A flexible electrochemical energy storage device and a method for preparing the same

By using transition metal compound-doped lignin/rubber composites in flexible electrochemical energy storage devices, combined with pre-stretching and laser direct writing technology, the problems of insufficient energy density and stretchability in the existing technology are solved and achieved. Flexible electrochemical energy storage devices with high energy density and stretchability are suitable for wearable smart electronic devices.

CN115512978BActive Publication Date: 2024-10-11WUHAN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211184324.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-27
Publication Date
2024-10-11
Estimated Expiration
2042-09-27

AI Technical Summary

Technical Problem

Existing flexible electrochemical energy storage devices can only achieve bending and low tensile strain capabilities, and have limited energy density, making it difficult to meet high energy density and stretchability requirements, limiting their use in wearable smart electronic devices. application.

Method used

Transition metal compound-doped lignin/rubber composites are used to prepare elastic base membranes through emulsion blending or mechanical blending methods, and combined with pre-stretching and laser direct writing technology to form high energy density and stretchable flexibility. Electrochemical energy storage devices.

Benefits of technology

A flexible electrochemical energy storage device with low cost, high energy density and excellent stability has been achieved. It has high mechanical properties and good tensile cycle stability and is suitable for wearable smart electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115512978B_ABST
    Figure CN115512978B_ABST
Patent Text Reader

Abstract

The present invention discloses a flexible electrochemical energy storage device and a preparation method thereof. The steps are as follows: 1) an elastic base film of a lignin / rubber composite material doped with a transition metal compound is prepared by an emulsion blending method or a mechanical blending method; 2) the elastic base film obtained in step 1) is pre-stretched, then laser direct writing is performed for in-situ carbonization, and the pre-stretching is restored after laser direct writing to prepare a flexible electrochemical energy storage electrode based on a lignin / rubber composite material doped with a transition metal compound; 3) the energy storage electrode obtained in step 2) is encapsulated to obtain a flexible electrochemical energy storage device. The preparation method is simple, the raw materials are cheap and readily available, and the obtained energy storage device has high mechanical properties, high elasticity, high conductivity and good tensile cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of flexible and stretchable energy storage, and specifically relates to a flexible electrochemical energy storage device based on laser direct writing transition metal compound doped lignin / rubber composite material and a preparation method thereof. Background Art

[0002] With the development of artificial intelligence, the research on flexible wearable smart electronic devices has received widespread attention. However, the current research on flexible electronic devices is mostly concentrated in the field of flexible sensing, and less on flexible electrochemical energy storage devices. In addition, the existing flexible electrochemical energy storage devices can only achieve bending and low tensile strain capabilities. The research on stretchable micro-flexible electrochemical energy storage devices that can withstand large deformations and unpredictable tensions while maintaining stable electrochemical properties has not yet been found. Laser direct writing technology has been proven to be a high-throughput and scalable method that can be used to manufacture micro-flexible supercapacitors. At present, the preparation of these flexible energy storage devices by laser direct writing technology usually uses polyimide as a flexible substrate. The flexible energy storage devices prepared by this technology only have bending capabilities but no stretchability. At the same time, the limited energy density also hinders their practical application.

[0003] How to prepare low-cost, highly stretchable, high energy density and excellent stability electrodes for electrochemical energy storage devices has become the key. Summary of the invention

[0004] In view of the existing technical defects, the present invention provides a transition metal compound doped lignin / rubber composite material flexible electrochemical energy storage device and a preparation method thereof. The composite material flexible energy storage device of the present invention has the advantages of simple preparation process, low cost, stretchability and high energy density.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] A method for preparing a flexible electrochemical energy storage device is provided, comprising the following steps:

[0007] 1) preparing a transition metal compound-doped lignin / rubber composite elastic base film by an emulsion blending method or a mechanical blending method;

[0008] 2) pre-stretching the elastic substrate film obtained in step 1), then in-situ carbonizing it by laser direct writing, and restoring the pre-stretching after laser direct writing to prepare a transition metal compound-doped lignin / rubber composite material-based flexible electrochemical energy storage electrode;

[0009] 3) Encapsulating the energy storage electrode obtained in step 2) to obtain a flexible electrochemical energy storage device.

[0010] According to the above scheme, in the step 1), the rubber is natural rubber, nitrile rubber, carboxylated nitrile rubber, styrene-butadiene rubber, carboxylated styrene-butadiene rubber, styrene-butadiene-pyridine rubber or ethylene-propylene rubber.

[0011] According to the above scheme, in step 1), the transition metal in the transition metal compound is zinc, copper, manganese, iron, cobalt, nickel, or vanadium.

[0012] According to the above scheme, in step 1), the transition metal compound is a complex of one or more transition metal oxides, transition metal sulfides, transition metal hydroxides, transition metal carbides, transition metal chlorides, transition metal nitrates, sulfates, and acetates.

[0013] According to the above scheme, in step 1), the specific steps of the emulsion blending method are:

[0014] Lignin and transition metal compounds are added to pre-vulcanized latex to prepare a composite emulsion, which is then poured into a mold and dried to obtain a film. The film is placed in deionized water and heated at 50-100°C for 1-3 hours to obtain a transition metal compound-doped lignin / rubber composite elastic base film.

[0015] Preferably, the latex is natural rubber latex, nitrile latex, styrene butadiene latex, carboxylated nitrile latex or carboxylated styrene butadiene latex.

[0016] Preferably, the mass ratio of lignin to latex dry glue is 1-100:100; the mass ratio of transition metal compound to latex dry glue is 1-30:100.

[0017] Preferably, the composite material emulsion is poured into the mold and dried under the following conditions: forced air drying at 60-100° C. for 1-3 hours.

[0018] Preferably, the process for preparing the pre-vulcanized latex is as follows: a certain amount of vulcanizing agent, accelerator, KOH, casein and latex are stirred at room temperature to prepare the pre-vulcanized latex.

[0019] More preferably, the vulcanizing agent is a complex of one or more of sulfur, dicumyl peroxide, and potassium persulfate; the accelerator is a complex of one or more of zinc oxide, stearic acid, triallyl isocyanurate, zinc diethyldithiocarbamate, N,N-tetramethyldithiodithiocarbamate, 2-mercaptobenzothiazole, xanthogenic acid, 2,2'-dithiodibenzothiazole, N-cyclohexyl-2-benzothiazole sulfenamide, tetramethylthiuram disulfide or diphenylguanidine.

[0020] More preferably, the mass ratio of the vulcanizing agent, the accelerator, KOH, casein and the latex dry rubber is 2-4:2-4:0.05-0.2:1.3-1.6:100.

[0021] According to the above scheme, in step 1), the specific steps of the mechanical blending method are: adding lignin, vulcanizing agent, accelerator and transition metal compound to rubber raw rubber, and mixing them in a double-roll open mill, and then molding them at 120°C-160°C to obtain a transition metal compound-doped lignin / rubber composite elastic base film.

[0022] Preferably, the mass ratio of lignin to raw rubber is 1-100:100; the mass ratio of transition metal compound to raw rubber is 1-30:100; the mass ratio of vulcanizing agent, vulcanization accelerator and raw rubber is 1-4:2-12:100.

[0023] More preferably, the vulcanizing agent is a complex of one or more of sulfur, dicumyl peroxide, and potassium persulfate; the accelerator is a complex of one or more of zinc oxide, stearic acid, triallyl isocyanurate, zinc diethyldithiocarbamate, N,N-tetramethyldithiodithiocarbamate, 2-mercaptobenzothiazole, xanthogenic acid, 2,2'-dithiodibenzothiazole, N-cyclohexyl-2-benzothiazole sulfenamide, tetramethylthiuram disulfide or diphenylguanidine.

[0024] Preferably, the raw rubber is natural rubber, nitrile rubber, carboxylated nitrile rubber, styrene-butadiene rubber, carboxylated styrene-butadiene rubber, styrene-butadiene-pyridine rubber, or ethylene-propylene rubber.

[0025] According to the above scheme, in step 2), the pre-stretching ratio is 0-1000%, preferably 20-600%.

[0026] According to the above scheme, in step 2), the specific method of laser direct writing is: placing the pre-stretched elastic substrate on a laser operating table, using a laser as a laser source, and controlling the laser scanning path through a program to form a patterned circuit on the surface of the elastic substrate.

[0027] According to the above scheme, in step 2), the laser is CO 2 (wavelength 10.6μm), fiber (wavelength 1040nm) or ultraviolet (wavelength 355nm) laser.

[0028] According to the above scheme, in step 2), the laser power is 0.1-80w, the scanning speed is 0.1-100mm / s, and the laser spot is 100-300μm.

[0029] According to the above scheme, in step 3), the gel electrolyte is coated on the patterned circuit surface of the energy storage electrode, dried at room temperature for 1-24 hours, and then encapsulated with rubber latex or solution to obtain an energy storage device.

[0030] Preferably, the gel electrolyte is a polyvinyl alcohol or polyacrylamide polymer hydrogel containing potassium hydroxide, sodium sulfate, sulfuric acid, zinc sulfate or phosphoric acid.

[0031] Preferably, the rubber emulsion or solution is a latex or solution of natural rubber, nitrile rubber, styrene-butadiene rubber, ethylene-propylene rubber or silicone rubber.

[0032] Provided is a flexible electrochemical energy storage device prepared by the above preparation method.

[0033] The present invention provides a method for preparing a transition metal compound doped lignin / rubber composite material flexible electrochemical energy storage device, by using an emulsion blending method and a mechanical blending method, low-cost, renewable low-density lignin is dispersed in a rubber matrix at a nanoscale, which not only effectively reduces the production cost of rubber, but also effectively avoids the adverse effects of lignin on rubber performance after addition, so that the rubber composite material has high elasticity and high mechanical strength, thereby increasing the detection range and mechanical durability of the flexible sensor device. In addition, lignin has a very high carbon content. In the laser direct writing process, it can be used as a carbon precursor to generate conductive carbon material in situ on the surface of the rubber composite material substrate, thereby constructing a sensing circuit with rapid response to stress or strain. More importantly, in the process of lignin and rubber compounding, hydrogen bonds, covalent bonds or π-π effects can be formed between lignin and rubber molecules, so that lignin and rubber molecules have good compatibility, so that in the laser patterning process, the conductive carbon material generated in situ by lignin and the rubber substrate have good interface bonding, and maintain certain mechanical properties and good morphology during the stretch recovery process, thereby enhancing the cycle stability of the flexible sensor device. At the same time, some transition metal compounds are reduced to transition metal elements during the laser carbonization process, which improves the conductivity of the energy storage electrode. The doping of transition metal compounds gives the patterned carbon electrode good electrochemical activity, thereby improving the energy density of the energy storage device.

[0034] The present invention combines pre-stretching as an out-of-plane buckling method with laser direct writing technology, so that the pre-stretched elastic substrate forms a transverse and longitudinal multi-level wrinkle structure during the recovery process after laser carbonization, and the tensile deformation of the conductive material is converted into a bending deformation. Moreover, by adjusting the parameters of the laser, the thickness of the conductive layer and the interface bonding can be further regulated, thereby avoiding the interface stratification problem caused by the mismatch of the modulus of the two, and achieving high conductivity, high stretching and high cycle stability. In addition, laser direct writing can prepare a variety of patterned flexible circuits such as serpentine, mesh, and interdigitated electrodes, and through circuit integration and packaging deployment, a sensor device array can be formed to expand its application range.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] 1. The present invention provides a method for preparing a transition metal compound doped lignin / rubber composite material flexible electrochemical energy storage device. Low-cost, renewable lignin is dispersed in a rubber matrix at the nanoscale. On the one hand, it not only reduces the cost of the elastic substrate, but also ensures the high mechanical properties and high elasticity of the rubber composite material. On the other hand, the high carbon content of lignin can be used as a carbon precursor for preparing graphitized patterns by laser direct writing, giving the rubber composite material a conductive function. At the same time, the good compatibility of lignin and rubber molecules enables the conductive carbon material generated in situ by lignin to have a good interface with the rubber substrate, thereby enhancing the tensile cycle stability of the flexible sensing electrode; and the doping of transition metal compounds can increase the energy density of the energy storage device, and the transition metal compound is partially reduced to a transition metal element during the laser carbonization process, thereby improving the conductivity of the energy storage electrode; the energy storage device has high mechanical properties, high elasticity, high conductivity and good tensile cycle stability.

[0037] 2. The raw materials of the present invention are cheap and easily available, and the preparation process is simple. The application of laser direct writing technology in the preparation process of energy storage devices can produce the energy storage devices quickly and on a large scale, which greatly simplifies the manufacturing process and reduces production costs and operational complexity. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a schematic diagram of the structure of an energy storage device based on a transition metal compound doped-lignin-rubber composite material obtained in an embodiment of the present invention.

[0039] Figure 2 This is the process for preparing the energy storage device according to the embodiment of the present invention. DETAILED DESCRIPTION

[0040] The present invention is further described in detail below in conjunction with specific embodiments and drawings, but the present invention is not limited thereto.

[0041] A schematic diagram of the structure of an energy storage device based on a transition metal doped-lignin-rubber composite material is shown in the following specific embodiment of the present invention: Figure 1 , including an elastic substrate, a patterned circuit, a gel electrolyte and an encapsulation layer.

[0042] Example 1

[0043] Provided is a method for preparing a transition metal-doped lignin / rubber composite material flexible electrochemical energy storage device, comprising the following steps:

[0044] (1) Preparation of Nano-Co by Emulsion Blending 3 O 4 Doped lignin / natural rubber composites with elastic substrates.

[0045] 3 g of sulfur, 2.4 g of triallyl isocyanurate, 0.1 g of KOH, 1.5 g of casein and a latex containing 100 g of natural rubber were stirred at room temperature to prepare a pre-cured latex. 3 O 4 Add to natural rubber latex to prepare a composite material emulsion. Pour the composite rubber emulsion into a mold and dry it at 80°C for 3 hours. Then take out the prepared membrane from the mold and put it into deionized water and heat it at 95°C for 3 hours to prepare Co 3 O 4 Doped lignin / natural rubber composites with elastic substrates.

[0046] (2) Preparation of patterned flexible energy storage electrodes by laser direct writing in situ carbonization.

[0047] The elastic substrate pre-stretched by 300% was placed on the laser operating table, and a fiber laser was used as the laser source (power P = 6w, scanning speed 80mm / s, laser spot 300μm). The laser scanning path was controlled by a program to form a patterned circuit on the surface of the elastic substrate. After laser direct writing, the pre-stretching was restored, and finally an energy storage electrode was obtained.

[0048] (3) Assembly of energy storage devices.

[0049] A polyacrylamide hydrogel electrolyte containing 6M potassium hydroxide is coated on the patterned circuit surface of the energy storage electrode, dried at room temperature, and then encapsulated with natural rubber latex to obtain a supercapacitor.

[0050] The flexible supercapacitor prepared in Example 1 of the present invention has a maximum stretching rate of 300%, a specific capacitance of 338 F / g, and a capacitance retention rate of 95% after 1000 charge and discharge cycles.

[0051] Example 2

[0052] Provided is a method for preparing a transition metal-doped lignin / rubber composite material flexible electrochemical energy storage device, comprising the following steps:

[0053] (1) Preparation of nano-Fe by emulsion blending method 2 O 3 The lignin / natural rubber composite elastic substrate was prepared. 3 g sulfur, 2.4 g triallyl isocyanurate, 0.1 g KOH, 1.5 g casein and 100 g natural rubber latex were stirred at room temperature to prepare a pre-vulcanized latex. Then 50 g lignin and 1 g nano-Fe 2 O 3Add to natural rubber latex to prepare a composite material emulsion. Pour the composite rubber emulsion into a mold and air dry it at 80°C for 3 hours. Then take out the prepared film from the mold and put it into deionized water and heat it at 95°C for 3 hours to prepare nano-Fe 2 O 3 Doped lignin / natural rubber composites with elastic substrates.

[0054] (2) Laser direct writing in-situ carbonization to prepare patterned flexible energy storage electrodes. The pre-stretched 100% elastic substrate was placed on the laser operating table and carbonized using CO 2 The laser was used as a laser source (power P = 10w, scanning speed 50mm / s, laser spot 300μm), and the laser scanning path was controlled by a program to form a patterned circuit on the surface of the elastic substrate. After laser direct writing, the pre-stretching was restored to finally obtain an energy storage electrode.

[0055] (3) Assembly of energy storage device: A polyvinyl alcohol hydrogel electrolyte containing 6M potassium hydroxide was coated on the patterned circuit surface of the energy storage electrode, dried at room temperature, and then encapsulated with natural rubber latex to obtain a supercapacitor.

[0056] The flexible supercapacitor prepared in Example 2 of the present invention has a maximum stretching rate of 100%, a specific capacitance of 215 F / g, and a capacitance retention rate of 90% after 1000 charge and discharge cycles.

[0057] Example 3

[0058] Provided is a method for preparing a transition metal-doped lignin / rubber composite material flexible electrochemical energy storage device, comprising the following steps:

[0059] (1) Preparation of nano-MnO by mechanical mixing 2 The mechanical blending method is to mix 50g lignin, 2g sulfurized, 5 stearic acid, 1g zinc oxide, 1g N-cyclohexyl-2-benzothiazole sulfonamide, 1.5g 2, 2'-dithiodibenzothiazole and 2g nano MnO 2 Add it into 100g of nitrile rubber, mix it in a double-roll mill, and then press it at 160℃ to prepare nano MnO 2 Doped lignin / nitrile rubber composites with elastic substrates.

[0060] (2) Laser direct writing in-situ carbonization to prepare patterned flexible energy storage electrodes. The elastic substrate pre-stretched by 200% was placed on the laser operating table, and an ultraviolet laser was used as the laser source (power P = 3w, scanning speed of 20mm / s, laser spot of 250μm). The laser scanning path was controlled by a program to form a patterned circuit on the surface of the elastic substrate. After laser direct writing, the pre-stretching was restored to finally obtain an energy storage electrode.

[0061] (3) Assembly of energy storage device: A polyvinyl alcohol hydrogel electrolyte containing 6M potassium hydroxide was coated on the patterned circuit surface of the energy storage electrode, dried at room temperature, and then encapsulated with nitrile rubber latex to obtain a supercapacitor.

[0062] The flexible supercapacitor prepared in Example 3 of the present invention has a maximum stretching rate of 200%, a specific capacitance of 550 F / g, and a capacitance retention rate of 81% after 1000 charge and discharge cycles.

[0063] Example 4

[0064] Provided is a method for preparing a transition metal-doped lignin / rubber composite material flexible electrochemical energy storage device, comprising the following steps:

[0065] (1) Preparation of FeCl by mechanical mixing 3 The mechanical blending method is to mix 30g lignin, 1.5g sulfurized, 5-stearic acid, 1g zinc oxide, 0.5g tetramethylthiuram disulfide, 1g 2,2'-dibenzothiazole disulfide and 1g FeCl 3 Add 100 g of nitrile rubber into the raw rubber and mix them in a two-roll mill, and then press mold them at 160 ° C to prepare FeCl 3 Doped lignin / nitrile rubber composites with elastic substrates.

[0066] (2) Laser direct writing in-situ carbonization to prepare patterned flexible energy storage electrodes. The elastic substrate pre-stretched by 300% was placed on the laser operating table, and an ultraviolet laser was used as the laser source (power P = 3w, scanning speed of 20mm / s, laser spot of 250μm). The laser scanning path was controlled by a program to form a patterned circuit on the surface of the elastic substrate. After laser direct writing, the pre-stretching was restored to finally obtain an energy storage electrode.

[0067] (3) Assembly of energy storage device: A polyvinyl alcohol hydrogel electrolyte containing 6M potassium hydroxide was coated on the patterned circuit surface of the energy storage electrode, dried at room temperature, and then encapsulated with nitrile rubber latex to obtain a supercapacitor.

[0068] The flexible supercapacitor prepared in Example 4 of the present invention has a maximum stretching rate of 300%, a specific capacitance of 397 F / g, and a capacitance retention rate of 91% after 1000 charge and discharge cycles.

[0069] Example 5

[0070] Provided is a method for preparing a transition metal-doped lignin / rubber composite material flexible electrochemical energy storage device, comprising the following steps:

[0071] (1) Preparation of FeCl by mechanical mixing 3 The mechanical blending method is to mix 30g lignin, 1g sulfurized, 4-stearic acid, 1g zinc oxide, 1.5g tetramethylthiuram disulfide, 1g N-cyclohexyl-2-benzothiazole sulfonamide and 1g FeCl 3 Add 100 g of styrene-butadiene rubber raw rubber, mix in a two-roll mill, and then press mold at 150 ° C to prepare FeCl 3 Doped lignin / styrene butadiene rubber composites with elastic substrates.

[0072] (2) Laser direct writing in-situ carbonization to prepare patterned flexible energy storage electrodes. The elastic substrate pre-stretched by 300% was placed on the laser operating table, and an ultraviolet laser was used as the laser source (power P = 3w, scanning speed of 60mm / s, laser spot of 250μm). The laser scanning path was controlled by a program to form a patterned circuit on the surface of the elastic substrate. After laser direct writing, the pre-stretching was restored to finally obtain an energy storage electrode.

[0073] (3) Assembly of energy storage device: A polyvinyl alcohol hydrogel electrolyte containing 6M potassium hydroxide was coated on the patterned circuit surface of the energy storage electrode, dried at room temperature, and then encapsulated with styrene-butadiene rubber latex to obtain a supercapacitor.

[0074] The flexible supercapacitor prepared in Example 5 of the present invention has a maximum stretching rate of 300%, a specific capacitance of 441 F / g, and a capacitance retention rate of 86% after 1000 charge and discharge cycles.

Claims

1. A method for preparing a flexible electrochemical energy storage device, characterized in that: The following steps are involved: 1) An elastic base film of a lignin / rubber composite material doped with a transition metal compound is prepared by an emulsion blending method or a mechanical blending method; wherein: The transition metal in the transition metal compound is zinc, copper, manganese, iron, cobalt, nickel or vanadium; the transition metal compound is a complex of one or more of transition metal oxides, transition metal sulfides, transition metal hydroxides, transition metal carbides, transition metal chlorides, transition metal nitrates, transition metal sulfates and transition metal acetates; The specific steps of the emulsion blending method are: Adding lignin and a transition metal compound to a pre-cured latex to prepare a composite material emulsion, then pouring it into a mold and drying it to obtain a film, and placing the film in deionized water and heating it at 50-100° C. for 1-3 hours to obtain a transition metal compound-doped lignin / rubber composite elastic base film; The specific steps of mechanical blending are: Adding lignin, a vulcanizing agent, an accelerator and a transition metal compound into raw rubber, mixing them in a double-roll mill, and then molding them at 120° C.-160° C. to obtain an elastic base film of a lignin / rubber composite material doped with a transition metal compound; 2) pre-stretching the elastic substrate film obtained in step 1), then in-situ carbonizing it by laser direct writing, and restoring the pre-stretching after laser direct writing to prepare a transition metal compound-doped lignin / rubber composite material-based flexible electrochemical energy storage electrode; 3) Encapsulating the energy storage electrode obtained in step 2) to obtain a flexible electrochemical energy storage device.

2. The preparation method according to claim 1, characterized in that: In the step 1), the rubber is natural rubber, nitrile rubber, carboxylated nitrile rubber, styrene-butadiene rubber, carboxylated styrene-butadiene rubber, styrene-butadiene-pyridine rubber or ethylene-propylene rubber.

3. The preparation method according to claim 1, characterized in that: In the emulsion blending process, the mass ratio of lignin to latex dry glue is 1-100:100; the mass ratio of transition metal compound to latex dry glue is 1-30:100; in the mechanical blending process, the mass ratio of lignin to rubber raw rubber is 1-100:100; the mass ratio of transition metal compound to rubber raw rubber is 1-30:100, and the mass ratio of vulcanizing agent, accelerator and rubber raw rubber is 1-4:2-12:

100.

4. The preparation method according to claim 1, characterized in that: In the emulsion blending process, the pre-vulcanized latex preparation process is: a certain amount of vulcanizing agent, accelerator, KOH, casein and latex are stirred at room temperature to prepare the pre-vulcanized latex; wherein the mass ratio of the vulcanizing agent, accelerator, KOH, casein and latex dry rubber is 2-4:2-4:0.05-0.2:1.3-1.6:

100.

5. The preparation method according to claim 1, characterized in that: In the step 2), the pre-stretching ratio is 0-1000%.

6. The preparation method according to claim 1, characterized in that: In the step 2), the specific method of laser direct writing is: placing the pre-stretched elastic substrate on a laser operating table, using a laser as a laser source, and controlling the laser scanning path through a program to form a patterned circuit on the surface of the elastic substrate.

7. The preparation method according to claim 1, characterized in that: In the step 3), the gel electrolyte is coated on the patterned circuit surface of the energy storage electrode, dried at room temperature for 1-24 hours, and then encapsulated with rubber latex or solution to obtain an energy storage device.

8. A flexible electrochemical energy storage device prepared by the preparation method according to any one of claims 1 to 7.