethylene terephthalate (PET) arranged between two sheets of polyvinyl butyral (PVB), one of which advantageously has sound attenuation properties, or a sheet of polyvinyl butyral (PVB) advantageously having sound attenuation properties arranged between two sheets of polyvinyl butyral (PVB).
[0124] In this first configuration of the glazing 10 as a side window pane, the first glass sheet 20 and the second glass sheet 30 have a curved shape. Alternatively, the first glass sheet 20 and the second glass sheet 30 have a flat shape.
[0125] Preferably, the first and second glass sheets 20, 30 are thermally strengthened, in particular semi-tempered or hardened. In an alternative, they are chemically tempered.
[0126] The first glass sheet 20 and the second glass sheet 30 each have a thickness e 20 and thickness e 30 .
[0127] Preferably, the thickness e 20 and thickness e 30 In an alternative embodiment, the thickness e 20 Less than thickness e 30 In another alternative, the thickness e 20 Greater than thickness e 30 .
[0128] The intermediate layer 40 has a thickness e 40 , preferably between 0.3 mm and 1.2 mm, and the intermediate layer 40 comprises a hollowed-out portion 41, i.e. a cut, which preferably has a cylindrical shape and an inner contour 42. In an alternative, the hollowed-out portion 41 has a shape different from a cylindrical shape, such as a square, a rectangle, an ellipse or an oval. The hollowed-out portion 41 is formed before assembling the glazing 10.
[0129] The glazing 10 also comprises an insert 50 housed in a cutout 41 provided in the intermediate layer 40 , said cutout 41 advantageously having a shape complementary to that of the insert 50 .
[0130] Preferably, the insert 50 is in direct contact with the inner surface 24 of the first glass sheet 20 and the inner surface 34 of the second glass sheet 30. Thus, the insert 50 is inserted between the first glass sheet 20 and the second glass sheet 30.
[0131] The insert 50 comprises at least one hole 51. Preferably, the hole 51 is cylindrical. Alternatively, the hole 51 has a square, rectangular, elliptical or oval shape.
[0132] In yet another alternative, the hole 51 has a first cylindrical shape having a first diameter and a second cylindrical shape having a second diameter, the first diameter being greater than the second diameter.
[0133] Therefore, the hole 51 is not limited to the various shapes mentioned, but on the contrary, the hole 51 is limited to any shape obtainable by means of a device equipped with a laser source, which shapes are not exhaustively described in this description.
[0134] The insert 50 has an outer contour 52 and an inner contour 53, which is delimited by the hole 51 of the insert. The inner contour 53 thus has a shape corresponding to the shape of the hole 51, ie here circular.
[0135] The hardness of the insert 50 is greater than the hardness of the intermediate layer 40 . The Shore hardness D of the material of the insert is, for example, between 70 and 90.
[0136] like Figure 1 As shown, the insert 50 has an annular shape, for example here the shape of a circular disc or a flat ring.
[0137] Preferably, the outer diameter of the insert 50 is between 10 mm and 30 mm, or between 15 mm and 25 mm.
[0138] The thickness of the insert 50 is equal to ±10% of the thickness of the intermediate layer 40 , preferably equal to ±5% of the thickness of the intermediate layer 40 , and more preferably equal to ±2% of the thickness of the intermediate layer 40 .
[0139] The inner contour 42 of the hollowed-out portion 41 and the outer contour 52 of the insert 50 are advantageously complementary, so that at least a portion (here the entirety) of the insert 50 is in contact with the intermediate layer 40 .
[0140] By virtue of the hollowed-out portion 41 in the intermediate layer 40 , there is polymer material only around the insert 50 , along its inner contour 42 , while no polymer material is present at the hole 51 of the insert 50 .
[0141] Advantageously, insert 50 makes it possible to form a spacer capable of limiting creep of the polymer material of interlayer 40 , in particular during assembly of glazing 10 , which is usually carried out in an autoclave at a temperature of about 140° C., or subsequently due to the clamping forces exerted by the fixings.
[0142] In contrast, the material of the insert 50 is selected such that it does not creep at temperatures below 140°C.
[0143] Advantageously, the insert 50 is made of a plastic material, in particular polyamide (PA), for example PA 6-6, polyoxymethylene (POM) (also known as polymethylaldehyde or polyacetal), polybutylene terephthalate (PBT) or polyethylene terephthalate (PE).
[0144] Preferably, the interlayer 40 and the insert 50 are two separate elements independent of each other. In an alternative, the insert 50 is connected to the interlayer 40, for example by means of an adhesive tape or any other equivalent means, so that the insert 50 and the interlayer 40 form a single assembly, by means of which it is facilitated to be placed between the first glass sheet 20 and the second glass sheet 30 during assembly.
[0145] Reference now Figure 2 , which schematically shows a laminated glazing 100 according to a second configuration in a side view, comprising a first glass sheet 120 , a second glass sheet 130 and an interlayer 140 .
[0146] Next, we will compare the Figure 1 The laminated glazing 10 of the first configuration shown in FIG. Figure 2 The second configuration of the laminated glazing 100 makes the previously disclosed embodiment variants and other examples applicable to the laminated glazing 100 mutatis mutandis.
[0147] The first glass sheet 120 includes an outer surface 122 and an inner surface 124 , and the second glass sheet 130 includes an outer surface 132 and an inner surface 134 .
[0148] Preferably, the interlayer 140 comprises a single sheet of polymeric material, for example a sheet of polyvinyl butyral. As a variant, the interlayer 140 is a multilayer structure, i.e. composed of more than one sheet, in particular two sheets ("double-layer") or three sheets ("triple-layer"), as described above with respect to the laminated glazing 10.
[0149] The first glass sheet 120 and the second glass sheet 130 of the laminated glazing 100 have a curved shape, which forms a side window similar to the laminated glazing 10 according to the first configuration.
[0150] Alternatively, the first glass sheet 120 and the second glass sheet 130 have a planar shape. Preferably, the first and second glass sheets 120, 130 are thermally strengthened, in particular semi-tempered or hardened. In an alternative, they are chemically tempered.
[0151] The first and second glass sheets 120, 130 have a thickness e 120 and thickness e 130 Preferably, the thickness e 120 and thickness e 130 Basically equal.
[0152] In an alternative embodiment, the thickness e 120 Less than thickness e 130 .
[0153] In another alternative, the thickness e 120 Greater than thickness e 130 The intermediate layer 140 has a thickness e 140 , preferably between 0.3 mm and 1.2 mm.
[0154] The glazing 100 also comprises an insert 150 which is housed in a recess provided in the intermediate layer 140 and which advantageously has a complementary shape.
[0155] The insert 150 comprises at least one hole 151. The insert 150 has an outer contour 152 and an inner contour 153 which delimits the hole 151.
[0156] In this second configuration, the insert 150 is in contact with the intermediate layer 140 only over a portion of its outer contour 152 .
[0157] Contrary to the first configuration in which the hollow portion 41 is a closed shape that accommodates the insert 50 inside, the hollow portion provided in the intermediate layer 140 is here a shape that is open toward the end direction of the glass sheets 120 , 130 .
[0158] Therefore, if Figure 2 As shown, a portion of the insert 150 (the portion not in contact with the interlayer 140 ) is flush with the first and second glass sheets 120 , 130 .
[0159] The insert 150 is generally in the shape of a plate, and its outer periphery 152 may have different geometric shapes, such as a square or a rectangle, preferably a trapezoid.
[0160] Preferably, the hole 151 is cylindrical. As a variant, the hole 151 has any other geometric shape, such as square, rectangular, elliptical or oval. Therefore, the hole 151 is not limited to the various shapes mentioned, but on the contrary, the hole 151 is limited to any shape that can be obtained by means of a device equipped with a laser source, which shapes are not exhaustively described in this description.
[0161] The hardness of the insert 150 is greater than the hardness of the intermediate layer 140 , and the Shore hardness D of the insert material is, for example, between 70 and 90.
[0162] The thickness of the insert 150 is equal to ±10% of the thickness of the intermediate layer 140 , preferably equal to ±5% of the thickness of the intermediate layer 140 , and more preferably equal to ±2% of the thickness of the intermediate layer 140 .
[0163] Advantageously, the insert 150 can form a spacer capable of limiting creep of the polymer material of the intermediate layer 140 , in particular during assembly of the glazing 10 or subsequently due to clamping forces exerted by fixings.
[0164] Advantageously, insert 150 is made of a plastic material, such as those described above with respect to insert 50 .
[0165] Preferably, the insert 150 and the intermediate layer 140 are separate. In an alternative embodiment, the insert 150 is integrally connected with the intermediate layer 140, that is, the insert 150 and the intermediate layer 140 form a single assembly.
[0166] International application PCT / FR2021 / 050485 (not published), filed on March 25, 2020, claiming priority from French application FR2002921, described and presents other embodiments of laminated glazings comprising such an insert and other advantages, and reference will therefore be made advantageously for more details.
[0167] In the following description of the method according to the present invention, reference is made to Figure 1 The laminated glazing 10 according to the first configuration is shown. The method is described for Figure 2 The second configuration of the laminated glazing 100 shown is also effective.
[0168] Fig. 9 The various steps of the cutting method according to the present invention are schematically shown, and the dotted lines correspond to optional steps.
[0169] refer to Figure 3 , which schematically shows the first step of the method according to the invention, namely the detection step 201. In this step, the visual device 300 checks the glazing 10 in order to detect the inner contour 53 of the hole 51 of the insert 50, here shown through the second glass sheet 30, preferably through the first glass sheet 20 in the following description. Of course, the detection step 201 can also be performed through one and / or the other of the glass sheets 20, 30.
[0170] Preferably, the vision device 300 is a "smart" camera equipped with electronics that enable the capture, storage and processing of images. Such a camera is known in the field of industrial vision. It is called "smart" because it combines inside it the usual functions of a computer, but in a more compact way. It comprises in particular a digital sensor of the CCD or CMOS type, a processor and a memory.
[0171] Preferably, the vision device 300 communicates in particular with a manipulating member such as a robotic manipulator arm (not shown). Alternatively, the vision device 300 comprises a laser sighting system or an optical transceiver system with a reflector. These systems are also known.
[0172] The vision device 300 detects the inner contour 53 of the hole 51 of the insert 50. In the second step of the method according to the invention, the calculation step 202, the path to be traveled for cutting the glass sheets 20, 30 is determined with the aid of the image acquired in the detection step 201. The vision device 300 sends the inner contour 53 of the hole 51 of the insert 50 to the operating member (not shown) of the laser source 401, and therefore the path to be traveled by the operating member in the next step.
[0173] In the third step of the method according to the present invention, i.e., the cutting step 203, the laser source 401 is caused to emit a beam 402, such as Figure 4 Preferably, the laser source 401 is manipulated by a robot manipulator arm (not shown).
[0174] Preferably, the laser source 401 is a nanosecond laser with a length of 532 nm, a pulse period between 10 ns and 20 ns, a frequency of 60 kHz, and a power of 12 W. Alternatively, the laser source 401 is a picosecond laser or a femtosecond laser.
[0175] In the cutting step 203, the first glass sheet 20 is cut along the path calculated in the calculating step 202. After the cutting step 203, the first glass sheet 20 then includes the hole 21, such as Figure 5 As shown, and glass fragments are generated.
[0176] Advantageously, the roughness of the holes 21 obtained by laser cutting is less than 3 μm, preferably less than 2 μm, more preferably less than 1 μm.
[0177] Advantageously, the path calculated in calculation step 202 takes into account the contraction relative to the inner contour 53 of the hole 51 of the insert 50 , so that the beam 402 emitted by the laser source 401 does not hit the insert 50 .
[0178] Preferably, the shrinkage is between 0.1 mm and 1 mm, or between 0.5 mm and 1 mm.Therefore, only the first glass sheet 20 is cut.
[0179] Optionally, in a finishing step 204 , a laser source 401 is used to chamfer the edge 25 of the hole 21 in order to eliminate sharp edges or to form a taper, thereby facilitating the subsequent introduction of components such as sensors.
[0180] By applying the method according to the invention, until the cutting step 203 or until the finishing step 204 , only one cutout is formed, which forms a cavity 11 in the glazing 10 in order to accommodate a device such as a sensor (for example a capacitive sensor or an IR sensor), or a light diffuser or a LiDAR.
[0181] When the expectation is to obtain Figure 7 When the glazing 10 including the through hole 21 ′ is shown, the cutting step 203 is modified.
[0182] In the modified cutting step 203 , the laser source 401 is caused to emit a beam 402 having the same characteristics as in the cutting step 203 .
[0183] First, the first glass sheet 20 is cut along the path calculated in the calculation step 202 , and then the beam 402 is refocused, for example within a few tenths of a second, and then the second glass sheet 30 is cut along the path calculated in the calculation step 202 .
[0184] Preferably, in the modified cutting step 203, the laser source 401 is always on the side of the first glass sheet 20. Optionally, in the finishing step 204, the laser source 401 is used to form a chamfer on the edges 25a, 25b of the hole 21' to eliminate sharp edges or form a taper to facilitate the subsequent introduction of components.
[0185] Alternatively, when it is desired to obtain a glazing 10 including a through hole 21 ′, Figure 7 As shown, the method according to the invention comprises an additional cutting step 203'.
[0186] In the additional cutting step 203', as Figure 6 As shown, the cutting step 203 is applied as follows: a first laser source 401a disposed on the side of the first glass sheet 20 is used to emit a beam 402a having the same characteristics as mentioned above for the cutting step 203, and a second laser source 401b disposed on the side of the second glass sheet 30 is used to emit a beam 402b having the same characteristics as mentioned above for the cutting step 203.
[0187] Preferably, the first laser source 401a and the second laser source 401b are activated simultaneously to reduce the cutting time. Alternatively, either the first laser source 401a is activated first and then the second laser source 401b is activated, or the second laser source 401b is activated first and then the first laser source 401a is activated.
[0188] Optionally, in a finishing step 204 , a chamfer is produced on edge 25a of hole 21 ′ with laser source 401a and another chamfer is produced on edge 25b of hole 21 ′ with laser source 401b in order to eliminate sharp edges or form a taper to facilitate the subsequent introduction of components.
[0189] The method according to the invention makes it possible to obtain very small or even no alignment defects between the holes present in the first glass sheet 20 , the holes present in the second glass sheet 30 and the holes 51 of the insert 50 .
[0190] Advantageously, the laminated glazing 10 , 100 comprises a hole 21 in the first glass sheet 20 , 120 or a through hole 21 ′ through the first glass sheet 20 , 120 and the second glass sheet 30 , 130 , coaxial with said hole 51 , 151 of the insert 50 , 150 .
[0191] Thus, the shafts of the fixings passing through the glazing 10 do not damage the glass sheets due to the better distribution of forces. Compared to laminated glazings having alignment defects at the fixing holes, such glazing 10 has increased robustness.
[0192] During the cutting step, glass chips are formed and are advantageously removed, for example, by gravity or reduced pressure.
[0193] The method according to the invention may be implemented by a data processing system, such as a computer integrated into the vision device 300 .
[0194] Furthermore, the present invention may implement an algorithm, also referred to as a computer program product, comprising a sequence of instructions stored and readable by a processor (e.g. a processor of a computer integrated into the visual device 300) which, after being read by the processor, causes the execution of the steps of the method according to the present invention.
[0195] A computer (eg, a computer integrated into the vision device 300) readable medium may include the algorithm.
[0196] Reference now Figure 8 , schematically shows a laminated glazing 80 forming a side window of a motor vehicle, the laminated glazing 80 comprising a first hole 81 a and a second hole 81 b obtained by the method according to the invention.
[0197] The laminated glazing 80 comprises a so-called visible region 82 and a so-called non-visible region 84 which extend on both sides of a visibility limit LV of the glazing, the non-visible region 84 corresponding to the lower part of the glazing which is permanently concealed in the vehicle door.
[0198] To illustrate the visibility limit LV, this limit is shown in dotted lines. The visibility limit LV generally corresponds to a glass sealing strip mounted integrally with the vehicle door, said glass sealing strip being arranged to cooperate with the laminated glazing 80, in particular when said glazing 80 slides relative to the vehicle door.
[0199] The laminated glass 80 includes at least one fixing portion 86 in the non-visible area 84 below the visibility limit LV, the fixing portion 86 including a first fixing hole 81a and a second fixing hole 81b for accommodating a fixing member for fixing the glass 80 to a driving device (not shown) of the glass 80 .
[0200] The fixing between the glazing 80 and the drive device comprises for example at least a first shaft and a second shaft intended to pass through the fixing portion 86 of the glazing 80 through a first fixing hole 81a and a second fixing hole 81b respectively. The fixing associated with the glazing 80 is for example a screw fixing.
[0201] In a known manner, such a fastening element is designed to be integral with the window pane 80 and exerts a clamping force laterally on each fastening part 86 as a result of screwing.
[0202] A drive device (sometimes referred to as a "proportional lifter") is selectively controlled to move the assembly glass 80 in a translational motion in a height direction at least between a high position and a low position, wherein the high position is referred to as a position for closing the door window and the low position is referred to as a position for fully or partially opening the window.
[0203] The laminated glazing 80 comprises at least an outer glass sheet and an inner glass sheet assembled together by means of an interlayer. The laminated glazing 80 used here as a side window glazing is delimited by a periphery in the shape of a substantially parallelepiped.
[0204] The outer glass sheet comprises an outer surface and an inner surface facing the vehicle exterior and the vehicle interior, respectively.
[0205] like Figure 8 As shown, the outer glass sheet continuously includes an upper edge, a rear edge, a lower edge and a front edge, the upper edge and the lower edge opposite to each other extend substantially in the longitudinal direction, and the rear edge and the front edge opposite to each other extend substantially in the vertical direction.
[0206] Depending on the type of laminated glazing 80 , ie symmetrical or asymmetrical, the at least one fastening portion 86 can in particular consist of all or only part of the pane forming the glazing 80 .
[0207] The inner glass sheet includes an outer surface and an inner surface facing the vehicle exterior and the vehicle interior, respectively.
[0208] In such a laminated glazing 10 , 100 or 80 , at least one of the glass sheets 20 , 120 , 30 , 130 is advantageously heat strengthened.
[0209] Preferably, the first glass sheet 20, 120 and the second glass sheet 30, 130 are heat strengthened, preferably the heat strengthening is of the semi-quenching or hardening type.
[0210] Preferably, the first glass sheet 20, 120 and the second glass sheet 30, 130 have the same composition, in particular a composition of the soda-lime, aluminosilicate, borosilicate type.
[0211] As a variant, the first glass sheet 20 , 120 and the second glass sheet 30 , 130 have different compositions.
[0212] Depending on the use and type of the laminated glazing, the first glass sheet 20, 120 and the second glass sheet 30, 130 have the same thickness, e20, e120, e30, e130 respectively for the first and second configurations described previously, thereby forming a symmetrical laminated glazing.
[0213] Preferably, in such symmetrical glazing, the thickness of the glass sheet 20, 120, 30, 130 is between 0.7 mm and 3 mm, preferably between 1.1 mm and 2.6 mm.
[0214] The first glass sheet 20, 120 and the second glass sheet 30, 130 have different thicknesses to form an asymmetric laminated glazing, the first glass sheet 20, 120 having a thickness e20, e120 between 1.5 mm and 3.5 mm, and the second glass sheet 30, 130 having a thickness e30, e130 between 0.4 mm and 2.6 mm, preferably between 0.7 mm and 1.6 mm.
[0215] Preferably, the first glass sheet 20 , 120 and the second glass sheet 30 , 130 have the same color tone, in particular clear glass, green glass or dark (or grey) glass.
[0216] As a variant, the first glass sheet 20 , 120 and the second glass sheet 30 , 130 have different hues.
[0217] The method according to the invention is also applicable to asymmetrical glazings, for which individual glass sheets are cut. The invention is not limited to the application of the method to side windows, but can also be applied, for example, to roofs or rear windows of motor vehicles, or to laminated glazings intended for use in fields other than motor vehicles.
Claims
1. A method for cutting a laminated glazing (10, 80, 100), the laminated glazing (10, 80, 100) comprising at least a first glass sheet (20, 120) and a second glass sheet (30, 130) assembled together by an intermediate layer (40, 140) comprising at least one sheet of polymeric material, the glazing (10, 80, 100) further comprising an insert (50, 150) having a hole (51, 151), the hole (51, 151) being defined by an inner contour (53, 153), the insert (50, 150) being received in a hollowed-out portion (41) provided in the intermediate layer (40, 140), the method comprising the following steps: - a detection step (201) of detecting the inner contour (53, 153) by means of a visual device (300); - a calculation step (202) of the cutting path to be followed based on the detection of said inner contour (53, 153); A cutting step (203) of cutting at least the first glass sheet (20, 120) according to the calculated cutting path by means of a laser source (401, 401a) having a beam (402, 402a).
2. The method according to claim 1, characterized in that: In the calculation step (202), a shrinkage relative to the inner contour (53, 153) is calculated, which is between 0.1 mm and 1 mm, or between 0.5 mm and 1 mm, so that the beam (402, 402b) does not touch the insert (50, 150) in the cutting step (203).
3. The method according to claim 1, characterized in that The method further comprises: - a beveling step (204) by means of said laser source (401), comprising making at least one beveling cut on the edge (25) of the hole (21) of said first glass sheet (20, 120) resulting from the cutting step (203).
4. The method according to any one of claims 1 to 3, characterized in that In the cutting step (203), the second glass sheet (30, 130) is also cut according to the calculated cutting path by means of the laser source (401).
5. The method according to claim 3, characterized in that: The method further comprises: - performing at least one beveling step (204) by means of the laser source (401) on the edge (25a) of the first glass sheet (20, 120) of the through hole (21') produced by the cutting step (203) and / or on the edge (25b) of the second glass sheet (30, 130).
6. The method according to any one of claims 1 to 3, characterized in that The method further comprises: - an additional cutting step (203') of additionally cutting the second glass sheet (30, 130) according to the calculated cutting path by means of an additional laser source (401b) having a beam (402b).
7. The method according to claim 6, characterized in that The cutting step (203) and the additional cutting step (203') are performed simultaneously.
8. The method according to claim 6, characterized in that The cutting step (203) and the additional cutting step (203') are performed sequentially.
9. Laminated glazing (10, 80, 100) comprising at least one cut obtained by the method according to any one of claims 1 to 8, by means of which the glazing (10, 80, 100) comprises a hole (21) in a first glass sheet (20, 120) or a through hole (21') through the first glass sheet (20, 120) and the second glass sheet (30, 130) coaxial with the hole (51, 151) of the insert (50, 150).
10. The laminated glazing (10, 80, 100) according to claim 9, characterized in that The roughness of the cutting is less than 3 μm.
11. The laminated glazing (10, 80, 100) according to claim 9, characterized in that The roughness of the cutting is less than 2 μm.
12. The laminated glazing (10, 80, 100) according to claim 9, characterized in that The roughness of the cutting is less than 1 μm.
13. The laminated glazing (10, 80, 100) according to claim 9, characterized in that The first glass sheet (20, 120) and / or the second glass sheet (30, 130) are heat strengthened.
14. The laminated glazing (10, 80, 100) according to claim 13, characterized in that Heat strengthening is of semi-quenching type.
15. The laminated glazing (10, 80, 100) according to claim 9, characterized in that The first glass sheet (20, 120) and the second glass sheet (30, 130) have the same composition, or the first glass sheet (20, 120) and the second glass sheet (30, 130) have different compositions.
16. The laminated glazing (10, 80, 100) according to claim 9, characterized in that The first glass sheet (20, 120) and the second glass sheet (30, 130) have the same thickness (e 20 , e 120 , e 30 , e 130 ), thereby forming a symmetrical laminated glazing, and wherein the thickness of the glass sheet is between 0.7 mm and 3 mm.
17. The laminated glazing (10, 80, 100) according to claim 16, characterized in that The thickness of the glass sheet is between 1.1 mm and 2.6 mm.
18. The laminated glazing (10, 80, 100) according to claim 9, characterized in that The first glass sheet (20, 120) and the second glass sheet (30, 130) have different thicknesses, thereby forming an asymmetric laminated glazing, the first glass sheet (20, 120) having a thickness (e) between 1.5 mm and 3.5 mm. 20 , e 120 ) and the second glass sheet (30, 130) has a thickness (e) between 0.4 mm and 2.6 mm 30 , e 130 ).
19. The laminated glazing (10, 80, 100) according to claim 18, characterized in that The second glass sheet (30, 130) has a thickness (e) between 0.7 mm and 1.6 mm. 30 , e 130 ).
20. The laminated glazing (10, 80, 100) according to claim 9, characterized in that The first glass sheet (20, 120) and the second glass sheet (30, 130) have the same color tone, or the first glass sheet (20, 120) and the second glass sheet (30, 130) have different color tones.
Citation Information
Patent Citations
Composite glass hole cutting method
CN104326649A
FR2002921A1
FR2204992A5
Apparatus for bending and tempering glass sheets.
FR2549465A1
Protective material with a ceramic multilayer structure.
FR2642419A1