A multi-level filler-constructed dental composite resin and a preparation method thereof

By constructing dental composite resin using multi-stage fillers, and combining porous SiO2 and silanized non-porous SiO2 fillers, the problems of insufficient mechanical properties and high polymerization shrinkage of dental composite resin are solved, achieving higher filler loading and lower cost.

CN115501121BActive Publication Date: 2024-11-26DONGHUA UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211210553.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-30
Publication Date
2024-11-26
Estimated Expiration
2042-09-30

AI Technical Summary

Technical Problem

Existing dental composite resins have insufficient mechanical properties, high polymerization shrinkage, and low filler content, leading to increased costs.

Method used

A multi-level filler is used to construct dental composite resin. A combination of porous SiO2 filler and silanized non-porous SiO2 filler is used. The particle size and ratio are calculated by using an equisional spherical close packing model to form a multi-level filler structure, which is combined with the resin matrix and photoinitiator.

Benefits of technology

The mechanical properties of dental composite resin were improved, the polymerization shrinkage rate was reduced, and the filler content was increased, thereby reducing the manufacturing cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115501121B_ABST
    Figure CN115501121B_ABST
Patent Text Reader

Abstract

The present invention relates to a multi-level filler-constructed dental composite resin and a preparation method thereof. The composite resin comprises the following components by mass percentage: 33-89% of multi-level filler; 15-67% of resin matrix; and 0.1-1% of photoinitiator. Compared with traditional dental restoration composite resins, the multi-level filler-constructed dental composite resin prepared by the present invention has further improved mechanical properties by adjusting the component addition ratio, and exhibits a lower polymerization shrinkage rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of dental restoration, and particularly relates to a multi-level filler-constructed dental composite resin and a preparation method thereof. Background Art

[0002] The oral cavity is a very important organ in the human body. Its internal environment is complex. Under the influence of multiple factors inside and outside the body, it often develops a common and frequently occurring disease - dental caries. This disease has been listed by the World Health Organization (WHO) as one of the three major non-communicable diseases that need to be focused on prevention and treatment in the 21st century. According to the results of the four national oral health epidemiological survey reports, as people age, the dental caries rate increases year by year. The average dental caries rate in my country is now as high as more than 80%. If not treated in time, it will seriously affect human health and quality of life. The cause of dental caries is relatively complex. The main mechanism of its formation is: bacteria form plaque on the surface of the hard tissue of the tooth, and metabolize carbohydrates to produce organic acids. The acid acts on the teeth to dissolve the hydroxyapatite crystals in the teeth. If this process cannot be well controlled, dental caries will eventually form.

[0003] Composite resin has completely replaced traditional silver-mercury alloy in most countries and regions due to its beautiful color, good physical and chemical properties, low cytotoxicity and convenient clinical operation. It has become the preferred material for filling and repairing tooth defects at home and abroad. Composite resin is mainly composed of organic monomers, inorganic fillers and a small amount of photoinitiator system. The organic resin contains polymerizable groups. Under the action of light curing, it forms a three-dimensional network structure, which can give the material a certain shape. The inorganic filler mainly gives the composite material excellent mechanical properties and reduces the polymerization shrinkage of the composite resin. It is reported that the fracture of resin restorations due to insufficient mechanical properties, the occurrence of microleakage and secondary caries due to large polymer shrinkage, and the cost increase due to low filling amount of inorganic fillers are the main reasons for the unsatisfactory clinical effect of dental composite resin. In order to solve the above problems, people have tried to improve the mechanical properties of composite resins by developing new structural fillers and optimizing the organic-inorganic interface. For example, patent CN 104083289 A silanizes the surface of silica nanofibers to obtain a composite resin with a bending strength of 79.8-93.2 MPa. The composite resin obtained by this method has a weak force formed at the organic-inorganic interface and is prone to hydrolysis during long-term service (T. Nihei. Journal of Oral Science, 2016, 58, 151-155.); Patent CN 108852858A designs a rambutan-like SiO2 filler, the surface of which has a "sawtooth"-like protrusion structure, which can increase the friction between particles and the contact area between particles and the resin matrix, and improve the phase interface performance, but the "sawtooth" structure only exists on the surface of the rambutan-like SiO2 filler, so the organic monomer can only penetrate the surface of the filler and cannot effectively penetrate the interior of the filler, thereby limiting the degree of improvement in the organic-inorganic phase interface bonding; Patent CN112206171A designs a dendritic silica filler with adjustable pore size, through the physical micromechanical interlocking effect of the filler-resin, a "cross-stitch"-like hinged mesh structure is formed, thereby improving the interfacial bonding force of the organic-inorganic phase and enhancing the mechanical properties of the dental composite resin, but the low filling amount of the filler leads to a high cost of the composite resin, and the polymerization shrinkage rate is not well improved. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a multi-level filler constructed dental composite resin and a preparation method thereof, the composite resin overcomes the defect of low filling amount of dental composite resin using dendritic porous SiO2 as inorganic filler alone, further improves the mechanical properties of the dental composite resin and reduces its polymerization shrinkage.

[0005] The present invention provides a multi-level filler-constructed dental composite resin, wherein the composite resin comprises the following components by mass percentage:

[0006] Multi-stage filler 33-89%;

[0007] Resin matrix 15-67%;

[0008] Photoinitiator 0.1-1%; the sum of the mass percentages of each component is 100%;

[0009] Wherein, the multi-stage filler is composed of porous SiO2 filler and silanized non-porous SiO2 filler in a mass ratio of 1:9-9:1.

[0010] The pore size of the porous SiO2 filler is 2-3.5 nm, and the particle size is 0.03 μm-1.5 μm; the particle size of the silanized non-porous SiO2 filler is 0.05 μm-1.2 μm.

[0011] The resin matrix is ​​two of bisphenol A-dimethacrylate glycidyl ester Bis-GMA, triethylene glycol dimethacrylate TEGDMA, bisphenol A polyoxyethylene ether dimethacrylate EBPDMA, and dimethacrylate urethane UDMA, with a mass ratio of 1-6:1.

[0012] The photoinitiator consists of camphorquinone CQ and ethyl 4-dimethylaminobenzoate 4-EDMAB, with a mass ratio of 1:4-6.

[0013] The present invention also provides a method for preparing a multi-level filler-constructed dental composite resin, comprising the following steps:

[0014] (1) Preparation of porous SiO2 filler: alcohol, cyclohexane and tetraethyl orthosilicate TEOS are stirred into a mixed solution, and then a mixed solution of surfactant, urea and water is added, hydrothermally reacted, and naturally cooled, centrifuged and washed, and calcined to obtain the filler;

[0015] (2) Preparation of silanized non-porous SiO2 filler: first, tetraethyl orthosilicate TEOS is added to a stirred mixed solution of ethanol, ammonium hydroxide and water, and then the mixture is stirred and refluxed in an oil bath, cooled, centrifuged and washed, and vacuum dried to obtain non-porous SiO2; then, the non-porous SiO2 is dispersed in cyclohexane, and then a mixed solution of n-propylamine and γ-MPS is added, stirred at room temperature, and finally cooled, centrifuged and washed, and vacuum dried to obtain the mixture;

[0016] (3) Construction of multi-level fillers: A composite of porous SiO2 fillers with equal particle sizes and silanized non-porous SiO2 fillers is selected as the primary filler. Then, the maximum size of silanized non-porous SiO2 fillers (secondary fillers) with different particle sizes filled in the regular tetrahedral voids and regular octahedral voids of the primary filler is calculated by using the equal sphere close packing model theory to obtain a multi-level filler.

[0017] (4) Preparation of dental composite resin: The multi-level filler, resin matrix and photoinitiator are mixed evenly to obtain an uncured composite resin paste, which is then photocured to obtain a multi-level filler-constructed dental composite resin.

[0018] The alcohol in step (1) is one of ethanol, isopropanol, n-pentanol, n-butanol, n-hexanol and n-heptanol; the surfactant is hexadecyltrimethylammonium bromide (CTAB) or polyoxyethylene polyoxypropylene ether block copolymer F127.

[0019] The volume ratio of alcohol, cyclohexane and tetraethyl orthosilicate TEOS in step (1) is 1:10-30:1-10; the mass ratio of surfactant, urea and water is 1:0.1-0.5:10-30. The volume ratio between the two mixed solutions is 1.1-1.4:1.

[0020] The process parameters of the hydrothermal reaction in the step (1) are: in a polytetrafluoroethylene high temperature and high pressure hydrothermal reactor, the reaction temperature is 80-250° C. for 2-7 hours; the process parameters of the calcination are: the calcination temperature is 420-680° C., and the calcination time is 4-10 hours.

[0021] The volume ratio of ethanol, ammonium hydroxide and water in step (2) is 3-20:2-10:1; the volume ratio of cyclohexane, n-propylamine and γ-MPS is 100-150:0.1-2:0.3-1.5; the mass volume ratio of non-porous SiO2 and cyclohexane is 1-10g:100-150mL.

[0022] The process parameters of the oil bath reaction in step (2) are: reacting in a 50-80° C. oil bath for 1-3 hours; the process parameters of the vacuum drying are: drying temperature of 70-120° C., and drying time of 8-14 hours.

[0023] The particle size of the primary filler in step (3) is 200-550 nm, and the particle size of the filled silanized non-porous SiO2 secondary filler is 60-190 nm. The interface bonding effect between the silanized non-porous SiO2 filler and the resin matrix is ​​better.

[0024] The cooling method in steps (1) and (2) is natural cooling; the process conditions for centrifugal washing are: centrifugal washing with ethanol, acetone or deionized water.

[0025] In the step (3), the mass ratio of the primary filler to the secondary filler of the multi-stage filler is 1-4:1.

[0026] The process conditions of light curing in step (4) are as follows: fill the uncured composite resin paste into the silicone rubber mold and use LED lamp to cure for 10-230s, and then obtain the composite resin specimen after demoulding. Then, store the specimen in the dark at room temperature for 2-3 days, and polish the sample surface with silicon carbide sandpaper before testing to remove the uncured layer on the resin surface.

[0027] Beneficial Effects

[0028] (1) The multi-level filler prepared by the present invention is used to construct a dental composite resin. The preparation method is simple, the reaction conditions are mild, and the multi-level filler has a good mixing effect with the resin matrix. Compared with the dendritic porous SiO2 used alone as an inorganic filler, the filler filling amount is significantly increased, and it can be applied to the field of dental composite restoration resins;

[0029] (2) Compared with conventional dental restoration composite resins, the multi-level filler-constructed dental composite resin prepared by the present invention has further improved mechanical properties by adjusting the addition ratio of porous SiO2 and silanized non-porous SiO2, while exhibiting a lower polymerization shrinkage rate. At the same time, due to the combination of SiO2 inorganic fillers of different particle sizes, the filling amount of the inorganic filler in the composite resin is greatly increased, and the mass fraction of the composite resin monomer is reduced, thereby significantly reducing the production cost of the composite resin. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a SEM image of the dendritic porous SiO2 particles obtained in Example 1;

[0031] Figure 2 This is a SEM image of the silanized non-porous SiO2 particles obtained in Example 1;

[0032] Figure 3 is the flexural strength of the composite resins obtained in Examples 1-3 and Comparative Example 1;

[0033] Figure 4 is the compressive strength of the composite resins obtained in Examples 1-3 and Comparative Example 1;

[0034] Figure 5 is the polymerization shrinkage of the composite resins obtained in Examples 1-3 and Comparative Example 1;

[0035] Figure 6 It is the maximum filling amount of the composite resin obtained in Examples 1-3 and Comparative Example 1. DETAILED DESCRIPTION

[0036] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0037] Example 1

[0038] (1) Preparation of dendritic porous SiO2 particles

[0039] 1.5 ml of amyl alcohol, 30 ml of cyclohexane and 2.5 ml of TEOS were mixed and stirred to form a mixed solution, and then a mixed solution of 1.8 g of CTAB, 1 g of urea and 30 g of water was added to the mixed solution. The mixed solution was poured into a polytetrafluoroethylene high temperature and high pressure hydrothermal autoclave, reacted at 130 ° C for 4 hours, and naturally cooled to room temperature after the reaction was completed. After centrifugation, acetone and deionized water washing, calcined at 550 ° C for 6 hours, and a dendritic porous SiO2 particle size of 500 nm was obtained. The SEM results are as follows: Figure 1 As shown, the SEM image shows that the SiO2 particles have a uniform particle size and a uniformly distributed pore structure on the particle surface.

[0040] (2) Preparation of silanized nonporous SiO2 particles

[0041] 460 mL of ethanol, 320 mL of ammonium hydroxide and 70 mL of deionized water were mixed and stirred to form a mixed solution, and then 40 mL of tetraethyl orthosilicate was added. The mixture was refluxed and stirred for 2 h in an oil bath at 60 °C and cooled to room temperature. After centrifugal washing with anhydrous ethanol and deionized water, vacuum drying at 110 °C for 12 h, it was ultrasonically dispersed in 100 mL of cyclohexane, and then 0.14 mL of propylamine and 0.53 mL of γ-MPS were added. The mixture was stirred at room temperature for 30 min and then at 60 °C for 1 h. After the reaction was completed, it was naturally cooled to room temperature, centrifuged and washed with cyclohexane and deionized water, and dried in a vacuum oven at 80 °C for 12 h to obtain silanized non-porous SiO2 particles with a particle size of 500 nm. The SEM results are shown in the following figure. Figure 2 As shown, the SEM image shows that the SiO2 particles have a uniform particle size and are a non-porous spherical structure. According to the above reaction sequence and conditions, the amounts of ethanol, ammonium hydroxide, deionized water, and TEOS reagents were changed to 780mL, 40mL, 70mL, and 40mL, respectively, and the amounts of other reagents remained unchanged, and finally silanized non-porous SiO2 particles with a particle size of 190nm were obtained.

[0042] (3) Construction of “porous + non-porous” multi-level packing

[0043] Dendritic porous SiO2 and silanized nonporous SiO2 with a particle size of 500nm were selected as primary fillers in a mass ratio of 3:7. The maximum sizes of the tetrahedral voids and octahedral voids of the primary fillers were then calculated using the equi-sphere close packing model theory. Silanized nonporous SiO2 with a particle size of 190nm was selected as the secondary filler to obtain a "porous + nonporous" multi-level filler.

[0044] (4) Preparation of composite resin

[0045] According to the formula shown in Table 1, the dendritic porous SiO2 and silanized non-porous SiO2, organic monomers and photoinitiator systems with a particle size of 500 nm were first mixed by manual premixing. When the inorganic filler was fully wetted by the resin matrix, it was put into a three-roll mill (EXAKT 80E, Germany) for secondary mixing, and after vacuum negative pressure treatment, an uncured composite resin paste was obtained. Subsequently, it was cured by visible light (wavelength of 430-490 nm) to obtain a dental composite resin.

[0046] Table 1 Components of composite resin and content of each component

[0047]

[0048] (5) Characterization of composite resin

[0049] According to the international standard "ISO 4049-2009", the flexural strength and compressive strength of the composite resin were tested by a universal testing machine (Instron 5900, USA), which were 105.9±8.0MPa and 389.5±35.1MPa respectively; according to the Archimedean principle, the density of the repair resin before and after curing was tested by a density balance (ML 204, Switzerland), and the polymerization shrinkage of the composite resin was calculated to be 5.5±0.5%; the inorganic filler, organic matrix and photoinitiator were uniformly mixed by manual premixing using a three-roll grinder (EXAKT 80E, Germany), and the maximum filler filling amount was weighed and calculated to be 65.0±1.0wt% using an analytical balance (AL204).

[0050] Example 2

[0051] (1) Preparation of dendritic porous SiO2 particles

[0052] 1.5 ml of amyl alcohol, 30 ml of cyclohexane and 2.5 ml of TEOS were mixed and stirred into a mixed solution, and then a mixed solution of 1.8 g of CTAB, 1 g of urea and 30 g of water was added to the mixed solution. The mixed solution was poured into a polytetrafluoroethylene high temperature and high pressure hydrothermal autoclave, reacted at 130°C for 4 hours, and naturally cooled to room temperature after the reaction was completed. After centrifugation, washing with acetone and deionized water, calcined at 550°C for 6 hours to obtain dendritic porous SiO2 particles with a particle size of 500 nm.

[0053] (2) Preparation of silanized nonporous SiO2 particles

[0054] 460mL of ethanol, 320mL of ammonium hydroxide and 70mL of deionized water were mixed and stirred into a mixed solution, and then 40mL of tetraethyl orthosilicate was added. The mixture was refluxed and stirred for 2h under 60℃ oil bath conditions and cooled to room temperature. After centrifugal washing with anhydrous ethanol and deionized water, vacuum drying at 110℃ for 12h, it was ultrasonically dispersed in 100mL of cyclohexane, and then 0.14mL of propylamine and 0.53mL of γ-MPS were added. The mixture was stirred at room temperature for 30min and then at 60℃ for 1h. After the reaction was completed, it was naturally cooled to room temperature, centrifuged and washed with cyclohexane and deionized water, and dried in a vacuum oven at 80℃ for 12h to obtain silanized non-porous SiO2 particles with a particle size of 500nm. According to the above reaction sequence and conditions, the amounts of ethanol, ammonium hydroxide, deionized water and TEOS reagents were changed to 400mL, 30mL, 10mL and 90mL respectively, and the amounts of other reagents remained unchanged, and finally silanized non-porous SiO2 particles with a particle size of 60nm were obtained.

[0055] (3) Construction of “porous + non-porous” multi-level packing

[0056] Dendritic porous SiO2 and silanized non-porous SiO2 with a particle size of 500 nm were selected. 20 The composite was used as the primary filler with a mass ratio of 3:7. The tetrahedral voids and octahedral voids of the primary filler were calculated theoretically with the aid of the equal-sphere close packing model. Silanized non-porous SiO2 with a particle size of 60 nm was selected as the secondary filler to obtain a "porous + non-porous" multi-level filler.

[0057] (4) Preparation of composite resin

[0058] According to the formula shown in Table 2, the dendritic porous SiO2 and silanized non-porous SiO2, organic monomers and photoinitiator systems with a particle size of 500 nm were first mixed by manual premixing. When the inorganic filler was fully wetted by the resin matrix, it was put into a three-roll mill (EXAKT 80E, Germany) for secondary mixing, and after vacuum negative pressure treatment, an uncured composite resin paste was obtained. Subsequently, it was cured by visible light (wavelength of 430-490 nm) to obtain a dental composite resin.

[0059] Table 2 Components of composite resin and content of each component

[0060]

[0061] (5) Characterization of composite resin

[0062] According to the international standard ISO 4049-2009, the flexural strength and compressive strength of the composite resin were tested by a universal testing machine (Instron 5900, USA), which were 128.8±8.6MPa and 366.6±12.3MPa, respectively. According to the Archimedean principle, the density of the repair resin before and after curing was tested by a density balance (ML 204, Switzerland), and the polymerization shrinkage of the composite resin was calculated to be 4.6±0.8%. The inorganic filler, organic matrix and photoinitiator were uniformly mixed by manual premixing using a three-roll grinder (EXAKT 80E, Germany), and the maximum filler filling amount was weighed and calculated to be 69.0±2.0wt% using an analytical balance (AL204).

[0063] Example 3

[0064] (1) Preparation of dendritic porous SiO2 particles

[0065] 1.5 ml of amyl alcohol, 30 ml of cyclohexane and 2.5 ml of TEOS were mixed and stirred into a mixed solution, and then a mixed solution of 1.8 g of CTAB, 1 g of urea and 30 g of water was added to the mixed solution. The mixed solution was poured into a polytetrafluoroethylene high temperature and high pressure hydrothermal autoclave, reacted at 130°C for 4 hours, and naturally cooled to room temperature after the reaction was completed. After centrifugation, washing with acetone and deionized water, calcined at 550°C for 6 hours to obtain dendritic porous SiO2 particles with a particle size of 500 nm.

[0066] (2) Preparation of silanized nonporous SiO2 particles

[0067] 460mL of ethanol, 320mL of ammonium hydroxide and 70mL of deionized water were mixed and stirred into a mixed solution, and then 40mL of tetraethyl orthosilicate was added, refluxed and stirred for 2h under 60℃ oil bath conditions and cooled to room temperature. After centrifugal washing with anhydrous ethanol and deionized water, vacuum drying at 110℃ for 12h, it was ultrasonically dispersed in 100mL of cyclohexane, and then 0.14mL of propylamine and 0.53mL of γ-MPS were added, first stirred at room temperature for 30min, and then stirred at 60℃ for 1h. After the reaction was completed, it was naturally cooled to room temperature, centrifuged and washed with cyclohexane and deionized water, and dried in a vacuum oven at 80℃ for 12h to obtain silanized non-porous SiO2 particles with a particle size of 500nm. According to Example 1-2, by changing the amount of ethanol, ammonium hydroxide, deionized water, and TEOS reagent, silanized non-porous SiO2 with a particle size of 60nm and 190nm were synthesized respectively.

[0068] (3) Construction of “porous + non-porous” multi-level packing

[0069] Dendritic porous SiO2 and silanized nonporous SiO2 with a particle size of 500nm were selected as primary fillers in a mass ratio of 3:7. The tetrahedral voids and octahedral voids of the primary fillers were theoretically calculated with the help of the equal-sphere close packing model. Silanized nonporous SiO2 with a particle size of 60nm and 190nm were selected as secondary fillers to obtain a "porous + nonporous" multi-level filler.

[0070] (4) Preparation of composite resin

[0071] According to the formula shown in Table 3, the dendritic porous SiO2 and silanized non-porous SiO2, organic monomers and photoinitiator system with a particle size of 500 nm were first mixed by manual premixing. When the inorganic filler was fully wetted by the resin matrix, it was put into a three-roll mill (EXAKT 80E, Germany) for secondary mixing, and after vacuum negative pressure treatment, an uncured composite resin paste was obtained. Subsequently, it was cured by visible light (wavelength of 430-490 nm) to obtain a dental composite resin.

[0072] Table 3 Components of composite resin and content of each component

[0073]

[0074] (5) Characterization of composite resin

[0075] According to the international standard ISO 4049-2009, the flexural strength and compressive strength of the composite resin were tested by a universal testing machine (Instron 5900, USA), which were 153.2±9.2MPa and 430.8±17.4MPa, respectively. According to the Archimedean principle, the density of the repair resin before and after curing was tested by a density balance (ML 204, Switzerland), and the polymerization shrinkage of the composite resin was calculated to be 2.6±0.4%. The inorganic filler, organic matrix and photoinitiator were uniformly mixed by manual premixing using a three-roll grinder (EXAKT 80E, Germany), and the maximum filler filling amount was 75.0±2.0wt% by weighing using an analytical balance (AL204).

[0076] Comparative Example 1

[0077] According to Example 1, a dendritic porous SiO2 inorganic filler with a particle size of 500 nm was prepared, and a dental restoration composite resin was prepared according to the formula shown in Table 4. First, the dendritic porous SiO2 particles, organic monomers and photoinitiator system were mixed by manual premixing. When the inorganic filler was fully wetted by the resin matrix, it was put into a three-roll grinder (EXAKT 80E, Germany) for secondary mixing. After vacuum negative pressure treatment, an uncured composite resin paste was obtained. Subsequently, it was cured by visible light to obtain a dental composite resin, which was used as control group 1.

[0078] Table 4 Components of composite resin and content of each component

[0079]

[0080] The maximum filler loading, flexural strength, compressive strength and polymerization shrinkage of the composite resins prepared in this comparative example and in Examples 1-3 are shown as follows: Figure 3-6 As shown, it can be seen that compared with the composite resin filled with the dendritic porous SiO2 inorganic filler alone (control group 1), the maximum filling amount and mechanical properties of the dental composite resin filler constructed by the "porous + non-porous" multi-level filler of the present invention are higher than those of the control group 1, and the polymerization shrinkage rate is lower than that of the control group 1, that is, the "porous + non-porous" multi-level filler constructed by the present invention is beneficial to improving the filler filling amount and mechanical properties of the dental composite resin, and reducing its polymerization shrinkage rate.

[0081] Comparative Example 2

[0082] According to Example 1, a silanized non-porous SiO2 inorganic filler with a particle size of 500 nm was prepared, and a dental restoration composite resin was prepared according to the formula shown in Table 5. First, the dendritic porous SiO2 particles, organic monomers and photoinitiator system were mixed by manual premixing. When the inorganic filler was fully wetted by the resin matrix, it was put into a three-roll mill (EXAKT 80E, Germany) for secondary mixing. After vacuum negative pressure treatment, an uncured composite resin paste was obtained. Subsequently, it was cured by visible light to obtain a dental composite resin, which was used as control group 1.

[0083] Table 5 Components of composite resin and content of each component

[0084]

[0085] The maximum filler loading, flexural strength, compressive strength and polymerization shrinkage of the composite resins prepared in this comparative example and in Examples 1-3 are shown as follows: Figure 3-6 As shown, it can be seen that compared with the silanized non-porous SiO2 inorganic filler alone filling the composite resin (control group 2), the maximum filling amount and mechanical properties of the dental composite resin filler constructed by the "porous + non-porous" multi-level filler of the present invention are higher than those of the control group 2, and the polymerization shrinkage rate is lower than that of the control group 2, that is, the "porous + non-porous" multi-level filler constructed by the present invention is beneficial to improving the filler filling amount and mechanical properties of the dental composite resin, and reducing its polymerization shrinkage rate.

Claims

1. A multi-level filler-based dental composite resin, characterized in that: The composite resin comprises the following components by mass percentage: The inorganic filler is 500nm dendritic porous SiO2 11.1wt%, 500nm particle size silanized non-porous SiO2 25.9wt%, 60nm particle size silanized non-porous SiO2 27.5wt%, 190nm particle size silanized non-porous SiO2 10.5wt%; The organic monomers are Bis-GMA 12wt%, TEGDMA 12wt%; The photoinitiator is CQ 0.2wt%, 4-EDMAB 0.8wt%.

2. A method for preparing the multi-level filler-structured dental composite resin as claimed in claim 1, comprising the following steps: (1) Preparation of porous SiO2 filler: by stirring alcohol, cyclohexane and tetraethyl orthosilicate TEOS into a mixed solution, then adding a mixed solution of surfactant, urea and water, hydrothermal reaction, and naturally cooling, centrifugal washing, and calcining to obtain the filler; (2) Preparation of silanized non-porous SiO2 filler: first, tetraethyl orthosilicate (TEOS) was added to a stirred mixed solution of ethanol, ammonium hydroxide and water, and then the mixture was stirred and refluxed in an oil bath, cooled, centrifuged and washed, and vacuum dried to obtain non-porous SiO2; then, the non-porous SiO2 was dispersed in cyclohexane, and then a mixed solution of n-propylamine and γ-MPS was added, stirred at room temperature, and finally cooled, centrifuged and washed, and vacuum dried to obtain the filler; (3) Construction of multi-level fillers: A composite of porous SiO2 fillers with equal particle sizes and silanized non-porous SiO2 fillers is selected as the primary filler. Then, the tetrahedral voids and octahedral voids of the primary filler are calculated using the equal sphere close packing model theory, and the maximum size of the silanized non-porous SiO2 fillers with different particle sizes is filled to obtain a multi-level filler. (4) Preparation of dental composite resin: The multi-level filler, resin matrix and photoinitiator are mixed evenly to obtain an uncured composite resin paste, which is then photocured to obtain a multi-level filler-constructed dental composite resin.

3. The preparation method according to claim 2, characterized in that: The alcohol in step (1) is one of ethanol, isopropanol, n-pentanol, n-butanol, n-hexanol and n-heptanol; the surfactant is hexadecyltrimethylammonium bromide (CTAB) or polyoxyethylene polyoxypropylene ether block copolymer F127.

4. The preparation method according to claim 2, characterized in that: In the step (1), the volume ratio of alcohol, cyclohexane and tetraethyl orthosilicate TEOS is 1:10-30:1-10; the mass ratio of surfactant, urea and water is 1:0.1-0.5:10-30.

5. The preparation method according to claim 2, characterized in that: The process parameters of the hydrothermal reaction in step (1) are: in a polytetrafluoroethylene high temperature and high pressure hydrothermal reactor, the reaction temperature is 80-250° C. for 2-7 hours; the process parameters of the calcination are: the calcination temperature is 420-680° C., and the calcination time is 4-10 hours.

6. The preparation method according to claim 2, characterized in that: The volume ratio of ethanol, ammonium hydroxide and water in step (2) is 3-20:2-10:1; the volume ratio of cyclohexane, n-propylamine and γ-MPS is 100-150:0.1-2:0.3-1.5; the mass volume ratio of non-porous SiO2 and cyclohexane is 1-10g:100-150mL.

7. The preparation method according to claim 2, characterized in that: The process parameters of the oil bath reaction in step (2) are: reacting in an oil bath at 50-80° C. for 1-3 hours; the process parameters of the vacuum drying are: drying temperature of 70-120° C., and drying time of 8-14 hours.